Resin composition for shrink labels
The resin composition for shrinkable labels, incorporating an aqueous acrylic resin emulsion and carboxyl group-containing silicone compound, addresses flexibility and whitening issues, enhancing adhesion and resistance properties in coating films.
Patent Information
- Application Number
- JP2023073427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional resin compositions for shrinkable labels, particularly those using water-based varnishes, suffer from reduced flexibility and whitening after heat shrinkage, compromising hot water resistance and adhesion.
A resin composition comprising an aqueous acrylic resin emulsion, a carboxyl group-containing silicone compound, and an aqueous medium, with specific ratios and optional additives like crosslinking agents, to achieve excellent adhesion, abrasion resistance, hot water resistance, whitening property, and leveling property.
The resulting coating film exhibits improved adhesion, abrasion resistance, hot water resistance, whitening property, and leveling property, maintaining flexibility and stability over time.
Smart Images

Figure 2024158313000001 
Figure 2024158313000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for shrink labels. More specifically, the present invention relates to a resin composition for shrink labels which provides a coating film excellent in adhesion, abrasion resistance, hot water resistance, whitening resistance, slippage and leveling properties. [Background technology]
[0002] Shrink labels are heat-shrinkable plastic films, and are laminated films using heat-shrinkable polyester films, polystyrene films, polyolefin films, etc. as base films. Shrink labels are attached to the containers of various products (e.g., PET bottle drinks, alcoholic beverages, daily necessities, medicines, food and beverages, etc.) and are widely used as labels that display information, designs, etc. of the products.
[0003] Shrink labels are attached to containers by wrapping a heat-shrinkable film around the container and then heating it to shrink (heat shrink) the film and make it adhere closely to the container. Known heating methods are steam and hot air. When using the steam method, the shrink label is required to be hot water resistant (no blocking occurs even when exposed to hot water such as steam).
[0004] In recent years, in order to address environmental issues, when a resin composition for shrink labels is used as a varnish composition, it is desired that the composition be an aqueous varnish composition, in addition to the conventional solvent-based varnish composition. In general, the coating film of an aqueous varnish tends to have lower hot water resistance than the coating film of a solvent-based varnish. Therefore, when the aqueous varnish composition is used for shrink labels, a technique has been proposed in which a crosslinking agent is added (two-part) to improve the hot water resistance (for example, Patent Documents 1-2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2020-501935 [Patent Document 2] Patent No. 7122482 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the inks described in Patent Documents 1 and 2 contain a large amount of crosslinking agent to improve hot water resistance. Therefore, the resulting coating film has low flexibility and whitening occurs after thermal shrinkage. Therefore, a resin composition for shrink labels that has excellent performance in both hot water resistance and whitening properties has not yet been known.
[0007] The present invention has been made in consideration of such conventional problems, and has an object to provide a resin composition for shrink labels which provides a coating film having excellent adhesion, abrasion resistance, hot water resistance, whitening properties, slip properties and leveling properties. [Means for solving the problem]
[0008] The present invention, which solves the above problems, mainly comprises the following configuration.
[0009] (1) A resin composition for a shrink label, comprising an aqueous acrylic resin emulsion, a carboxyl group-containing silicone compound, and an aqueous medium, the content of the carboxyl group-containing silicone compound being 0.1 to 1.1 mass% in the resin composition for a shrink label.
[0010] According to such a constitution, the resulting coating film has excellent adhesion, abrasion resistance, hot water resistance, whitening resistance, slipping property and leveling property.
[0011] (2) The resin composition for shrink labels according to (1), further comprising a pigment.
[0012] According to this constitution, when the resin composition for shrink labels is an ink composition, the resulting coating film has excellent adhesion, abrasion resistance, hot water resistance, whitening properties, slip properties and leveling properties.
[0013] (3) The resin composition for shrink labels according to (1) or (2), further comprising a crosslinking agent.
[0014] According to such a constitution, the resulting coating film has an excellent balance between hot water resistance and whitening property.
