Perfluoropolyether derivative, lubricant and magnetic recording medium
The use of a perfluoropolyether derivative with ester groups and carboxylic acid ammonium salts at one end addresses the friction and durability issues in magnetic recording media, achieving reduced friction and improved durability.
Patent Information
- Application Number
- JP2023072701
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional lubricants for magnetic recording media, such as long-chain hydrocarbon esters and perfluoropolyether derivatives, fail to adequately reduce friction and maintain durability, leading to increased friction coefficients and reduced playback output over time.
A perfluoropolyether derivative with specific structural modifications, including the incorporation of two or more ester groups and carboxylic acid ammonium salts at one end, is used to enhance lubricity and durability by improving the alignment and adsorption to the magnetic layer.
The modified lubricant significantly reduces the coefficient of friction and maintains low friction even after long-term use, enhancing the durability and reliability of magnetic recording media.
Smart Images

Figure 2024157980000035 
Figure 2024157980000036 
Figure 2024157980000037
Abstract
Description
[Technical field]
[0001] The present invention relates to a perfluoropolyether derivative, a lubricant, and a magnetic recording medium. [Background technology]
[0002] Magnetic tape systems, which are one of the data recording methods, are widely used as a medium for recording large volumes of data because of their high recording density per unit volume. To improve the recording and playback characteristics of magnetic tape, it is necessary to smooth the magnetic tape surface and reduce the spacing between the magnetic head and the magnetic tape (media) as much as possible. In recent years, the smoothing of tape surfaces has progressed, resulting in increased friction between the magnetic head and the magnetic tape. For this reason, there is a demand for the development of lubricants that can improve the coefficient of friction between the magnetic head and the magnetic recording medium and improve the durability of the magnetic recording medium.
[0003] In conventional magnetic recording media, long-chain hydrocarbon esters, carboxylic acids, or mixtures thereof have been used as lubricants. However, when these are applied to the surface of a magnetic recording medium, the friction coefficient of the smoothed surface of the magnetic recording medium is high, and the thermal stability is poor, so the lubricant deteriorates over long-term storage. For this reason, lubricants based mainly on perfluoroalkyl groups or perfluoropolyether (PFPE) derivatives have been molecular-designed and synthesized.
[0004] Among these, Patent Document 1 proposes a perfluoroalkyl carboxylate ammonium salt, and Patent Document 2 proposes an ammonium salt of PFPE having a carboxyl group at its terminal, as a lubricant for thin-film magnetic recording media.
[0005] In addition, Patent Document 3 proposes a compound in which one carboxylic acid of succinic acid is partially esterified with an alkyl fluoride and the other carboxylic acid is an ammonium salt as a lubricant for thin-film magnetic recording media. Patent Document 4 discloses a dicarboxylate derivative of PFPE having hydroxyl groups at both ends modified with a succinic acid derivative. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Unexamined Patent Publication No. 1-9961 [Patent Document 2] Japanese Patent Application Publication No. 3-252921 [Patent Document 3] JP 2000-353310 A [Patent Document 4] JP 2003-55310 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the field of magnetic recording media, particularly magnetic recording media with a lubricant applied to the surface, further improvements in practical characteristics are required, such as a drop in playback output during running tests due to insufficient performance of the lubricant used. In addition, the coefficient of friction increases with long-term use, leaving concerns about reliability.
[0008] One aspect of the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a lubricant that can improve the durability of a magnetic recording medium. [Means for solving the problem]
[0009] As a result of intensive research into solving the above problems, the inventors have found that a compound having a specific structure can reduce the coefficient of friction of a magnetic recording medium compared to the prior art and improve its durability, and have completed the present invention. That is, the present invention includes the following configurations.
