Image formation system, and image formation method
The image forming system addresses image defects in toners with reduced bisphenol A derivatives by using amorphous polyester and an aluminum alloy developing sleeve, ensuring low-temperature fixability and heat resistance.
Patent Information
- Application Number
- JP2023073381
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing toners with reduced bisphenol A derivatives suffer from image defects such as black spots and fog, particularly at increased print speeds and in compact machines, due to the rigidity of bisphenol A derivatives affecting meltability and causing heat generation issues.
An image forming system using electrostatic image developing toners with amorphous polyester containing 10 mol% or less structural units derived from bisphenol A derivatives and a developing sleeve made of an aluminum alloy with more than 0.6% by mass silicon to suppress heat generation and improve low-temperature fixability and heat resistance.
The system effectively suppresses image defects like black spots and fog while maintaining excellent low-temperature fixability and heat resistance, even at high print speeds and in compact machines.
Smart Images

Figure 2024158293000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an image forming system and an image forming method, and more particularly to an image forming system and the like that is capable of suppressing image defects such as black spots and fogging and has excellent low-temperature fixing properties and heat resistance. [Background technology]
[0002] From the viewpoint of energy saving in recent years, it is desired that the toner for developing electrostatic images used during image formation has excellent low-temperature fixing properties. Regarding the toner for developing electrostatic images (hereinafter, also simply referred to as "toner"), for example, as in Patent Document 1, a toner containing an amorphous polyester and a crystalline polyester as a binder resin has been developed.
[0003] By the way, bisphenol A derivatives are often used in the production of amorphous polyesters. However, the bisphenol A derivatives have a structure containing many aromatic rings, so the molecules are rigid and very difficult to move, which inhibits the melting of the resin. For this reason, it is disadvantageous for low-temperature fixing, and there are also concerns about the environmental impact.
[0004] For this reason, there is a demand for the development of a toner that uses a small amount of bisphenol A derivative, as in Patent Document 2. However, it has been found that when the amount of bisphenol A derivative used is reduced, problems occur in which image defects such as black spots occur. In particular, it has been found that these image defects become more pronounced with the recent trend toward higher printing speeds and more compact machines. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-279714 A [Patent Document 2] JP 2017-062344 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide an image forming system and an image forming method that suppress image defects such as black spots and fog and have excellent low-temperature fixing properties and heat resistance. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have investigated the causes of the above problems, and have found that the above problems can be solved by an image forming system having an electrostatic image developing toner including toner particles containing an amorphous polyester in which the content of structural units derived from bisphenol A derivatives is equal to or less than a certain numerical value, and a developing sleeve having an aluminum alloy containing more than 0.6 mass % of silicon, thereby arriving at the present invention. That is, the above problems according to the present invention are solved by the following means.
[0008] 1. An image forming system having a toner for developing an electrostatic image and a developing sleeve for transporting the toner for developing an electrostatic image, the toner particles contained in the electrostatic image developing toner contain an amorphous polyester, the amorphous polyester is a polycondensate of a polycarboxylic acid and a polyhydric alcohol, a content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less based on the total structural units derived from the polyhydric alcohol; The developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon. 1. An image forming system comprising:
[0009] 2. A member that generates magnetic flux is provided inside the developing sleeve. 2. The image forming system according to claim 1,
[0010] 3. The toner particles contain a crystalline resin. 2. The image forming system according to claim 1,
[0011] 4. The crystalline resin contains a crystalline polyester, The crystalline polyester is a polycondensation product of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms. 4. The image forming system according to claim 3,
[0012] 5. The polyhydric alcohol contains an aliphatic polyhydric alcohol having 5 or more carbon atoms. 2. The image forming system according to claim 1,
[0013] 6. The silicon content in the aluminum alloy is more than 0.8% by mass. 2. The image forming system according to claim 1,
[0014] 7. The toner particles contain a release agent having a melting point in the range of 70 to 91°C. 2. The image forming system according to claim 1,
[0015] 8. The toner particles contain silica particles having an average particle diameter in the range of 90 to 130 nm as an external additive. 2. The image forming system according to claim 1,
[0016] 9. An image forming method using a toner for developing an electrostatic image and a developing sleeve for transporting the toner for developing an electrostatic image, the toner particles contained in the electrostatic image developing toner contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, a content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less based on the total structural units derived from the polyhydric alcohol; The developing sleeve comprises an aluminum alloy containing more than 0.6% by weight of silicon. 1. An image forming method comprising: Effect of the Invention
[0017] According to the above-mentioned means of the present invention, it is possible to provide an image forming system and an image forming method which can suppress image defects such as black spots and fog, and have excellent low-temperature fixing properties and heat resistance. Although the mechanism of the manifestation or action of the effects of the present invention is not clear, it is speculated as follows.
[0018] The image forming system of the present invention comprises a toner for developing electrostatic images, the toner particles containing an amorphous polyester in which the content of structural units derived from bisphenol A derivatives is 10 mol % or less relative to all structural units derived from polyhydric alcohols, and a developing sleeve having an aluminum alloy containing more than 0.6 mass % silicon.
[0019] As described above, since the bisphenol A derivative has a structure containing many aromatic rings in the molecule, the molecule is characterized by being very rigid and difficult to move. Therefore, in the present invention, the content of the structural unit derived from the bisphenol A derivative in the amorphous polyester is set to 10 mol % or less with respect to the total structural units derived from the polyhydric alcohol, thereby facilitating the movement of charge in the molecule and accelerating the rise of the charge amount.
[0020] However, when the content of the structural unit derived from a bisphenol A derivative is set to 10 mol % or less as described above, the glass transition temperature (Tg) of the toner decreases, and the amount of heat generated on the developing sleeve during image formation increases, which causes the toner to aggregate and results in image defects such as black spots.
[0021] The developing sleeve used in the image forming system of the present invention has an aluminum alloy containing more than 0.6% by mass of silicon, and has a high surface resistance, which suppresses heat generation during image formation.
[0022] In the image forming system of the present invention, the content of the structural unit derived from the bisphenol A derivative is set within the above range during image formation, and the above developing sleeve is used in combination with the above developing sleeve, which is presumably capable of suppressing the adverse effects of reducing the amount of bisphenol A derivative used while preventing excessive heat generation on the developing sleeve and suppressing image defects such as black spots. [Brief description of the drawings]
[0023] [Figure 1] External view of a developing roller equipped with a developing sleeve [Diagram 2] Cross-sectional view of a developing roller with a shaft that does not pass through the magnet roller [Diagram 3] Cross-sectional view of a developing roller with a shaft passing through a magnet roller [Figure 4] Partially enlarged view of the cross section of the developing sleeve [Diagram 5] FIG. 1 is an explanatory cross-sectional view showing an example of a configuration of an electrophotographic image forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The image forming system of the present invention is an image forming system having a toner for developing electrostatic images and a developing sleeve for transporting the toner for developing electrostatic images, characterized in that the toner particles contained in the toner for developing electrostatic images contain an amorphous polyester, the amorphous polyester is a polycondensate of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less relative to all structural units derived from the polyhydric alcohol, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon. This feature is a technical feature common to or corresponding to each of the following embodiments (aspects).
[0025] As an embodiment of the present invention, even if a member that generates a magnetic flux, such as the above-mentioned magnet roller, is provided inside the developing sleeve, this is preferable from the viewpoint of suppressing heat generation on the developing sleeve.
[0026] It is preferable that the toner particles contain a crystalline resin from the viewpoint of achieving both low-temperature fixability and high-temperature storage stability.
[0027] It is preferable that the crystalline resin contains a crystalline polyester, and the crystalline polyester is a polycondensate of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms, from the viewpoints of improving low-temperature fixability and improving the rise of charge amount while ensuring heat-resistant storage stability of the toner.
[0028] From the viewpoint of suppressing toner fogging, it is preferable that the polyhydric alcohol contains an aliphatic polyhydric alcohol having 5 or more carbon atoms.
[0029] It is preferable that the silicon content in the aluminum alloy exceeds 0.8% by mass from the viewpoint of suppressing heat generation on the developing sleeve.
[0030] The toner particles preferably contain a release agent having a melting point in the range of 70 to 91° C. in terms of separability from the fixing member, low-temperature fixability, and heat-resistant storage stability of the toner particles.
[0031] From the viewpoint of heat-resistant storage stability, it is preferable that the toner particles contain silica particles having an average particle size within a range of 90 to 130 nm as an external additive.
[0032] The image forming method according to the present invention is an image forming method using a toner for developing electrostatic images and a developing sleeve that transports the toner for developing electrostatic images, the toner particles contained in the toner for developing electrostatic images contain an amorphous polyester that is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less relative to all structural units derived from the polyhydric alcohol, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon, and can be suitably used in the image forming system of the present invention.
[0033] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower and upper limits.
[0034] [Overview of the image forming system of the present invention] 1. Image forming system The image forming system of the present invention is an image forming system having a toner for developing electrostatic images and a developing sleeve for transporting the toner for developing electrostatic images, characterized in that the toner particles contained in the toner for developing electrostatic images contain an amorphous polyester, the amorphous polyester is a polycondensate of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less relative to all structural units derived from the polyhydric alcohol, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon.
[0035] In the present invention, the "image forming system" refers to a collection of devices or apparatuses with specific functions, toner or developer, recording media, etc., which are used as the means elements necessary for each step of image formation. These as a whole perform the function of image formation. Each means element may be disposed separately in different locations, or may be gathered together in a certain space as a single device to form a system device.
[0036] The image forming system of the present invention may use an image forming apparatus described below as a device or apparatus for forming an image. However, as long as the system is a form or mode in which an image is formed using the toner and developing sleeve, the means constituting the image forming system are not limited.
[0037] The image forming system of the present invention may also include a means for recording and storing the recording and copying information as electronic data, and a means for wirelessly transmitting the electronic data. For example, it is preferable that the image forming system has a wireless interface for transmitting and receiving data to and from the information processing means by wireless communication such as Bluetooth (registered trademark) or Wi-Fi (registered trademark).
