Manufacturing method of semiconductor wafer and manufacturing method of semiconductor device

By employing a semiconductor wafer support structure with sloping angles and controlled RTA conditions, the method addresses slips during RTA processing, enhancing wafer quality and device reliability.

JP2024158114APending Publication Date: 2024-11-08GLOBALWAFERS JAPAN
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023073006
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing semiconductor wafer manufacturing methods face issues with slips during Rapid Thermal Annealing (RTA) processing due to thermal and self-weight stress, leading to device failures, which conventional techniques have not adequately addressed.

Method used

The method involves RTA treatment with a semiconductor wafer placed on a support member having a sloping surface, forming obtuse angles between the wafer backside and bevel, with specific angle ranges (θ1≧5°, θ2≧5°, and |θ1−θ2|≦5°) to minimize contact area and thermal stress, along with controlled temperature and cooling rates.

Benefits of technology

This approach effectively suppresses slips during RTA, ensuring gettering properties and reducing device failures by minimizing contact area and thermal stress, thereby improving wafer quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158114000001_ABST
    Figure 2024158114000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a semiconductor wafer which suppress slipping caused by implementing RTA processing.SOLUTION: A manufacturing method of a semiconductor wafer includes a step of performing RAT processing and performs the RTA processing in a state where the wafer is mounted in a wafer support member 2 including a supporting surface 2a inclined downward toward the inside. The manufacturing method of the semiconductor wafer further includes a bevel processing step of making a corner, which is formed by a wafer rear face 1a and a rear face side bevel 1b, into an obtuse angle and processing the semiconductor wafer in such a manner that an apex 1c of the obtuse angle is in contact with the supporting surface 2a when performing the RTA processing. In the RTA processing, a semiconductor wafer 1 is generated in such a manner that an angle θ1 of a corner which is at a contact position with the supporting surface 2a and formed by the wafer rear face 1a and the supporting surface 2a and an angle θ2 of a corner formed by the rear face side bevel 1b and the supporting surface 2a respectively satisfy θ1≥5° and θ2≥5° and further that a differential between the angle θ1 and the angle θ2 satisfies |θ1-θ2|≤5°.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor wafer, which includes a step of performing an RTA (Rapid Thermal Annealing) process. [Background technology]

[0002] Semiconductor wafers obtained by slicing semiconductor single crystal ingots grown by the CZ (Czochralski) method have numerous grown-in defects on their surfaces and surface layers. However, because semiconductor wafers are required to have surfaces and surface layers that are almost defect-free, RTA processing has been used for some time as a method for eliminating defects on the surface and surface layers.

[0003] The rapid heating and cooling heat treatment by RTA not only eliminates defects on the surface and surface layer of the semiconductor wafer, but also forms a high density of BMD (Bulk Micro Defects) in the bulk portion. The BMD in the bulk portion acts as a gettering site for metal impurities that are diffused during the semiconductor device fabrication process and affect the device characteristics.

[0004] For example, as a method for manufacturing a silicon wafer having a step of performing an RTA treatment, Patent Document 1 listed below discloses a method in which an RTA treatment is performed on a silicon wafer in an oxidizing atmosphere at a temperature of 1300° C. or higher and 1400° C. or lower, and a large amount of vacancies, which are point defects, are left in the bulk of the silicon wafer, thereby forming a high density of BMDs during a subsequent precipitation heat treatment.

[0005] Furthermore, as a pre-process before performing heat treatment by RTA, the following Patent Documents 2 and 3 describe, for example, slicing a silicon single crystal ingot grown by the Czochralski method into wafers using an inner diameter blade or a wire saw, and then subjecting the sliced ​​silicon wafers to processing steps such as chamfering the outer periphery, lapping, etching, and mirror polishing on both sides to prepare silicon wafers before heat treatment.

[0006] Furthermore, the following Patent Documents 4 and 5 disclose techniques for specifying the angle of the wafer bevel and the inclination angle of the wafer support member (such as a susceptor) in order to suppress slippage caused by the RTA process.

