Cosmetic, method for producing the same and ultraviolet protective agent composition

The organic-inorganic composite UV absorber with BMBM and UV protection enhancers addresses solubility and coloring issues, achieving high UV-A protection and safety in cosmetics.

JP2024158041APending Publication Date: 2024-11-08JO COSMETICS +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023072871
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing UV-A absorbers like 4-tert-butyl-4'-methoxydibenzoylmethane (BMBM) face solubility issues in cosmetic oils, leading to precipitation and reaction with inorganic powders and metal ions, resulting in coloring and inadequate UV protection.

Method used

A cosmetic formulation using an organic-inorganic composite UV absorber with a positively charged base layer and negatively charged intermediate layer, containing BMBM, combined with a polyhydric alcohol fatty acid ester type nonionic surfactant, polyoxyethylene alkyl ether phosphate, silicone surfactant, clay mineral, or silica to enhance UV protection and prevent precipitation.

Benefits of technology

The formulation provides high UV-A protection with reduced metal ion coloring and improved safety, allowing efficient production of cosmetics with enhanced UV protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158041000001
    Figure 2024158041000001
  • Figure 2024158041000002
    Figure 2024158041000002
  • Figure 2024158041000003
    Figure 2024158041000003
Patent Text Reader

Abstract

To provide a cosmetic having high sunscreen efficacy, especially high ultraviolet A protection efficacy, less coloration and excellent safety, an efficient method for producing the same and an ultraviolet protective agent composition suitable for producing the same.SOLUTION: There is provided a cosmetic which contains a liquid oil (C) as an oil phase component comprising: an ultraviolet protective agent (A) composed of a layered double hydroxide, having positively charged basic layers composed of divalent metal ions, trivalent metal ions and hydroxide ions, and a negatively charged intermediate layer disposed between the two basic layers and containing organic acid ions and t-butyl methoxydibenzoylmethane; and at least one ultraviolet protection ability improver (B) selected from the group consisting of polyhydric alcohol fatty acid ester-based nonionic surfactants, polyoxyethylene alkyl ether phosphoric acid or salts thereof, silicone-based surfactants, polyhydroxy fatty acid, clay minerals and silica.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cosmetic having a high ultraviolet protection effect, a method for producing the same, and an ultraviolet protection agent composition suitable for producing the cosmetic. [Background technology]

[0002] Among the ultraviolet rays that have adverse effects on the human body, 4-tert-butyl-4'-methoxydibenzoylmethane (cosmetic label name: t-butyl methoxydibenzoylmethane, sometimes abbreviated as "BMBM" in this specification) is widely used as an organic ultraviolet absorbing agent for protecting against long-wavelength ultraviolet rays (UV-A) with wavelengths of 320 to 400 nm. However, this BMBM has low solubility in oils commonly used in cosmetics, making it difficult to include it in high concentrations, and even if it is dissolved, there is a problem that it is prone to crystallization over time, and further there is a problem that it is prone to coloration due to reaction with inorganic powders blended into cosmetics and metal ions derived from manufacturing equipment.

[0003] Therefore, development of a new ultraviolet absorber that improves the drawbacks of BMBM is underway, and for example, Patent Document 1 discloses an organic-inorganic composite ultraviolet absorber having a structure in which the interlayer water contained in the intermediate layer of hydrotalcites, which is a layered double hydroxide consisting of a positively charged base layer and a negatively charged intermediate layer, is replaced with a polar and nonionic organic ultraviolet absorber, for example, BMBM, as a new ultraviolet absorber (see claims 1 and 6). The document also describes that this organic-inorganic composite ultraviolet absorber is confined inside the layered crystals of hydrotalcites, so that the organic ultraviolet absorber can be protected from light and prevented from coming into contact with transition metals or skin (see paragraph 0006), and also discloses that this organic-inorganic composite ultraviolet absorber is used for cosmetics (see claim 9). However, there is no description of a specific example of a cosmetic using this organic-inorganic composite ultraviolet absorber, and no disclosure of an embodiment for use as a cosmetic. Thus, the organic-inorganic composite ultraviolet absorber described in Patent Document 1 has excellent UV-A protection capabilities, but in recent years, there has been a demand in the market for the development of sunscreen cosmetics with even higher performance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2021-161367 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention was completed against this background technology, and its main object is to provide a cosmetic preparation which has a high sunscreen effect, in particular a high protective effect against ultraviolet A rays (UV-A), is less discolored, and is highly safe. Another object is to provide a method for efficiently producing the cosmetic preparation, and a further object is to provide an ultraviolet protection agent composition suitable for producing the cosmetic preparation. [Means for solving the problem]

[0006] As a result of intensive research by the present inventors to solve the above problems, they discovered that in the case of the organic-inorganic composite ultraviolet absorber described in Patent Document 1, which contains BMBM as an ultraviolet absorber in the intermediate layer, it is useful to have a specific compound coexist when dispersing the organic-inorganic composite ultraviolet absorber in the oil phase, and thus completed the present invention.

[0007] Thus, according to the present invention, as a first invention, there is provided a cosmetic comprising an ultraviolet protection agent (A) consisting of a layered double hydroxide having a positively charged base layer composed of divalent metal ions, trivalent metal ions, and hydroxide ions, an organic acid ion and BMBM present between the two base layers, and a negatively charged intermediate layer, and a liquid oil (C) containing at least one ultraviolet protection enhancer (B) selected from the group consisting of polyhydric alcohol fatty acid ester type nonionic surfactants, polyoxyethylene alkyl ether phosphoric acid or its salt, silicone surfactants, polyhydroxy fatty acids, clay minerals, and silica. As another invention, there is provided a method for producing the cosmetic comprising a step of mixing the components (A), (B), and (C) to prepare an oil dispersion, and as a further invention, there is provided a composition for ultraviolet protection comprising the components (A), (B), and (C). Effect of the Invention

[0008] The cosmetic of the present invention has a high sunburn prevention effect, especially a high UV-A protection effect, is less colored by metal ions, and is also excellent in safety because the possibility of BMBM coming into contact with the skin is reduced. Furthermore, the production method and ultraviolet protection ability enhancer of the present invention allow the above-mentioned cosmetic to be produced efficiently. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The cosmetic of the present invention contains, as essential components, an organic-inorganic composite (A), an ultraviolet protection enhancer (B), and a liquid oil (C). Each component will be described in detail below.