[0038] As mentioned above, bisphenol A derivatives are often used in the production of amorphous polyesters contained in toners. However, since the bisphenol A derivatives have a structure containing many aromatic rings, the molecules are rigid and very difficult to move, which inhibits the melting of the resin. For this reason, it is required to reduce the amount of bisphenol A derivatives used, but the drop in glass transition temperature (Tg) increases the amount of heat generated, which causes the toner to aggregate and results in image defects such as black spots.
[0039] The image forming system of the present invention uses a developing sleeve having a high surface resistivity while suppressing the content of structural units derived from bisphenol A derivatives to a low level during image formation. Specifically, the content of structural units derived from bisphenol A derivatives in the amorphous polyester is set to 10 mol % or less relative to the total structural units derived from polyhydric alcohols, which facilitates the movement of charges within the molecule and speeds up the rise of the charge amount.In addition, a developing sleeve with a high surface resistance and an aluminum alloy containing more than 0.6 mass % silicon is used, which suppresses heat generation during image formation.
[0040] From the above, while suppressing the adverse effects caused when the amount of bisphenol A derivative used is reduced, heat generation on the developing sleeve is suppressed from becoming excessive, and image defects such as black spots can be suppressed.
[0041] The components of the image forming system of the present invention will be described below in order.
[0042] (1.1) Toner for developing electrostatic images In the present invention, the term "toner for developing electrostatic images" refers to an aggregate of toner particles. Hereinafter, the term "toner for developing electrostatic images" is also simply referred to as "toner". The toner particles may be composed of only toner base particles, or may be composed of toner base particles and an external additive attached to the surface of the toner base particles. The term "toner base particles" refers to a material that constitutes the base of the toner particles. The toner base particles contain a binder resin such as amorphous polyester, and may also contain a colorant, a release agent (wax), a charge control agent, etc., as necessary.
[0043] The toner particles contained in the toner for developing electrostatic images according to the present invention contain an amorphous polyester, the amorphous polyester being a polycondensate of a polycarboxylic acid and a polyhydric alcohol, and the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less based on the total structural units derived from the polyhydric alcohol.
[0044] (1.1.1) Amorphous polyester From the viewpoint of low-temperature fixability, the toner according to the present invention contains an amorphous polyester. The term "amorphous polyester" refers to a polyester obtained by a polymerization reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyhydric alcohol), which exhibits amorphous properties. In addition, from the viewpoint that bisphenols can be esterified in the same manner as alcohols, in the present invention, the "polyhydric alcohol" includes bisphenol A derivatives. The bisphenol A derivative also includes bisphenol A itself.
[0045] "Amorphous" means that it does not have a melting point. In other words, "amorphous" means that it does not have a clear endothermic peak when heated in an endothermic curve obtained by differential scanning calorimetry (DSC). "Clear endothermic peak" means a peak with a half-width of 15°C or less in an endothermic curve when heated at a heating rate of 10°C / min.
[0046] The amorphous polyester according to the present invention is a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol, and the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less relative to the total structural units derived from the polyhydric alcohol. It is particularly preferable that the content is 0 mol %. This can further suppress toner fogging.
[0047] (Content of structural units derived from bisphenol A derivatives) The content of structural units derived from bisphenol A derivatives in the amorphous polyester contained in the toner particles can be analyzed by a nuclear magnetic resonance (NMR) device. For example, the toner particles to be measured can be dissolved in a deuterium solvent and analyzed using a proton nuclear magnetic resonance (1H-NMR) device. Specifically, it can be obtained by the following method.
[0048] First, the toner particles are analyzed together with an internal standard substance of known concentration. Next, only the target component (e.g., linear aliphatic diol, etc.) of known concentration and the internal standard substance are analyzed. By comparing the spectra obtained by these, the structural units derived from bisphenol A derivatives and all structural units derived from polyhydric alcohols in the amorphous polyester can be calculated.
[0049] (Synthesis method) The amorphous polyester can be synthesized by esterifying a polyvalent carboxylic acid and a polyhydric alcohol through polycondensation using a known esterification catalyst.
[0050] [Polyhydric alcohol] Examples of polyhydric alcohols other than bisphenol A derivatives that can be used in the synthesis of amorphous polyesters include dihydric or trihydric alcohols such as ethylene glycol, propylene glycol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, glycerin, sorbitol, 1,4-sorbitan, and trimethylolpropane.
[0051] The bisphenol A derivative includes bisphenol A and its derivatives. Examples of the bisphenol A derivative include bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.
[0052] From the viewpoint of low temperature fixability, it is preferable to include an aliphatic polyhydric alcohol. Since the molecules are easily mobile, low temperature fixability is improved. The polyhydric alcohol component is preferably any one of ethylene glycol, neopentyl glycol, propane glycol, and 1,5-pentanediol. In addition, from the viewpoint of suppressing toner fogging, it is preferable that the polyhydric alcohol contains an aliphatic polyhydric alcohol having 5 or more carbon atoms.
[0053] Since the structural unit derived from the aliphatic polyhydric alcohol having 5 or more carbon atoms contained in the amorphous polyester has a large degree of freedom of molecular motion, the inclusion of the structural unit facilitates the movement of charges within the molecule of the amorphous polyester. Therefore, the inclusion of the structural unit derived from the aliphatic polyhydric alcohol having 5 or more carbon atoms in the amorphous polyester can further suppress toner fogging.
[0054] For the above reasons, in the synthesis of the amorphous polyester according to the present invention, it is preferable to use an aliphatic polyhydric alcohol having 5 or more carbon atoms. As the aliphatic polyhydric alcohol having 5 or more carbon atoms, neopentyl glycol is particularly preferable.
[0055] [Polycarboxylic acid] Examples of polyvalent carboxylic acids that can be used in the synthesis of the amorphous polyester include phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, mesaconic acid, dimethyl isophthalate, fumaric acid, dodecenylsuccinic acid, 1,10-dodecanedicarboxylic acid, etc. Among these, terephthalic acid, fumaric acid, and dodecenylsuccinic acid are preferred.
[0056] 〔catalyst〕 Examples of catalysts that can be used in the synthesis of the amorphous polyester include metal-containing compounds, phosphorous compounds, phosphoric acid compounds, and amine compounds.
[0057] Examples of the metal contained in the metal-containing compound include sodium, lithium, magnesium, calcium, aluminum, zinc, manganese, antimony, titanium, tin, zirconium, germanium, etc. These may be used alone or in combination of two or more.
[0058] Specific examples of tin-containing compounds include dibutyltin oxide, tin octoate, tin dioctoate, and salts thereof.
[0059] Examples of titanium-containing compounds include titanium alkoxides, titanium acylates, and titanium chelates. Examples of titanium alkoxides include tetra-normal-butyl titanate (Ti(On-Bu)4), tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate. Examples of titanium acylates include polyhydroxytitanium stearate. Examples of titanium chelates include titanium tetraacetylacetonate, titanium lactate, and titanium triethanolamine.
[0060] Examples of germanium-containing compounds include germanium dioxide.
[0061] Examples of aluminum-containing compounds include polyaluminum hydroxide, aluminum alkoxide, tributylaluminate, and the like.
[0062] (Polymerization temperature) The polymerization temperature is not particularly limited, but is preferably within the range of 150 to 250° C. The polymerization time is not particularly limited, but is preferably within the range of 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0063] (Glass transition temperature and weight average molecular weight) From the viewpoint of achieving both sufficient low-temperature fixability and heat-resistant storage stability, the glass transition point (Tg) of the amorphous polyester is preferably within a range of 25 to 60° C., and more preferably within a range of 35 to 55° C. The glass transition point (Tg) can be measured using a differential scanning calorimeter, for example, Diamond DSC (manufactured by PerkinElmer).
[0064] The weight average molecular weight Mw of the amorphous polyester can be within the range of 10000 to 100000. The weight average molecular weight Mw can be measured by gel permeation chromatography (GPC).
[0065] (others) The amorphous polyester may be a hybrid amorphous polyester having a graft copolymer structure of an amorphous polyester polymer segment and a styrene-acrylic polymer segment.
[0066] The content of the amorphous polyester is preferably within a range of 50 to 100% by mass, and more preferably within a range of 70 to 90% by mass, based on the total amount of the resin contained in the toner base particles.
[0067] (1.1.2) Crystalline resins The toner particles according to the present invention preferably contain a crystalline resin from the viewpoint of achieving both low-temperature fixability and high-temperature storage stability. From the viewpoint of low-temperature fixability, the crystalline resin is more preferably a crystalline polyester.
[0068] "Crystalline" means having a melting point. In other words, "crystalline" means having a clear endothermic peak when heated in an endothermic curve obtained by differential scanning calorimetry (DSC). A "clear endothermic peak" means a peak with a half-width of 15°C or less in an endothermic curve when heated at a heating rate of 10°C / min.
[0069] The melting point (Tm) of the crystalline resin is more preferably within a range of 62 to 82° C. in order to obtain sufficient low-temperature fixability and high-temperature storage stability.
[0070] The crystalline resin is not particularly limited, but may be a polyolefin resin, a polydiene resin, or a polyester resin. Among these, it is more preferable to contain a crystalline polyester. This can ensure the heat-resistant storage property of the toner while improving the low-temperature fixability and also improve the charge build-up.
[0071] (Crystalline polyester) Crystalline polyester is a crystalline polyester obtained by a polymerization reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol). Crystalline polyester can be produced by esterifying a polyvalent carboxylic acid and a polyalcohol through polycondensation using a known esterification catalyst.
[0072] [Polycarboxylic acid] Examples of divalent polycarboxylic acids that can be used in the synthesis of crystalline polyesters include saturated aliphatic dicarboxylic acids, unsaturated aliphatic dicarboxylic acids, and unsaturated aromatic dicarboxylic acids. Examples of saturated aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Examples of unsaturated aliphatic dicarboxylic acids include methylenesuccinic acid, fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid. Examples of unsaturated aromatic dicarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylene diacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, anthracene dicarboxylic acid, etc. Lower alkyl esters and acid anhydrides of these dicarboxylic acids can also be used as polyvalent carboxylic acids.