[0015] (4) The resin composition for shrink labels according to (3), wherein the solid content of the crosslinking agent in the resin composition for shrink labels is 0.5 to 6.5% by mass.
[0016] According to this configuration, the resulting coating film has a better balance between hot water resistance and whitening property.
[0017] (5) The resin composition for shrink labels according to (3) or (4), wherein the crosslinking agent is at least one of an epoxy-based crosslinking agent and an aziridine-based crosslinking agent.
[0018] According to this configuration, the resulting printed matter can exhibit high durability even when aged in a mild environment around room temperature. Effect of the Invention
[0019] According to the present invention, it is possible to provide a resin composition for shrink labels which gives a coating film excellent in adhesion, abrasion resistance, hot water resistance, whitening resistance, slipping property and leveling property. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] <Resin composition for shrink labels> The shrink label resin composition according to one embodiment of the present invention contains an aqueous acrylic resin emulsion, a carboxyl group-containing silicone compound, and an aqueous medium. The content of the carboxyl group-containing silicone compound in the shrink label resin composition is 0.1 to 1.1% by mass. The shrink label resin composition according to this embodiment provides a coating film excellent in adhesion, abrasion resistance, hot water resistance, whitening, slippage, and leveling. Therefore, the shrink label resin composition is useful as a varnish composition capable of forming a coating film having the above-mentioned characteristics, for example. In addition, the shrink label resin composition is useful as an ink composition capable of forming a coating film having the above-mentioned characteristics by including an appropriate pigment. Each of these will be described below.
[0021] (Water-based acrylic resin emulsion) The aqueous acrylic resin emulsion refers to a resin liquid in which the aqueous acrylic resin is emulsion-stabilized in a particulate form. The aqueous acrylic resin emulsion is not particularly limited. For example, the aqueous acrylic resin emulsion may be an ethylene / vinyl acetate / (meth)acrylic acid derivative copolymer emulsion, an ethylene / (meth)acrylic acid derivative copolymer emulsion, a poly(meth)acrylic acid derivative emulsion, a styrene / (meth)acrylic acid derivative copolymer emulsion, or a vinyl acetate / (meth)acrylic acid derivative emulsion. The (meth)acrylic acid derivative is an acid derivative such as acrylic acid and / or methacrylic acid, or an ester thereof.
[0022] (Meth)acrylic acid derivatives include acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, acrylonitrile, methacrylonitrile, acrylamide, and methacrylamide.
[0023] By incorporating the aqueous acrylic resin emulsion, the resin composition for shrink labels has excellent adhesion to the overcoat layer when used as a varnish composition, and has an excellent balance of adhesion and blocking resistance of the printing layer when used as an ink composition.
[0024] The acid value of the resin component contained in the aqueous acrylic resin emulsion is not particularly limited. For example, the acid value is preferably 10 mgKOH / g or more, more preferably 20 mgKOH / g or more. The acid value is preferably 180 mgKOH / g or less, more preferably 100 mgKOH / g or less. When the acid value is within the above range, the balance between the dispersibility of the emulsion in the aqueous medium and the stability of the resin composition for shrink labels is excellent. In this embodiment, the acid value is a theoretical acid value obtained by arithmetically calculating the number of mg of potassium hydroxide theoretically required to neutralize 1 g of the aqueous acrylic resin emulsion based on the composition of the monomers used to synthesize the aqueous acrylic resin emulsion.
[0025] The glass transition temperature (Tg) of the resin component contained in the aqueous acrylic resin emulsion is preferably −30 to 150° C., and more preferably −25 to 120° C. When the Tg is within the above range, the resin composition for shrink labels has an excellent balance of heat resistance, adhesion, and flexibility of the overcoat layer when used as a varnish composition. In addition, the resin composition for shrink labels has an excellent balance of heat resistance, adhesion, and flexibility when used as an ink composition.
[0026] The method for producing the aqueous acrylic resin emulsion is not particularly limited. For example, the aqueous acrylic resin emulsion can be obtained by a known production method, for example, by emulsion polymerization of polymerizable monomers, which are raw materials for synthetic resins, in water or a water-containing solvent using a polymerization initiator in the presence of an emulsifier.