[0010] (A: Organic-inorganic composite) The organic-inorganic composite used as component (A) of the present invention is a layered double hydroxide having a positively charged basic layer composed of divalent metal ions, trivalent metal ions, and hydroxide ions, and a negatively charged intermediate layer that contains organic acid ions and BMBM and is present between the two basic layers.

[0011] A typical example of a layered double hydroxide is hydrotalcite, a type of clay mineral. The typical composition of hydrotalcite is Mg6Al2(OH). 16 It is CO3·4H2O. Hydrotalcite has a layered crystal structure like talc and smectite, and a metal double hydroxide with a regular octahedral structure in which some of the Mg in magnesium hydroxide is replaced with Al forms a positively charged basic layer (also called the host layer), and CO3 ions that electrically neutralize the charge form an intermediate layer (also called the guest layer), and it is known that the intermediate layer contains water molecules. The water molecules contained in the intermediate layer are called interlayer water.

[0012] A large number of layered double hydroxides (sometimes referred to as "hydrotalcite-like compounds") having a structure similar to hydrotalcite are also known, in which the Mg in hydrotalcite is replaced with another divalent metal, the Al is replaced with another trivalent metal, the ratio of the two is changed, or the CO ions are replaced with other anions. These are usually represented by the composition formula shown in Formula (1) below. [(M 2+ ) 1-x (M 3+ ) x (OH)2][(A n- ) x / n (H2O) m ]····(1) (M in the formula 2+ is a divalent metal ion, M3+ represents a trivalent metal ion, A n- represents an n-valent anion respectively, n represents an integer from 1 to 6, x represents a number where 0.1 < x < 0.5, and m represents a number greater than 0.) As the divalent metal ion, Mg 2+ , Zn 2+ , Ca 2+ , Mn 2+ , Ni 2+ , Co 2+ etc. are exemplified, and preferably at least one of Mg 2+ and Zn 2+ . As the trivalent metal ion, Fe 3+ , Al 3+ , Ga 3+ .Cr 3+ , La 3+ , In 3+ etc. are exemplified, and preferably Al 3+ . As the n-valent anion, CO3 2- ,SO4 2- , NO3 - , PO4 3- etc. are exemplified.

[0013] The hydrotalcite-like compound can be easily obtained as a precipitate by coprecipitation reaction with an alkali that is almost equivalent to an aqueous solution of a mixed metal salt of divalent and trivalent. The interlayer anion of the hydrotalcite-like compound has ion exchangeability, and various anions have been inserted by utilizing its characteristics, so-called intercalation studies have been conventionally conducted, but there are few reports on the exchange of interlayer water. Patent Document 1 is one of the few reports, and the organic-inorganic composite described in that document is obtained by substituting the interlayer water of the hydrotalcite-like compound with a polar non-ionic organic ultraviolet absorber. In the present invention, among the organic-inorganic composites described in Patent Document 1, the one using BMBM as the organic ultraviolet absorber is used as the component (A).

[0014] The basic layer of the organic-inorganic composite used as component (A) of the present invention is formed of a double hydroxide of a divalent metal and a trivalent metal. The divalent metal used is Mg, Ca, Zn, Ni, Cu, etc., preferably Mg or Zn. The trivalent metal is Al, Fe, In, etc., preferably Al. The divalent metal and the trivalent metal may be used alone or in combination of two or more kinds.

[0015] The anion forming the intermediate layer of the organic-inorganic composite is an organic acid ion having a larger ionic radius than carbonate ion or sulfate ion, and preferably has an ionic radius such that the thickness (unit layer thickness) of the intermediate layer is 10 Å or more, and further 13 Å or more. If the thickness of the intermediate layer is smaller than the molecular diameter of BMBM (about 8.3 Å), it becomes difficult to insert BMBM between the layers, and it becomes difficult to obtain an organic-inorganic composite with a large BMBM content. Specific examples of preferred organic acid ions include ions of higher fatty acids having 10 or more carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid, and ions of ferulic acid and phenylbenzimidazole sulfonic acid, which are known to have ultraviolet absorbing ability, and among them, stearic acid ion, which has a large unit layer thickness of 31 Å, is particularly preferably used. The anion forming the intermediate layer may be a single component or multiple components.

[0016] The organic-inorganic composite contains BMBM in the intermediate layer. BMBM is inserted in a form that replaces water molecules originally contained therein, and some water molecules may coexist. The BMBM content in the organic-inorganic composite is preferably 2 to 80% by mass, more preferably 5 to 70% by mass, and particularly preferably 10 to 60% by mass. If the BMBM content is too small, it is not possible to impart a high ultraviolet protection effect to the cosmetic, and if it is too large, it is difficult to insert BMBM between the layers, making production difficult.

[0017] Such an organic-inorganic composite is a known substance from Patent Document 1 (JP 2021-161367 A) and can be produced according to the method described in the same document. The outline of the method is as follows. Phase 1 A hydrotalcite-like compound is produced by co-precipitation reaction of a mixed aqueous solution of water-soluble divalent and trivalent metal salts (metal chlorides, nitrates, bromides, sulfates, etc., preferably chlorides and nitrates) with an equivalent amount of alkali (sodium hydroxide, potassium hydroxide, ammonia, sodium carbonate, calcium hydroxide, etc.) approximately equal to the equivalent amount of the metal ions, followed by hydrothermal treatment at 100 to 250°C, preferably 150 to 250°C, for 5 to 20 hours. <Second Stage> The anions in the intermediate layer of the hydrotalcite-like compound are ion-exchanged with organic acid ions. <Third Stage> The hydrotalcite-like compound with an increased unit layer thickness in the second step is mixed with an organic solvent solution in which BMBM has been dissolved, and heated under stirring at a temperature below the boiling point of the organic solvent, preferably at 50 to 70°C, to replace the interlayer water with BMBM. Specific examples of organic solvents that dissolve BMBM include alcohols such as ethyl alcohol and isopropyl alcohol, and hydrocarbons such as n-hexane and cyclohexane, and are preferably alcohols. The amount of BMBM used in this replacement reaction is 1 to 150 parts by mass, preferably 10 to 100 parts by mass, relative to 100 parts by mass of the hydrotalcite-like compound. Thereafter, an organic-inorganic composite to be used as component (A) is obtained by appropriately selecting and using conventional processes such as filtration, washing, drying, pulverization, and classification.