[0007] Furthermore, Patent Document 6 listed below discloses a heat treatment tool that can prevent not only slippage but also scratches on the back surface of the wafer and chamfered portions by forming the support surface of a support member that supports the back surface of the wafer during heat treatment into a convex curved shape. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2015-204326 A [Patent Document 2] JP 2022-050071 A [Patent Document 3] JP 2013-201314 A [Patent Document 4] JP 2007-036105 A [Patent Document 5] JP 2006-19625 A [Patent Document 6] JP 2006-5271 A Summary of the Invention [Problem to be solved by the invention]

[0009] As described in the above Patent Document 1, it is desirable to perform an RTA treatment at 1300°C or higher in order to eliminate surface and surface layer defects of a semiconductor wafer and form BMD in the bulk part, but when an RTA treatment is performed, slip occurs due to the temperature difference within the wafer surface and stress caused by the weight of the semiconductor wafer. In particular, when the wafer support member is an edge ring that supports the semiconductor wafer from the outer periphery of the back surface, the stress caused by the weight of the wafer and the thermal stress caused by the temperature difference between the semiconductor wafer and the wafer support member occur simultaneously at the contact position between the semiconductor wafer and the wafer support member, which makes it easy for slip to occur on the outer periphery of the wafer.

[0010] Furthermore, as described in Patent Documents 2 and 3 above, if the semiconductor wafer (particularly the back surface and back surface bevel of the wafer) is mirror-polished before heat treatment, the contact area between the semiconductor wafer and the wafer support member increases when the RTA treatment is performed, making it easier for slippage due to welding to occur.

[0011] Since the above-mentioned slips can cause device defects, there is a demand for heat treatments that can suppress the slips.

[0012] On the other hand, the above Patent Documents 4 and 5 describe techniques for specifying the angle of the wafer bevel and the inclination angle of the wafer support member, etc., in order to suppress slip due to the implementation of RTA processing, and the above Patent Document 6 describes forming the support surface of the wafer support member that supports the back surface of the wafer during heat treatment into a convex curved shape. However, since the effect of heat dissipation in the wafer contact area (the back surface side and the back surface bevel side of the wafer) during cooling is not taken into consideration, there is room for further improvement in terms of suppressing slip due to thermal stress.

[0013] Furthermore, a method for suppressing slip caused by the RTA process is required not only for semiconductor wafers but also for manufacturing semiconductor devices from semiconductor wafers.

[0014] The present invention has been made in view of the above problems, and has an object to provide a method for manufacturing a semiconductor wafer that suppresses slip caused by the RTA treatment. Another object of the present invention is to provide a method for manufacturing a semiconductor device that suppresses slip caused by the RTA treatment. [Means for solving the problem]

[0015] The method for manufacturing a semiconductor wafer according to the present invention includes a step of performing an RTA treatment, and is a method for manufacturing a semiconductor wafer in which the RTA treatment is performed while the wafer is placed on a wafer support member having a support surface that slopes downward inward. The method includes a bevel processing step of forming an obtuse angle between the back surface of the wafer and a back surface bevel, and processing the semiconductor wafer so that the apex of this obtuse angle contacts the support surface during the RTA treatment. In the step of performing the RTA treatment, the angle θ1 between the back surface of the wafer and the support surface formed at the contact position between the apex of the obtuse angle and the support surface, and the angle θ2 between the back surface bevel and the support surface are set to θ1≧5° and θ2≧5°, respectively, and further, the difference between angle θ1 and angle θ2 is set to |θ1-θ2|≦5°.

[0016] According to the semiconductor wafer manufacturing method of the present invention, even when performing RTA treatment at 1300°C or higher, which can ensure gettering properties against metal impurities, slip occurring at the contact portion between the semiconductor wafer and the wafer support member can be reduced.

[0017] Furthermore, in the semiconductor wafer manufacturing method according to the present invention, it is desirable that the surface roughness of the semiconductor wafer at the contact position is 5.0 nm≦Ra≦30.0 nm, and further, it is desirable that the angle θ3 between the back surface of the wafer and the back surface bevel is 157°≦θ3≦167°.