[0010] <1> A perfluoropolyether derivative represented by the following formula (1). [ka] In formula (1), Each X is independently represented by the following formula (2) or an arbitrary substituent, and at least one of X is represented by the following formula (2): [ka] (In formula (2), m is an integer of 0 to 10, R is a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom, R' is a cyclic hydrocarbon group, and R1, R2, R3, and R4 are each a hydrocarbon group having 30 or less carbon atoms or a hydrogen atom, at least one of which is a hydrocarbon group having 30 or less carbon atoms.) R f is expressed by the following equation (3). [ka] (In formula (3), j, k, p, q, r, and s are each a real number from 3 to 70.) <2> A perfluoropolyether derivative represented by the following formula (4): [ka] In formula (4), X is represented by the following formula (2): [ka] (In formula (2), m is an integer of 0 to 10, R is a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom, R' is a cyclic hydrocarbon group, and R1, R2, R3, and R4 are each a hydrocarbon group having 30 or less carbon atoms or a hydrogen atom, at least one of which is a hydrocarbon group having 30 or less carbon atoms.) R f is expressed by the following equation (3). [ka] (In formula (3), j, k, p, q, r, and s are each a real number from 3 to 70.) <3> <1> or <2> A perfluoropolyether composition comprising at least one of the perfluoropolyether derivatives described in 1. <4> <1> or <2> A lubricant comprising the perfluoropolyether derivative according to claim 1. <5> The magnetic recording medium comprises a non-magnetic support and a magnetic layer laminated on the non-magnetic support, the magnetic layer comprising: <4> A magnetic recording medium comprising the lubricant according to claim 1. <6> The present invention relates to a magnetic recording medium comprising: a non-magnetic support; a magnetic layer laminated on the non-magnetic support; and a lubricant layer laminated on the magnetic layer, the lubricant layer comprising: <4> A magnetic recording medium comprising the lubricant according to claim 1. Effect of the Invention
[0011] According to one aspect of the present invention, a lubricant capable of improving the durability of a magnetic recording medium can be provided. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view of a magnetic tape according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a sample in which a lubricant is applied to a magnetic tape used in friction measurement according to one embodiment of the present invention. [Diagram 3] 2 is a structure of the magnetic layer 1 of FIG. 1 according to one embodiment of the present invention. [Figure 4] 2 illustrates a structure of the nonmagnetic layer 2 of FIG. 1 according to one embodiment of the present invention. [Diagram 5] 1 is a schematic cross-sectional view of a magnetic disk according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to this, and various modifications are possible within the scope described, and embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more, B or less."
[0014] 1. Overview of the Invention Long-chain hydrocarbon esters, carboxylic acids, or mixtures thereof that have been used as lubricants for conventional magnetic recording media have a high friction coefficient on the surface of the magnetic recording medium when applied to the surface of the magnetic recording medium. In addition, the lubricant has poor thermal stability, so deterioration of the lubricant during long-term storage is inevitable. Therefore, lubricants mainly composed of perfluoroalkyl groups or perfluoropolyether (PFPE) derivatives have been molecular designed and synthesized, but even when lubricants such as those disclosed in Patent Documents 1 to 4 are applied to the surface of the magnetic recording medium, the friction coefficient is still high and the durability is low on the magnetic recording medium with a smooth surface.
[0015] Therefore, the present inventors conducted extensive research to solve the above problems and discovered that by using a perfluoropolyether derivative containing a total of two or more polar groups, an ester group and a carboxylate ammonium salt, at one end of the perfluoropolyether, the friction generated between a magnetic recording medium with a smoothed surface and a head can be further reduced.
[0016] [2. Perfluoropolyether derivatives] A perfluoropolyether derivative according to one embodiment of the present invention is represented by the following formula (1).
[0017] [ka] In formula (1), X's are each independently the following formula (2) or any substituent, and at least one of them is formula (2). Examples of the optional substituent include a hydrogen atom, a hydroxyl group, an alkoxy group, a thiol group, a halogen atom, and a group having an ether bond or an ester bond. [ka] In formula (2), m is an integer of 0 to 10. When m is within this range, the friction coefficient can be reduced and lubricity can be improved. From the viewpoint of synthesis, which will be described later, m is preferably an integer of 0 to 8.
[0018] In formula (2), R is a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom. The lower limit of the carbon number of the hydrocarbon group is not particularly limited, and is usually 1 or more. If R is within this range, the resulting perfluoropolyether derivative reduces the friction of the magnetic tape and is likely to improve lubricity. From the viewpoint of improving lubricity, R is preferably a hydrocarbon group, and the carbon number of the hydrocarbon group is more preferably 8 or more. From the viewpoint of solubility in a solvent, R is preferably a hydrogen atom or a hydrocarbon group having 18 or less carbon atoms. The carbon number of the hydrocarbon group can be determined taking into consideration the solubility of the resulting perfluoropolyether derivative in a solvent.
[0019] In formula (2), R' is a cyclic hydrocarbon group. Usually, the cyclic hydrocarbon group has 3 to 12 carbon atoms. Examples of the cyclic hydrocarbon group include aromatic rings and alicyclic hydrocarbons. Examples of the aromatic ring include a benzene ring and a naphthalene ring. Examples of the alicyclic hydrocarbon include cyclohexane and cyclopentane.
[0020] In formula (2), R1, R2, R3, and R4 are each a hydrocarbon group having 30 or less carbon atoms or a hydrogen atom, and at least one of them is a hydrocarbon group having 30 or less carbon atoms. R1, R2, R3, and R4 are preferably a hydrocarbon group having 24 or less carbon atoms or a hydrogen atom, more preferably a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom, and even more preferably a hydrocarbon group having 18 or less carbon atoms or a hydrogen atom. From the viewpoint of reducing the friction coefficient, the total number of carbon atoms contained in R1 to R4 is preferably 10 to 48, and more preferably 20 to 48.
[0021] When R, R1, R2, R3 and R4 are hydrocarbon groups, they may be linear or may contain a branched chain, a double bond, fluorine, an aromatic ring, a hetero element, a heterocycle, etc. From the viewpoint of reducing the friction coefficient, it is more preferable that they are linear.
