Method for producing valuable metal

By controlling the mass ratios of calcium and lithium oxides in the slag and adjusting heating temperatures during reduction melting, the method addresses safety and efficiency issues in recovering valuable metals from waste lithium ion batteries, enhancing productivity and reducing costs.

JP2024158388AInactive Publication Date: 2024-11-08SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023073545
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for recovering valuable metals from waste lithium ion batteries, such as those described in Patent Document 1, face safety issues due to erosion of the furnace walls and high costs due to the use of expensive materials like magnesia, and inefficiencies due to excessive slag production.

Method used

A method involving controlled reduction melting with specific mass ratios of calcium oxide to aluminum oxide and lithium oxide in the slag, along with controlled slag heating temperatures, minimizes the use of magnesia and optimizes slag viscosity, forming a protective coating on the furnace walls, thereby enhancing safety and efficiency.

Benefits of technology

This approach allows for safe and efficient recovery of valuable metals by reducing refractory erosion and slag generation, improving metal productivity and recovery rates while maintaining operational safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158388000001_ABST
    Figure 2024158388000001_ABST
Patent Text Reader

Abstract

To provide a method capable of safely and efficiently recovering valuable metals from a raw material containing waste lithium ion batteries or the like.SOLUTION: The present invention is a method for producing valuable metals from a raw material containing valuable metals, comprising a step of preparing a raw material containing lithium, aluminum, and valuable metals, and a step of applying a reductive melting process to the raw material to obtain a reducing product containing an alloy containing valuable metals and slag, and a step of separating the slug from the reducing product to recover the alloy, wherein the step of adding a flux containing calcium to the raw material to apply a reduction melting treatment is performed so that a mass ratio of calcium oxide / (aluminum oxide+calcium oxide) in the generated slag is 0.20 or more and 0.25 or less, and the mass ratio of lithium oxide / (lithium oxide+aluminum oxide) is 0.27 or more and 0.32 or less, and a reductive melting process is performed by setting a slag heating temperature at 1500°C or more and 1600°C or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing valuable metals from raw materials such as waste lithium ion batteries. [Background technology]

[0002] In recent years, lithium ion batteries have become popular as lightweight, high-power secondary batteries. The well-known lithium ion battery has a structure in which a negative electrode material, a positive electrode material, a separator, and an electrolyte are enclosed in an outer can.

[0003] For example, the exterior can is made of a metal such as aluminum (Al) or iron (Fe). The negative electrode material is made of a negative electrode active material (graphite, etc.) attached to a negative electrode current collector (copper foil, etc.). The positive electrode material is made of a positive electrode active material (lithium nickel oxide, lithium cobalt oxide, etc.) attached to a positive electrode current collector (aluminum foil, etc.). The separator is made of a porous resin film such as polypropylene. The electrolyte contains an electrolyte such as lithium hexafluorophosphate (LiPF6).

[0004] One of the main uses of lithium-ion batteries is in hybrid and electric vehicles. For this reason, it is expected that a large amount of lithium-ion batteries installed in these vehicles will be discarded in the future according to their life cycle. In addition, some lithium-ion batteries are discarded as defective products during manufacturing. There is a demand for recycling such used batteries and defective batteries generated during manufacturing (hereinafter referred to as "waste lithium-ion batteries") as resources.

[0005] As a method of recycling, a pyrometallurgical process has been proposed in which all used lithium-ion batteries are melted in a high-temperature furnace. In the pyrometallurgical process, crushed used lithium-ion batteries are melted and the valuable metals to be recovered, such as cobalt (Co), nickel (Ni), and copper (Cu), are separated and recovered from low-value-added metals, such as iron (Fe) and aluminum (Al), by utilizing the difference in oxygen affinity between them. In this method, low-value-added metals are oxidized as much as possible to produce slag, while oxidation of valuable metals is suppressed as much as possible to recover them as alloys.

[0006] Patent Document 1 discloses a method for recovering valuable metals including nickel and cobalt from waste lithium-ion batteries that contain nickel and cobalt. Specifically, the method includes a melting step in which waste batteries are melted to obtain a molten material, an oxidation step in which the molten material or the waste batteries before the melting step are subjected to an oxidation treatment of the waste batteries, and a slag separation step in which slag is separated from the molten material to recover an alloy containing valuable metals, and the melting step proposes a process in which calcium oxide is added to lower the liquidus temperature of the slag to recover valuable metals. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6819827 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the technology disclosed in Patent Document 1 still has problems. For example, in the method disclosed in Patent Document 1, if the slag liquidus temperature (hereinafter also referred to as the "slag melting point") is lowered too much by adding flux, the refractory material in the furnace wall of the treatment furnace is corroded. If such erosion occurs, there is a risk of the treated material leaking outside the furnace, which is a safety problem. In addition, the cost required for maintaining the refractory material in the furnace wall becomes enormous, making it impossible to recover valuable metals at low cost.