[0018] In the semiconductor wafer manufacturing method according to the present invention, it is preferable to perform the RTA treatment under the conditions of holding the maximum temperature of 1300°C to 1350°C for 1 s to 60 s in an oxidizing atmosphere and cooling to 1000°C at a cooling rate of 50°C / s to 120°C / s. In the semiconductor wafer manufacturing method according to the present invention, it is preferable to set the diameter of the semiconductor wafer to be subjected to the RTA treatment to 300 mm or more. In the semiconductor wafer manufacturing method according to the present invention, it is preferable to set the difference between the angle θ1 and the angle θ2 to |θ1-θ2|=0°.

[0019] The method for manufacturing a semiconductor device according to the present invention includes a step of performing an RTA treatment, and the RTA treatment is performed while the semiconductor wafer is placed on a semiconductor wafer support member having a support surface that slopes downward inward, the semiconductor wafer being processed so that an obtuse angle is formed between the back surface of the wafer and a back surface bevel, and an apex of the obtuse angle contacts the support surface during the RTA treatment, and in the step of performing the RTA treatment, an angle θ1 formed between the back surface of the wafer and the support surface at a contact position between the apex of the obtuse angle and the support surface, and an angle θ2 formed between the back surface bevel and the support surface are set to θ1≧5° and θ2≧5°, respectively, and further, a difference between angle θ1 and angle θ2 is set to |θ1-θ2|≦5°. Effect of the Invention

[0020] According to the method for producing a semiconductor wafer or a method for producing a semiconductor device of the present invention, slip caused by carrying out an RTA process can be suppressed. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of a method for producing a semiconductor wafer according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of an RTP device. [Diagram 3]FIG. 3 is a diagram showing an example of a cause of slippage. [Figure 4] FIG. 4 is a diagram showing an example of a cause of slippage. [Diagram 5] FIG. 5 is a diagram showing the results of measuring the distortion area ratio by SIRD for each of the silicon wafers produced by the methods of the example and comparative examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of a method for manufacturing a semiconductor wafer according to the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to this embodiment.

[0023] <Manufacturing method> FIG. 1 is a cross-sectional view showing a schematic diagram of a method for manufacturing a semiconductor wafer (sometimes simply called a wafer) according to the present embodiment. The method for manufacturing a semiconductor wafer according to the present embodiment includes a step of performing an RTA process, in which the semiconductor wafer 1 is placed on a wafer support member 2 having a support surface 2a that is inclined downward toward the inside. Furthermore, the method for manufacturing a semiconductor wafer according to the present embodiment includes a bevel processing step of processing the wafer so that the angle between the wafer back surface 1a and the back surface bevel 1b is formed to be an obtuse angle, and the apex 1c of the obtuse angle contacts the support surface 2a when the RTA process is performed. During the RTA process, the semiconductor wafer 1 is generated so that the angle θ1 between the wafer back surface 1a and the support surface 2a formed at the contact position with the support surface 2a, and the angle θ2 between the back surface bevel 1b and the support surface 2a are θ1≧5° and θ2≧5°, respectively, and further, the difference between the angle θ1 and the angle θ2 is |θ1-θ2|≦5°.

[0024] In the method for manufacturing a semiconductor wafer according to this embodiment, an RTA treatment is performed under an oxidizing atmosphere while maintaining the maximum temperature at 1250°C or higher (preferably 1300°C or higher and 1350°C or lower) for 1 second or more and 60 seconds or less, and then cooling at a cooling rate of 50°C / s or higher and 120°C / s or lower until 1000°C or lower. Thereby, a semiconductor wafer having sufficient gettering characteristics for metal impurities can be manufactured.

[0025] In this embodiment, even when performing an RTA treatment at 1300°C or higher that can ensure gettering characteristics for metal impurities, a method for manufacturing a semiconductor wafer capable of reducing slips generated from the contact portion between the semiconductor wafer 1 and the wafer support member 2 is proposed.

[0026] <RTA treatment> Here, the RTA treatment in the process of manufacturing the semiconductor wafer 1 will be described. The RTP (Rapid Thermal Process) apparatus 10 used in this embodiment includes, for example, as shown in FIG. 2, a chamber (reaction tube) 20 having an atmosphere gas inlet 20a and an atmosphere gas outlet 20b, a plurality of lamps 30 spaced apart and disposed above the chamber 20, and a wafer support portion 40 that supports the semiconductor wafer 1 in the reaction space 25 within the chamber 20.