[0027] The emulsifier is not particularly limited, and examples thereof include anionic, nonionic, cationic or amphoteric surfactants and protective colloids such as polyvinyl alcohol.
[0028] The solid content of the aqueous acrylic resin emulsion contained in the varnish composition is not particularly limited. As an example, the solid content of the aqueous acrylic resin emulsion in the varnish composition is preferably 10.0 to 40.0 mass%, more preferably 15.0 to 35.0 mass%. When the solid content of the aqueous acrylic resin emulsion is within the above range, the shrink label resin composition has an excellent balance between the adhesion and blocking resistance of the overcoat layer when used as a varnish composition. In addition, the shrink label resin composition has an excellent balance between the adhesion and blocking resistance of the printing layer when used as an ink composition.
[0029] (Other water-based resin emulsions) In the resin composition for shrink labels of this embodiment, a part of the above-mentioned aqueous acrylic resin emulsion may be appropriately replaced with another aqueous emulsion.
[0030] The other aqueous resin emulsion is not particularly limited, and examples of the other aqueous resin emulsion include an aqueous urethane-based resin emulsion and an aqueous acrylic urethane-based emulsion.
[0031] The aqueous urethane resin emulsion refers to a resin liquid in which the aqueous urethane resin is in a particulate emulsion state. Examples of the aqueous urethane resin emulsion include polyester urethane, polyether urethane, polycarbonate urethane, and other resin emulsions.
[0032] The acid value of the resin component contained in the aqueous urethane resin emulsion is not particularly limited. For example, the acid value is preferably 10 mgKOH / g or more, more preferably 20 mgKOH / g or more. The acid value is preferably 60 mgKOH / g or less, more preferably 50 mgKOH / g or less. By having the acid value within the above range, the balance between the dispersibility of the emulsion in the aqueous medium and the stability of the resin composition for shrink labels is excellent.
[0033] The solid content of the aqueous urethane resin emulsion contained in the shrink label resin composition is not particularly limited. As an example, the solid content of the aqueous urethane resin emulsion is preferably 10.0 to 40.0 mass %, more preferably 15.0 to 35.0 mass %, in the shrink label resin composition. When the solid content of the aqueous urethane resin emulsion is within the above range, the shrink label resin composition has an excellent balance between the adhesion and blocking resistance of the overcoat layer when used as a varnish composition. In addition, when the shrink label resin composition is used as an ink composition, the print layer has an excellent balance between the adhesion and blocking resistance.
[0034] The aqueous acrylic urethane resin emulsion refers to a resin liquid in which the aqueous acrylic urethane resin is emulsion-stabilized in a particulate form. The aqueous acrylic urethane resin is a resin containing an acrylic resin part and a urethane resin part. The resin containing an acrylic resin part and a urethane resin part may be an alternating copolymer of an acrylic unit and a urethane unit, and may have a urethane resin bonded as a side chain to an acrylic resin constituting a main chain, or may have an acrylic resin bonded as a side chain to a urethane resin constituting a main chain. For example, it can be produced by referring to the methods described in JP-A-4-103614 and JP-A-10-139839.
[0035] The acid value of the resin component contained in the aqueous acrylic urethane resin emulsion is not particularly limited. For example, the acid value is preferably 5 mgKOH / g or more, more preferably 25 mgKOH / g or more. The acid value is preferably 100 mgKOH / g or less, more preferably 80 mgKOH / g or less. By having the acid value within the above range, the balance between the dispersibility of the emulsion in the aqueous medium and the stability of the resin composition for shrink labels is excellent.
[0036] The solid content of the aqueous acrylic urethane resin emulsion contained in the shrink label resin composition is not particularly limited. As an example, the solid content of the aqueous acrylic urethane resin emulsion is preferably 10.0 to 40.0 mass %, more preferably 15.0 to 35.0 mass %, in the shrink label resin composition. When the solid content of the aqueous acrylic urethane resin emulsion is within the above range, the shrink label resin composition has an excellent balance between the adhesion and blocking resistance of the overcoat layer when used as a varnish composition. In addition, when the shrink label resin composition is used as an ink composition, the shrink label resin composition has an excellent balance between the adhesion and blocking resistance of the printing layer.