[0018] Such an organic-inorganic composite may be used as it is, but may be treated with a polyanion (polymeric anion) if desired. Specific examples of the polyanion used include polyacrylic acid, maleic anhydride-olefin copolymer, polystyrene sulfonic acid, alginic acid, polyphosphoric acid, polysilicic acid (water glass), and carboxymethyl cellulose, which are usually neutralized with an alkali such as NaOH before use. The treatment with a polyanion can be carried out by adding an aqueous solution of a polyanion to a hydrotalcite-like compound dispersed in a polar solvent such as water, and mixing the aqueous solution with stirring. The amount of polyanion used in the treatment is 0.01 to 20% by mass, preferably 0.5 to 10% by mass, based on the mass of the organic-inorganic composite. When the polyanion is treated, the openings of the intermediate layer of the hydrotalcite-like compound are blocked, and the BMBM can be trapped inside.

[0019] Since the organic-inorganic complex of component (A) is a powder containing BMBM between the layers of the layered double hydroxide, the BMBM content in the cosmetic is proportional to the powder blend amount. Therefore, the greater the BMBM content in the organic-inorganic complex, and the greater the content of the organic-inorganic complex in the cosmetic, the greater the BMBM blend amount. BMBM is a substance that is difficult to dissolve in oils commonly used in cosmetics, so if BMBM is dissolved in an oil by a normal method, it is difficult to blend BMBM at a concentration above its solubility. However, according to the present invention, by increasing the BMBM content of the organic-inorganic complex and increasing the blend amount of the organic-inorganic complex, BMBM can be blended at a concentration above its solubility in the oil. Incidentally, the solubility of BMBM in liquid paraffin, which is used as an oil in cosmetics, is 1% by mass at room temperature.

[0020] The cosmetic of the present invention preferably contains 1 to 50% by mass of the organic-inorganic complex of component (A) in the cosmetic. More preferably, it is 2 to 40% by mass, and particularly preferably, it is 5 to 30% by mass. Moreover, the organic-inorganic complex of component (A) is preferably blended in such a ratio that the amount of BMBM contained therein is 0.5 to 20% by mass of the entire cosmetic, more preferably, the amount of BMBM is 1 to 15% by mass, and particularly preferably, the amount of BMBM is 2 to 10% by mass. If the content of component (A) in the cosmetic is too low, a high ultraviolet protection effect cannot be obtained, and if it is too high, the solids concentration in the cosmetic becomes high, making it difficult to spread on the skin.

[0021] (B: UV protection enhancer) The organic-inorganic composite of component (A) used in the present invention has the advantage that it does not precipitate BMBM crystals even when blended at a high concentration, and is less likely to be discolored by contact with metal ions, but it is still not sufficient in terms of UV protection effect. Therefore, in the present invention, at least one selected from the group consisting of polyhydric alcohol fatty acid ester type nonionic surfactant, polyoxyethylene alkyl ether phosphoric acid or its salt, silicone surfactant, polyhydroxy fatty acid, clay mineral, and silica is blended as component (B) as an UV protection ability enhancer to improve the UV protection ability of component (A).

[0022] The mechanism by which component (B) improves the UV protection effect is not clear; however, in the case of powders such as clay minerals and silica, it is presumed that it functions to prevent the complex of component (A) from agglomerating or reagglomerating in liquid oil, and in the case of other organic compounds, it is presumed that it functions to improve the wettability of the complex of component (A) and prevent reagglomeration in liquid oil.

[0023] Examples of polyhydric alcohol fatty acid ester type nonionic surfactants used as component (B) include sucrose fatty acid esters such as polysucrose polystearate and sucrose tetrastearate triacetate; glycerin fatty acid esters such as glyceryl stearate and glyceryl diisostearate; polyglycerin fatty acid esters such as polyglyceryl-2 oleate, polyglyceryl-2 isostearate and polyglyceryl-6 polyricinoleate; fatty acid sorbitan esters such as sorbitan isostearate, sorbitan sesquiisostearate, sorbitan oleate and sorbitan sesquioleate; polyoxyethylene sorbitan fatty acid esters such as PEG-4 sorbitan triisostearate; polyoxyethylene glycerin fatty acid esters such as PEG-5 glyceryl stearate; polyoxyethylene fatty acid esters such as PEG-3 isostearate and PEG-2 stearate; polyoxyethylene hydrogenated castor oils such as PEG-5 hydrogenated castor oil and PEG-7 hydrogenated castor oil. Among these, polyglyceryl-2 oleate, polyglyceryl-2 isostearate, sorbitan isostearate, sorbitan sesquiisostearate, sorbitan oleate, and sorbitan sesquioleate are preferably used because they have a high rate of improvement in ultraviolet protection ability.

[0024] The polyhydric alcohol fatty acid ester type nonionic surfactant used as component (B) is preferably lipophilic since it is used by dissolving or dispersing in the oil used in the cosmetic preparation, and its HLB value is usually 8 or less, preferably 2 to 8, and particularly preferably 3 to 6. Note that HLB is an index showing the balance between hydrophilicity and lipophilicity of a nonionic surfactant as a value from 0 to 20, with the closer to 0 the higher the lipophilicity, and the closer to 20 the higher the hydrophilicity. There are various known methods for calculating the HLB value, and the value is also listed in catalogs provided by manufacturers.

[0025] Commercially available polyhydric alcohol fatty acid ester type nonionic surfactants include, for example, NIKKOL SI-15RV (manufactured by Nikko Chemicals Co., Ltd.), which is a sorbitan sesquiisostearate, Cosmol 41V (manufactured by Nisshin Oillio Co., Ltd.), which is a polyglyceryl-2 isostearate, and NIKKOL HEXAGLYN PR-15 (manufactured by Nikko Chemicals Co., Ltd.), which is a polyglyceryl-6 polyricinoleate.

[0026] Examples of polyoxyethylene alkyl ether phosphate or its salt used as component (B) include polyoxyethylene lauryl ether phosphate, polyoxyethylene myristyl ether phosphate, polyoxyethylene cetyl ether phosphate, polyoxyethylene stearyl ether phosphate, polyoxyethylene behenyl ether phosphate, and sodium salts thereof. Examples of commercially available polyoxyethylene alkyl ether phosphate or its salt include NIKKOL TLP-4, which is trilaureth-4 phosphate, and DLP-10, which is dilaureth-10 phosphate (both manufactured by Nikko Chemicals Co., Ltd.).