[0073] Examples of trivalent or higher polyvalent carboxylic acids that can be used in the synthesis of crystalline polyester include trimellitic acid and pyromellitic acid.
[0074] [Polyhydric alcohol] Examples of dihydric polyhydric alcohols that can be used in the synthesis of the crystalline polyester include saturated aliphatic diols, unsaturated aliphatic diols, and aromatic diols.
[0075] Examples of saturated aliphatic diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentyl glycol.
[0076] Examples of the unsaturated aliphatic diol include 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, 9-octadecene-7,12-diol, and the like.
[0077] Examples of aromatic diols include bisphenols and alkylene oxide adducts of bisphenols. Examples of bisphenols include bisphenol A and bisphenol F. Examples of alkylene oxide adducts of bisphenols include ethylene oxide adducts of bisphenols and propylene oxide adducts of bisphenols. Derivatives of these diols can also be used as polyhydric alcohols.
[0078] The crystalline polyester according to the present invention is preferably a polycondensate of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms, from the viewpoints of improving the low-temperature fixing property and improving the rise of the charge amount while ensuring the heat-resistant storage stability of the toner.
[0079] Also, when the structural unit of the crystalline polyester is an ester, it is preferable that the number of carbon atoms, including the ester moiety, is 6 to 14, from the viewpoints of ensuring the heat-resistant storage stability of the toner, improving the low-temperature fixability, and improving the rise of the charge amount.
[0080] The smaller the carbon number of the acid and alcohol constituting the crystalline polyester, the easier it is for the toner particles containing the resin to melt, and the better the low-temperature fixability becomes. On the other hand, if the toner particles melt too easily, their heat resistance decreases, and they may aggregate when stored in a heated state, for example, in a developing device.
[0081] Therefore, by making the number of carbon atoms of both the acid and alcohol constituting the crystalline polyester to be 6 to 14, it is possible to improve the low-temperature fixability while ensuring the heat-resistant storage property of the toner.
[0082] In addition, when the carbon number of the acid and alcohol constituting the crystalline polyester is increased, the polarity of the crystalline polyester is decreased, and the crystalline polyester is less compatible with other resins. Therefore, when the carbon number of the acid and alcohol constituting the crystalline polyester is increased, the domain of the crystalline polyester in the binder resin is increased. On the other hand, when the carbon number of the acid and alcohol constituting the crystalline polyester is decreased, the polarity of the crystalline polyester is increased, and the crystalline polyester is more easily compatible with other resins. Therefore, when the carbon number of the acid and alcohol constituting the crystalline polyester is decreased, the crystalline polyester is more finely dispersed in the binder resin.
[0083] When the dispersion state of the crystalline polyester is appropriate, the distance between the domains of the crystalline polyester becomes short. This reduces the resistance to charge transfer in the toner particles, making it easier for the charge amount to rise. Therefore, from the viewpoint of the dispersion state that makes the charge amount rise well, it is preferable that the carbon numbers of the acid and alcohol constituting the crystalline polyester are both within the range of 6 to 14.
[0084] For the synthesis of the crystalline polyester, the above-mentioned catalysts that can be used for the synthesis of the amorphous polyester can be used.
[0085] The polymerization temperature is not particularly limited, but is preferably within the range of 70 to 250° C. The polymerization time is not particularly limited, but is preferably within the range of 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.
[0086] The crystalline polyester may be a hybrid crystalline polyester having a graft copolymer structure of a crystalline polyester polymerized segment and a styrene-acrylic polymerized segment.
[0087] The weight average molecular weight Mw of the crystalline polyester is preferably within the range of 1000 to 29000. The weight average molecular weight Mw can be measured by gel permeation chromatography (GPC).
[0088] The content of the crystalline polyester is preferably within a range of 5 to 30% by mass, and more preferably within a range of 10 to 20% by mass, based on the total amount of the resin contained in the toner base particles.
[0089] (1.1.3) Vinyl resins The toner particles according to the present invention may contain a vinyl resin. The vinyl resin is a polymer of a monomer having a vinyl group (hereinafter referred to as a vinyl monomer) that exhibits amorphous nature. Examples of the vinyl resin that can be used include styrene-acrylic resin, styrene resin, acrylic resin, etc., and among them, styrene-acrylic resin that has excellent heat resistance is preferable. Examples of the vinyl monomer that can be used include the following, and one of these can be used alone or two or more can be used in combination.
[0090] (1) Styrene-based monomers Monomers having a styrene structure, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, and derivatives thereof (2) (Meth)acrylic acid ester monomers Monomers having a (meth)acrylic group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and derivatives thereof. (3) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (4) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (5) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (6) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (7)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid derivatives such as acrylonitrile, methacrylonitrile, and acrylamide, and methacrylic acid derivatives, etc.
[0091] As the vinyl monomer, a monomer having an ionically dissociable group such as a carboxy group, a sulfonic acid group, or a phosphoric acid group is preferred because it makes it easier to control the affinity with the crystalline resin.
[0092] Examples of monomers having a carboxy group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.
[0093] Examples of the monomer having a sulfonic acid group include styrenesulfonic acid, allylsulfosuccinic acid, and 2-acrylamido-2-methylpropanesulfonic acid.
[0094] An example of a monomer having a phosphoric acid group is acidophosphooxyethyl methacrylate.
[0095] A polymer having a crosslinked structure can be obtained by using a polyfunctional vinyl as the vinyl monomer. Examples of the polyfunctional vinyl include divinylbenzene, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, neopentyl glycol dimethacrylate, and neopentyl glycol diacrylate.
[0096] (1.1.4) Release agents The toner particles according to the present invention preferably contain a release agent. The release agent is not particularly limited, and various known waxes can be used.
[0097] Examples of the release agent that can be used include branched chain hydrocarbon waxes, long chain hydrocarbon waxes, dialkyl ketone waxes, ester waxes, amide waxes, etc. Examples of the branched chain hydrocarbon waxes include polyolefin waxes such as polyethylene wax and polypropylene wax, and microcrystalline waxes. Examples of the long chain hydrocarbon waxes include paraffin wax and sazol wax. Examples of the dialkyl ketone waxes include distearyl ketone. Examples of the ester waxes include carnauba wax, montan wax, behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, tristearyl trimellitate, distearyl maleate, and stearyl stearate. Examples of amide waxes include ethylenediamine behenylamide and trimellitic acid tristearylamide.
[0098] Examples of commercially available release agents include HNP-0190, HNP-51, and FNP-0090 manufactured by Nippon Seiro Co., Ltd., and C80 manufactured by Sasol Co., Ltd. These release agents may be used alone or in combination of two or more.
[0099] The content of the release agent can be usually within a range of 1 to 30% by mass, and preferably within a range of 5 to 20% by mass, based on the total amount of the resin contained in the toner base particles. By keeping the content of the release agent within the above range, sufficient fixing separation property can be obtained.
[0100] (Melting point of release agent) It is preferable that the toner particles contain a release agent having a melting point in the range of 70 to 91°C from the viewpoints of separability from the fixing member, low-temperature fixability, and heat-resistant storage stability of the toner particles. By having a melting point (Tm) of 91°C or less, the release agent is easily exuded from the toner particles during fixing, and the amount of the release agent on the surface of the image increases. This improves the separability from the fixing member and the low-temperature fixability. In addition, by having a melting point (Tm) of 70°C or more, the release agent is less likely to be arranged on the surface of the toner particles during production due to the difference in viscosity with the binder resin, and the heat-resistant storage stability of the toner particles is improved.
[0101] The melting point (Tm) of the release agent is determined by differential scanning calorimetry (DSC), for example, by the following procedure. A differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI) are used. 0.5 mg of the measurement sample is placed in an AI autosampler sample container φ6.8 H2.5mm (manufactured by HITACHI). This is sealed using an AI autosampler cover (manufactured by HITACHI). This is set in the sample holder of the "AS3 / DX".
[0102] The measurement conditions are: measurement temperature 0-200°C, temperature rise rate 10°C / min, temperature fall rate 10°C / min. Heat-cool-Heat temperature control is performed, and the data from the 1st Heat is analyzed. An empty aluminum pan is used for the reference measurement.
[0103] The peak top temperature of the endothermic peak derived from the crystalline resin in the 1st heat is taken as the melting point (Tm). If multiple endothermic peaks are detected, the peak top temperature of the highest endothermic peak is taken as the melting point (Tm) of the release agent.
[0104] (1.1.5) Colorants The toner particles according to the present invention may contain a colorant. A known inorganic or organic colorant may be used as the colorant. Carbon black, magnetic powder, organic pigment, inorganic pigment, dye, etc. may be used as the colorant. The content of the colorant is preferably 1 to 30% by mass, more preferably 2 to 20% by mass, based on the toner particles.
[0105] (1.1.6) Charge control agents The toner particles according to the present invention may contain a charge control agent. As the charge control agent, known compounds such as nigrosine dyes, metal salts of naphthenic acid, metal salts of higher fatty acids, alkoxylated amines, quaternary ammonium salts, azo metal complexes, and metal salicylic acid salts can be used. By using the charge control agent, a toner with excellent charging properties can be obtained. The content of the charge control agent can be usually within a range of 0.1 to 5.0% by mass based on the total amount of resin contained in the toner base particles.
[0106] (1.1.7) External additives The toner particles according to the present invention preferably contain an external additive. Examples of the external additive include inorganic oxide fine particles, inorganic stearic acid compound fine particles, inorganic titanic acid compound fine particles, zirconia particles, etc. The external additives may be used alone or in combination of two or more kinds.
[0107] Examples of inorganic oxide particles include silica particles, alumina particles, titanium oxide particles, zinc oxide particles, chromium oxide particles, cerium oxide particles, antimony oxide particles, tungsten oxide particles, tin oxide particles, tellurium oxide particles, manganese oxide particles, boron oxide particles, etc. Examples of inorganic stearic acid compound particles include aluminum stearate particles and zinc stearate particles, etc. Examples of inorganic titanic acid compound particles include strontium titanate and zinc titanate, etc.