[0009] In response to such problems, the present applicant has proposed a method of adding magnesia (MgO) together with flux when performing reduction melting of raw materials (Patent Application No. 2022-155194). According to this method, a slag coating layer can be effectively formed on the furnace wall of the treatment furnace, and wear of the furnace can be suppressed, making it possible to perform safe and efficient treatment. However, although magnesia facilitates the generation of slag coating, it is a relatively expensive material, so it is desirable to reduce the amount of magnesia used. In addition, the addition of magnesia may increase the amount of slag generated, which may reduce the efficiency of the treatment.

[0010] The present invention has been proposed in consideration of the above-mentioned circumstances, and aims to provide a method for safely and efficiently recovering valuable metals from raw materials including waste lithium-ion batteries, etc. [Means for solving the problem]

[0011] The present inventors conducted extensive research and found that the above-mentioned problems can be solved without adding materials such as magnesia by controlling the mass ratios of calcium oxide / (calcium oxide + aluminum oxide) and lithium oxide / (lithium oxide + aluminum oxide) in the slag produced by reducing and melting the raw materials to fall within a specific range, and by controlling the slag heating temperature to fall within a specific range during the reducing and melting process, thereby completing the present invention.

[0012] (1) A first aspect of the present invention is a method for producing valuable metals from raw materials containing the valuable metals, the method comprising: a preparation step of preparing raw materials containing at least lithium (Li), aluminum (Al), and the valuable metals; a reduction and melting step of subjecting the raw materials to a reducing and melting treatment to obtain a reduced product containing an alloy containing the valuable metal and slag; and a slag separation step of separating the slag from the reduced product to recover the alloy. In either or both of the preparation step and the reducing and melting step, a flux containing calcium (Ca) is added to the raw materials, and in the reducing and melting step, the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the slag produced is 0.20 to 0.25 and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is 0.27 to 0.32, and the reducing and melting treatment is performed at a slag heating temperature of 1500°C to 1600°C.

[0013] (2) A second aspect of the present invention is a method for producing valuable metals according to the first aspect of the present invention, wherein the raw material includes discarded lithium-ion batteries.

[0014] (3) A third aspect of the present invention is a method for producing valuable metals according to the first or second aspect of the present invention, wherein the melting furnace used in the reduction melting process is provided with a means for cooling the furnace wall from the outside.

[0015] (4) A fourth aspect of the present invention is a method for producing valuable metals according to any one of the first to third aspects of the present invention, further comprising, prior to the reducing melting treatment, an oxidizing roasting step of oxidizing roasting the raw material to obtain an oxidized roasted product, and the oxidized roasted product obtained is subjected to the reducing melting treatment. Effect of the Invention

[0016] According to the present invention, it is possible to provide a method for safely and efficiently recovering valuable metals from raw materials including waste lithium ion batteries and the like. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a process diagram showing an example of the flow of a method for recovering valuable metals from waste lithium-ion batteries. [Diagram 2] FIG. 1 is a diagram showing a phase diagram of the Al2O3-CaO-Li2O system calculated using thermodynamic calculation software (FactSage), and is a diagram plotting the results of a melting test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described below. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.

[0019] ≪1. How to recover valuable metals≫ The method for producing valuable metals according to the present embodiment is a method for separating and recovering valuable metals from raw materials containing at least lithium (Li), aluminum (Al), and valuable metals. Therefore, it can also be said to be a method for recovering valuable metals. The method according to the present embodiment is mainly a method using a dry smelting process, but may be composed of a dry smelting process and a wet smelting process.

[0020] Specifically, the method according to the present embodiment includes a step of preparing raw materials containing at least lithium, aluminum, and valuable metals (preparation step), a step of subjecting the prepared raw materials to a reducing melting treatment to obtain a reduced product (melt) containing an alloy containing valuable metals and slag (reducing melting step), and a step of separating the slag from the reduced product to recover the alloy (slag separation step).

[0021] In this method, a flux containing calcium (Ca) is added to the raw materials in either or both of the preparation process and the reduction and melting process to lower the slag melting point.Then, in the reduction and melting process, the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the generated slag is set to 0.20 to 0.25, and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is set to 0.27 to 0.32, and the reduction and melting process is performed with the slag heating temperature set to 1500°C to 1600°C in order to operate at the melting point of the slag with these mass ratios.

[0022] In this method, no materials such as magnesia (MgO) are added, which would facilitate the formation of a slag coating on the refractory walls of the melting furnace.

[0023] Here, the valuable metal is a material to be recovered, and is, for example, at least one metal or alloy selected from the group consisting of copper (Cu), nickel (Ni), cobalt (Co), and combinations thereof. Note that, in the following, copper, nickel, and cobalt will be taken as examples of valuable metals for explanation.

