Electrode material for use in water electrolysis

By incorporating iron-containing oxides and hydroxides with nickel and cobalt in specific ratios, the electrode materials reduce overvoltage, enhancing conductivity and electrochemical activity for efficient hydrogen production in water electrolysis.

JP2024158424APending Publication Date: 2024-11-08SAKAI CHEM IND CO LTD

Patent Information

Application Number
JP2023073613
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional water electrolysis electrodes suffer from high overvoltage, which leads to energy inefficiency in hydrogen production, and there is a need for materials that can reduce this overvoltage effectively.

Method used

The use of electrode materials comprising at least one compound selected from iron-containing oxides and hydroxides, nickel, and cobalt, with a specific mass ratio of these components, enhances conductivity and electrochemically effective surface area, thereby reducing overvoltage.

Benefits of technology

The proposed electrode materials achieve lower overvoltage in water electrolysis, improving the efficiency of hydrogen production by increasing conductivity and electrochemical activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158424000001
    Figure 2024158424000001
Patent Text Reader

Abstract

To provide an electrode material for use in water electrolysis, having a lower overvoltage in water electrolysis relative to conventional electrode materials for use in water electrolysis.SOLUTION: An electrode material for use in water electrolysis includes at least one compound (A) selected from the group consisting of oxides containing iron and hydroxides containing iron, and at least one metal-containing component (B) selected from the group consisting of nickel, cobalt and oxides thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode material for water electrolysis, and more particularly to an electrode material for water electrolysis useful for producing hydrogen and oxygen, etc. [Background technology]

[0002] Hydrogen has been attracting attention in recent years as an environmentally friendly alternative to fossil fuels. There are various methods for producing hydrogen, such as reforming fossil fuels, using by-product gases from industrial processes, and gasifying biomass. However, a method for electrolyzing water using renewable energy is being developed as a clean method that does not emit carbon dioxide.

[0003] In water electrolysis, oxygen is generated at the anode and hydrogen is generated at the cathode when an electric current is passed through the water. In order for the electrode reaction to proceed, a voltage that is excessive relative to the theoretical voltage (overvoltage) must be applied to activate the reactant, water. However, because overvoltage is a cause of energy loss in electrolysis, technology to reduce the overvoltage is needed.

[0004] Concerning the technology for reducing the anode overvoltage, Non-Patent Document 1 discloses a composite oxide catalyst based on iron and calcium, such as CaFe2O4. However, since CaFe2O4 has no electrical conductivity, Non-Patent Document 1 adds carbon as an electrical conductivity assistant to measure the oxygen generation capacity, but carbon cannot be used in the anode environment of water electrolysis because it easily decomposes. CaFe2O4 alone has almost no electronic conductivity, so the electrochemically effective surface area is low, making it difficult to use CaFe2O4 as an anode catalyst under practical conditions.

[0005] Patent Document 1 discloses an anode for water electrolysis having a nickel porous substrate and a thin film containing a metal oxide with a perovskite structure having a composition represented by a specific formula formed on at least a part of the surface of the substrate. Patent Document 2 also discloses an anode for water electrolysis using a composite oxide catalyst with a perovskite structure. Patent Document 3 discloses a catalyst contained in an anode for generating oxygen by electrolysis of water, the catalyst being goethite particles with a cobalt content of 5 mol% to 45 mol% relative to iron, and having a Tafel gradient of 26 mV / dec to 55 mV / dec. Patent Document 4 discloses an electrode containing copper oxide, at least one selected from the group consisting of nickel, iron, and cobalt, and at least one selected from the group consisting of manganese, titanium, vanadium, chromium, molybdenum, and tungsten on a copper-containing electrode substrate. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2017 / 047792 [Patent Document 2] International Publication No. 2018 / 155503 [Patent Document 3] JP 2019-112697 A [Patent Document 4] JP 2021-070864 A [Non-patent literature]

[0007] [Non-Patent Document 1] Y Sugawara and 3 others, Applied Energy Materials, 2021, Vol. 4, p3057-3066 Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, various electrodes for water electrolysis have been developed, and techniques for reducing overvoltage have been investigated. However, conventional electrodes for water electrolysis are insufficient in reducing overvoltage, and there has been a demand for electrode materials for water electrolysis that have a lower overvoltage in water electrolysis than conventional electrode materials for water electrolysis.