[0037] (Carboxyl group-containing silicone compound) The carboxyl group-containing silicone compound is a compound in which a part of the side chain of dimethyl silicone oil or the methyl groups at both ends or one end are replaced with a group containing a carboxyl group. The shrink label resin composition of this embodiment contains a carboxyl group-containing silicone compound among silicone compounds. This allows the shrink label resin composition to provide a coating film with excellent hot water resistance and leveling properties.
[0038] The viscosity of the carboxyl group-containing silicone compound is 25 mm. 2 / s or more is preferable, and 50 mm 2 The viscosity of the carboxyl group-containing silicone compound is preferably 3000 mm / s or more. 2 / s or less is preferable, and 2500 mm2 / s or less is more preferable. By having a viscosity within the above range, the shrink label resin composition has an excellent balance between hot water resistance and whitening property. In this embodiment, the viscosity can be measured at 25°C using a Cannon-Fenske viscometer based on JIS Z 8803:2011.
[0039] The specific gravity of the carboxyl group-containing silicone compound is preferably 0.92 or more, more preferably 0.95 or more. The specific gravity of the carboxyl group-containing silicone compound is preferably 1.03 or less, more preferably 1.00 or less. When the specific gravity is within the above range, the shrink label resin composition has excellent stability over time of the printed matter. In this embodiment, the specific gravity can be measured using a hydrometer based on JIS Z 8804.
[0040] The refractive index of the carboxyl group-containing silicone compound is preferably 1.37 or more, more preferably 1.40 or more. The refractive index of the carboxyl group-containing silicone compound is preferably 1.45 or less, more preferably 1.42 or less. When the refractive index is within the above range, the resin composition for shrink labels has excellent stability over time of the printed matter. In this embodiment, the refractive index can be measured based on JIS K 0062 using a device called a digital refractometer (model number: RX-5000, seller: Atago Co., Ltd.).
[0041] The functional group equivalent of the carboxyl group-containing silicone compound is preferably 500 g / mol or more, more preferably 1000 g / mol or more. The functional group equivalent of the carboxyl group-containing silicone compound is preferably 6000 g / mol or less, more preferably 5000 g / mol or less. By having the functional group equivalent within the above range, the resin composition for shrink labels can achieve both hot water resistance and appropriate slip properties.
[0042] The content of the carboxyl group-containing silicone compound in the resin composition for shrink labels may be 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. The content of the carboxyl group-containing silicone compound in the resin composition for shrink labels may be 1.1% by mass or less, preferably 1.0% by mass or less, and more preferably 0.9% by mass or less. By having the content of the carboxyl group-containing silicone compound within the above range, the resin composition for shrink labels has excellent hot water resistance and whitening properties of the coating film obtained. The carboxyl group-containing silicone compound is obtained by collecting low molecular weight components by GPC, 1 H-NMR analysis, 13 Quantitation can be achieved by combining C-NMR analysis, LC-MS, GC-MS, etc.
[0043] (aqueous medium) The aqueous medium is not particularly limited, and examples of the aqueous medium include water and various water-soluble organic solvents.
[0044] The water-soluble organic solvent is not particularly limited. For example, the water-soluble organic solvent is an alcohol or polyhydric alcohol solvent, and examples thereof include methanol, ethanol, propanol, butanol, hexanol, octanol, decanol, ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monooctyl ether, diethylene glycol, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ... Examples of the monoethylene glycol monopropyl ether include triethylene glycol monobutyl ether, propylene glycol, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monopropyl ether, tripropylene glycol monobutyl ether, and glycerin.
[0045] The content of the aqueous medium in the varnish composition is preferably 50.0% by mass or more, and more preferably 60.0% by mass or more. The content of the aqueous medium in the varnish composition is preferably 90.0% by mass or less, and more preferably 80.0% by mass or less. By having the content of the aqueous medium within the above range, the varnish composition has an excellent balance between cleaning ability and drying ability.