[0024] [Preparation process] In the preparation step, the raw material to be treated is prepared. The raw material is the subject of treatment to recover valuable metals, and as described above, contains lithium and aluminum, as well as at least one valuable metal selected from the group consisting of copper, nickel, and cobalt. The raw material may contain these components (Li, Al, Cu, Ni, Co) in the form of metal, or in the form of a compound such as an oxide. The raw material may also contain inorganic or organic components other than these components.

[0025] The raw material is not particularly limited, and examples thereof include waste lithium ion batteries, dielectric materials (capacitors), magnetic materials, etc. Furthermore, the form of the raw material is not limited as long as it is suitable for the treatment in the reduction melting process described below. Furthermore, in the preparation process, the raw material may be subjected to a crushing process or the like to obtain a suitable form. Furthermore, in the preparation process, the raw material may be subjected to a heat treatment or a separation process to remove unnecessary components such as moisture and organic matter.

[0026] In the preparation step, a flux containing calcium (Ca) can be added to the raw material. The added flux will be described in detail later. In the method according to the present embodiment, the flux is added in either one or both of the preparation step and the reduction melting step.

[0027] [Reduction melting process] In the reduction melting process, the prepared raw materials are charged into a melting furnace and heated to perform a reduction melting process to obtain a reduced product, which contains the alloy and slag separately.

[0028] The reduction melting process is a process in which raw materials are heated and reduced and melted in a melting furnace to produce a reduced product. The purpose of this process is to convert low-value-added metals (e.g., Al) contained in the raw materials into oxides, while valuable metals (Cu, Ni, Co) are reduced and melted to recover as an integrated alloy. After the reduction melting process, a molten alloy is obtained. If the oxidizing roasting process described below is performed prior to the reduction melting process, the obtained oxidizing roasted product is charged into a melting furnace and heated to reduce and melt. This keeps low-value-added metals (e.g., Al) oxidized by the oxidizing roasting process as oxides, while valuable metals (Cu, Ni, Co) are reduced and melted to recover as an integrated alloy.

[0029] In the reduction melting treatment, it is preferable to introduce a reducing agent. In addition, it is preferable to use carbon and / or carbon monoxide as the reducing agent. Carbon has the ability to easily reduce valuable metals (Cu, Ni, Co) to be recovered. For example, 1 mole of carbon can reduce 2 moles of valuable metal oxides (copper oxide, nickel oxide, etc.). In addition, reduction methods using carbon or carbon monoxide are extremely safer than methods using metal reducing agents (for example, thermite reaction method using aluminum).

[0030] As the carbon, artificial graphite and / or natural graphite can be used, and coal or coke can also be used if there is no risk of impurity contamination.

[0031] The alloy produced by reduction melting contains valuable metals. Therefore, it is possible to separate components (alloys) containing valuable metals from other components in the reduction product. This is because low-value-added metals (such as Al) have high oxygen affinity, whereas valuable metals have low oxygen affinity. For example, aluminum (Al), lithium (Li), carbon (C), manganese (Mn), phosphorus (P), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu) are generally oxidized in the order of Al>Li>C>Mn>P>Fe>Co>Ni>Cu. In other words, aluminum (Al) is most easily oxidized, and copper (Cu) is least easily oxidized. Therefore, low-value-added metals (such as Al) are easily oxidized to become slag, and valuable metals (Cu, Ni, Co) are reduced to become metals (alloys). In this way, low-value-added metals and valuable metals can be efficiently separated into slag and alloys.

[0032] In the method according to the present embodiment, a flux containing calcium (Ca) can be added to the raw material during the reducing melting process. Specifically, the flux is added in either or both of the preparation process and the reducing melting process. The flux is mainly composed of calcium (Ca), and examples of the flux include calcium oxide (CaO) and calcium carbonate (CaCO3). However, if the raw material to be treated contains a necessary amount of calcium, it is not necessary to add a flux.

[0033] Additionally, the method does not add materials such as magnesia (MgO) to facilitate the formation of a slag coating at any step.

[0034] The method according to the present embodiment is characterized in that the amount of calcium-containing flux added is minimized and the raw materials are mixed, and a reduction melting process is performed so that the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the resulting slag is 0.20 to 0.25, and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is 0.27 to 0.32.

[0035] Here, since the alloy containing copper, nickel, and cobalt contains at least copper, the melting point of the alloy is 1300°C to 1400°C. In order to smoothly obtain an alloy (hereinafter also referred to as "metal") with such a melting point, it is necessary to set the heating temperature of the metal (hereinafter also simply referred to as "metal heating temperature") to 1350°C to 1450°C, and in order to maintain this metal heating temperature, it is necessary to set the heating temperature of the slag (hereinafter also simply referred to as "slag heating temperature") located on and in contact with the metal layer to 1500°C to 1600°C. In order to obtain such a slag heating temperature, the slag melting point needs to be 1400°C to 1500°C.