[0022] In formula (1), R f is expressed by the following equation (3). [ka]
[0023] In formula (3), j, k, p, q, r, and s each represent an average degree of polymerization and are real numbers from 3 to 70. When j, k, p, q, r, and / or s are less than 3, the molecular weight is small and lubricating effect is not expected. When j, k, p, q, r, and / or s are more than 70, the compound is difficult to dissolve in a hydrocarbon solvent. j, k, p, q, r, and s are preferably real numbers from 5 to 50, and more preferably real numbers from 5 to 30. The skeleton represented by formula (3) is also called, from the top, a Fomblin skeleton, a C2 skeleton, a Demnam skeleton, a Krytox skeleton, and a C4 skeleton.
[0024] Moreover, a perfluoropolyether derivative according to another embodiment of the present invention is represented by the following formula (4). [ka] In formula (4), X is represented by the above formula (2). In formula (4), R f is shown in the above formula (3).
[0025] Hereinafter, the perfluoropolyether derivative represented by the formula (4) is also referred to as “derivative A,” and the perfluoropolyether derivative represented by the formula (1) is also referred to as “derivative B.”
[0026] Conventionally, perfluoropolyether compounds represented by the following formulas (5) and (6) are known. The perfluoropolyether compound represented by the following formula (5) is also called D2M, and the perfluoropolyether compound represented by the following formula (6) is also called DDOH. [ka] [ka] In the above formulas (5) and (6), k is a real number from 3 to 70.
[0027] Derivative A and derivative B each have a structure in which at least a part of the hydroxyl groups of D2M and DDOH are modified. Specifically, in derivative A, the hydroxyl group of D2M is substituted with a functional group having an ester group and an ammonium carboxylate. In derivative B, at least one of the two hydroxyl groups is similarly substituted with a functional group having an ester group and an ammonium carboxylate. In other words, derivative B is a compound in which only one of the hydroxyl groups is modified, or a compound in which two of the hydroxyl groups are modified.
[0028] The perfluoropolyether derivative contains a total of two or more polar ester groups and ammonium carboxylates at one end of the perfluoropolyether. Therefore, when a lubricant containing the perfluoropolyether derivative is applied to a magnetic layer, it is more strongly oriented and adsorbed to the magnetic layer than a conventional lubricant containing a compound having two or less hydroxyl groups, such as a compound represented by D2M or DDOH. Therefore, the lubricant containing the perfluoropolyether derivative can reduce the friction coefficient of the magnetic recording medium more than a conventional lubricant. In addition, the lubricant containing the perfluoropolyether derivative can maintain a low friction coefficient. Therefore, it is possible to improve the durability of the magnetic recording medium, especially the durability of the magnetic recording medium having high electromagnetic conversion characteristics with smoothness that enables high-density recording, which is currently required.
[0029] 3. Method for Producing Perfluoropolyether Derivatives The method for producing the perfluoropolyether derivatives represented by the formulas (1) and (4) is not particularly limited. For example, first, a perfluoropolyether compound is reacted with a dicarboxylic anhydride such as succinic anhydride to obtain a succinic anhydride-modified product. Then, the obtained succinic anhydride-modified product is reacted with an amine compound to obtain the perfluoropolyether derivative.
[0030] Examples of the perfluoropolyether compound include, but are not limited to, the above-mentioned D2M and DDOH. Examples of dicarboxylic acid anhydrides include succinic anhydride, maleic anhydride, malonic anhydride, glutaric anhydride, adipic anhydride, and the like, and methylsuccinic anhydride, butylsuccinic anhydride, hexylsuccinic anhydride, octylsuccinic anhydride, dodecylsuccinic anhydride, hexadecylsuccinic anhydride, octadecylsuccinic anhydride, and the like, which are obtained by substituting these with a hydrocarbon group having 1 to 30 carbon atoms. The side chain of this succinic anhydride derivative corresponds to the hydrocarbon group represented by R in the above-mentioned derivatives A and B. In addition, the amine compound can be ammonia and / or a primary to tertiary amine compound, and is preferably a tertiary amine compound. The total carbon of the amine compound is usually 0 to 120. Examples of the amine compound include dimethyloctadecylamine, trioctylamine, and the like.
[0031] Specifically, the derivative A can be synthesized by the following method. First, D2M and 1 equivalent of a succinic anhydride derivative are reacted in an oil bath while being heated and stirred. After the reaction is completed, the resulting reaction product is dissolved in a solvent, impurities are filtered out, the solvent is removed, and the product is purified by silica gel chromatography to obtain a modified succinic anhydride product. The oil bath temperature is preferably 110 to 150°C, and the reaction time is preferably 5 to 15 hours. Examples of the solvent to be used for dissolving the product after the reaction are diisopropyl ether, diethyl ether, Vertrel ether, and the like. TM -XF (manufactured by Mitsui DuPont Fluorochemicals). Next, the resulting succinic anhydride modified product is reacted with one equivalent of an amine compound at 100-150°C for 2-8 hours with heating and stirring. The reaction mixture is then cooled and the n-hexane soluble portion is removed to obtain derivative A.