[0108] The amount of the external additive is preferably in the range of 0.05 to 5% by mass, more preferably in the range of 0.1 to 3% by mass, based on the total amount of the toner base particles. When a plurality of external additives are used, the amount is the total amount. Among the above, the toner particles according to the present invention preferably have silica particles or strontium titanate particles as the external additive.
[0109] (Silica particles) Silica particles are particles mainly composed of silica (SiO2). Silica particles may be either crystalline or amorphous. Silica particles may be particles manufactured using silicon compounds such as water glass and alkoxysilane as raw materials, or may be particles obtained by crushing quartz.
[0110] The silica particles may be, for example, sol-gel silica particles, aqueous colloidal silica particles, alcoholic silica particles, fumed silica particles obtained by a gas phase method, fused silica particles, etc. Among the above, the silica particles are preferably sol-gel silica particles.
[0111] Sol-gel silica particles can be obtained, for example, as follows: Tetraalkoxysilane (TMOS, etc.) is dropped into an alkaline catalyst solution containing an alcohol compound and aqueous ammonia, and the tetraalkoxysilane is hydrolyzed and condensed to obtain a suspension containing sol-gel silica particles. The solvent is then removed from the suspension to obtain a granular material. The granular material is then dried to obtain the sol-gel silica particles.
[0112] The silica particles may be silica particles that have been hydrophobized with a hydrophobizing agent. Examples of the hydrophobizing agent include known organosilicon compounds having an alkyl group (e.g., a methyl group, an ethyl group, a propyl group, a butyl group, etc.). Specific examples of the hydrophobizing agent include an alkoxysilane compound, a siloxane compound, a silazane compound, etc. Among the above, the hydrophobizing agent is preferably at least one of a siloxane compound and a silazane compound. Examples of the siloxane compound include silicone oil, silicone resin, etc. The silicone oil is preferably dimethyl silicone oil. Examples of the silazane compound include hexamethyldisilazane, tetramethyldisilazane, etc. The silazane compound is preferably hexamethyldisilazane (HMDS). The hydrophobizing agent may be used alone or in combination of two or more.
[0113] The amount of the hydrophobizing agent such as a silazane compound attached to the surface of the silica particles is preferably within a range of 0.01 to 5 mass %, more preferably within a range of 0.05 to 3 mass %, and even more preferably within a range of 0.10 to 2 mass %, based on the silica particles, from the viewpoint of improving the hydrophobization degree of the silica particles.
[0114] Examples of the method for subjecting silica particles to a hydrophobic treatment using a hydrophobic treatment agent include the following methods. [1] A method in which a hydrophobic treatment agent is dissolved in supercritical carbon dioxide and applied to the surface of silica particles. [2] A method in which a solution containing a hydrophobizing agent is applied (for example, sprayed or coated) to the surface of silica particles in the air. [3] A method in which a solution containing a hydrophobizing agent is added to a silica particle dispersion liquid and maintained in the atmosphere, and then the mixed liquid is dried.
[0115] From the viewpoint of heat-resistant storage stability, it is preferable that the number-average particle diameter of the silica particles is within the range of 90 to 130 nm. When the number-average particle diameter is 90 nm or more, the silica particles are more likely to exhibit a spacer effect with other toner particles. As a result, even when the toner base particles have high melting properties, the toner particles are less likely to aggregate together, improving the heat-resistant storage stability. When the number-average particle diameter is 130 nm or less, the silica particles are less likely to detach from the toner base particles, and deterioration of the heat-resistant storage stability due to exposure of the toner base particles can be suppressed.
[0116] The number average particle size of the silica particles can be determined by the following procedure. (1) Toner particles are dispersed in methanol, stirred at room temperature (23°C), and then treated in an ultrasonic bath to separate the external additives from the toner base particles. The toner base particles are allowed to settle by centrifugation, and the dispersion liquid in which the external additives are dispersed is recovered. Methanol is distilled off from the dispersion liquid, and the external additives are extracted. (2) The extracted external additive is dispersed in resin particles (polyester, weight average molecular weight Mw=50,000) having a volume average particle diameter of 100 μm. (3) The resin particles with the dispersed external additives were analyzed using an energy dispersive X-ray analyzer (EDX device, manufactured by Horiba, Ltd., EMAX Evolution X-Max 80 mm) 2 Images are taken at a magnification of 40,000 times using a scanning electron microscope (SEM, Hitachi High-Technologies Corporation, S-4800) equipped with a 40000 times magnification. At this time, more than 300 primary silica particles are identified within one field of view based on the presence of Si by EDX analysis. SEM observation is performed with an acceleration voltage of 15 kV, an emission current of 20 μA, and a WD of 15 mm. EDX analysis is performed under the same conditions with a detection time of 60 minutes. (4) The obtained images are imported into an image analyzer (LUZEXIII, manufactured by Nireco Corporation). The area of each particle is determined by analyzing the imported images. (5) From the measured area value, the particle diameter of the silica particles is calculated as the equivalent circle diameter. (6) Select 100 silica particles having an equivalent circle diameter of 80 nm or more. (7) The number average particle size is calculated from the particle sizes of the selected silica particles.
[0117] (Strontium titanate particles) Strontium titanate particles are particles whose main component is strontium titanate (SrTiO3). Strontium titanate particles are positively charged. Therefore, by using strontium titanate particles as an external additive, the strontium titanate particles promote the negative charging of the toner base particles, thereby suppressing fogging.
[0118] The number-average primary particle diameter of the strontium titanate particles is preferably within a range of 30 to 100 nm, more preferably within a range of 30 to 80 nm, and even more preferably within a range of 30 to 60 nm. When the number-average primary particle diameter of the strontium titanate particles is 30 nm or more, embedding of the strontium titanate particles in the toner base particles is suppressed. When the number-average primary particle diameter of the strontium titanate particles is 100 nm or less, the surface coverage of the toner base particles is easily increased.
[0119] The number-average primary particle size of the strontium titanate particles can be measured in the same manner as the number-average primary particle size of the silica particles described above. In the EDX analysis, 300 or more primary particles of strontium titanate are identified in one field of view based on the presence of Ti and Sr.
[0120] The strontium titanate particles preferably have a rounded shape. For example, the average circularity of the strontium titanate particles is preferably within the range of 0.82 to 0.94, more preferably within the range of 0.84 to 0.94, and even more preferably within the range of 0.86 to 0.92. When the strontium titanate particles have an average circularity of 0.82 or more, the dispersibility in the toner base particles is easily improved. When the strontium titanate particles have an average circularity of 0.94 or less, the mobility on the surface of the toner base particles is reduced, and the uniform dispersibility on the surface is easily improved.
[0121] (1.1.8) Toner manufacturing method The toner can be produced by producing toner base particles and adding external additives thereto as necessary. Examples of methods for producing toner base particles include a kneading and grinding method, a suspension polymerization method, an emulsion aggregation method, a dissolution suspension method, a polyester elongation method, and a dispersion polymerization method. Among these, the emulsion aggregation method is preferred from the viewpoints of uniformity of particle size, which is advantageous for high image quality and high stability, controllability of shape, and ease of forming a core-shell structure.
[0122] The emulsion aggregation method is carried out, for example, by the following procedure. A dispersion liquid in which resin particles are dispersed with a surfactant or a dispersion stabilizer is mixed with a dispersion liquid of colorant particles, etc. An aggregating agent is added to this system, and the particles are aggregated until the desired particle size is reached. Thereafter, or simultaneously with the aggregation, the resin particles are fused together, and the shape is controlled to produce toner base particles.
[0123] The resin particles may contain internal additives such as a release agent, a charge control agent, etc. The resin particles may be composite particles formed of two or more layers composed of resins with different compositions.
[0124] From the viewpoint of toner structure design, it is also preferable to add different types of resin particles during aggregation to form toner base particles having a core-shell structure.
[0125] The resin particles can be produced, for example, by emulsion polymerization, mini-emulsion polymerization, phase inversion emulsification, etc. When an internal additive is contained in the resin particles, the resin particles are preferably produced by mini-emulsion polymerization.
[0126] In the drying process of the toner base particles, the drying conditions are adjusted as necessary to make the moisture content of the toner particles as described above. For example, the drying conditions are adjusted so that the toner base particles are not overdried, in other words, so that a certain amount of moisture remains in the toner base particles.
[0127] The method for drying the toner base particles is not particularly limited, but from the viewpoint of productivity, freeze drying, flash jet drying, vibration type fluidized drying, etc. are preferred. Among these, flash jet drying is more preferred. Examples of conditions for preventing the toner base particles from being overdried during flash jet drying include the following methods. [1] Increase the temperature of the gas being blown in (inlet temperature). [2] Lower the temperature of the exhaust gas (outlet temperature). [3] Lower the temperature of both the incoming and outgoing gases without changing the temperature difference between them. [4] Increase the airflow volume.
[0128] A suitable example of a method for adding an external additive to a toner base particle is a dry method in which the external additive is added in powder form to a dried toner base particle. Examples of a mixing device include a mechanical mixing device such as a Henschel mixer or a coffee mill.
[0129] (1.1.9) Developer The toner according to the present invention may be used alone as a magnetic or non-magnetic one-component developer, or may be mixed with carrier particles to be used as a two-component developer. As the carrier particles, for example, magnetic particles made of a conventionally known material may be used. Examples of magnetic particles include metals such as iron, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead. As the carrier particles, ferrite particles are particularly preferred.
[0130] As the carrier particles, coated carrier particles in which the surfaces of magnetic particles are coated with a coating agent such as resin, or dispersed carrier particles in which magnetic fine powder is dispersed in a binder resin may be used. From the viewpoint of suppressing adhesion of the carrier particles to the photoreceptor, coated carrier particles are preferred.
[0131] The volume-based median diameter of the carrier particles is preferably within a range of 20 to 100 μm, and more preferably within a range of 25 to 80 μm. The volume-based median diameter of the carrier particles can be measured, for example, by a laser diffraction particle size distribution measuring device (HELOS, SYMPATEC) equipped with a wet disperser.
[0132] The carrier particles may be mixed in an appropriate amount with the toner particles. Examples of the mixing device used for the mixing include a Nauta mixer, a W-type mixer, a V-type mixer, and the like.