[0009] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide an electrode material for water electrolysis that has a smaller overvoltage during water electrolysis than conventional electrode materials for water electrolysis. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into electrode materials for water electrolysis and found that overvoltage in water electrolysis can be reduced by using an electrode material that contains at least one compound selected from the group consisting of iron-containing oxides and iron-containing hydroxides, and at least one metal-containing component selected from the group consisting of nickel, cobalt, and oxides thereof. They then came to the conclusion that the above-mentioned problems can be solved in an excellent manner, and completed the present invention.

[0011] The present invention includes the following electrode materials for water electrolysis, etc. [1] An electrode material for water electrolysis, comprising: at least one compound (A) selected from the group consisting of iron-containing oxides and iron-containing hydroxides; and at least one metal-containing component (B) selected from the group consisting of nickel, cobalt, and oxides thereof. [2] The electrode material for water electrolysis according to [1] above, wherein the content of the metal-containing component (B) is 0.5 to 95 mass% relative to 100 mass% in total of the compound (A) and the metal-containing component (B). [3] The electrode material for water electrolysis according to [1] or [2] above, which is an electrode material for alkaline water electrolysis. [4] An electrode comprising the electrode material for water electrolysis according to any one of [1] to [3] above. [5] A water electrolysis cell comprising the electrode according to [4] above. Effect of the Invention

[0012] The electrode material for water electrolysis of the present invention has the above-mentioned configuration and has a smaller overvoltage in water electrolysis than conventional electrode materials for water electrolysis, and therefore can be suitably used for producing hydrogen by electrolysis of water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The preferred embodiments of the present invention are specifically described below, but the present invention is not limited to the following description, and can be modified as appropriate within the scope of the present invention. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below also falls within the preferred embodiments of the present invention.

[0014] 1. Electrode materials for water electrolysis The electrode material for water electrolysis of the present invention contains at least one compound (A) selected from the group consisting of iron-containing oxides and iron-containing hydroxides, and at least one metal-containing component (B) selected from the group consisting of nickel, cobalt, and oxides thereof. The electrode material for water electrolysis may contain the compound (A) and the metal-containing component (B), but it is preferable that the compound (A) and the metal-containing component (B) are at least partially adhered to each other. When the compound (A) and the metal-containing component (B) are adhered to each other, an interface is formed between the compound (A) and the metal-containing component (B). The electrode material for water electrolysis is more preferably in a form in which the metal-containing component (B) is supported on the compound (A). The electrode material for water electrolysis, by combining the compound (A) with the metal-containing component (B), can enhance the electrical conductivity of the iron-containing compound (A) which has low electronic conductivity, and facilitate the conduction of electrons from the catalyst surface to the electrode, thereby increasing the electrochemically effective area of ​​the water electrolysis electrode and increasing the electrolysis current value, thereby improving the mass activity.

[0015] The proportion of the metal-containing component (B) in the electrode material for water electrolysis is not particularly limited, but is preferably 0.5 to 95 mass% relative to 100 mass% in total of the compound (A) and the metal-containing component (B), thereby enabling the overvoltage in water electrolysis to be more sufficiently reduced. The proportion of the metal-containing component (B) is more preferably 1 to 95 mass%, even more preferably 5 to 90 mass%, even more preferably 10 to 85 mass%, still more preferably 20 to 80 mass%, even more preferably 30 to 75 mass%, and particularly preferably 35 to 70 mass%.

[0016] The electrode material for water electrolysis contains nickel and / or cobalt in the metal-containing component (B), and the ratio thereof is not particularly limited, but the ratio of nickel and / or cobalt is preferably 1 to 99 mol %, more preferably 50 to 90 mol %, relative to 100 mol % in total of nickel and / or cobalt in the metal-containing component (B) and iron in the compound (A).