[0032] The obtained compound can be identified, for example, by nuclear magnetic resonance spectroscopy (NMR) or Fourier transform infrared spectroscopy (FTIR). When identifying by FTIR measurement, it is possible to confirm whether or not the compound is the target compound by measuring the IR peaks assigned to the hydroxyl group, ester group, or carboxyl group.
[0033] Derivative B can be obtained by using 1 or 2 equivalents of DDOH and a succinic anhydride derivative. When 1 equivalent is used, one of X is a hydroxyl group. In addition, a perfluoropolyether composition containing one X and two Xs can be obtained by changing the molar ratio of the succinic anhydride derivative reacted with DDOH in the range of 1 to 2 equivalents, and the ratio can be easily changed by changing the molar ratio of the compound used in the reaction step.
[0034] One embodiment of the present invention also includes a composition containing derivative A and / or B. In this specification, the composition is also referred to as a perfluoropolyether composition. When derivative A and B are mixed, the mixing ratio is not particularly limited. The perfluoropolyether composition may contain other components within a range that does not impair the performance of derivative A and B. When the perfluoropolyether composition contains a compound other than derivative A and B, the content of derivative A and / or B is preferably more than 50 wt%, more preferably 80 wt% or more, and even more preferably 90 wt% or more.
[0035] [4. Lubricants] The lubricant according to one embodiment of the present invention comprises the above-mentioned perfluoropolyether derivative or the above-mentioned perfluoropolyether composition. In other words, the lubricant according to one embodiment of the present invention comprises at least one of derivatives A and B. In addition, as long as it comprises at least one of derivatives A and B, it may be mixed with other compounds.
[0036] In particular, in magnetic recording media with a smoothed surface, a lubricant is applied to the surface. Conventionally, due to the insufficient performance of this lubricant, for example, the playback output of the magnetic tape may decrease during a running test. In this case, the practical characteristics are unsatisfactory. Furthermore, if the friction coefficient increases due to repeated running tests, there is a concern about the long-term reliability. From these points of view, the present inventor has studied a lubricant that can improve the durability of magnetic recording media.
[0037] By using the lubricant according to one embodiment of the present invention in a magnetic recording medium, excellent lubricity is maintained under various conditions of use, and the lubricating effect is sustained even after long-term use. This provides excellent running properties, wear resistance, durability, etc. In addition to the magnetic recording medium, it is also possible to improve the lubricating properties of polymer films and the like that do not include a magnetic layer and have improved durability.
[0038] The lubricant may contain other components than the derivative A and the derivative B, as long as the lubricant does not impair its performance. For example, the lubricant according to one embodiment of the present invention may further contain a solvent. Examples of the solvent include hydrocarbon solvents such as diisopropyl ether, n-hexane, methyl ethyl ketone, toluene, cyclohexanone, and methanol; Vertrel; TM Fluorine-based solvents such as fluorine-based solvents (manufactured by Mitsui DuPont Fluorochemicals) and the like, and mixed solvents thereof.
[0039] The contents of Derivative A and Derivative B in the lubricant containing the solvent are not particularly limited as long as they are within a range that does not impair the performance of the lubricant, but are preferably 0.001 to 40.0 g / L, and more preferably 0.05 to 20.0 g / L.
[0040] 5. Magnetic Recording Media A magnetic recording medium according to one embodiment of the present invention comprises a non-magnetic support and a magnetic layer laminated on the non-magnetic support, and the magnetic layer may contain the above-mentioned lubricant (the lubricant may be internally added to the magnetic layer). Alternatively, a magnetic recording medium according to one embodiment of the present invention comprises a non-magnetic support, a magnetic layer laminated on the non-magnetic support, and a lubricant layer laminated on the magnetic layer, and the lubricant layer may contain the above-mentioned lubricant.
[0041] In this specification, the term "magnetic recording medium" includes magnetic tapes, magnetic disks, etc. From the viewpoint of reducing the coefficient of friction and facilitating improvement in durability, the magnetic recording medium is preferably a magnetic tape or a magnetic disk.
[0042] 1 and 2 are schematic cross-sectional views showing the structure of a magnetic tape according to an embodiment of the present invention. The magnetic tape 15 in FIG. 1 is formed by laminating a magnetic layer 1, a non-magnetic layer 2, a base film 3 as a support, and a backcoat layer 4 in this order. In the magnetic tape in FIG. 1, a lubricant is added to the magnetic layer 1 and the non-magnetic layer 2. FIG. 3 shows the structure of the magnetic layer 1, which contains a pigment 6 such as an abrasive, a magnetic powder 7, and an organic layer 8 containing a binder, a lubricant, etc. Therefore, the lubricant seeps out from the inside of the magnetic layer 1 to the surface, and the friction coefficient of the magnetic tape surface is continuously reduced. FIG. 4 shows the structure of the non-magnetic layer 2, which contains a pigment 6, a non-magnetic powder 9, and an organic layer 8 containing a binder, a lubricant, etc.