[0036] For example, if the slag melting point is less than 1400°C, the temperature difference with the slag heating temperature becomes large, making it difficult to form a slag coating on the refractory of the furnace wall of the treatment furnace used in the reduction melting process, which may result in the refractory of the furnace wall being eroded. Also, if the slag melting point exceeds 1500°C, the temperature difference with the slag heating temperature becomes small, which increases the viscosity of the slag generated, making it difficult to obtain metal smoothly, i.e., at a high recovery rate.

[0037] Therefore, in the method according to the present embodiment, the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the slag generated by the reduction melting treatment is set to 0.20 to 0.25 and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is set to 0.27 to 0.32 while adding a minimum amount of calcium-containing flux, thereby minimizing the melting point of the slag to a level at which a slag coating can be generated.

[0038] In this way, the reduction melting process is performed so that the slag produced has the above-mentioned composition by mass ratio, and a slag coating layer is produced on the furnace wall of the melting furnace, so there is no need to add materials such as magnesia to lower the viscosity of the slag and make it easier to produce the slag coating, and the amount of material used can be reduced. Furthermore, by not using materials such as magnesia and minimizing the amount of flux added to lower the slag melting point, the amount of slag produced can be reduced, and metal productivity can be greatly improved.

[0039] Lithium (Li) and calcium (Ca) contribute to lowering the melting temperature of the slag. Therefore, by controlling the composition of the slag to be within the above-mentioned mass ratio range in the generated slag, the melting temperature of the slag can be made, for example, 1600°C or lower. Furthermore, if there is a large amount of calcium in the slag, it becomes easier to remove phosphorus when it is contained in the raw material. This is because phosphorus becomes an acidic oxide when oxidized, whereas calcium becomes a basic oxide when oxidized. Therefore, the more calcium there is in the slag, the more basic the slag composition becomes, and as a result, it becomes easier to incorporate phosphorus into the slag and remove it.

[0040] Regarding the composition of the slag produced, if the mass ratio (conveniently referred to as "mass ratio A") expressed by calcium oxide / (aluminum oxide + calcium oxide) or the mass ratio (conveniently referred to as "mass ratio B") expressed by lithium oxide / (lithium oxide + aluminum oxide) is excessively high, specifically, if the mass ratio A exceeds 0.25 or the mass ratio B exceeds 0.32, the liquidus temperature of the slag drops too much and the melting point becomes, for example, less than 1400°C, and it becomes difficult to form a coating layer of the slag even if the furnace wall is cooled. Here, since the melting point of the obtained alloy composed of copper, nickel, and cobalt is about 1300°C to 1400°C, for example, in order to operate so that the metal heating temperature is 1350°C to 1450°C, that is, in order to give heat from the slag to the metal, it is necessary to set the slag temperature to 1500°C to 1600°C. However, if the melting point of the slag is less than 1400°C, the coating cannot be formed effectively and the refractory material of the furnace wall may be eroded.

[0041] Furthermore, if mass ratio A or mass ratio B is excessively low, specifically if mass ratio A is less than 0.20 or mass ratio B is less than 0.27, the liquidus temperature of the slag will be high, and the raw material to be melted will not be able to be sufficiently melted, which may make it difficult to efficiently recover valuable metals.

[0042] For this reason, as described above, the reducing melting process is carried out so that the mass ratio (mass ratio A) of calcium oxide / (aluminum oxide + calcium oxide) in the slag produced is 0.20 to 0.25, and the mass ratio (mass ratio B) of lithium oxide / (lithium oxide + aluminum oxide) is 0.27 to 0.32. This makes it possible to carry out the process safely while suppressing the erosion of the refractory material constituting the sidewall of the reducing melting furnace, and to recover valuable metals at a high recovery rate.

[0043] The amount of slag components (e.g., Al, Li, Ca) can be easily controlled by adjusting the composition of the raw materials and the amount of flux added to the raw materials. Specifically, for example, the amount of calcium (Ca) in the slag can be controlled by adding a calcium-containing flux to the material to be processed and adjusting the amount of the flux added. As described above, examples of calcium-containing flux include calcium oxide (CaO) and calcium carbonate (CaCO3). The amount of lithium (Li) and aluminum (Al) in the slag can be controlled by adjusting the composition of the raw materials in the preparation process.

[0044] In the reduction melting process, the heating temperature (slag heating temperature) is set to 1500°C or more and 1600°C or less. If the slag heating temperature exceeds 1600°C, thermal energy is wasted and the refractory materials such as the crucible constituting the melting furnace are rapidly worn out, which may reduce productivity. In particular, since lithium is contained in the slag by reducing and melting the raw material containing lithium, the wear of the refractory becomes significant, and for example, operation at a slag heating temperature exceeding 1600°C is difficult from the viewpoint of the wear of the refractory and the life of the melting furnace (furnace wall). In view of the upper limit of the slag heating temperature, it is preferable for the metal heating temperature to be in the range of 1350°C to 1450°C and the metal melting point to be in the range of 1300°C to 1400°C for smooth operation, i.e., for the separation of the metal and the slag, and for the formation of a slag coating on the refractory. In order to achieve such a metal melting point, it is preferable for the metal to contain copper (Cu).