[0133] (1.2) Developing sleeve The developing sleeve according to the present invention has a role of transporting a developer containing a toner and a carrier. The developing sleeve is characterized by having an aluminum alloy containing more than 0.6% by mass of silicon. The developing sleeve is provided on a developing roller.
[0134] The "developing sleeve" according to the present invention is a means having a function of carrying a moderately charged developer and supplying the developer to a photoconductor on which an electrostatic image is formed, and is, for example, a part of a developing roller of a developing device provided in an electrophotographic image forming apparatus, and the developing roller is composed of a developing sleeve, a flange, a shaft, and a magnet roller. However, a developing roller having the "developing sleeve" according to the present invention as a part of its configuration does not have to include a magnet portion such as a magnet roller as a part of its configuration.
[0135] According to the present invention, even if a member that generates a magnetic flux, such as the above-mentioned magnet roller, is provided inside the developing sleeve, heat generation on the developing sleeve can be suppressed.
[0136] Aluminum alloy is a conductive material with a relatively small electrical resistance, and when the developing sleeve is rotated relative to the magnet roller, the developing sleeve crosses the magnetic field lines generated by the magnet roller. This causes electromagnetic induction, which generates heat due to eddy currents around the surface of the developing sleeve. When the current density of the eddy current is high, the heat generated increases, causing the toner and carrier to thermally fuse and begin to aggregate, which causes image defects such as black spots.
[0137] In particular, due to the recent demand for faster printing speeds and more compact machines, the developing sleeve is required to have a small diameter. In addition, the developing sleeve is required to rotate at high speed while maintaining a high magnetic flux density. This further increases the heat generated by the developing sleeve due to eddy currents. This makes image defects such as black spots more noticeable.
[0138] In the present invention, the aluminum alloy of the developing sleeve contains more than 0.6% by mass of silicon, so that the surface resistance of the developing sleeve is increased. In addition, since silicon has almost the same chargeability as aluminum, it does not interfere with the chargeability between the toner carrier. Therefore, appropriate chargeability can be maintained during image formation. As a result, even if the developing sleeve has a member that generates magnetic flux inside, the generation of eddy currents can be suppressed, and heat generation can be suppressed. Therefore, it is presumed that the occurrence of image defects such as black spots can be suppressed even if the content of structural units derived from bisphenol A derivatives in the amorphous polyester contained in the toner particles contained in the electrostatic image developing toner used during image formation is low.
[0139] Fig. 1 is an external view of a developing roller equipped with a developing sleeve. The developing sleeve is rotatable and cylindrical, and plays a role in carrying and transporting a developer on its surface. As shown in Fig. 1, a plurality of grooves 20 extending in the axial direction of the developing roller 10 are formed at predetermined intervals in the circumferential direction on the surface of the developing sleeve 11. Note that the surface of the developing sleeve according to the present invention may be configured without the above-mentioned grooves.
[0140] 2 and 3 are examples of the developing sleeve according to the present invention, each of which is an axial cross-sectional view of a developing roller having a magnet roller and a shaft configuration with different shapes. However, a developing roller having the developing sleeve according to the present invention as part of its configuration does not need to include a magnet portion as part of its configuration, such as a magnet roller, and is not limited to the configurations shown in FIGS. 2 and 3.
[0141] 2 is a cross-sectional view of a developing roller in which the shaft does not pass through the magnet roller. As shown in Fig. 2, the developing roller 10 has a shaft 16 fixed by inserting the shaft into a hole formed in the magnet roller 12, and is provided with a developing sleeve 11 made of a non-magnetic material on the outer periphery of the magnet roller 12.
[0142] 3 is a cross-sectional view of a developing roller in which the shaft passes through the magnet roller. As shown in FIG. 3, the developing roller 10 has a magnet roller 12 fixed around the periphery of a shaft 16, and a developing sleeve 11 made of a non-magnetic material attached to the outer periphery of the magnet roller 12.
[0143] The developing sleeve 11 is connected to the magnet roller 12 with a predetermined gap therebetween via a bearing portion 17 such as a bearing provided on the outside of the magnet roller 12. A non-driving side flange 18 and a driving side flange 19 are connected to the developing sleeve 11 on the outside of the axial bearing portion 17 of the developing sleeve 11. Note that the non-driving side flange 18 and the driving side flange 19 may be reversed, and are not limited to this. The non-driving side flange 18 and the driving side flange 19 are rotated together with the developing sleeve 11 while being held relative to the developing container.
[0144] (1.2.1) Silicon content in aluminum alloys From the viewpoint of suppressing heat generation on the developing sleeve, the silicon content is preferably more than 0.8% by mass, more preferably 1.4% by mass or more. In addition, if the silicon content is too high, the unevenness of the developing sleeve surface increases, and charge leakage is likely to occur, so the silicon content is preferably 4.4% by mass or less.
[0145] The aluminum alloy of the developing sleeve according to the present invention does not include the materials constituting the flange, shaft and magnet roller (see FIGS. 1, 2 and 3).
[0146] (1.2.2) Surface condition of developing sleeve The developing sleeve according to the present invention has a role of transporting a developer containing a toner and a carrier, and therefore, by imparting an appropriate surface roughness to the surface of the developing sleeve, the transportability of the developer is improved and maintained.
[0147] Although there is no particular limitation on the method for imparting an appropriate roughness to the surface of the developing sleeve according to the present invention, it is preferable that the surface of the developing sleeve is subjected to sandblasting in terms of improving the transportability of the developer. By performing sandblasting, unevenness is formed on the surface of the developing sleeve, thereby maintaining the appropriate roughness of the outer peripheral surface and ensuring excellent transportability.
[0148] When silicon is contained, the silicon is removed differently on the surface of the developing sleeve during sandblasting in the areas containing silicon and the areas not containing silicon, so that an appropriate surface roughness can be imparted.
[0149] Sandblasting is a process in which a blasting material is projected onto the surface of a developing sleeve to indent the surface with the blasting material, thereby forming an uneven shape. More specifically, examples of sandblasting include air blasting, wet sandblasting, and shot blasting.
[0150] There are no particular limitations on the materials that can be used for sandblasting, and any known materials can be used as appropriate.Specific examples include glass beads, alumina particles, silica particles, titania particles, and zirconia particles.Organic fine particles can also be used, such as melamine resin particles, benzoguanamine resin particles, and crosslinked acrylic resin particles.
[0151] As materials applicable to sandblasting, from the viewpoint of applying an impact force that dents the elastic layer but does not tear the surface of the outer layer, spherical glass beads and alumina beads are particularly preferable. These materials may be used alone or in combination of two or more.
[0152] The volume average particle size of the above material varies depending on the size of the irregularities on the surface of the desired developing sleeve, but is preferably within the range of 3 to 200 μm, more preferably within the range of 10 to 100 μm, and even more preferably within the range of 20 to 80 μm.
[0153] From the viewpoint of improving the transportability of the developer, it is preferable that the surface of the developing sleeve according to the present invention has a groove. Fig. 4 is a partially enlarged view of a cross section of the developing sleeve. The groove 20 is a V-shaped groove formed by an upstream wall surface 21 located on the upstream side with respect to the rotation direction X of the developing sleeve 11 and a downstream wall surface 22 located on the downstream side. The cross-sectional shape of the developing sleeve according to the present invention is not limited to a V-shaped groove shape such as the groove 20 shown in Fig. 4, and may be a flat-bottom shape or an arc shape.
[0154] The developing sleeve 11 having the grooves 20 formed on its surface in this way has excellent wear resistance and excellent developer transportability when the developer is supported on the surface. For example, by forming a plurality of grooves extending in the axial direction of the developing sleeve at predetermined intervals in the circumferential direction, the durability of the developing sleeve during long-term use is improved and the developer transportability is also improved.
[0155] The depth D of the groove is preferably within a range of 40 to 120 μm from the viewpoint of excellent transportability. The depth D of the groove can be calculated by photographing the groove using a laser microscope (model: VKX-200) manufactured by Keyence Corporation.
[0156] The apex angle α of the groove is preferably 80° or more from the viewpoint of suppressing deterioration of transportability due to clogging of the developer, and is preferably 120° or less from the viewpoint of improving transportability of the developer.
[0157] The number of grooves in the circumferential direction of the developing sleeve is preferably within a range of 40 to 120.
[0158] The groove angle β in FIG. 4 is 9° when the number of grooves is 40, and is 3° when the number of grooves is 120.
[0159] In addition, the groove angle β in FIG. 4 is calculated by drawing a perpendicular line from a direction perpendicular to the surface of the developing sleeve to a specific vertex (vertex A) of the groove, and then measuring the line L. A Draw a perpendicular line from the direction perpendicular to the surface of the developing sleeve to the vertex (vertex B) adjacent to the specific vertex A of the groove, and define the straight line as L. B Then, the line is L A and the line L B The groove angle is less than 90°.
[0160] 2. Image forming method The image forming method according to the present invention is an image forming method using a toner for developing electrostatic images and a developing sleeve that transports the toner for developing electrostatic images, the toner particles contained in the toner for developing electrostatic images contain an amorphous polyester that is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less relative to all structural units derived from the polyhydric alcohol, and the developing sleeve has an aluminum alloy containing more than 0.6 mass % silicon, and can be suitably used in the image forming system of the present invention.
[0161] 3. Electrophotographic Image Forming Apparatus An electrophotographic image forming apparatus that can be used in the image forming system and image forming method of the present invention includes, for example, a charging unit, an exposure unit, a developing unit, and a transfer unit.
[0162] 5 is an explanatory cross-sectional view showing an example of the configuration of an electrophotographic image forming apparatus. The image forming apparatus 100 shown in FIG. 5 is called a tandem type color image forming apparatus, and has four image forming units 110Y, 110M, 110C, and 110Bk, a paper feed conveying means 150, and a fixing means 170.
[0163] An original image reading device SC is disposed on the upper portion of the main body of the image forming apparatus 100.