[0027] The wafer support portion 40 includes an annular wafer support member 40a (corresponding to the above-described wafer support member 2) that supports the outer peripheral portion of the semiconductor wafer 1, and a stage 40b that supports the wafer support member 40a. Further, the wafer support portion 40 includes a rotating means (not shown) that rotates the semiconductor wafer 1 at a predetermined speed around its central axis.

[0028] 2, when performing RTA processing on the semiconductor wafer 1, the semiconductor wafer 1 is introduced into the reaction space 25 through a wafer inlet (not shown) provided in the chamber 20, and the semiconductor wafer 1 is placed on the wafer support member 40a. Then, while introducing atmospheric gas from the atmospheric gas inlet 20a and rotating the semiconductor wafer 1 by the rotating means, the wafer surface is irradiated with light from the lamps 30.

[0029] The temperature control within the reaction space 25 in this RTP device 10 is performed by measuring the temperatures at multiple points on the wafer surface in the wafer radial direction below the semiconductor wafer 1 using multiple radiation thermometers 50 embedded in the stage 40b, and controlling the multiple lamps 30 (such as individually controlling the ON-OFF of each lamp and controlling the emission intensity of the emitted light) based on the measured temperatures.

[0030] <Production method details> Next, the method for producing a semiconductor wafer according to the present embodiment will be described in detail with reference to the drawings.

[0031] In the method for manufacturing a semiconductor wafer according to this embodiment, first, a semiconductor single crystal ingot grown by the CZ method is obtained, and then the semiconductor single crystal ingot is sliced ​​into wafers using a wire saw or the like. Then, the semiconductor wafer obtained by slicing is subjected to beveling. After that, the uneven layer formed during slicing is removed in a lapping process and a grinding process, and the flatness and surface roughness are adjusted. Then, the processing damage introduced in the lapping and grinding processes is removed in an etching process.

[0032] In this embodiment, the semiconductor wafer 1 is produced in which the angle between the wafer back surface 1a and the back surface bevel 1b is formed to be an obtuse angle by the above-mentioned manufacturing process (Slicing → Beveling → Lapping → Grinding → Etching) as shown in FIG. 1. Here, as an example, a semiconductor wafer 1 having a diameter of 300 mm or more is produced. At that time, when the semiconductor wafer 1 is placed on the support surface 2a (support surface 2a inclined downward toward the inside) of the wafer support member 2, the semiconductor wafer 1 is processed so that the boundary portion (apex 1c of the obtuse angle) between the wafer back surface 1a and the back surface bevel 1b contacts the support surface 2a. Specifically, as shown in FIG. 1, the angle θ1 between the wafer back surface 1a and the support surface 2a formed at the contact position and the angle θ2 between the back surface bevel 1b and the support surface 2a are set to θ1≧5° and θ2≧5°, respectively, and further, the difference between the angle θ1 and the angle θ2 is set to |θ1-θ2|≦5°.

[0033] The adjustment of angles θ1 and θ2 is performed by a method of controlling angle θ3 between wafer back surface 1a and back surface bevel 1b during the bevel processing step, and a method of adjusting the angle of support surface 2a of wafer support member 2. In the semiconductor wafer manufacturing method of this embodiment, after RTA processing is performed on semiconductor wafer 1 generated in the above-mentioned manufacturing step, mirror polishing is performed on the wafer front surface.

[0034] By producing the semiconductor wafer 1 for performing the RTA process as described above, the contact area between the semiconductor wafer 1 and the wafer support member 2 is minimized (see FIG. 1), and therefore slip caused by welding can be suppressed. Furthermore, by defining the angles θ1 and θ2 as described above, the difference in heat dissipation between the wafer back surface 1a side and the back surface bevel 1b side at the contact position between the semiconductor wafer 1 and the wafer support member 2 is suppressed (see FIG. 1), and thermal stress occurring at the contact portion between the semiconductor wafer 1 and the wafer support member 2 is suppressed, and therefore slip caused by thermal stress can also be minimized.