[0046] (optional ingredient) The resin composition for shrink labels of this embodiment may contain a crosslinking agent, a pigment, a leveling agent, an antifoaming agent, a wax, a viscosity modifier, a polymerization inhibitor, a solvent, an antiblocking agent, a light stabilizer, an ultraviolet absorber, an infrared absorber, a thickener (thixotropic agent), an antibacterial and antifungal agent, and the like.
[0047] (Crosslinking agent) The crosslinking agent is not particularly limited. For example, the crosslinking agent may be an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a melamine-based crosslinking agent, a peroxide-based crosslinking agent, a urea-based crosslinking agent, a metal alkoxide-based crosslinking agent, a metal chelate-based crosslinking agent, a metal salt-based crosslinking agent, a carbodiimide-based crosslinking agent, a hydrazine-based crosslinking agent, an amine-based crosslinking agent, a silane coupling agent, or the like. Among these, the crosslinking agent is preferably at least one of an epoxy-based crosslinking agent and an aziridine-based crosslinking agent. This allows the resin composition for shrink labels to obtain a coating film having excellent hot water resistance and abrasion resistance.
[0048] When a crosslinking agent is blended, the content of the crosslinking agent is not particularly limited. For example, the solid content of the crosslinking agent can be appropriately determined depending on the type of the crosslinking agent. For example, the solid content of the crosslinking agent in the resin composition for shrink labels is preferably 0.5% by mass or more, more preferably 1.0% by mass or more. In addition, the solid content of the crosslinking agent in the resin composition for shrink labels is preferably 6.5% by mass or less, more preferably 6.0% by mass or less. By having the content of the crosslinking agent within the above range, the resin composition for shrink labels has an excellent balance between hot water resistance and whitening properties.
[0049] The aziridine crosslinking agent is not particularly limited. For example, the aziridine crosslinking agent may be trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(1-(2-methyl)aziridinylpropionate)], etc.
[0050] When an aziridine-based crosslinking agent is used, the solid content of the aziridine-based crosslinking agent in the resin composition for shrink labels is preferably 0.5% by mass or more, and more preferably 1.0% by mass or more. The content of the aziridine-based crosslinking agent in the resin composition for shrink labels is preferably 4.5% by mass or less, and more preferably 4.0% by mass or less. By having the content of the aziridine-based crosslinking agent within the above range, the resin composition for shrink labels has an excellent balance between hot water resistance and whitening properties.
[0051] The epoxy crosslinking agent is not particularly limited. For example, the epoxy crosslinking agent is one having two or more epoxy groups in one molecule, such as N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, etc.
[0052] When an epoxy-based crosslinking agent is used, the solid content of the epoxy-based crosslinking agent in the resin composition for shrink labels is preferably 1.0% by mass or more, more preferably 3.0% by mass or more. The content of the epoxy-based crosslinking agent in the resin composition for shrink labels is preferably 6.5% by mass or less, more preferably 6.0% by mass or less. By having the content of the epoxy-based crosslinking agent within the above range, the resin composition for shrink labels has an excellent balance between hot water resistance and whitening properties.
[0053] The metal chelate crosslinking agent is not particularly limited. For example, the metal chelate crosslinking agent is a zirconium chelate crosslinking agent, a titanium chelate crosslinking agent, an aluminum chelate crosslinking agent, etc. Among these, the metal chelate crosslinking agent is preferably a zirconium chelate crosslinking agent such as ZrOCl2, ZrO(NO3)2K2ZrO(CO3)2, K2Zr(CO3)2(OH2)2, (NH4)2ZrO(CO3)2, (NH4)2Zr(CO3)2(OH2)2, ZrO(C2H3O2)2, Zr(C2H3O2)4, Zr(C5H7O2)4, or Zr(On-C4H9)3(C5H7O2).