[0043] 2, a lubricant topcoat layer 5 containing the lubricant is formed on the magnetic layer 1. In this case, the lubricant topcoat layer 5 is strongly oriented and adsorbed to the magnetic layer 1, thereby reducing the coefficient of friction and maintaining the durability of the magnetic tape 15. In this case, the magnetic layer 1 may or may not have a lubricant added thereto.
[0044] Examples of the pigment 6 include abrasives such as alumina, carbon black powder, etc. Examples of the magnetic powder 7 include ferromagnetic iron oxide particles such as γ-Fe2O3 and cobalt-coated γ-Fe2O3, ferromagnetic chromium dioxide particles, ferromagnetic metal particles made of metals such as Fe, Co, and Ni, and alloys containing these, and hexagonal ferrite fine particles having a hexagonal plate shape. Examples of the magnetic powder 7 include hexagonal ferrite, epsilon-type iron oxide (ε iron oxide), Co-containing spinel ferrite, gamma hematite, magnetite, chromium dioxide, and cobalt-coated iron oxide.
[0045] Examples of the binder contained in the organic layer 8 include polymers of vinyl chloride, vinyl acetate, vinyl alcohol, vinylidene chloride, acrylic acid esters, methacrylic acid esters, styrene, butadiene, acrylonitrile, etc., or copolymers of two or more of these, polyurethane resins, polyester resins, epoxy resins, etc. In order to improve the dispersibility of the magnetic powder, hydrophilic polar groups such as sulfonic acid groups, carboxyl groups, and phosphoric acid groups may be introduced into the binder. There are no particular limitations on the binder as long as it is one that is generally used in magnetic recording media, and examples of the binder include polyurethane resins or vinyl chloride resins that have undergone a crosslinking reaction, thermosetting resins, and reactive resins.
[0046] The base film 3 is a layer that functions as a support for the magnetic tape. Examples of materials for the base film 3 include one or more of polyester, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), polycyclohexylene dimethylene terephthalate (PCT), polyethylene-p-oxybenzoate (PEB), aramid (aromatic polyamide), and polyethylene bisphenoxycarboxylate.
[0047] The backcoat layer 4 is a layer for improving the running properties of the magnetic tape. Examples of materials for the backcoat layer 4 include polyurethane resins containing carbon and calcium carbonate, nitrocellulose resins, and polyester resins.
[0048] 5 is a cross-sectional schematic diagram showing the configuration of a magnetic disk according to one embodiment of the present invention. A magnetic disk 16 is formed by laminating a lubricant layer 10, a protective layer 11, a magnetic layer 12, an underlayer 13, and a substrate 14 in this order, and the lubricant layer 10 contains the lubricant. In another embodiment, the magnetic disk may include an underlayer below the magnetic layer, a soft magnetic underlayer disposed below the underlayer, and an adhesive layer disposed below one or more soft magnetic layers.
[0049] Each layer of the magnetic disk, other than the lubricant layer, may comprise materials known in the art to be suitable for the individual layers of the magnetic disk, for example, protective layer 11 may be a carbon film.
[0050] The method for obtaining layers other than the lubricating layer is not particularly limited, and the layers may be synthesized based on known techniques, or commercially available products may be used. EXAMPLES
[0051] Hereinafter, one embodiment of the present invention will be described in more detail based on examples and comparative examples, but the embodiment of the present invention is not limited to these.
[0052] <Magnetic tape sample preparation> A magnetic tape sample having the structure shown in Figure 2 was prepared as follows. A commercially available magnetic tape, Ultrium 7 (manufactured by Fujifilm Corporation), was prepared. The magnetic tape sample was obtained by dipping the magnetic tape surface with the compounds and comparative compounds shown in Tables 1 and 2 at a concentration of 8 g / L. The solvents used are shown in Table 3.
[0053] <Friction test method> The coefficient of friction was measured using a tribogear friction and wear tester TYPE:40 (manufactured by Heidon). As a specific measurement method, at 25 °C, a magnetic tape coated with a lubricant was fixed on a glass plate, a 10 mmφ SUS ball was brought into contact with the magnetic tape, and a load of 50 g was applied. In this state, the SUS ball was moved on the sample at a moving speed of 1 mm / s, and the running distance of 5 mm was run 5 times and 20 times (10 round trips). At that time, the frictional force generated was measured with a strain gauge. The moving speed of the ball was set assuming the low-speed running of the magnetic tape.
[0054] <FTIR measurement> The FTIR measurement was performed by the ATR method (diamond prism) using a Fourier transform infrared spectrometer (manufactured by Thermo Fisher Scientific, product name: Nicolet iS10 FTIR).