[0035] For example, when an RTA process is performed using a semiconductor wafer that has been mirror-polished after an etching process, the boundary between the back surface of the wafer and the back surface bevel becomes smooth, and the contact area between the semiconductor wafer and the wafer support member 2 tends to increase (see FIG. 3), which causes slippage due to welding during RTA process at 1300°C or higher.

[0036] Furthermore, when the angle θ1 is 0°, the wafer support member 2 and the back surface of the wafer are in close contact with each other (see FIG. 4(a)), and when the angle θ2 is 0°, the wafer support member 2 and the back surface bevel are in close contact with each other (see FIG. 4(b)). As a result, for example, slippage due to welding occurs in an RTA process at 1300°C or higher.

[0037] Furthermore, if the angles θ1 and θ2 are too small (for example, less than 5°), heat is not easily dissipated from the contact area between the semiconductor wafer and the wafer support member 2 during rapid cooling (see FIG. 4(c)), causing slippage due to thermal stress.

[0038] Furthermore, if the difference between angles θ1 and θ2 is large (for example, if the difference exceeds 5°), a difference in heat dissipation occurs between the back surface side and the back surface bevel side of the wafer at the contact position between the semiconductor wafer and the wafer support member 2 (see Figure 4(d)), causing slippage due to thermal stress.

[0039] That is, in this embodiment, by setting θ1 ≧ 5° and θ2 ≧ 5°, a space is secured in which heat can be dissipated during rapid cooling while minimizing the contact area between the semiconductor wafer 1 and the wafer support member 2, and further, by setting |θ1-θ2|≦ 5°, the difference in heat dissipation between the wafer back surface 1a side and the back surface bevel 1b side of the contact portion is suppressed. This makes it possible to suppress slip occurring from the contact portion during rapid cooling.

[0040] In this embodiment, in order to further reduce slippage caused by the RTA process, it is preferable to set the surface roughness of the semiconductor wafer 1 around the contact position between the semiconductor wafer 1 and the wafer support member 2 to 5.0 nm≦Ra≦30.0 nm in the above-mentioned manufacturing process. This reduces the contact area between the semiconductor wafer 1 and the wafer support member 2, and can further suppress slippage caused by welding. If Ra<5.0 nm, the contact area between the semiconductor wafer and the wafer support member 2 becomes large, which is undesirable because slippage caused by welding is likely to occur. Also, if Ra>30.0 nm, it is undesirable because the surface of the semiconductor wafer is too rough, which causes variation in the wafer contact area, which makes slippage caused by self-weight stress more likely to occur.

[0041] In this embodiment, it is preferable that the angle θ3 between the wafer back surface 1a and the back surface bevel 1b is 157°≦θ3≦167°. This makes it possible to reduce the contact area between the semiconductor wafer 1 and the wafer support member 2 while preventing chipping and cracking of the wafer end surface that occurs during wafer transport during manufacturing, thereby suppressing slippage caused by welding. If θ3<157°, chipping and cracking are likely to occur on the wafer back surface during wafer transport, which is not preferable. If θ3>167°, chipping and cracking are likely to occur on the wafer end surface during wafer transport, which is not preferable.

[0042] In the semiconductor device manufacturing method of this embodiment, a semiconductor wafer (the above-mentioned semiconductor wafer 1) is used, which is processed so that the angle between the wafer back surface and the back surface bevel is formed as an obtuse angle, and the apex of this obtuse angle contacts the support surface 2a of the wafer support member 2 during the RTA process. In addition, a conventionally known method can be adopted as the semiconductor device manufacturing process, and in the RTA process, the angle θ1 between the wafer back surface and the support surface 2a formed at the contact position between the apex of the obtuse angle and the support surface 2a, and the angle θ2 between the back surface bevel and the support surface 2a are set to θ1≧5° and θ2≧5°, respectively, and further, the difference between the angle θ1 and the angle θ2 is set to |θ1-θ2|≦5°. As a result, the contact area between the semiconductor wafer 1 and the wafer support member 2 is minimized as described above, so that the semiconductor device manufacturing method can also suppress slip caused by welding. Furthermore, by specifying the angles θ1 and θ2 as described above, the difference in heat dissipation between the back side of the wafer and the back side bevel side at the contact position between the semiconductor wafer 1 and the wafer support member 2 is suppressed, and thermal stress generated at the contact portion between the semiconductor wafer 1 and the wafer support member 2 is suppressed, so that slip due to thermal stress can also be minimized. EXAMPLES

[0043] Next, the method for producing a semiconductor wafer according to the present invention will be further described based on examples, although the present invention is not limited to the following examples.