[0027] Examples of silicone surfactants used as component (B) include silicone surfactants having polyoxyalkylene groups such as PEG-3 dimethicone, PEG-8 dimethicone, PEG-9 dimethicone, PEG-10 dimethicone, PEG-9 polydimethylsiloxyethyl dimethicone, lauryl PEG-9 polydimethylsiloxyethyl dimethicone, cetyl PEG / PPG-10 / 1 dimethicone, etc.; silicone surfactants having glycerin groups such as polyglyceryl-3 disiloxane dimethicone, polyglyceryl-3 polydimethylsiloxyethyl dimethicone, lauryl polyglyceryl-3 polydimethylsiloxyethyl dimethicone, etc. The HLB value of the silicone surfactant is preferably 8 or less, more preferably 2 to 8. The HLB value is particularly preferably 3 to 6.

[0028] Examples of commercially available silicone surfactants include silicone surfactants having a polyoxyalkylene group, such as KF-6016, KF-6011P, KF-6012, KF-6013, KF-6018, KF-6019, KF-6017, KF-6028P, and KF-6038 (all manufactured by Shin-Etsu Chemical Co., Ltd.), ABIL EM-90, ABIL EM-97 (all manufactured by Evonik Goldschmidt), SH-3772M, and SH3775M (all manufactured by Dow Toray Industries, Inc.), and SILWET L-7604 (manufactured by Momentive Performance Materials, Inc.), and silicone surfactants having a glycerin group, such as KF-6104, KF-6105, and KF-6106 (all manufactured by Shin-Etsu Chemical Co., Ltd.).

[0029] Examples of polyhydroxy fatty acids used as component (B) include polyhydroxystearic acid, polyricinoleic acid, etc. Commercially available polyhydroxy fatty acids include, for example, polyhydroxystearic acid Salacos HS-6C (manufactured by Nisshin Oillio Co., Ltd.).

[0030] Examples of clay minerals used as component (B) include water-swelling clay minerals such as bentonite, montmorillonite, hectorite, saponite, silicate (Li / Mg / Na), and silicate (Al / Mg); organically modified clay minerals such as disteardimonium hectorite (dimethyl distearyl ammonium hectorite), quaternium-18 hectorite, stearalkonium hectorite (benzyl dimethyl stearyl ammonium hectorite), and aluminum magnesium silicate treated with distearyl dimethyl ammonium chloride; non-swelling clay minerals such as talc, kaolin, mica, synthetic mica, and sericite; and examples of silica include fumed silica and wet silica. Among these ultraviolet protection enhancers, organically modified clay minerals have a high improvement rate of ultraviolet protection effect and can be preferably used. Commercially available organically modified clay minerals include Sumecton SAN-P (Kunimine Kogyo Co., Ltd.), which is a quaternium-18 hectorite, Esben WV60 (Hojun Co., Ltd.), which is a quaternium-18 bentonite, Benton 38VCG (Elementis Japan Co., Ltd.), which is a disteardimonium hectorite, and Benton 27 (Elementis Japan Co., Ltd.), which is a stearalkonium hectorite.

[0031] As the ultraviolet protection enhancer, a compound having an ultraviolet protection index of 1.2 or more, particularly 1.5 or more, as determined by the following evaluation method is preferably used. Examples of compounds having an ultraviolet protection index of 1.5 or more include polyhydric alcohol fatty acid ester-type nonionic surfactants, polyoxyethylene alkyl ether phosphates or salts thereof, silicone surfactants, polyhydroxy fatty acids, clay minerals, and silica, with organically modified clay minerals having a particularly high ultraviolet protection index.

[0032] (Evaluation method of UV protection index) The base layer is Mg 0.75 Al 0.2513.9 parts by mass of an organic-inorganic complex having a composition of (OH)2 and a BMBM content of 36% by mass and 13.9 parts by mass of isotridecyl isononanoate are mixed using a three-roll mill, and then 72.2 parts by mass of isotridecyl isononanoate are added to the resulting mixture to prepare a total of 100 parts by mass of oil dispersion (1). The amount of BMBM contained in this oil dispersion (1) is 5% by mass. The ultraviolet protection factor (UVAPF) of this oil dispersion (1) is measured according to the Colipa (European Federation of Perfume and Cosmetics Industry) guidelines (Method for in vitro determination of UVA protection, 2009), and the value is used as the reference value.

[0033] On the other hand, 100 parts by mass of oil dispersion (2) is prepared in the same manner as above, except that 1 part by mass of ultraviolet protection performance enhancer is added when mixing 13.9 parts by mass of organic-inorganic composite and 13.9 parts by mass of isotridecyl isononanoate using a three-roll mill, and the amount of isotridecyl isononanoate added is reduced to 71.2 parts by mass, and the UVAPF is measured and this value is designated as UVAPF-1. The amount of BMBM contained in oil dispersion (2) is 5% by mass, and the amount of ultraviolet protection performance enhancer is 1% by mass. The ratio of the obtained UVAPF-1 to the reference value (UVAPF-1 / reference value) is calculated, and this ratio is designated as the ultraviolet protection performance improvement index of the ultraviolet protection performance enhancer. An ultraviolet protection performance improvement index of more than 1 indicates that the addition of the ultraviolet protection performance enhancer has improved ultraviolet protection performance compared to when the ultraviolet protection performance enhancer is not added. For example, an ultraviolet protection performance improvement index of 1.2 indicates that the addition of the ultraviolet protection performance enhancer has improved ultraviolet protection performance by 20% compared to when the ultraviolet protection performance enhancer is not added.

[0034] In the cosmetic of the present invention, the content of the ultraviolet protection enhancer of component (B) is preferably 0.001 to 20% by mass, based on the total amount of the cosmetic. More preferably, it is 0.01 to 10% by mass. In addition, in the cosmetic of the present invention, the content of component (B) in the oil phase is preferably 0.01 to 40% by mass, based on the total amount of the oil phase. More preferably, it is 0.02 to 20% by mass. By having the amount of component (B) within this range, a high sunscreen effect is achieved. In addition, the mass ratio of component (B) to component (A) [(B) / (A)] is preferably 1 / 99 to 50 / 50, more preferably 2 / 98 to 30 / 70.

[0035] (C: Liquid oil) In the present invention, the above-mentioned components (A) and (B) are mixed with (C) liquid oil as essential components. Here, "liquid oil" refers to oil that has fluidity at room temperature (25°C) and semi-solid oil with a melting point of less than 50°C.