[0054] When a zirconium chelate crosslinking agent is used, the solid content of the zirconium chelate crosslinking agent in the resin composition for shrink labels is preferably 2.5% by mass or more, more preferably 3.0% by mass or more. The content of the zirconium chelate crosslinking agent in the resin composition for shrink labels is preferably 6.5% by mass or less, more preferably 6.0% by mass or less. By having the content of the zirconium chelate crosslinking agent within the above range, the resin composition for shrink labels has an excellent balance between hot water resistance and whitening properties.
[0055] (Pigments) The pigment is preferably blended when the resin composition for shrink labels is an ink composition. The pigment is not particularly limited. For example, the pigment is various organic pigments and inorganic pigments. The organic pigment is a dye lake pigment, an azo pigment, a benzimidazolone pigment, a phthalocyanine pigment, a quinacridone pigment, an anthraquinone pigment, a dioxazine pigment, an indigo pigment, a thioindigo pigment, a perylene pigment, a perinone pigment, a diketopyrrolopyrrole pigment, an isoindolinone pigment, a nitro pigment, a nitroso pigment, a flavanthrone pigment, a quinophthalone pigment, a pyranthrone pigment, an indanthrone pigment, or the like.
[0056] The inorganic pigments include carbon black, titanium oxide, zinc oxide, red iron oxide, graphite, iron black, chromium oxide green, and aluminum hydroxide.
[0057] The pigment may be surface-treated with a known surface treatment agent.
[0058] Yellow pigments include CI Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 42, 73, 74, 75, 81, 83, 87, 93, 95, 97, 98, 108, 109, 114, 120, 128, 129, 138, 139, 150, 151, 155, 166, 180, 184, 185, 213, etc.
[0059] Magenta pigments include CI Pigment Red 5, 7, 12, 22, 38, 48:1, 48:2, 48:4, 49:1, 53:1, 57, 57:1, 63:1, 101, 102, 112, 122, 123, 144, 146, 149, 168, 177, 178, 179, 180, 184, 185, 190, 202, 209, 224, 242, 254, 255, 270, CI Pigment Violet 19, and the like.
[0060] Cyan pigments include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 18, 22, 27, 29, 60, and the like.
[0061] The black pigment is carbon black (CI Pigment Black 7) or the like.
[0062] The white pigment is titanium oxide, aluminum oxide, etc. The white pigment may be surface-treated with various materials such as alumina, silica, etc.
[0063] The content of the pigment is not particularly limited. For example, the content of the pigment in the ink composition is preferably 0.5% by mass or more, and more preferably 10% by mass or more. The content of the pigment in the ink composition is preferably 45% by mass or less, and more preferably 40% by mass or less.
[0064] <Method for preparing resin composition for shrink label> The method for preparing the resin composition for shrink labels of the present embodiment is not particularly limited. As an example, the resin composition for shrink labels can be prepared by adding all of the components and stirring and mixing them with a stirring device.
[0065] <Shrink film> The shrink film (shrinkable plastic film) to which the resin composition for shrink labels of the present embodiment is applied is not particularly limited. Examples of the shrink film include a shrinkable polypropylene film, a shrinkable polyvinyl chloride film, and a shrinkable polyethylene phthalate film.
[0066] <Printing method for shrink label resin composition> The method of producing a printed matter by printing the resin composition for shrink labels of the present embodiment on a shrink film is not particularly limited. As an example, the printed matter is obtained by printing the resin composition for shrink labels on the above-mentioned shrink film, which is a printing substrate, preferably by using a gravure printing machine or a flexographic printing machine. Conventionally known conditions are appropriately adopted as printing conditions.
[0067] A coating film of the resin composition for shrink labels of the present embodiment is formed on the printed matter. The coating film has excellent adhesion to shrink films, abrasion resistance, hot water resistance, whitening resistance, slipping properties and leveling properties. EXAMPLES
[0068] The present invention will be described in more detail below with reference to the following examples. The present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass". The materials used in the following examples and comparative examples are as follows. The units of values in the columns relating to each component and the total in the tables are "% by mass".