[0045] On the other hand, if the slag heating temperature is less than 1500°C, the separation between the generated slag and the alloy may become poor, and the recovery rate of valuable metals may decrease.

[0046] It is preferable that the melting furnace is provided with a mechanism for cooling the furnace walls from the outside by water cooling or the like. By cooling the furnace walls from the outside, the temperature of the slag in contact with the inner refractory surface can be lowered below the liquidus temperature of the slag, and a solidified layer of slag (slag coating layer) is effectively formed on the refractory surface. When the slag coating layer is formed in this way, the refractory is protected and erosion of the refractory can be more effectively prevented.

[0047] The melting furnace is preferably a submerged arc furnace. As described above, in order to transfer heat from the slag to the metal, the temperature of the slag layer located on the upper side must be higher than that of the metal layer located on the lower side. In a submerged arc furnace, the slag layer itself generates heat as the electrodes are immersed in the slag, so that the operating temperature of the slag layer can be maintained at the highest level, which is preferable.

[0048] When an oxidizing roasting treatment (oxidizing roasting step) is performed prior to the reducing melting treatment, it is not necessary to perform an oxidation treatment during the reducing melting treatment. However, when the oxidation in the oxidizing roasting treatment is insufficient or when the purpose is to further adjust the degree of oxidation, an additional oxidation treatment may be performed during or after the reducing melting treatment. By performing the additional oxidation treatment, it is possible to adjust the degree of oxidation more precisely.

[0049] An example of a method for performing the additional oxidation treatment is to blow an oxidizing agent into the melt produced by the reducing melting treatment. Specifically, a metal tube (lance) is inserted into the melt produced by the reducing melting treatment, and the oxidizing agent is blown in by bubbling to perform the oxidation treatment. In this case, a gas containing oxygen, such as air, pure oxygen, or oxygen-enriched gas, can be used as the oxidizing agent.

[0050] Furthermore, in the reduction melting process, harmful substances such as dust and exhaust gas may be generated, but these can be rendered harmless by carrying out a known treatment such as exhaust gas treatment.

[0051] [Oxidation roasting process] In the method according to the present embodiment, a step of oxidizing roasting the raw material to obtain an oxidizing roasted product (oxidizing roasting step) can be further provided, as necessary, prior to the reducing melting treatment.

[0052] The oxidizing roasting process (oxidizing process) is a process in which raw materials are oxidized and roasted to produce oxidizing roasted products. Even if the raw materials contain carbon, the carbon can be oxidized and removed, and this makes it possible to promote the alloy integration of valuable metals in the reducing melting process. Specifically, in the reducing melting process, valuable metals are reduced to localized molten fine particles, and at this time, the carbon contained in the charge becomes a physical obstacle when the molten fine particles (valuable metals) aggregate, hindering the aggregation and integration of the molten fine particles and the resulting separation of metal (alloy) and slag, which may reduce the recovery rate of valuable metals. In this regard, by subjecting the raw materials to the oxidizing roasting process prior to the reducing melting process, the carbon in the raw materials can be effectively removed, which promotes the aggregation and integration of the molten fine particles (valuable metals) generated in the reducing melting process, thereby further increasing the recovery rate of valuable metals.

[0053] In the oxidizing roasting process, the degree of oxidation can be adjusted as follows. That is, as described above, aluminum (Al), lithium (Li), carbon (C), manganese (Mn), phosphorus (P), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu) are generally oxidized in the order of Al>Li>C>Mn>P>Fe>Co>Ni>Cu. In the oxidizing roasting process, the process is advanced until all of the aluminum is oxidized. The process may be accelerated until a portion of the iron is oxidized, but it is preferable to minimize the oxidation of cobalt and keep the oxidation degree at a level where the cobalt is not oxidized and recovered as slag.

[0054] In adjusting the degree of oxidation in the oxidation roasting process, it is preferable to introduce an appropriate amount of oxidizing agent. In particular, when using raw materials containing waste lithium-ion batteries, it is preferable to introduce an oxidizing agent and perform the treatment. Lithium-ion batteries contain metals such as aluminum and iron as exterior materials. They also contain aluminum foil and carbon materials as positive and negative electrode materials. Furthermore, in the case of battery packs, plastic is used as the external package. Since all of these materials act as reducing agents, the oxidation degree can be adjusted to an appropriate range by introducing an oxidizing agent.

[0055] The oxidizing agent is not particularly limited as long as it can oxidize carbon and low-value-added metals (such as Al), but it is preferable to use an oxygen-containing gas such as air, pure oxygen, or oxygen-enriched gas, which is easy to handle. The amount of oxidizing agent introduced is approximately 1.2 times (e.g., approximately 1.15 to 1.25 times) the amount (chemical equivalent) required for oxidation of each substance to be subjected to the oxidizing roasting treatment.