[0036] The liquid oil (C) is not particularly limited as long as it is one that is commonly used in cosmetics, and may be any of animal oils, vegetable oils, and synthetic oils. Specific examples of liquid oils include esters such as triethylhexanoin, tri(capryl / capric acid)glyceryl, neopentyl glycol dicaprate, isononyl isononanoate, isotridecyl isononanoate, ethylhexyl palmitate, isopropyl myristate, isopropyl palmitate, octyldodecyl myristate, diisostearyl malate, oligomer esters of dimer acid and dimer diol, pentaerythritol tetraisostearate, diglyceryl tetraisostearate, cetyl isooctanoate, cholesterol fatty acid esters, and jojoba oil; hydrocarbons such as volatile isoparaffin, (C13-15) alkanes, (C15-19) alkanes, butylene, heavy liquid isoparaffin, liquid paraffin, α-olefin oligomers, squalane, and petrolatum; oils and fats such as olive oil, castor oil, mink oil, and macadamia nut oil; Fatty acids such as isostearic acid and oleic acid; higher alcohols such as oleyl alcohol and isostearyl alcohol; silicone oils such as low polymerization degree dimethylpolysiloxane, cyclic silicone, high polymerization degree dimethylpolysiloxane, methylphenylpolysiloxane, methyltrimethicone, caprylyl trimethicone, crosslinked organopolysiloxane, and fluorine-modified polysiloxane; fluorine-based oils such as perfluoropolyether; lanolin derivatives such as lanolin, lanolin acetate, lanolin fatty acid isopropyl, and lanolin alcohol.

[0037] Among these liquid oils, ester oils have excellent dispersibility for component (A), and when ester oils are used as liquid oils, cosmetics exhibiting good UVAPF can be easily obtained.Specific examples of ester oils include triethylhexanoin, tri(caprylic / capric acid)glyceryl, neopentyl glycol dicaprate, isononyl isononanoate, isotridecyl isononanoate, ethylhexyl palmitate, and isopropyl myristate.

[0038] The viscosity of the liquid oil at 25°C is usually 0.5 to 5,000 mPa·s, preferably 1 to 500 mPa·s, and more preferably 5 to 500 mPa·s. The viscosity of the liquid oil is measured with a B-type viscometer. In particular, an ester oil having a viscosity of 1 to 200 mPa·s at 25°C is preferably used, and its content is preferably 10 to 100 mass% based on the total liquid oil.

[0039] The content of the liquid oil (C) is preferably 7 to 98% by mass, more preferably 10 to 95% by mass, and even more preferably 12 to 90% by mass, based on the total amount of the cosmetic. If the amount of the component (C) is too small, it becomes difficult to disperse the organic-inorganic composite of the component (A), and the ease of spreading decreases. If the amount is too large, the cosmetic lacks freshness and feels sticky when used.

[0040] The cosmetic of the present invention may be in any form, such as a lotion (liquid), gel, emulsion, suspension, cream, ointment, aerosol, mist, solid, or solid stick. This cosmetic can be used not only as a sunscreen cosmetic, but also as other cosmetic with ultraviolet protection. Specific examples of other cosmetic include makeup cosmetics such as foundation and base, skin care cosmetics such as emulsion, cream, beauty essence, BB cream, CC cream, and hair cosmetics.

[0041] In addition to the above-mentioned components (A), (B), and (C), the cosmetic of the present invention may appropriately contain other components. The other components are not particularly limited as long as they are generally used in the field of cosmetics, and the amount of the other components is not particularly limited as long as the effects of the present invention are not essentially impaired. Specific examples of the other components include solid oils, oil-soluble resins, oil-based gelling agents, ultraviolet absorbers (e.g., dimethicodethyl benzalomalonate, ethylhexyl methoxycinnamate, etc.), ultraviolet scattering agents (e.g., titanium oxide, zinc oxide, etc.), polyhydric alcohols (e.g., glycerin, propylene glycol, butanediol, etc.), lower alcohols (e.g., ethanol, isopropyl alcohol, etc.), surfactants, water-soluble polymers, vitamins, moisturizers, fragrances, antioxidants, whitening agents, pH adjusters, chelating agents, preservatives, antifoaming agents, fibers, and various extracts.

[0042] Although the above component (A) has excellent protection against UV-A, its protection against short-wavelength UV is insufficient, so when the cosmetic composition of the present invention is used for sunscreen purposes, it is preferable to blend an oil-soluble ultraviolet absorber or ultraviolet scattering agent that has excellent protection against short-wavelength ultraviolet rays (UV-B). The oil-soluble ultraviolet absorber and ultraviolet scattering agent will be described below.

[0043] Examples of oil-soluble UV absorbers that can be blended include cinnamic acid-based UV absorbers such as benzyl paramethoxycinnamate, 2-ethylhexyl paramethoxycinnamate, and glyceryl di-paramethoxycinnamate mono-2-ethylhexanoate; benzophenone-based UV absorbers such as hydroxymethoxybenzophenone, dihydroxymethoxybenzophenone, dihydroxybenzophenone, and tetrahydroxybenzophenone; benzoic acid ester-based UV absorbers such as paraaminobenzoic acid, ethyl paraaminobenzoate, glyceryl paraaminobenzoate, amyl paradimethylaminobenzoate, octyl paradimethylaminobenzoate, ethyl 4-[N,N-di(2-hydroxypropyl)amino]benzoate, and diethylaminohydroxybenzoylhexylbenzoate; salicylic acid-based UV absorbers such as ethylene glycol salicylate, phenyl salicylate, octyl salicylate, benzyl salicylate, para-tert-butylphenyl salicylate, and homomenthyl salicylate; Triazine-based ultraviolet absorbers such as ethylhexyl triazone (2,4,6-tris[4-(2-ethylhexyloxycarbonyl)anilino]1,3,5-triazine) and bis-ethylhexyloxyphenol methoxyphenyl triazine; other ultraviolet absorbers such as menthyl anthranilate, 2-(2-hydroxy-5-methylphenyl)benzotriazole, dimethoxybenzylidene dioxoimidazolidinepropionate 2-ethylhexyl, octocrylene, dimethicodethyl benzalmalonate, etc. Also, free BMBM can be contained within a range that does not impair the effects of the present invention.

[0044] When an oil-soluble ultraviolet absorber is blended, its content is 2 to 30% by mass, preferably 5 to 25% by mass, and more preferably 8 to 22% by mass, based on the total mass of the cosmetic.

[0045] Examples of the ultraviolet scattering agent that can be blended include fine particle metal oxides. More specifically, fine particle titanium oxide, fine particle zinc oxide, fine particle iron oxide, fine particle cerium oxide, fine particle zirconium oxide, etc. The shape of these fine particles is not particularly limited, and may be any of amorphous, granular, spherical, needle-like, spindle-like, plate-like, etc.