[0069] The raw materials used in this example are shown below. (Acrylic resin A) Acid value 50mgKOH / g, Tg=0℃, solid content 37.0% by mass <Preparation of Acrylic Resin A> A copolymer composed of acrylic acid, methyl methacrylate, and styrene was dissolved in aqueous ammonia to obtain an aqueous solution as a polymeric emulsifier. Next, to form the core, methyl methacrylate, 2-ethylhexyl acrylate, and diacetone acrylamide were added and emulsion polymerization was carried out by a conventional method. After that, 1% by mass of adipic acid dihydrazide (ADH) was added to the obtained acrylic emulsion solution to prepare an acrylic emulsion liquid (acrylic resin A). (Water-soluble acrylic resin) Joncryl HPD 196: BASF, acid value 200 mg KOH / g, solid content 36.0 mass% Hiros-X DL-4036: Seiko PMC Corporation, acid value 80 mg KOH / g, solid content 20.7% by mass (Silicone compounds) Carboxyl group-containing silicone compounds X-22-162C: Shin-Etsu Chemical Co., Ltd., modified at both ends, viscosity (25°C): 220 mm 2 / s, specific gravity: 0.98, refractive index: 1.406, functional group equivalent: 2300g / mol X-22-3701E: Shin-Etsu Chemical Co., Ltd., side chain modified, viscosity (25°C): 2000mm 2 / s, specific gravity: 0.98, refractive index: 1.409, functional group equivalent: 4000g / mol X-22-3710: Shin-Etsu Chemical Co., Ltd., one-end modified, viscosity (25°C): 60 mm 2 / s, specific gravity: 0.97, refractive index: 1.412, functional group equivalent: 1450g / mol Amino-modified silicone compounds KF-865: Shin-Etsu Chemical Co., Ltd., side chain modified, viscosity (25°C): 110mm 2 / s, specific gravity: 0.97, refractive index: 1.405, functional group equivalent: 5000g / mol (Crosslinking agent) Denacol EX-614B: Epoxy crosslinking agent, Nagase ChemteX Corporation, solid content 100% by mass SU-125F: Aziridine-based crosslinking agent, manufactured by Meisei Chemical Industry Co., Ltd., solid content 20% by mass (others) Surfynol 104E: Leveling agent, manufactured by Nissin Chemical Industry Co., Ltd., solid content 50% by mass TEGO Foamex 825: Defoamer, manufactured by EVONIK, solid content 20% by weight Chemipearl W-401: Wax, manufactured by Mitsui Chemicals, Inc., solid content 40% by mass SN Thickener 601: Viscosity modifier, manufactured by San Nopco Ltd., solid content 40% by mass
[0070] <Examples 1 to 15 and Comparative Examples 1 to 9> (Preparation of Resin Composition for Shrink Label) According to the recipes shown in Tables 1 and 2, the materials were mixed by stirring to prepare respective resin compositions for shrink labels.
[0071] [Table 1]
[0072] [Table 2]
[0073] The obtained resin composition for shrink labels was used to prepare print samples, which were then evaluated as follows. The results are shown in Tables 1 and 2.
[0074] <Preparation of printed sample> Each shrink label resin composition was applied to a shrinkable PET film (Toyobo Co., Ltd., SP809#40μm) in a wet coating amount of 4.0g / m2 using a proofer. 2 Then, the coating was dried to prepare a print sample.