[0055] [Example 1] The synthesis of Compound 1 was carried out as shown in the following formula (7). [Chemical formula]
[0056] 20.28 g of a perfluoropolyether (DDOH) with a molecular weight of 2010 having two hydroxyl groups at the ends and 3.52 g of octadecyl succinic anhydride in an equivalent amount to DDOH were reacted for 3 hours while stirring in an oil bath at 150 °C. After completion of the reaction, it was dissolved in diisopropyl ether and filtered. Silica gel column chromatography was performed for purification to obtain a DDOH mono-octadecyl succinic acid modified product. To the DDOH octadecyl succinic acid modified product, 1 equivalent amount of dimethyloctadecylamine was added, and it was heated and stirred at 80 °C for 1 hour. Then, it was cooled, and the n-hexane soluble portion was removed after cooling to obtain Compound 1.
[0057] The obtained compound was identified by FTIR measurement. In the DDOH mono-octadecyl succinic acid modified product, the peak of the carbonyl group attributed to the ester group was at 1770 cm -1The carbonyl group peak attributable to the carboxyl group is at 1710 cm -1 Compound 1 showed no change in the peak position of the carbonyl group assigned to the ester group, while the peak position at 1710 cm -1 The carbonyl peak attributable to the carboxyl group disappears, and the carbonyl peak attributable to the carboxylate appears at 1600 cm -1 It appeared near the peak. This suggested that the carboxylic acid reacted with the amine compound to form an ammonium carboxylate. As for other absorptions, the following peaks were observed, which indicated that the compound obtained contained hydroxyl groups, hydrocarbon groups, ester groups, carboxylates, and perfluoropolyether groups. This identified the compound obtained as Compound 1. In Compound 1, k=11. Peak assigned to hydroxyl group: 3443 cm -1 Peak assigned to CH stretching vibration: 2937 cm -1 Peaks assigned to CF stretching vibration: 1110-1250 cm -1
[0058] Example 2 Compound 2 was synthesized according to the following scheme (8). [ka]
[0059] 20.85 g of DDOH and 7.19 g of octadecyl succinic anhydride (2 equivalents relative to DDOH) were reacted and purified in the same manner as in Example 1 to obtain a DDOH bisoctadecyl succinic anhydride modified product. 2 equivalents of dimethyloctadecylamine were added to the DDOH bisoctadecyl succinic anhydride modified product, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 2 represented by formula (8).
[0060] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as Compound 2. In Compound 2, k=11. Peak assigned to CH stretching vibration: 2926 cm -1 and 2857 cm -1 Peak of carbonyl group assigned to ester group: 1751 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1602 cm -1 Peaks assigned to CF stretching vibration: 1120-1270 cm -1
[0061] Example 3 Compound 3 was synthesized according to the following scheme (9). [ka]
[0062] In the same manner as in Example 1, 20.55 g of DDOH and 3.56 g of hexadecylsuccinic anhydride (1 equivalent relative to DDOH) were reacted and purified in the same manner as in Example 1 to obtain a DDOH monohexadecylsuccinic acid modified product. One equivalent of dimethyloctadecylamine was added to the DDOH monohexadecylsuccinic acid modified product, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 3.
[0063] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as compound 3. In compound 3, k=11. Peak assigned to CH stretching vibration: 2927 cm -1 and 2858 cm -1 Carbonyl group peak attributable to ester group: 1740 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1601 cm -1 Peaks assigned to CF stretching vibration: 1120-1270 cm -1
[0064] Example 4 Compound 4 was synthesized according to the following scheme (10). [ka]
[0065] As in Example 2, 20.55 g of DDOH was reacted with 6.49 g of hexadecylsuccinic anhydride (2 equivalents relative to DDOH) in the same manner as in Example 2, and purified to obtain a DDOH bishexadecylsuccinic acid-modified product. To the DDOH bishexadecylsuccinic acid-modified product, 2 equivalents of dimethyloctadecylamine was added, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 4.
[0066] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as compound 4. In compound 2, k=11. Peak assigned to CH stretching vibration: 2925 cm -1 and 2856 cm -1 Peak of carbonyl group assigned to ester group: 1745 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1590cm -1 Peaks assigned to CF stretching vibration: 1115-1280 cm -1
[0067] Example 5 Compound 5 was synthesized according to the following scheme (11). [ka]
[0068] In the same manner as in Example 1, 21.35 g of DDOH was reacted with 3.06 g of dodecylsuccinic anhydride (1 equivalent relative to DDOH) in the same manner as in Example 1, and purified to obtain a monododecylsuccinic acid-modified DDOH. One equivalent of dimethyloctadecylamine was added to the monododecylsuccinic acid-modified DDOH, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 5.
[0069] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. This indicated that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. This identified the obtained compound as Compound 5. Peak assigned to CH stretching vibration: 2928 cm -1 and 2859 cm -1 Peak of carbonyl group assigned to ester group: 1735 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1600cm -1 Peaks assigned to CF stretching vibration: 1110-1270cm -1
[0070] Example 6 Compound 6 was synthesized according to the following scheme (12). [ka]
[0071] As in Example 2, 25.00 g of DDOH was reacted with 6.52 g of dodecylsuccinic anhydride (2 equivalents relative to DDOH) in the same manner as in Example 2, and purified to obtain a DDOH bisdodecylsuccinic acid modified product. To the DDOH bisdodecylsuccinic acid modified product, 2 equivalents of dimethyloctadecylamine was added, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 6.