[0046] Since the ultraviolet scattering agent is usually added to the oil phase, it is preferable to use the one whose surface is hydrophobized from the viewpoint of dispersibility in the oil phase. Such a surface hydrophobization method is not particularly limited, and examples thereof include hydrophobized products using silicone, metal soap, N-acylamino acid salt, perfluoroalkyl compound, etc. as a treatment agent. The hydrophobization treatment can be carried out by using a single treatment agent or a combination of two or more treatment agents.

[0047] The ultraviolet scattering agent is usually a fine particle having a number average particle size of 5 nm to 100 nm, preferably 8 nm to 85 nm, more preferably 10 nm to 35 nm. If the number average particle size is too small, the ultraviolet protection effect is reduced, and if it is too large, the ultraviolet protection effect is reduced and the transparency is reduced.

[0048] When the cosmetic is an emulsion cosmetic such as an oil-in-water type or water-in-oil type, the UV scattering agent can be blended in the aqueous phase, but from the viewpoint of the durability of the sunburn prevention effect, it is preferable to blend it in the oil phase.

[0049] In the present invention, a solid oil can be contained in the oil phase. By containing a solid oil, it is possible to adjust the feel of the cosmetic such as the long-lasting effect and moisturizing feeling. In addition, by blending this, it is possible to make a compact or stick-shaped oil-based solid cosmetic or a solid W / O type cosmetic, and it is possible to impart functions such as portability and ease of use when applied to specific areas. In the present invention, the solid oil is an oil that is solid at room temperature (25°C) and has a melting point of 50 to 120°C, preferably 55°C to 105°C.

[0050] Specific examples of such solid oils include hydrocarbon waxes such as paraffin wax, polyethylene wax, ethylene-propylene copolymer, microcrystalline wax, ceresin, ozokerite, and Fischer-Tropsch wax, as well as Japan wax, carnauba wax, candelilla wax, rice wax, beeswax (beeswax), hydrogenated jojoba oil, hardened oil, higher alcohol, and silicone wax.

[0051] The formulation of the cosmetic of the present invention is not particularly limited, and may be, for example, an oil-based cosmetic, a water-in-oil (W / O) emulsion cosmetic, or an oil-in-water (O / W) emulsion cosmetic. Each formulation type will be described below.

[0052] (Oily based cosmetics) When the cosmetic of the present invention is an oil-based cosmetic, it can be in the form of an oily liquid, oily paste, or oily solid, containing components (A), (B), and (C) as essential components.

[0053] When the formulation is an oily paste or oily solid, it is preferable to contain one or more selected from an oily gelling agent and a solid oil. Examples of the oily gelling agent include dextrin fatty acid ester, sucrose fatty acid ester, starch fatty acid ester, aluminum stearate, etc. The content of the oily gelling agent and / or solid oil is usually 1 to 30% by mass, preferably 2 to 20% by mass, and more preferably 3 to 15% by mass, based on the total weight of the cosmetic.

[0054] (Water-in-oil emulsion cosmetics) When the sunscreen cosmetic of the present invention is a water-in-oil type emulsion cosmetic, it may contain water, a water-soluble component, and a water-dispersible component that form an aqueous phase, in addition to the components (A), (B), and (C). From the viewpoint of emulsion stability, the water-in-oil type emulsion cosmetic may contain a lipophilic surfactant that does not fall under component (B), and it is preferable that the aqueous phase contains an inorganic salt such as sodium chloride or magnesium sulfate in an amount of 0.01 to 3 mass% based on the total weight of the cosmetic.

[0055] In the water-in-oil emulsion cosmetic, the content of the oil phase is preferably 20 to 95% by mass, more preferably 30 to 90% by mass, based on the total weight of the cosmetic, and the content of the water phase is preferably 5 to 80% by mass, more preferably 10 to 70% by mass, based on the total weight of the cosmetic.

[0056] (oil-in-water emulsion cosmetics) When the cosmetic of the present invention is an oil-in-water emulsion cosmetic, it may contain water, a water-soluble component, and a water-dispersible component that form an aqueous phase, in addition to the components (A), (B), and (C). From the viewpoint of emulsion stability, it is preferable that the aqueous phase of the oil-in-water emulsion cosmetic contains a hydrophilic surfactant, a water-soluble polymer, and a polyhydric alcohol. Examples of hydrophilic surfactants include anionic surfactants, amphoteric surfactants, and nonionic surfactants with an HLB value of more than 8.

[0057] In the case of an oil-in-water emulsion cosmetic, the content of the aqueous phase is preferably 30 to 80% by mass, more preferably 40 to 75% by mass, based on the total weight of the cosmetic, and the content of the oil phase is preferably 20 to 70% by mass, more preferably 25 to 60% by mass, based on the total weight of the cosmetic.

[0058] (Method of manufacturing cosmetics) The cosmetic of the present invention can be prepared according to a conventional method, but it is preferable to prepare an oily dispersion containing each of the components (A), (B), and (C) in advance, and then add and mix other components as necessary to form an oil phase in which the organic-inorganic composite is dispersed. According to this production method, a cosmetic having excellent sun protection effect, feel, and usability can be efficiently produced.

[0059] The method for preparing the oil dispersion is not particularly limited, but it is preferable to use a dispersing machine to produce it from the viewpoint of improving the sunburn prevention effect. Examples of dispersing machines include roll mills such as two-roll and three-roll, ball mills such as ball mills and vibration ball mills, paint shakers, bead mills such as continuous disk bead mills and continuous annular bead mills, Henschel mixers, dispersing mixers, homomixers, high-pressure homogenizers, planetary mixers, kneaders, etc. Among these, it is preferable to use a roll mill because of its high dispersing power and ease of equipment cleaning.

[0060] When preparing an oil-based dispersion using a dispersing machine, the total amount of components (A), (B) and (C) constituting the dispersion may be put into the dispersing machine, or the dispersion may be dispersed using components (A), (B) and a part of component (C) in advance, and then diluted with the remaining component (C). When preparing a dispersion using a kneading machine such as a three-roll mill, the mass ratio of the amount of component (A) to the total amount of components (B) and (C) during dispersion [(A):[(B)+(C)]] is preferably 2:8 to 8:2, more preferably 4:6 to 7:3. If this mass ratio is small, it is difficult to obtain a fine dispersion, and if this mass ratio is too large, the oil agent does not become a continuous phase, making it difficult to obtain a dispersion.