[0075] <Adhesiveness> Adhesion was evaluated according to the following criteria based on the degree to which the overcoat layer peeled off when cellophane tape was applied to the overcoat layer (varnish surface) of the printed sample and then quickly peeled off. (Evaluation Criteria) ◯: The percentage of the overcoat layer peeled off from the base film was less than 5% in terms of area. Δ: The percentage of the overcoat layer peeled off from the base film was 5% or more and less than 30% in terms of area ratio. ×: The area ratio of the overcoat layer peeled off from the base film was 30% or more. <Abrasion resistance> The overcoat layer (varnish surface) of the printed sample was rubbed back and forth 1,000 times with a Gakushin tester (Daiei Scientific Instruments Manufacturing Co., Ltd.) using a K-liner as the friction element and a load of 500 g, and the abrasion resistance was evaluated from the degree to which the overcoat layer fell off. (Evaluation Criteria) ◯: The overcoat layer did not fall off. Δ: Fall-off of the overcoat layer occurred in less than 50% by area. ×: The overcoat layer fell off in an area ratio of 50% or more. <Hot water resistance> The printed sample was wrapped around a commercially available PET bottle (500ml square bottle) with the printed side facing outwards, and then exposed to hot water at 90°C to shrink the printed sample and attach it to the bottle. The inside of the PET bottle with the printed sample attached was filled with hot water at 90°C, and the wet PET bottles were stacked in a state of close contact with each other. After cooling naturally in this state for 30 minutes, the water in the contents was removed and the bottle was dried in a 40°C oven. After drying, the hot water resistance of the printed material was evaluated based on the presence or absence of blocking of the printed material. (Evaluation Criteria) ○: No blocking was observed. △: Some blocking was observed. ×: Considerable blocking was observed. <Whitening property> Both ends of the print sample were fixed to stainless steel plates and immersed in hot water at 90°C for 20 seconds to shrink and dry. The haze value of the print that had shrunk by 50% was measured using a haze meter to evaluate the whitening property. (Evaluation Criteria) A: The haze value was less than 50. Δ: The haze value was 50 or more and less than 70. ×: The haze value was 70 or more. <Slipperiness> The static and dynamic friction coefficients were measured using an autograph AGS-500B manufactured by Shimadzu Corporation. One printed sample was attached to a 200g weight with the printed surface facing outward, and another printed sample was fixed to the test stand with the printed surface facing outward. The weight was gently placed on the test stand, the tester was started, and the weight was pulled at a tensile speed of 100mm / min. The static friction force was observed as the maximum value recorded immediately after starting, and the dynamic friction force was observed as the average value recorded while the weight was moving. The static and dynamic friction coefficients were calculated using the following formula using the observed static and dynamic friction forces, and the slipperiness was evaluated. (Coefficient of friction) = (frictional force) / (weight of the weight) (Evaluation Criteria) ◯: The static and dynamic friction coefficients were 0.20 or more and less than 0.30. △: The static and dynamic friction coefficients were 0.15 or more and less than 0.20, or 0.30 or more and less than 0.50. ×: The static and dynamic friction coefficients were less than 0.15 or 0.50 or more. <Leveling ability> The printed sample was observed and evaluated for uneven printing caused by the varnish not spreading smoothly in the applied area. (Evaluation Criteria) ○: No unevenness was observed at all. △: Slight unevenness was observed. ×: Considerable unevenness was observed.
[0076] As shown in Table 1, the coating films obtained using the resin compositions for shrink labels of Examples 1 to 15 of the present invention exhibited excellent adhesion, abrasion resistance, hot water resistance, whitening resistance, slippage and leveling properties.
Claims
1. The composition includes an aqueous acrylic resin emulsion, a carboxyl group-containing silicone compound, and an aqueous medium, The content of the carboxyl group-containing silicone compound in the resin composition for shrink labels is 0.1 to 1.1% by mass.
2. 2. The resin composition for shrink labels according to claim 1, further comprising a pigment.
3. 3. The resin composition for shrink labels according to claim 1, further comprising a crosslinking agent.
4. 4. The resin composition for shrink labels according to claim 3, wherein the solid content of the crosslinking agent is 0.5 to 6.5% by mass in the resin composition for shrink labels.
5. 4. The resin composition for shrink labels according to claim 3, wherein the crosslinking agent is at least one of an epoxy-based crosslinking agent and an aziridine-based crosslinking agent.
Citation Information
Patent Citations
Water-based inks for shrinkable and non-shrinkable polymer films
JP2020501935A
Binder component, emulsion, emulsion manufacturing method, and water-based ink
JP7122482B1
Cited By
Water-based varnish compositions, laminates, and packaging materials
JP2026136490A
Water-based ink compositions, laminates, and packaging materials
JP2026136505A
Water-based varnish compositions, laminates, and packaging materials
JP7925101B2
Water-based ink compositions, laminates, and packaging materials
JP7925102B2