[0056] The heating temperature of the oxidizing roasting treatment is preferably 700° C. or higher and 1100° C. or lower, and more preferably 800° C. or higher and 1000° C. or lower. By setting the heating temperature at 700° C. or higher, it is possible to further increase the carbon oxidation efficiency and shorten the oxidation time. In addition, by setting the heating temperature at 1100° C. or lower, it is possible to reduce the thermal energy cost and increase the efficiency of the oxidizing roasting.

[0057] The oxidation roasting treatment can be carried out using a known roasting furnace. It is also preferable to use a furnace (backup furnace) different from the furnace used in the reduction melting treatment and carry out the treatment in the backup furnace. As the roasting furnace, any type of furnace can be used as long as it is possible to supply an oxidizing agent (oxygen, etc.) while roasting the ground material and carry out the treatment therein. Examples include a conventionally known rotary kiln and tunnel kiln (hearth furnace).

[0058] [Slag separation process] In the slag separation process, slag is separated from the reduced material obtained by the reduction melting process, and alloys containing valuable metals are recovered. Slag and alloys have different specific gravities, and since slag, which has a smaller specific gravity than alloys, collects on top of the alloys, they can be efficiently separated and recovered by gravity separation.

[0059] In addition, after the slag is separated from the reduced material in the slag separation process to recover the alloy, a sulfurization process may be performed to sulfurize the alloy obtained, or a crushing process may be performed to crush the mixture of the sulfide and the alloy obtained in the sulfurization process. Furthermore, the valuable metal alloy obtained through such a dry smelting process may be subjected to a hydrometallurgical process. By the hydrometallurgical process, impurity components can be removed, and valuable metals (Cu, Ni, Co) can be separated and refined and recovered. Examples of the treatment in the hydrometallurgical process include known methods such as neutralization and solvent extraction.

[0060] As described above, in the method according to the present embodiment, the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the resulting slag in the reducing melting treatment is set to 0.20 to 0.25, and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is set to 0.27 to 0.32. This allows the melting temperature of the slag to be at least 1600°C or less, for example 1500°C or less, and the viscosity of the slag can be reduced. The reducing melting treatment is then performed with the slag heating temperature set to 1500°C or more and 1600°C or less.

[0061] In this way, for example, when the melting temperature (melting point) of the slag is 1500°C, by setting the slag heating temperature to 1600°C, it is possible to obtain slag with a sufficiently low viscosity, and the slag and metal can be separated efficiently.

[0062] In addition, by not lowering the melting point of the slag too much, a coating (slag coating) can be applied between the slag and the furnace wall refractory, which protects the refractory on the side walls of the melting furnace and enables stable operation with a high level of safety.

[0063] At this time, the slag heating temperature is preferably 1500°C or higher, so that the metal temperature is about 1400°C or higher, and it is possible to ensure that the operating temperature of the metal is above the metal melting point, and the fluidity of the metal can be maintained. Note that it is preferable that the obtained alloy has a melting point of 1400°C or lower, that is, that it contains at least copper (Cu).

[0064] ≪2. Method for producing valuable metals from waste lithium-ion batteries≫ In the method according to the present embodiment, the raw material to be treated is not limited as long as it contains at least lithium (Li), aluminum (Al), and valuable metals. Among them, the raw material is preferably one containing a waste lithium ion battery.

[0065] Waste lithium-ion batteries contain lithium (Li) and valuable metals (Cu, Ni, Co), as well as low-value-added metals (Al, Fe) and carbon components. Therefore, by using waste lithium-ion batteries as a raw material, valuable metals can be efficiently separated and recovered. Note that the concept of waste lithium-ion batteries includes not only used lithium-ion batteries, but also defective products generated during the manufacturing process of the positive electrode material that constitutes the battery, residues from the manufacturing process, scraps, and other waste materials generated during the manufacturing process of lithium-ion batteries. Therefore, waste lithium-ion batteries can also be called lithium-ion battery waste materials.

[0066] Fig. 1 is a process diagram showing an example of the flow of a method for producing valuable metals from waste lithium-ion batteries. As shown in Fig. 1, this method includes a waste battery pretreatment process (S1) for removing the electrolyte and outer cans of the waste lithium-ion batteries, a crushing process (S2) for crushing the contents of the waste batteries to obtain a crushed material, an oxidation roasting process (S3) for oxidizing and roasting the crushed material, a reduction melting process (S4) for reducing and melting the oxidizing roasted material to obtain an alloy, and a slag separation process (S5) for separating slag from the reduced material obtained by the reduction melting process to recover the alloy.

[0067] In addition, although not shown, a sulfurization process for sulfurizing the obtained alloy and a crushing process for crushing the mixture of the sulfide obtained in the sulfurization process and the alloy may be provided after the slag separation process (S5). The details of each process are described below.