[0164] The image forming units 110Y, 110M, 110C, and 110Bk are arranged in a vertical line. The image forming units 110Y, 110M, 110C, and 110Bk each include a rotating drum-shaped photoconductor 111Y, 111M, 111C, and 111Bk, charging means 113Y, 113M, 113C, and 113Bk, exposure means 115Y, 115M, 115C, and 115Bk, developing means 117Y, 117M, 117C, and 117Bk, primary transfer rollers (primary transfer means) 133Y, 133M, 133C, and 133Bk, and cleaning means 119Y, 119M, 119C, and 119Bk, which are arranged in sequence along the rotation direction of the photoconductor in the outer circumferential surface area of the drum-shaped photoconductor 111Y, 111M, 111C, and 111Bk.
[0165] A configuration is adopted in which toner images of yellow (Y), magenta (M), cyan (C) and black (Bk) are formed on the photoconductors 111Y, 111M, 111C and 111Bk, respectively.
[0166] In the following description, the image forming unit 110Y will be taken as an example when referring to the drawings.
[0167] <Charging means> The charging means is a means for uniformly charging the surface of the photoreceptor. The charging means may be of a contact type such as a charging roller, a charging brush, or a charging blade, or of a non-contact type such as a corona charger (such as a corotron charger or a strocotton charger). The charging means provided in the image forming apparatus may be of either a contact type or a non-contact type. The contact type has the advantage that the amount of harmful ozone gas generated during the charging process is small. The non-contact type has the advantage that filming is less likely to occur because it is not a close-proximity discharge, as compared to the contact type.
[0168] It is preferable that the charging means is a proximity charging roller or a contact charging roller, since this reduces the amount of harmful ozone gas generated during the charging process and is advantageous for achieving high image quality and miniaturization of the apparatus.
[0169] 5 is of a contact type. The charging unit 113Y in this example is made up of a charging roller disposed in contact with the surface of the photoconductor 111Y, and a power source that applies a voltage to the charging roller.
[0170] <Exposure means> The exposure means is a means for exposing the photoconductor, which has been given a uniform potential by the charging means, based on an image signal to form an electrostatic latent image corresponding to the image. Examples of the exposure means include those consisting of LEDs and imaging elements in which light emitting elements are arranged in an array in the axial direction of the photoconductor, and those consisting of a laser optical system.
[0171] <Developing method> The developing means (developing machine) is a means for supplying a developer to the surface of the photoconductor to develop the electrostatic latent image formed on the surface of the photoconductor to form a toner image. Note that as the developer, a developer containing the above-mentioned toner and carrier is used.
[0172] The developing means may be provided with a lubricant supplying means for supplying a lubricant to the developer, and it is preferable that the developer supplied by the developing means contains a lubricant from the viewpoint of improving abrasion resistance. It is more preferable that the lubricant is a metal soap from the viewpoint of improving abrasion resistance.
[0173] The developing means 117Y shown in FIG. 5 is specifically composed of a developing roller 118Y that has a built-in magnet and rotates while holding a developer, and a voltage application device (not shown) that applies a DC and / or AC bias voltage between the photoconductor 111Y and the developing roller 118Y.
[0174] The developing roller is composed of the developing sleeve, the flange, the shaft, and the magnet roller as described above. The aluminum alloy of the developing roller has a silicon content of more than 0.6 mass %.
[0175] The developer is transported to the photoconductor 111Y by the rotation of the developing roller 118Y. Then, a thin layer of toner on the developing roller 118Y comes into contact with the photoconductor 111Y to develop the electrostatic latent image on the photoconductor 111Y.
[0176] The developing roller 118Y is connected to a voltage application device. This voltage application device applies a DC and / or AC bias voltage to the developing roller 118Y. The developing bias can be adjusted to a desired value by controlling the voltage applied to the developing roller 118Y.
[0177] Due to a potential difference (development potential difference) between the potential of the electrostatic latent image carried by the developing roller 118Y and the photoconductor 111Y, an electric field is formed in a developing section where the developing roller 118Y and the photoconductor 111Y face each other.
[0178] The toner in the developer transported to the developing section by the rotation of the developing roller 118Y moves due to the force exerted by the electric field, and is attracted to the electrostatic latent image on the photoconductor 111Y.
[0179] The electrostatic latent image carried on the photoconductor 111Y is visualized, so that a toner image corresponding to the shape of the electrostatic latent image is formed on the surface of the photoconductor 111Y.
[0180] <Transfer Method> The transfer means is a means for transferring the toner image on the photoreceptor to a transfer body (intermediate transfer body or transfer material). When an intermediate transfer body is used, the primary transfer roller becomes the transfer means. Since the "transfer means" in the present invention is a means for transferring the "toner image on the photoreceptor", the secondary transfer roller used when transferring from the intermediate transfer body to the transfer material is not included in the "transfer means".
[0181] 5 transfers the toner image formed on the photoconductor 111Y onto the endless belt-like intermediate transfer body 131. The primary transfer roller 133Y is disposed in contact with the intermediate transfer body 131.
[0182] In the image forming apparatus 100 shown in FIG. 5, an intermediate transfer method is adopted in which the toner images formed on the photoconductors 111Y, 111M, 111C, and 111Bk are transferred to the intermediate transfer body 131 by primary transfer rollers (primary transfer means) 133Y, 133M, 133C, and 133Bk, and each toner image transferred to the intermediate transfer body 131 is transferred to the transfer material P by a secondary transfer roller (secondary transfer means) 217, but a direct transfer method may also be adopted in which the toner images formed on the photoconductors are transferred directly to the transfer material P by a transfer means. EXAMPLES
[0183] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.
[0184] A. Preparation of developing sleeve 1 (A.1) Preparation of hollow cylindrical tube made of aluminum alloy The aluminum alloy containing silicon (Si) was used to prepare a hollow cylindrical tube, in which the content of silicon (Si) was 0.7 mass % relative to the total mass of the aluminum alloy.
[0185] (A.2) Groove formation The developing sleeve 1 was produced by forming V-groove surface shapes at equal intervals in the circumferential direction on the hollow cylindrical tube, and spraying glass beads with a blast gun to sandblast the outer peripheral surface of the cylinder. As shown in FIG. 4, for example, the V-groove has a groove depth D of 75±25 μm, a V-groove apex angle α of 100°, 40 grooves in the circumferential direction of the developing sleeve, and a groove angle β of 9°. The developing sleeve 1 had an outer diameter of 16 mm and a thickness of 1 mm. The processing conditions for the sandblasting treatment were as follows:
[0186] <Processing conditions> Glass bead type: FGB#80 (manufactured by Fuji Manufacturing) Glass beads feed rate: 200g / min Distance from blast gun to cylinder: 100mm Blast gun movement speed: 5.0cm / sec Compressed air pressure: 0.23MPa Cylinder rotation speed: 545 rpm
[0187] The surface of the developing sleeve 1 was photographed with a laser microscope (model: VKX-200) manufactured by Keyence Corporation, and the depth D of the grooves in the circumferential direction of the support was measured. Specifically, 12 points in total, 3 points in the axial direction of the support and 4 points in the circumferential direction, were photographed at 500x magnification. The photographed images were binarized using image analysis software, and the depth D of all linear grooves on the image was calculated. The range of the depth D of linear grooves that accounted for 90% or more of the total was calculated from the calculated linear groove depths, and was found to be 100 μm.
[0188] B. Preparation of developing sleeves 2 to 7 (B.1) Preparation of aluminum alloy and fabrication of hollow cylindrical tube The hollow cylindrical tube was produced using an aluminum alloy containing silicon (Si) as shown in Table I. The developing sleeve 7 contained 0.7 mass % of lithium (Li).
[0189] (B.2) Groove formation Grooves were formed in the hollow cylindrical tube at equal intervals in the circumferential direction to form a V-groove surface shape. For example, as shown in Fig. 4, the V-groove was formed with a groove depth D of 75±25μm, a V-groove apex angle α of 100°, 40 grooves in the circumferential direction of the developing sleeve, and a groove angle β of 9°, similar to that of the developing sleeve 1.
[0190] The developing sleeves 2 to 19 all had an outer diameter of 16 mm and a thickness of 1 mm.
[0191] [Table 1]
[0192] C. Preparation of amorphous polyester particle dispersion (C.1) Amorphous polyester particle dispersion (AP1) (C.1.1) Synthesis of amorphous polyester The following amorphous polyester monomers were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and were heated to 170° C. to dissolve.
[0193] <Polyhydric alcohol> Ethylene glycol 50 parts by mole Neopentyl glycol 50 parts by mole
[0194] <Polycarboxylic acid> Terephthalic acid 55 parts by mole Fumaric acid 5 mole parts Dodecenyl succinic acid 40 mole parts
[0195] The mixture in the dropping funnel was dropped into a four-neck flask over 90 minutes under stirring, and after aging for 60 minutes, the unreacted monomer was removed under reduced pressure (8 kPa). Then, Ti(OBu)4 was added as an esterification catalyst at 0.003 mass% based on the total amount of polyvalent carboxylic acid components, and the mixture was heated to 235°C and reacted under normal pressure (101.3 kPa) for 5 hours. The mixture was further reacted under reduced pressure (8 kPa) for 1 hour. The mixture was then cooled to 200°C and reacted under reduced pressure (20 kPa), after which the solvent was removed to synthesize amorphous polyester [a1].
[0196] (C.1.2) Preparation of amorphous polyester particle dispersion 108 parts by mass of the synthesized amorphous polyester [a1] was dissolved in 64 parts by mass of methyl ethyl ketone by stirring for 30 minutes at 70° C. Next, an aqueous solution in which sodium polyoxyethylene lauryl ether sulfate was dissolved in 26 parts by mass of ion-exchanged water to a concentration of 1% by mass was added to the solution.
[0197] Next, 3.4 parts by mass of a 25% by mass aqueous solution of sodium hydroxide was added. This solution was placed in a reaction vessel equipped with a stirrer, and 270 parts by mass of ion-exchanged water heated to 70° C. was added dropwise to the solution over a period of 70 minutes while stirring.
[0198] The liquid in the container became cloudy during the dropping process, and a uniform emulsion was obtained after the entire amount was dropped. The particle size of the oil droplets in this emulsion was measured using a laser diffraction particle size distribution analyzer "LA-750 (HORIBA)" and the volume average particle size was 90 nm.