[0044] <Example> Oxygen concentration: 1.0 x 10 18 / cm 3For a silicon wafer obtained by slicing a silicon single crystal ingot, the manufacturing process of the present embodiment described above (Beveling → Lapping → Grinding → Etching) was performed, and 10 first silicon wafers with a diameter of 300 mm (corresponding to the semiconductor wafer 1 described above: see FIG. 1) were produced so that Ra = 20 nm and θ3 = 160°. Then, using an RTP apparatus having a wafer support member with a support surface inclined downward by 10° toward the inside, the first silicon wafer was placed on the support surface so that θ1 = 10°, θ2 = 10°, and |θ1 - θ2| = 0°, and the following RTA treatment was performed to produce a silicon wafer (see FIG. 1). <RTA treatment conditions> The RTA treatment was performed under the condition of holding at a maximum temperature of 1350 °C for 30 s in an oxidizing atmosphere and cooling at a cooling rate of 120 °C / s to 1000 °C or lower.

[0045] <Comparative Example 1> Oxygen concentration: 1.0×10 18 / cm 3 For a silicon wafer obtained by slicing a silicon single crystal ingot, the manufacturing process of Comparative Example 1 (Beveling → Lapping → Grinding → Etching) was performed, and 10 second silicon wafers with a diameter of 300 mm (see FIG. 4(b)) were produced so that Ra = 20 nm and θ3 = 170°. Then, using the same RTP apparatus as in the example, the second silicon wafer was placed on the support surface of the wafer support member so that θ1 = 10°, θ2 = 0°, and |θ1 - θ2| = 10°, and the RTA treatment was performed under the same conditions as in the example to produce a silicon wafer (see FIG. 4(b)).

[0046] <Comparative Example 2> Oxygen concentration: 1.0×10 18 / cm 3The silicon wafer obtained by slicing the silicon single crystal ingot was subjected to the manufacturing process of Comparative Example 2 (Beveling → Lapping → Grinding → Etching) to produce 10 third silicon wafers (see FIG. 4(d)) having a diameter of 300 mm so that Ra=20 nm and θ3=150°. Then, using the same RTP device as in the example, the third silicon wafer was placed so that θ1=10°, θ2=20°, and |θ1-θ2|=10° relative to the support surface of the wafer support member, and an RTA process was performed under the same conditions as in the example to produce silicon wafers (see FIG. 4(d)).

[0047] <Comparative Example 3> Oxygen concentration: 1.0 x 10 18 / cm 3 The silicon wafer obtained by slicing the silicon single crystal ingot was subjected to the conventional manufacturing process (Beveling → Lapping → Grinding → Etching → Mirror Polishing) to produce ten fourth silicon wafers (Ra=5 nm, θ1=10°, θ2=5°, |θ1-θ2|=5°, θ3=165° relative to the support surface of the wafer support member before mirror polishing, see FIG. 3) having a diameter of 300 mm. Then, using the same RTP device as in the embodiment, the fourth silicon wafer was placed on the support surface of the wafer support member, and RTA processing was performed under the same conditions as in the embodiment to produce silicon wafers (see FIG. 3).

[0048] <Evaluation method> The silicon wafers produced by the methods of the embodiment and comparative examples 1 to 3 were measured by SIRD (Scanning Infrared Depolarization) to evaluate slip and strain area ratio. That is, the ratio of the area where the strain stress increased due to slip to the entire area of ​​the silicon wafer (strain area ratio) was calculated and evaluated. For example, the larger the strain area ratio, the worse the slip quality, and the smaller the strain area ratio, the better the slip quality.