[0017] The compound (A) in the electrode material for water electrolysis is at least one compound selected from the group consisting of iron-containing oxides and iron-containing hydroxides. The iron-containing oxide may be a composite oxide containing a metal element other than iron, so long as it contains iron and oxygen. The iron-containing oxide is represented by the following formula (1); Fe(III) x1 Fe(II) x2 M y O α1 (1) (In the formula, M represents a metal element other than iron. α1 represents the number of oxygen elements and is a number greater than 0. x1, x2, and y are the same or different and represent numbers greater than 0, with the proviso that at least one of x1 and x2 is a number greater than 0.)

[0018] M is not particularly limited as long as it is a metal element other than iron, and one or more kinds may be contained in the compound represented by the above formula (1). Examples of metals other than iron include monovalent to heptavalent metals.

[0019] The monovalent metal is not particularly limited, but examples thereof include lithium, sodium, potassium, rubidium, cesium, silver, copper(I), and the like.

[0020] The divalent metal is not particularly limited as long as it is other than iron, and examples thereof include nickel (II), cobalt (II), magnesium, calcium, barium, zinc, copper (II), manganese (II), chromium (II), etc. Among these, calcium is preferable.

[0021] The trivalent metal is not particularly limited as long as it is other than iron, but examples thereof include nickel (III), cobalt (III), aluminum, gallium, chromium (III), zirconium (III), manganese (III), yttrium, lanthanum, cerium (III), and gadolinium. The tetravalent metal is not particularly limited, but examples thereof include nickel (IV), cobalt (IV), titanium, zirconium (IV), manganese (IV), and the like.

[0022] Examples of the pentavalent metal include niobium, tantalum, and antimony. Examples of the hexavalent metal include molybdenum and tungsten. Heptavalent metals include manganese(VII) and technetium.

[0023] In the above formula (1), at least one of x1 and x2 may be a number greater than 0, but when x2 is 0, it is preferable that x1 is 1 or greater. When x1 is 0, x2 is preferably 1 or greater. Also, an embodiment in which x1 and x2 are each 1 or greater is one of the preferred embodiments. x1 and x2 are the same or different and are preferably a number of 5 or less, more preferably 4 or less, and further preferably 3 or less.

[0024] In the above formula (1), y represents the number of metal elements other than iron and is a number equal to or greater than 0. When the compound represented by the above formula (1) contains multiple types of metals other than iron, y represents the total number of metals other than iron. y is preferably a number of 5 or less, more preferably 4 or less, further preferably 3 or less, and particularly preferably 2 or less.

[0025] In the above formula (1), α1 represents the number of oxygen elements and is a number greater than zero. α1 is determined by x1, x2, and y in formula (1) and the valence m of the metal M, and satisfies α1 = 3 / 2x1 + x2 + 1 / 2Σ(m × y). In the above formula, Σ represents the sum of the products of the valences m and the number y of metals other than iron contained in the compound represented by formula (1).

[0026] M in the above formula (1) is preferably a metal other than iron and cobalt, and more preferably a metal other than iron, nickel and cobalt. The iron-containing oxide is preferably FeO, Fe2O3, Fe3O4, CaFe2O4, or the like, and more preferably Fe3O4 or CaFe2O4.

[0027] The iron-containing hydroxide may be a composite hydroxide containing a metal other than iron or O in addition to OH, so long as it contains iron and OH. The above-mentioned iron-containing hydroxide is preferably a hydroxide represented by the following formula (2); Fe(III) p1 Fe(II) p2 M q (OH) β O α2 (2) (wherein M represents a metal element other than iron; p1, p2, q, and α2 are the same or different and represent numbers of 0 or more, provided that at least one of p1 and p2 is a number greater than 0; and β represents the number of OH groups and is a number greater than 0). Specific examples of M in the above formula (2) are the same as M in formula (1).