[0199] Next, while keeping this emulsion at 70°C, a diaphragm vacuum pump "V-700" (manufactured by BUCHI) was used to stir the emulsion under a reduced pressure of 15 kPa (150 mbar) for 1 hour to distill off the methyl ethyl ketone, thereby preparing an amorphous polyester particle dispersion (AP1) in which fine particles of the amorphous polyester resin [a1] were dispersed.
[0200] The solid content of the obtained amorphous polyester particle dispersion (AP1) was 24%. As a result of measurement with a particle size distribution measuring device, the volume average particle size of the amorphous polyester [a1] fine particles in the amorphous polyester particle dispersion (AP1) was 94 nm.
[0201] (C.2) Amorphous polyester particle dispersions (AP2) to (AP7) Amorphous polyesters [a2] to [a7] were synthesized in the same manner as for amorphous polyester [a1], except that in the synthesis of the amorphous polyester, the monomers listed in Table II were added as polyhydric alcohol components. In addition, the same monomers as for amorphous polyester [a1] were added as polyvalent carboxylic acids in the same amounts. Amorphous polyester particle dispersions (AP2) to (AP7) were otherwise prepared in the same manner as for amorphous polyester particle dispersion (AP1).
[0202] [Table 2]
[0203] D. Preparation of Crystalline Polyester Particle Dispersion (D.1) Crystalline polyester particle dispersion (CP1) (D.1.1) Synthesis of crystalline polyester The raw material monomers for the polycondensation resin (crystalline polyester: CPEs) units listed below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and were heated to 170°C to dissolve.
[0204] Sebacic acid (polycarboxylic acid) 60 mol parts 1,6-Hexanediol (polyhydric alcohol) 40 mole parts
[0205] Next, the monomer was placed in a reaction vessel equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet tube, and the inside of the reaction vessel was replaced with dry nitrogen gas. Ti(OBu)4 was added to the resulting mixture in an amount of 0.003% by mass based on the total amount of polyvalent carboxylic acid components, and the mixture was heated to 235°C and reacted for 5 hours under normal pressure (101.3kPa). The reaction was further carried out for 1 hour under reduced pressure (8kPa). Next, the resulting reaction liquid was cooled to 200°C, and then reacted for 1 hour under reduced pressure (20kPa) to synthesize crystalline polyester [c1].
[0206] (D.1.2) Preparation of crystalline polyester particle dispersion 174 parts by mass of the synthesized crystalline polyester [c1] was added to 102 parts by mass of methyl ethyl ketone and dissolved by stirring for 30 minutes at 75° C. Next, an aqueous solution in which sodium polyoxyethylene lauryl ether sulfate was dissolved in 26 parts by mass of ion-exchanged water to a concentration of 1% by mass was added to the solution.
[0207] Next, 4.6 parts by mass of a 25% by mass aqueous solution of sodium hydroxide was added. This solution was placed in a reaction vessel equipped with a stirrer, and 375 parts by mass of water heated to 70°C was added dropwise to the solution over a period of 70 minutes while stirring. The liquid in the vessel became cloudy during the dropwise addition, and after the entire amount was added, a uniform emulsion state was obtained.
[0208] Next, while keeping this emulsion at 70°C, it was stirred for 1 hour under reduced pressure of 15 kPa (150 mbar) using a diaphragm vacuum pump "V-700" (BUCHI) to distill off the methyl ethyl ketone, and then cooled at a rate of 6°C / min to prepare a crystalline polyester particle dispersion (CP1) in which fine particles of the crystalline polyester [c1] were dispersed.
[0209] The solid content of the resulting crystalline polyester particle dispersion (CP1) was 25%. As a result of measurement with a particle size distribution measuring device, the volume average particle diameter of the crystalline resin particles in the crystalline resin particle dispersion was 202 nm.
[0210] (D.2) Crystalline polyester particle dispersions (CP2) to (CP4) Crystalline polyesters [c2] to [c4] were synthesized in the same manner as for crystalline polyester [c1], except that the monomers were added in the amounts shown in Table III as polyvalent carboxylic acid and polyhydric alcohol components in the synthesis of the crystalline polyesters. Otherwise, crystalline polyester particle dispersions (CP2) to (CP4) were prepared in the same manner as for crystalline polyester particle dispersion (CP1).
[0211] [Table 3]
[0212] E. Preparation of Colorant Particle Dispersion (Colorant particle dispersion (P1)) A solution of 226 parts by mass of sodium dodecyl sulfate added to 1600 parts by mass of ion-exchanged water was stirred, and 420 parts by mass of copper phthalocyanine (CI Pigment Blue 15:3) was gradually added thereto.
[0213] A colorant particle dispersion (P1) was prepared by dispersing using a stirring device Clearmix (manufactured by M Technique Co., Ltd., "Clearmix" is a registered trademark of the company). The colorant particles in the dispersion had a volume-based median diameter of 110 nm.
[0214] F. Preparation of release agent particle dispersion (F.1) Release agent particle dispersion (W1) The following components were heated to 110°C and dispersed using a homogenizer (IKA: Ultra Turrax T50), and then dispersed using a Manton-Gaulin high pressure homogenizer (Gaulin) to prepare a release agent dispersion (W1) (release agent concentration: 26% by mass) in which a release agent having an average particle size of 0.21 µm was dispersed.
[0215] <Ingredients> Release agent "HNP-9" (manufactured by Nippon Seiro Co., Ltd.) 50 parts by weight Anionic surfactant "Neogen RK" (Dai-ichi Kogyo Seiyaku Co., Ltd.) 5 parts by weight Ion-exchanged water 200 parts by weight
[0216] The volume average particle diameter of the fine particles in the release agent particle dispersion (W1) was measured with a Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) and was found to be 215 nm.
[0217] (F.2) Release agent particle dispersion (W2) to (W6) Release agent particle dispersions (W2) to (W6) were prepared in the same manner as for the preparation of the release agent particle dispersion (W1), except that 50 parts by mass of the release agent shown in Table IV was used instead of "HNP-9" (manufactured by Nippon Seiro Co., Ltd.).
[0218] [Table 4] G. Preparation of Toner Particles (G.1) Toner particles [1] The following materials were placed in a round stainless steel flask and 0.1 N nitric acid was added to adjust the pH to 3.5, after which an aqueous solution of polyaluminum chloride (PAC, Oji Paper Co., Ltd.: 30% powder product) 2.0 parts by mass dissolved in 30 parts of ion-exchanged water was added.
[0219] <Material> Ion-exchanged water 200 parts by weight Amorphous polyester particle dispersion (AP1) 150 parts by weight Crystalline polyester particle dispersion (CP1) 40 parts by weight Colorant particle dispersion (P1) 15 parts by weight Release agent particle dispersion (W1) 10 parts by weight Anionic surfactant (TaycaPower) 2.8 parts by weight
[0220] After dispersing at 30°C using a homogenizer (IKA Ultra Turrax T50), the mixture was heated to 45°C in a heating oil bath and maintained at this temperature until the volume average particle size of the toner particles made from the above materials reached 4.1 μm.
[0221] Thereafter, 60 parts by mass of amorphous polyester particle dispersion (AP1) was added and held for 30 minutes. Then, when the volume average particle size of the toner particles became 4.5 μm, 60 parts by mass of amorphous polyester particle dispersion (A1) was further added and held for 30 minutes.
[0222] Next, 20 parts by mass of a 10% NTA (nitrilotriacetic acid) metal salt aqueous solution (Chilest 70: manufactured by Chelesto Co., Ltd.) was added, and the pH was adjusted to 9.0 using a 1N aqueous sodium hydroxide solution. Then, 1.0 part by mass of an anionic activator (TaycaPower) was added, and the mixture was heated to 85°C while continuing to stir, and maintained for 5 hours.
[0223] The toner particles were then cooled to 20°C at a rate of 20°C / min, filtered, and thoroughly washed with ion-exchanged water. The resulting water-containing toner was dried using a continuous instantaneous airflow dryer "Flash Jet Dryer" (manufactured by Seishin Enterprise Co., Ltd., model: 2 inch) to produce toner particles [1] with a volume average particle size of 5.0 μm.
[0224] (G.2) Toner particles [2] to
[22] Toner particles [2] to
[22] were prepared in the same manner as in the preparation of toner particles [1], except that the amorphous polyester particle dispersion, the crystalline polyester particle dispersion, and the release agent particle dispersion were changed to those shown in Table V, respectively.
[0225] H. Preparation of external additives (H.1) External additives [1] 945 parts by mass of methanol, 45 parts by mass of 28% aqueous ammonia, and 135 parts by mass of water were added and mixed in a 3-liter reaction vessel equipped with a stirrer, dropping funnel, and thermometer. The temperature of this solution was adjusted to 35°C, and 405 parts by mass of tetramethoxysilane was dropped over 6 hours while stirring. After the dropwise addition, stirring was continued for another hour to perform hydrolysis, and a suspension of silica particles was obtained. This dispersion was distilled under reduced pressure and dried, and the fine particles were crushed to produce an external additive [1] (silica particles [S1]) with a particle size of 110 nm.
[0226] (H.2) External additive [2] (silica particle [S2]) to external additive [4] (silica particle [S4]) In producing the external additive [1] (silica particles [S1]), the mass ratio of methanol, aqueous ammonia and water, and the temperature of the solution were controlled to produce silica particles [S2] to [S4] having the number-average particle diameters shown in Table V.
[0227] I. Preparation of developer (I.1) Developer 1 (Preparation of Toner 1) Toner 1 was prepared by adding 1.5 parts by mass of external additive [1] (silica particles [1]) having a particle size of 110 nm to 100 parts by mass of toner particles [1] and mixing them in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotor peripheral speed of 35 mm / sec at 32°C for 20 minutes.
[0228] (Mixed Carriers) Then, toner 1 from which coarse particles had been removed using a sieve with 45 μm openings and ferrite carrier with a volume average particle size of 32 μm coated with acrylic resin were added and mixed so that the toner particle concentration was 6 mass %, thereby preparing developer 1.