[0072] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as Compound 6. In Compound 6, k=11. Peak assigned to CH stretching vibration: 2924 cm -1 and 2855 cm -1 Peak of carbonyl group assigned to ester group: 1750 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1590cm -1 Peaks assigned to CF stretching vibration: 1115-1285 cm -1
[0073] Example 7 Compound 7 was synthesized according to the following scheme (13). [ka]
[0074] As in Example 2, 20.55 g of DDOH was reacted with 2.25 g of octylsuccinic anhydride (2 equivalents relative to DDOH) in the same manner as in Example 2, and purified to obtain a DDOH-bisoctylsuccinic acid-modified product. To the DDOH-bisoctylsuccinic acid-modified product, 2 equivalents of trioctylamine was added, and the mixture was heated and stirred at 80° C. for 1 hour. The mixture was then cooled, and the n-hexane soluble portion was removed after cooling to obtain compound 7.
[0075] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as Compound 7. In Compound 7, k=11. Peak assigned to CH stretching vibration: 2925 cm -1 and 2859 cm -1 Peak of carbonyl group assigned to ester group: 1750 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1570cm -1 Peaks assigned to CF stretching vibration: 1115-1285 cm -1
[0076] Example 8 Compound 8 was synthesized according to the following scheme (14). [ka]
[0077] D2M40.05g and 1.4 equivalents of octadecyl succinic anhydride relative to D2M were reacted for 11 hours with stirring at an oil bath temperature of 150°C. At the beginning of the reaction, the mixture was separated, but the upper layer of succinic anhydride gradually decreased. After that, the mixture was cooled, and the excess octadecyl succinic anhydride added after cooling was removed, dissolved in diisopropyl ether, filtered, and the solvent was removed. One equivalent of dimethyloctadecylamine was added to the octadecyl succinic anhydride-modified product of D2M obtained after purification by column chromatography, and the mixture was heated and stirred at 80°C for 1 hour. After that, the mixture was cooled, and the n-hexane soluble portion was removed to obtain compound 8.
[0078] The obtained compound was identified by FTIR measurement in the same manner as in Example 1. The following peaks were observed. From this, it was found that the obtained compound contained a hydrocarbon group, an ester group, a carboxylate, and a perfluoropolyether group. From this, the obtained compound was identified as compound 8. In compound 8, k=10. Peak assigned to CH stretching vibration: 2927 cm -1 and 2856 cm -1 Carbonyl group peak attributable to ester group: 1740 cm -1 Broad peak of carbonyl group assigned to carboxylate: 1585 cm -1 Peaks assigned to CF stretching vibration: 1120-1275 cm -1
[0079] Comparative Example 1 The synthesis of comparative compound 1 was carried out according to the following formula (15). Comparative compound 1 is a DDOH monooctadecyl succinic anhydride modified product, which is an intermediate in formula (7) of Example 1. By comparing compound 1 with comparative compound 1, the effect of ammonium carboxylate on friction durability can be compared. In comparative compound 1, k=11. [ka]
[0080] Comparative Example 2 The synthesis of comparative compound 2 was carried out according to the following formula (16). Comparative compound 2 is a DDOH bisoctadecyl succinic anhydride modified product, which is an intermediate in formula (8) of Example 2. By comparing compound 2 with comparative compound 2, the effect of ammonium carboxylate on friction durability can be compared. In comparative compound 2, k=11. [ka]
[0081] Comparative Example 3 Comparative compound 3 was synthesized in the same manner as in Patent Document 4. [ka] Comparative compound 3 is a compound disclosed in Patent Document 4, where p = 1 to 9 and q = 1 to 9. Comparison with the compound according to the present invention makes it possible to compare whether the polar group is at both ends of the perfluoropolyether or at one end.
[0082] Comparative Example 4 Comparative compound 4 was synthesized in the same manner as in Patent Document 2. [ka] Comparative compound 4 is a compound disclosed in Patent Document 2, in which k is an integer of 3 to 70, and the polar group is only an ammonium carboxylate. By comparing compounds 1 to 6 with this comparative compound 4, it is possible to compare ammonium succinate derivatives having a plurality of polar groups including an ester group with the prior art in which the polar group is only an ammonium carboxylate.