[0061] (Ultraviolet protection composition) The present invention also provides an ultraviolet protection composition containing the organic-inorganic complex of component (A). The ultraviolet protection composition of the present invention is an oil-based dispersion containing the organic-inorganic complex of component (A) and the ultraviolet protection enhancer of component (B) in the liquid oil of component (C), and can be suitably used for preparing cosmetics.

[0062] The content of component (A) in the UV protection composition of the present invention is preferably 1 to 70 mass %, more preferably 2 to 50 mass %, of the composition. The content of component (B) in the composition is preferably 0.01 to 50 mass %, more preferably 0.02 to 40 mass %, of the composition. The content of component (C) in the composition is preferably 10 to 98 mass %, more preferably 20 to 90 mass %.

[0063] The ultraviolet protection composition of the present invention can be produced by mixing the organic-inorganic composite of component (A), the ultraviolet protection enhancer of component (B), and the liquid oil of component (C), together with other components added as required. The preparation method is the same as the preparation method of the oil dispersion in the above-mentioned cosmetic production method. EXAMPLES

[0064] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. In the following production examples, examples, and comparative examples, "parts" and "%" represent "parts by mass" and "% by mass relative to the total amount" unless otherwise specified. In addition, the cosmetic compositions in the following examples and comparative examples were evaluated as follows.

[0065] (UVAPF measurement) The UVAPF was measured using a Labshere SPF Analyzer UV-1000S. The sample application plate used in the measurement was Shiseido Irika Technology's SPFMASTER-PA01, and the application amount was 2 mg / cm. 2 Let us assume that.

[0066] (Coloring test) 20 g of the evaluation sample was placed in a 30 mL glass bottle, and an iron nail (iron round nail N32) was added and stored at 40°C for one day. The degree of coloration of the sample was then visually observed and judged on a four-point scale based on the following evaluation criteria.

[0067] (Evaluation Criteria) A: There is no color change. B: The area around the nail is slightly discolored red or brown. C: The area around the nail has darkened to red or brown. D: Extensive red or brown discoloration around the nail.

[0068] Manufacturing Example 1 (Production of organic-inorganic complex I) A 2L mixture of 1.5M / L magnesium chloride aqueous solution and 0.5M / L aluminum chloride aqueous solution and 2L of 4.0M / L sodium hydroxide aqueous solution were fed to a 5L reaction tank filled with 500mL of water under stirring at a flow rate of 100mL / min using a metering pump, and a coprecipitation reaction was carried out while maintaining the pH at about 9.4-9.6 and the temperature at about 35°C to obtain a hydrotalcite-like compound. A portion of the precipitate was collected and dissolved in hydrochloric acid to measure the amounts of Mg and Al by chelate titration, and the atomic ratio of Mg:Al was found to be 3:1. In addition, by comparing the X-ray diffraction pattern of the precipitate with the X-ray diffraction pattern of the hydrotalcite, it was found that the hydrotalcite-like compound contained Mg. 0.75 Al 0.25It was found that the double hydroxide having the composition of (OH)2 formed the basic layer, and the chloride ions and water molecules formed the intermediate layer. Next, the reaction product was filtered under reduced pressure, washed with water, and then redispersed in water with a chemical stirrer to make the total volume 5L. 1L of the reaction product was taken from the reaction product, placed in a 1L autoclave, and hydrothermally treated at 180°C for 15 hours. After cooling to about 90°C, it was transferred to a 2L beaker, and an equimolar aqueous solution of sodium stearate (about 90°C) with Al was added under stirring, and the reaction was carried out for 30 minutes, and the chloride ions between the layers were ion-exchanged with stearate ions. After this, the mixture was filtered, washed with hot water (about 90°C), dried (about 120°C for 3 hours), and sieved through a 100 mesh screen to obtain a powder of a hydrotalcite-like compound containing interlayer water and stearate ions as interlayer anions. (BMBM-free complex) 50 g of this powder was added to 800 mL of ethyl alcohol solution in which 38 g of BMBM had been dissolved, and the mixture was heated at 60 ° C for 1 hour to replace the interlayer water with BMBM. Then, 0.5 g of maleic anhydride / diisobutylene copolymer sodium salt (Polystar OMR, NOF Corp.) was added and stirred for another 20 minutes. After filtration under reduced pressure, the mixture was washed with alcohol and sieved at 120 ° C for 2 hours with a 100 mesh to obtain organic-inorganic composite I. The sieved powder was dissolved in hydrochloric acid, and diethyl ether was added to extract BMBM into diethyl ether. A portion of the extract was taken and the amount of BMBM was measured from the absorption intensity at a wavelength of 357 nm using a spectrophotometer, and the content of BMBM was 36%.

[0069] Manufacturing Example 2 (Production of organic-inorganic complex II) Except for using 800 mL of ethyl alcohol in which 45 g of BMBM was dissolved, instead of 800 mL of ethyl alcohol solution in which 38 g of BMBM was dissolved, organic-inorganic composite II was obtained in the same manner as in Production Example 1. When analyzed in the same manner as in Production Example 1, the content of BMBM was 43%.

[0070] Comparative Example 1 13.9 parts of the organic-inorganic composite I (BMBM content 36%) obtained in Production Example 1 and the same mass of isotridecyl isononanoate were kneaded using a three-roll mill, and 72.2 parts of isotridecyl isononanoate were further added and mixed to prepare a total of 100 parts of an oil dispersion. The amount of BMBM contained in this oil dispersion corresponds to 5% of the total. The UVAPF of this composition was measured and found to be 23.6. In the following Examples 1 to 13, the ultraviolet protection ability improvement index of the ultraviolet protection ability improver was calculated using this value as the reference value.

[0071] Example 1 In Comparative Example 1, an ultraviolet absorber composition was obtained in the same manner as in Comparative Example 1, except that 1 part by mass of sorbitan sesquiisostearate was added prior to kneading with a three-roll mill, and the amount of isotridecyl isononanoate added was 71.2 parts. The BMBM content of this composition was 5%, and the sorbitan sesquiisostearate content was 1%. The UVAPF of this composition was measured to be 36.5, and the ultraviolet protection ability improvement index of sorbitan sesquiisostearate was 1.5. That is, the UVAPF was improved by 1.5 times the above-mentioned standard value due to the coexistence of sorbitan sesquiisostearate.