[0229] (I.2) Developers 2 to 22 (Preparation of toners 2 to 22) Toners 2 to 22 were prepared in the same manner as in the preparation of toner 1, except that the external additive [1] (silica particles [1]) was changed to one shown in Table V, respectively.
[0230] (Mixed Carriers) Then, toners 2 to 22, from which coarse particles had been removed using a sieve with 45 μm openings, and ferrite carriers with a volume average particle size of 32 μm coated with acrylic resin were added and mixed so that the toner particle concentration was 6 mass %, to prepare developers 2 to 22.
[0231] [Table 5]
[0232] J. Evaluation (preparation) A magnet roller, a shaft and a flange were attached to each of the prepared developing sleeves 1 to 6 to prepare developing rollers 1 to 6, which were then attached in a normal temperature and normal humidity environment (NN environment; temperature 23°C, humidity 50% RH) as developing rollers used in developing means in "bizhub C658" (manufactured by Konica Minolta, Inc.) for each of the Examples and Comparative Examples. In addition, developers 1 to 22 were loaded into each of the Examples and Comparative Examples.
[0233] (J.1) Sunspots (Evaluation method) In a NN environment, 400,000 sheets of a character chart with an average print rate of 5% were printed continuously. After that, in a high temperature and humidity environment (HH environment; temperature 30°C, humidity 85% RH), POD gloss coat (A3 size, 100g / m 2 100 sheets of each color (Y, M, C, Bk) were printed on a paper mat (manufactured by Oji Paper Co., Ltd.).
[0234] A total of eight sheets, the 1st and 100th sheets for each of Y, M, C, and Bk, were visually observed and the images were evaluated according to the following evaluation criteria. The evaluation criteria used were "A," "B," and "D." "A" and "B" were determined to be at a level that is acceptable for practical use and were rated as passing. "D" was determined to be at a level that is problematic for practical use and were rated as failing. The evaluation results are shown in Table VI.
[0235] (Evaluation Criteria) A: No black dots or other image defects were observed in any of the eight sheets, and there were no practical problems. B: Black spots can be seen in at least one of the eight sheets, but this does not cause any problems in practical use. D: At least one of the eight sheets had conspicuous black spots, the quality was unacceptable, and image defects were observed to a level that was problematic for practical use.
[0236] (J.2) Cover (Evaluation method) The fog on the image was measured by printing an image with a pixel ratio of 45% on A4-size wood-free paper (64 g / m2) in a low-temperature, low-humidity environment (temperature 10°C, humidity 15% RH). 2After printing 5,000 sheets on the A4-sized paper, a blank sheet was printed and the blank sheet density of the transfer material was measured using a reflection densitometer "RD-918" (Macbeth) and evaluated according to the following evaluation criteria. The blank sheet density of the transfer material was measured at 20 points on an A4-sized sheet and the average value was taken as the blank sheet density. The evaluation criteria used were "A", "B", "C" and "D". "A", "B" and "C" were judged to be at a level that is acceptable for practical use and were rated as passing. "D" was judged to be at a level that is problematic for practical use and were rated as failing. The evaluation results are shown in Table VI.
[0237] (Evaluation Criteria) A: The fog density is less than 0.005, which is a good level. B: The fog density is 0.005 or more and less than 0.008, which is at a level that does not cause any practical problems. C: The fog density is 0.008 or more and less than 0.012, which is at a level that does not cause any practical problems. D: The fog density is 0.012 or more, which is a practically problematic level.
[0238] (J.3) Low-temperature fixability (Evaluation method) The fixing device of the multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta, Inc.) was modified to be able to change the surface temperatures of the upper fixing belt and the lower fixing roller, and two-component developers were loaded in sequence. The above device was also modified to be able to freely set the fixing temperature, toner adhesion amount, and system speed.
[0239] Under normal temperature and humidity conditions (temperature 20°C, humidity 50% RH), A4 size high-quality paper "NPI high-quality (127.9 g / m 2 ) (manufactured by Nippon Paper Industries Co., Ltd.) with a deposition rate of 11.3 g / m 2 It was set to be.
[0240] After that, a fixing experiment to fix an image of 100 mm x 100 mm size was performed by repeatedly changing the set fixing temperature from 110 °C to 180 °C in 2 °C increments. The lowest fixing temperature at which image staining due to fixing offset was not visually confirmed was defined as the minimum fixing temperature (UO avoidance temperature). The measured value of this minimum fixing temperature was used to evaluate according to the following evaluation criteria.
[0241] The evaluation criteria used were "A," "B," "C," and "D." "A," "B," and "C" were deemed acceptable for practical use and were rated as "pass." "D" was deemed problematic for practical use and was rated as "fail." The evaluation results are shown in Table VI.
[0242] (Evaluation Criteria) A The minimum fixing temperature is less than 130°C. B The minimum fixing temperature is 130°C or higher and lower than 135°C. C The minimum fixing temperature is 135°C or higher and lower than 140°C. D The minimum fixing temperature is 140°C or higher.
[0243] (J.4) Heat resistance of toner (Evaluation method) 0.5 g of each toner was placed in a 10 mL glass bottle with an inner diameter of 21 mm, the bottle was closed, and the bottle was shaken 600 times at room temperature using a shaker "Tap Denser KYT-2000" (manufactured by Seishin Enterprise Co., Ltd.) After that, the bottle was left for 2 hours with the lid open in an environment with a temperature of 55°C and a humidity of 35% RH.
[0244] Next, the toner was placed on a 48 mesh (350 μm mesh) sieve while being careful not to break up the toner aggregates, and then set in a "Powder Tester" (manufactured by Hosokawa Micron Corporation) and fixed with a presser bar and knob nut. The vibration intensity was adjusted to give a feed width of 1 mm, and vibration was applied for 10 seconds, after which the ratio (mass%) of the toner amount remaining on the sieve was measured, and the toner aggregation rate was calculated by the following formula (A).
[0245] Formula (A): Toner cohesion rate [%] = (mass of toner remaining on sieve [g]) / 0.5 [g] x 100)
[0246] Similar measurements were performed at temperatures of 57.5°C and 60°C, and the X-axis was plotted as temperature and the Y-axis as toner cohesion rate. An approximate line was drawn between two temperatures that sandwiched the region where the toner cohesion rate was 50% between temperatures of 55°C, 57.5°C, and 60°C, and the temperature where the toner cohesion rate was 50% was calculated by interpolation. The temperature at that time was measured, and this was regarded as the heat resistance temperature and evaluated according to the following evaluation criteria.
[0247] The evaluation criteria used were "A," "B," "C," and "D." "A," "B," and "C" were deemed acceptable for practical use and were rated as "pass." "D" was deemed problematic for practical use and was rated as "fail." The evaluation results are shown in Table VI.
[0248] (Evaluation Criteria) A is above 59°C. B. 58°C or higher but less than 59°C. C. Above 57°C and below 58°C. D Less than 57°C.
[0249] [Table 6]
[0250] (J.5) Overall evaluation As is clear from Table VI, the Examples are superior to the Comparative Examples, suppressing image defects such as black spots and fog, and are excellent in low-temperature fixing property and heat resistance, making it possible to suppress image defects. [Explanation of symbols]
[0251] 10 Developing roller 11 Developing sleeve 12 Magnet Roller 16 Shaft 17 Bearing section 18 Non-drive side flange 19 Drive side flange 20 grooves 21 Upstream wall of the groove 22 Downstream wall of the groove 100 Image forming device 110Y, 110M, 110C, 110Bk Image forming unit 111Y, 111M, 111C, 111Bk photoconductor 113Y, 113M, 113C, 113Bk Charging means (charging roller) 115Y, 115M, 115C, 115Bk Exposure means 117Y, 117M, 117C, 117Bk developing means 118Y, 118M, 118C, 118Bk developing roller 119Y, 119M, 119C, 119Bk Cleaning means 131 Intermediate transfer body 133Y, 133M, 133C, 133Bk Transfer means (primary transfer roller) 150 Paper feed conveying means 170 Fixing means 217 Secondary transfer roller (secondary transfer means) SC Original Image Scanner P Transfer material α Groove apex angle β Groove angle A, B groove apex L A A perpendicular line drawn from a direction perpendicular to the surface of the developing sleeve to vertex A L B A perpendicular line drawn from a direction perpendicular to the surface of the developing sleeve to vertex B
Claims
1. An image forming system having a toner for developing an electrostatic image and a developing sleeve for conveying the toner for developing an electrostatic image, the toner particles contained in the electrostatic image developing toner contain an amorphous polyester, the amorphous polyester is a polycondensate of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less based on the total structural units derived from the polyhydric alcohol; The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon.
1. An image forming system comprising:
2. A member generating a magnetic flux is provided inside the developing sleeve.
2. The image forming system according to claim 1,
3. The toner particles contain a crystalline resin.
2. The image forming system according to claim 1,
4. The crystalline resin contains a crystalline polyester, The crystalline polyester is a polycondensation product of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms.
4. The image forming system according to claim 3.
5. The polyhydric alcohol contains an aliphatic polyhydric alcohol having 5 or more carbon atoms.
2. The image forming system according to claim 1,
6. The silicon content in the aluminum alloy is more than 0.8% by mass.
2. The image forming system according to claim 1,
7. The toner particles contain a release agent having a melting point in the range of 70 to 91° C.
2. The image forming system according to claim 1,
8. The toner particles contain silica particles having an average particle size in the range of 90 to 130 nm as an external additive.
2. The image forming system according to claim 1,
9. An image forming method using a toner for developing an electrostatic image and a developing sleeve for transporting the toner for developing an electrostatic image, comprising the steps of: the toner particles contained in the electrostatic image developing toner contain an amorphous polyester which is a polycondensation product of a polycarboxylic acid and a polyhydric alcohol, the content of structural units derived from a bisphenol A derivative in the amorphous polyester is 10 mol % or less based on the total structural units derived from the polyhydric alcohol; The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon.
1. An image forming method comprising:
Citation Information
Patent Citations
Toner for electrostatic charge image development, method for manufacturing the same, image forming method, and image forming apparatus
JP2007279714A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method
JP2017062344A