[0068] (Waste battery pre-treatment process) The waste battery pretreatment step S1 is carried out for the purpose of preventing explosion and rendering harmless the raw material waste lithium ion batteries, and removing the outer cans. Lithium ion batteries are sealed systems and contain electrolytes and the like inside. If they are crushed in their original state, there is a risk of explosion, which is dangerous, so it is preferable to discharge them or remove the electrolyte by some method. Furthermore, the outer cans are often made of metals such as aluminum (Al) and iron (Fe), and it is relatively easy to collect these metal outer cans as they are. In this way, by removing the electrolyte and the outer cans in the waste battery pretreatment step (S1), safety can be improved and the recovery rate of valuable metals (Cu, Ni, Co) can be increased.

[0069] The specific method of treatment in the waste battery pretreatment step S1 is not particularly limited, but may be, for example, a method of physically opening holes in the waste battery with a needle-shaped blade to remove the electrolyte, or a method of burning the waste battery to render it harmless.

[0070] (Crushing process) In the crushing step S2, the contents of the waste lithium-ion batteries are crushed to obtain crushed material. The purpose of the crushing process in the crushing step S2 is to increase the reaction efficiency in the dry smelting process. By increasing the reaction efficiency, the recovery rate of valuable metals (Cu, Ni, Co) can be increased.

[0071] The specific pulverization method is not particularly limited, and pulverization can be performed using a conventionally known pulverizer such as a cutter mixer.

[0072] In addition, when aluminum (Al) and iron (Fe) contained in the outer cans are to be recovered, the crushed material may be sieved using a sieve shaker. Aluminum (Al) can be easily turned into powder by light crushing, and can be efficiently recovered. Iron (Fe) contained in the outer cans may also be recovered by magnetic separation.

[0073] The waste battery pretreatment step S1 and the pulverization step S2 together correspond to the above-mentioned "preparation step."

[0074] (Oxidation roasting process) In the oxidizing roasting step S3, the pulverized material obtained in the pulverizing step S2 is oxidizing roasted to obtain an oxidizing roasted material. This step corresponds to the above-mentioned "oxidizing roasting step", and the details are as described therein.

[0075] (Reduction melting process) In the reducing and melting step S4, the oxidizing roasted product obtained in the oxidizing roasting step S3 is subjected to a reducing and melting treatment to obtain a reduced product. This step corresponds to the above-mentioned "reducing and melting step", and the details are as described therein.

[0076] In particular, in the method according to the present embodiment, a flux containing calcium (Ca) is added to the raw material in one or more of the waste battery pretreatment process, the pulverization process, and the reduction melting process.The reduction melting process is characterized in that the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the generated slag is 0.20 to 0.25, and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is 0.27 to 0.32, and the slag heating temperature is 1500°C to 1600°C.

[0077] This allows safe processing while suppressing erosion of the refractory material constituting the side wall of the melting furnace, and also allows valuable metals to be recovered at a high recovery rate.

[0078] (Slag separation process) In the slag separation step S5, the slag is separated from the reduced material obtained in the reduction melting step S4 to recover the alloy. This step corresponds to the above-mentioned "slag separation step", and the details are as explained therein.

[0079] In addition, after the slag separation process, a sulfurization process and a pulverization process may be performed. Furthermore, the obtained valuable metal alloy may be subjected to a hydrometallurgical process. The details of the sulfurization process, the pulverization process, and the hydrometallurgical process are as described above. EXAMPLES

[0080] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0081] [Flow of valuable metal recovery processing (operations at each step)] A process to recover valuable metals was carried out using waste lithium-ion batteries containing lithium (Li), aluminum (Al), and valuable metals (Cu, Ni, Co) as raw materials.

[0082] (Waste battery pre-treatment process and crushing process) First, as waste lithium-ion batteries, 18650 type cylindrical batteries, used automotive prismatic batteries, and defective products collected during the battery manufacturing process were prepared. Then, these waste lithium-ion batteries were immersed in salt water to discharge them, after which the moisture was removed and the electrolyte was decomposed and removed by roasting at a temperature of 260°C in the air, to obtain the battery contents.

[0083] Next, the battery contents were pulverized using a pulverizer (product name: Good Cutter, manufactured by Ujiie Seisakusho Co., Ltd.) to obtain a pulverized product.

[0084] (Oxidation roasting process) Next, the obtained pulverized material was subjected to oxidative roasting in a rotary kiln at a heating temperature of 900° C. for 180 minutes in the air.

[0085] (Reduction melting process) Next, the obtained oxidized roasted product was mixed so that the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) in the resulting slag would be the value shown in Table 1 below, and graphite powder was added as a reducing agent in an amount of 0.6 times the total mole number of valuable metals (Cu, Ni, Co) (i.e., 1.2 times the mole number of graphite powder required to reduce valuable metals), and calcium oxide (CaO) was added as a flux. The flux was added and mixed in an amount such that the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the slag produced by the reduction melting treatment would be the value shown in Table 1 below.