[0049] 5 is a diagram showing the results of measurement of the distortion area ratio by SIRD for each silicon wafer produced by the method of the example and comparative examples 1 to 3. The silicon wafer produced by the method of comparative example 1 had an average distortion area ratio of 9.7×10 -4 In the silicon wafers produced by the method of Comparative Example 2, slippage occurred due to welding with the wafer support member. In addition, the average distortion area ratio was 5.5×10 -4 In addition, the silicon wafer produced by the method of Comparative Example 3 had the largest average area distortion ratio (7.5×10 -3 ) slippage due to welding to the wafer support member and slippage due to thermal stress had occurred.

[0050] On the other hand, the silicon wafer of the embodiment corresponding to the above-mentioned silicon wafer 1 (see FIG. 1) had the smallest average strain area ratio (4.1×10 -5 ), and slip was suppressed to the greatest extent. Furthermore, it was confirmed that the distortion area ratio of the peripheral portion was reduced by approximately 99% compared to the silicon wafer of Comparative Example 3. [Explanation of symbols]

[0051] 1. Semiconductor wafer 1a Wafer backside 1b Back side bevel 1c top 2 Wafer support member 2a Support surface 10 RTP device 20 Chamber (reaction tube) 20a Atmospheric gas inlet 20b Atmospheric gas exhaust port 25 Reaction Space 30 Lamp 40 Wafer support 40a Wafer support member 40b Stage 50 radiation thermometer

Claims

1. A method for manufacturing a semiconductor wafer, comprising a step of performing an RTA treatment, the method including the steps of: performing an RTA treatment on a wafer support member having a support surface that is inclined downward toward an inside of the wafer; a bevel processing step of forming an obtuse angle between the wafer back surface and a back surface bevel, and processing the semiconductor wafer so that an apex of the obtuse angle contacts the support surface during RTA processing; In a step of performing an RTA process, an angle θ1 between the back surface of the wafer formed at a contact position between the apex of the obtuse angle and the support surface and an angle θ2 between the back surface bevel and the support surface are set to θ1≧5° and θ2≧5°, respectively, and further, a difference between the angle θ1 and the angle θ2 is set to |θ1-θ2|≦5°. A method for manufacturing a semiconductor wafer comprising the steps of:

2. In the bevel processing step, the surface roughness of the semiconductor wafer at the contact position is set to 5.0 nm≦Ra≦30.0 nm.

2. The method for producing a semiconductor wafer according to claim 1.

3. In the bevel processing step, an angle θ3 between the back surface of the wafer and the back surface bevel is set to 157°≦θ3≦167°.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

4. The RTA treatment is carried out under the conditions of holding the maximum temperature of 1300° C. or more and 1350° C. or less for 1 s or more and 60 s or less in an oxidizing atmosphere, and cooling to 1000° C. or less at a cooling rate of 50° C. / s or more and 120° C. / s or less.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

5. The diameter of the semiconductor wafer to be subjected to the RTA treatment is 300 mm or more.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

6. The difference between the angle θ1 and the angle θ2 is |θ1-θ2|=0°.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

7. A method for manufacturing a semiconductor device, comprising: a step of performing an RTA treatment, the method including performing the RTA treatment in a state where a semiconductor wafer is placed on a semiconductor wafer support member having a support surface that is inclined downward toward an inside, the method comprising: the semiconductor wafer is a semiconductor wafer in which an angle between the wafer back surface and a back surface bevel is formed as an obtuse angle, and the apex of the obtuse angle is processed so as to contact the support surface during RTA treatment; In a step of performing an RTA process, an angle θ1 between the back surface of the wafer formed at a contact position between the apex of the obtuse angle and the support surface and an angle θ2 between the back surface bevel and the support surface are set to θ1≧5° and θ2≧5°, respectively, and further, a difference between the angle θ1 and the angle θ2 is set to |θ1-θ2|≦5°.

1. A method for manufacturing a semiconductor device comprising the steps of:

Citation Information

Patent Citations

  • Tool and method for heat treatment of semiconductor wafer

    JP2006005271A

  • JP2006‐19625A

  • Susceptor for silicon wafer

    JP2007036105A

  • Method for manufacturing silicon wafer

    JP2013201314A

  • Heat treatment method of silicon wafer and silicon wafer

    JP2015204326A