[0083] The structural formulae of the compounds and comparative compounds are shown in Tables 1 and 2, respectively. [Table 1] [Table 2]
[0084] <Magnetic tape friction test results> The compounds and comparative compounds in Tables 1 and 2 were diluted to a concentration of 8 g / L using the solvents in Table 3, and applied to magnetic tapes by dip coating. The results of the friction coefficients (5th and 20th times) and friction marks in the friction tests for the magnetic tapes of Examples 1 to 8 and Comparative Examples 1 to 3 are summarized in Table 3. [Table 3]
[0085] It is understood that the coefficient of friction of the Examples is suppressed to be lower than that of the Comparative Examples, and that the durability of the magnetic tape is excellent. Specifically, the coefficient of friction of the Examples 1 to 8 is lower and more stable than that of the Comparative Examples 1 and 2, which are carboxylic acid compounds before reacting with the amine compound. In addition, Comparative Example 3 has ammonium carboxylate salts at both ends of the perfluoropolyether, whereas the Examples 1 to 8 have ammonium carboxylate salts at only one end. In other words, it is understood that the presence of a polar group at one end of the perfluoropolyether can improve the coefficient of friction. It is also understood that the Examples 1 to 8, which have an ester group between the perfluoropolyether and the ammonium carboxylate salt, exhibit excellent friction characteristics compared to Comparative Example 4, which does not have the ester group.
[0086] Compounds 1 and 2 are compounds obtained by converting comparative compounds 1 and 2 into ammonium salts, respectively. It can be seen that the friction coefficient is reduced by converting them into ammonium salts, and the increase in the friction coefficient due to the increase in the number of runs is reduced. In an actual magnetic tape system, the magnetic tape runs repeatedly starting and stopping. The running speed is low when starting and stopping. If the friction coefficient is low in the friction measurement test using Tribogear, the friction at low running speeds is small, and durability is thought to be improved. This suggests that durability is improved by converting them into ammonium salts. It can also be seen that the latter is more effective at reducing friction than the mono-modified succinic acid and the bis-modified succinic acid.
[0087] In addition, when comparing the friction coefficients of compounds with one ammonium carboxylate group at one end of the perfluoropolyether (compounds 1, 3, 5, and 8) with those with two (compounds 2, 4, 6, and 7), the compounds with two have a lower friction coefficient. This shows that having two ammonium carboxylate groups at one end is effective in reducing friction. This is thought to be because compounds with two ammonium carboxylate groups at one end have twice as many adsorption sites per molecule compared to compounds with only one, resulting in a lower friction coefficient and increased durability against friction of the lubricating oil film on the tape surface. [Industrial Applicability]
[0088] The present invention can be suitably used as a lubricant for magnetic recording media. [Explanation of symbols]
[0089] 1 magnetic layer 2 Non-magnetic layer 3 Base film 4 Backcoat layer 5 Lubricant topcoat layer 6. Pigments 7 Magnetic powder 8 Organic layer 9 Non-magnetic powder 10 Lubricant layer 11 Protective layer 12 Magnetic layer 13 Base layer 14 Substrate 15 Magnetic Tape 16 Magnetic Disk
Claims
1. A perfluoropolyether derivative represented by the following formula (1): [Formula 1] In formula (1), Each X is independently represented by the following formula (2) or an arbitrary substituent, and at least one of X is represented by the following formula (2): [Case 2] (In formula (2), m is an integer of 0 to 10, R is a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom, R' is a cyclic hydrocarbon group, and R 1 , R 2 , R 3 , R 4 are each a hydrocarbon group having 30 or less carbon atoms or a hydrogen atom, and at least one of them is a hydrocarbon group having 30 or less carbon atoms. R f is expressed by the following formula (3). [C3] (In formula (3), j, k, p, q, r, and s are each a real number from 3 to 70.)
2. A perfluoropolyether derivative represented by the following formula (4): [C4] In formula (4), X is represented by the following formula (2): [C5] (In formula (2), m is an integer of 0 to 10, R is a hydrocarbon group having 20 or less carbon atoms or a hydrogen atom, R' is a cyclic hydrocarbon group, and R 1 , R 2 , R 3 , R 4 are each a hydrocarbon group having 30 or less carbon atoms or a hydrogen atom, and at least one of them is a hydrocarbon group having 30 or less carbon atoms. R f is expressed by the following formula (3). [C6] (In formula (3), j, k, p, q, r, and s are each a real number from 3 to 70.)
3. A perfluoropolyether composition comprising at least one of the perfluoropolyether derivatives according to claim 1 or 2.
4. A lubricant comprising the perfluoropolyether derivative according to claim 1 or 2.
5. A magnetic recording medium comprising a non-magnetic support and a magnetic layer laminated on the non-magnetic support, the magnetic layer containing the lubricant according to claim 4.
6. 5. A magnetic recording medium comprising: a non-magnetic support; a magnetic layer laminated on the non-magnetic support; and a lubricant layer laminated on the magnetic layer, the lubricant layer containing the lubricant according to claim 4.
Citation Information
Patent Citations
Perfluoroalkylcarboxylic acid amine salt and magnetic recording medium using said salt
JP1989009961A
Magnetic recording medium
JP1991252921A
Magnetic recording medium
JP2000353310A
Perfluoropolyalkyl ether-based compound, lubricant comprising the same, and recording medium using the lubricant
JP2003055310A