[0072] Examples 2 to 13 Except for using the compounds shown in Table 1 instead of sorbitan sesquiisostearate, ultraviolet absorbent compositions were prepared in the same manner as in Example 1, and the UVAPFs of the compositions were measured to calculate the ultraviolet protection ability improvement indexes of the respective compounds. The results are shown in Table 1.

[0073] [Table 1]

[0074] From the results in Table 1, it can be seen that the coexistence of polyhydric alcohol fatty acid ester type nonionic surfactants (Examples 1-3), polyoxyethylene alkyl ether phosphate or its salt (Example 4), silicone surfactants (Examples 5 and 6), polyhydroxy fatty acids (Example 7), clay minerals (Examples 8-12), and silica (Example 13) results in UVAPFs that greatly exceed the standard value. Among them, sorbitan sesquiisostearate (Example 1), sorbitan oleate (Example 2), trilaureth-4 phosphate (Example 4), PEG-10 dimethicone (Example 5), polyhydroxystearic acid (Example 7), clay minerals (Examples 8-12), and fumed silica (Example 13) greatly improved the ultraviolet protection ability, and in particular, it was found that the organically modified clay minerals (Examples 8 and 9) remarkably improved the ultraviolet protection ability.

[0075] Examples 14 and 15 and Comparative Examples 2 and 3 <Water-in-oil (W / O) sunscreen cosmetics> The water-in-oil sunscreen cosmetic compositions shown in Table 2 were prepared according to the following manufacturing procedures and evaluated using the above evaluation methods. The results are also shown in Table 2. (Manufacturing Procedure) (1) The components listed in Part A of Table 2 are mixed together using a three-roll mill to prepare an oil-based dispersion. (2) Prepare an oil phase by dissolving or dispersing the components described in Part B in the above oil dispersion and thoroughly mixing. Note that homosalate (homomenthyl salicylate), octocrylene, and octyl salicylate described in Part B are oil-soluble UV absorbers. (3) Prepare the aqueous phase by mixing the ingredients listed in Part C. Note that butylene glycol listed in Part C is a humectant. (4) At room temperature (around 25°C), the above water phase is added to the above oil phase with stirring to prepare the cosmetic preparation.

[0076] [Table 2]

[0077] As is clear from the results in Table 2, the water-in-oil type cosmetics of the present invention exhibit excellent UVAPF and are less likely to be colored by contact with metals (Examples 14 and 15). In contrast, the cosmetics containing no BMBM have extremely low UVAPF (Comparative Example 2), and the cosmetics containing BMBM without complexation and dissolved in the oil phase showed coloring due to contact with metals (Comparative Example 3).

[0078] Example 16 and Comparative Example 4 <W / O type emulsified foundation> An W / O type emulsified foundation having the composition shown in Table 3 was prepared according to the same production procedure as in Example 14 and evaluated by the above evaluation method. The results are also shown in Table 3. The hydrogen dimethicone-treated fine zinc oxide described in Part B is an ultraviolet scattering agent, and the aluminum distearate-treated titanium oxide is a colorant.

[0079]

Table 3

[0080] As is clear from the results in Table 3, the W / O type foundation of Example 16 exhibits a large UVAPF and is less likely to be colored by contact with metals. In contrast, the foundation of Comparative Example 4 containing BMBM dissolved in the oil phase has a lower UVAPF than the example and shows coloring due to contact with metals.

[0081] Example 17, Comparative Example 5 <Oil-in-water type sunscreen cosmetics> An oil-in-water type sunscreen cosmetics having the composition shown in Table 4 was prepared according to the following production procedure using the D-phase emulsification method and evaluated by the above evaluation method. The results are also shown in Table 4. (Production procedure) (1) The components of Part A are kneaded using a three-roll mill to prepare an oily dispersion. The triethoxycaprylylsilane-treated fine titanium oxide described in Part A is an ultraviolet scattering agent. (2) In Comparative Example 5, the components of Part B are dissolved and mixed, and then mixed with the components of Part A to form an oil phase. (3) Prepare Phase D (surfactant phase) by mixing the ingredients of Part C. (4) At room temperature, the oil phase (in the case of Comparative Example 5) or the oil-based dispersion (in the case of Example 17) is mixed in small portions into the D phase to prepare an O / D phase of a gel emulsion. (5) The aqueous phase prepared by mixing the ingredients of part D with the above O / D phase is added and mixed to prepare the cosmetic preparation.

[0082] [Table 4]

[0083] As is clear from the results in Table 4, the sunscreen cosmetic of Example 17 exhibited excellent UVA protection and did not become discolored due to contact with metals. In contrast, the sunscreen cosmetic of Comparative Example 5 exhibited good UVA protection but became significantly discolored due to contact with metals. [Industrial Applicability]

[0084] According to the present invention, there are provided a cosmetic preparation which has a high sunburn prevention effect, is less discolored by metal ions, and is excellent in safety, an efficient method for producing the cosmetic preparation, and an ultraviolet protection agent composition which is useful for preparing the cosmetic preparation.

Claims

1. A cosmetic preparation comprising, as an oil phase component, an ultraviolet protection agent (A) consisting of a layered double hydroxide having a positively charged base layer composed of divalent metal ions, trivalent metal ions, and hydroxide ions, and a negatively charged intermediate layer containing organic acid ions and t-butyl methoxydibenzoylmethane present between the two base layers, and a liquid oil (C) containing at least one ultraviolet protection enhancer (B) selected from the group consisting of polyhydric alcohol fatty acid ester type nonionic surfactants, polyoxyethylene alkyl ether phosphates or salts thereof, silicone surfactants, polyhydroxy fatty acids, clay minerals, and silica.

2. 2. The cosmetic preparation according to claim 1, wherein the divalent metal is at least one selected from magnesium and zinc, and the trivalent metal is aluminum.

3. 3. The cosmetic preparation according to claim 1, wherein the content of t-butyl methoxydibenzoylmethane in the layered double hydroxide is 2 to 80 mass %.

4. 3. The cosmetic preparation according to claim 1, wherein the content of said component (A) is 1 to 50 mass%, the content of said component (B) is 0.01 to 20 mass%, and the content of said component (C) is 7 to 98 mass%.

5. The method for producing a cosmetic preparation according to claim 1 or 2, comprising a step of mixing the component (A), the component (B), and the component (C) to prepare an oil-based dispersion.

6. An ultraviolet protection agent composition comprising the component (A), the component (B) and the component (C).

Citation Information

Patent Citations

  • Ultraviolet absorber

    JP2021161367A