[0086] In addition, a submerged arc furnace was used as the melting furnace for the reduction melting treatment, and the furnace wall was cooled from the outside by a water-cooled jacket. Each test sample was heated to a predetermined reduction melting temperature (slag heating temperature) shown in Table 1 below to perform the reduction melting treatment, and valuable metals were alloyed to obtain alloys and slag.

[0087] (Slag separation process) The slag was separated from the resulting reduced product, and the alloy was recovered as a recovered alloy.

[0088] [Slag composition analysis] The components of the slag separated from the reduced product were analyzed as follows: The obtained slag was cooled, pulverized, and analyzed by fluorescent X-rays.

[0089] (Valuable metal recovery rate) The recovery rate of valuable metal (Co) was calculated based on the following formula 1. The components in the recovered alloy were analyzed by fluorescent X-rays. Valuable metal recovery rate (%) = (Weight of Co in recovered alloy) ÷ (Weight of Co in recovered alloy + Weight of Co in slag) × 100 ...(Formula 1)

[0090] [Evaluation results] Table 1 below shows the results of cobalt recovery rate and confirmation of the presence or absence of wear in the furnace wall refractory when the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) and the mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the obtained slag were changed and the slag was heated at slag heating temperatures of 1500° C. and 1600° C. The presence or absence of wear in the refractory was confirmed by visual inspection after the submerged arc furnace was turned off after the completion of these tests, together with confirmation of the presence or absence of the formation of a slag coating layer.

[0091] Figure 2 is a phase diagram of Al2O3-CaO-Li2O slag, where the results of the test on the presence or absence of a slag coating layer are plotted. The dashed line in Figure 2 indicates the liquidus calculated by thermodynamic calculation software (FactSage). This phase diagram does not include magnesia (MgO).

[0092] [Table 1]

[0093] As can be seen from the results in Table 1, in Examples 1 and 2, a slag coating layer was formed on the furnace wall of the melting furnace to protect the refractory, no wear of the refractory was observed, and processing was performed safely. In addition, the separation of the slag and metal was good, and good results were obtained with a cobalt recovery rate of 95% or more in all samples.

[0094] In addition, in Examples 1 and 2, a good slag coating layer was formed and the refractory material was protected without the need to add magnesia (MgO) etc. Also, by minimizing the amount of flux containing calcium that was added to lower the slag melting point, metal productivity was greatly improved.

[0095] On the other hand, in Comparative Examples 1 and 2, although a slag coating layer was formed, the cobalt recovery rate was lower than in the Examples. This is presumably because the estimated slag melting point in the obtained slag composition was around 1550°C, the slag was not completely melted, and the viscosity of the slag was high, which resulted in poor separation of the slag and metal, and the presence of many small metal particles in the slag is thought to have resulted in the low cobalt recovery rate.

[0096] In Comparative Example 3, the slag coating layer was not formed, the refractory was not protected, and the refractory was significantly worn. This is presumably because the liquidus temperature of the obtained slag composition was too low, and the estimated slag melting point was 1370°C, so the slag hardly solidified even when the furnace wall was cooled, and therefore the slag coating layer was hardly formed.

[0097] Reference Example 1 is an example in which magnesia (MgO) was added together with the flux and a reducing melting treatment was carried out so as to generate slag having the composition shown in Table 1. In Reference Example 1, the addition of magnesia allowed the refractory to be protected by the easy formation of a slag coating layer, but the addition of expensive magnesia reduced the treatment efficiency and increased the amount of slag.

Claims

1. A method for producing valuable metals from a raw material containing the valuable metals, comprising the steps of: A preparation step of preparing a raw material containing at least lithium (Li), aluminum (Al), and a valuable metal; a reducing and melting process for performing a reducing and melting process on the raw material to obtain a reduced product including an alloy containing the valuable metal and slag; A slag separation step of separating slag from the reduced material to recover an alloy, In either or both of the preparation step and the reduction melting step, a flux containing calcium (Ca) is added to the raw material, In the reduction melting step, The mass ratio of calcium oxide / (aluminum oxide + calcium oxide) in the generated slag is 0.20 or more and 0.25 or less, and the mass ratio of lithium oxide / (lithium oxide + aluminum oxide) is 0.27 or more and 0.32 or less, The slag heating temperature is set to 1500°C or higher and 1600°C or lower to carry out reduction melting treatment. A method for producing valuable metals.

2. The raw material includes waste lithium ion batteries; The method for producing valuable metals according to claim 1.

3. The melting furnace used in the reduction melting process is provided with a means for cooling the furnace wall from the outside. The method for producing valuable metals according to claim 1.

4. The method further includes an oxidizing roasting step of oxidizing roasting the raw material to obtain an oxidized roasted product prior to the reducing melting treatment, and the obtained oxidized roasted product is subjected to the reducing melting treatment. The method for producing valuable metals according to claim 1.

Citation Information

Patent Citations

  • Method for recovering valuable metals from waste lithium-ion batteries

    JP6819827B2