[0028] In the above formula (2), at least one of p1 and p2 may be a number greater than 0, but when p2 is 0, it is preferable that p1 is 1 or greater. When p1 is 0, p2 is preferably 1 or more. In addition, p1 and p2 may each be 1 or greater. p1 and p2 may be the same or different and are preferably a number of 5 or less, more preferably 4 or less, and further preferably 3 or less.

[0029] In the above formula (2), q is a number of 0 or more. When the compound represented by the above formula (2) contains multiple types of metals other than iron, q represents the total number of metals other than iron. q is preferably a number of 5 or less, more preferably 4 or less, even more preferably 3 or less, and particularly preferably 2 or less. The embodiment in which q is 0 is also one of the preferred embodiments of the present invention.

[0030] In the above formula (2), α2 represents the number of oxygen atoms. It is preferably 5 or less, more preferably 3 or less, even more preferably 2 or less, and particularly preferably 1 or less. An embodiment in which α2 is 0 is also one of the preferred embodiments of the present invention. In the above formula (2), β represents the number of OH groups and is a number greater than 0. It is preferably 1 or more, and more preferably 2 or more. In addition, β is preferably a number of 5 or less, and more preferably 4 or less.

[0031] The above-mentioned iron-containing hydroxide is not particularly limited, but examples thereof include Fe(OH)2, Fe(OH)3, FeO(OH), iron-containing hydrotalcite, etc. Fe(OH)3 is preferred.

[0032] The metal-containing component (B) in the electrode material for water electrolysis is at least one selected from the group consisting of nickel, cobalt, and oxides thereof. The oxide may be an oxide of nickel and / or cobalt, and may be a composite oxide of nickel and cobalt. Nickel oxides include NiO and Ni2O3. Cobalt oxides include CoO, Co2O3, and Co3O4. The metal-containing component (B) is preferably metallic nickel, metallic cobalt, NiO, or Co3O4, and more preferably metallic nickel or NiO.

[0033] The above water electrolysis electrode material has a specific surface area of ​​5 to 250 m 2 / g. With such a specific surface area, the oil absorption amount when the electrode material for water electrolysis is applied to an electrode as a paste is in a suitable range. The specific surface area is more preferably 10 to 40 m 2 / g, more preferably 10 to 30 m 2 / g. The specific surface area can be measured by the method described in the Examples.

[0034] The above water electrolysis electrode material has a volume resistivity of 1.0×10 6 It is preferable that the volume resistivity is 5.0×10 or less. This increases the conductivity of the catalyst, and facilitates the electron conduction from the catalyst surface to the electrode and the electrical conduction between catalyst particles. 5 Ω cm or less, and more preferably 1.0×10 5 Ω·cm or less. The volume resistivity can be measured by the method described in the examples.

[0035] The water electrolysis electrode material may contain the compound (A) and the metal-containing component (B), but may also contain other components in addition to the compound (A) and the metal-containing component (B). The other components are not particularly limited, but examples thereof include hydroxides or oxides of metal elements other than iron, nickel and cobalt, metals, polymers, and the like. Examples of the metal other than iron, nickel and cobalt include the metals in M ​​described above. The content of the other components is not particularly limited, but is preferably 0 to 20 mass% relative to 100 mass% of the total of the compound (A) and the metal-containing component (B), more preferably 0 to 10 mass%, even more preferably 0 to 5 mass%, and most preferably 0 mass%.

[0036] 2. Manufacturing method of electrode material for water electrolysis The method for producing the electrode material for water electrolysis of the present invention is not particularly limited, and the electrode material can be produced by mixing compound (A) with the metal-containing component (B), or by mixing compound (A) and / or a raw material for compound (A) with the metal-containing component (B) and / or a raw material for metal-containing component (B), and calcining the mixture. The method for producing an electrode material for water electrolysis of the present invention preferably includes a step of mixing compound (A) and / or a raw material for compound (A) with metal-containing component (B) and / or a raw material for metal-containing component (B). The method for producing an electrode material for water electrolysis may include a step of firing the mixture obtained in the mixing step. When the raw material of the compound (A) and / or the raw material of the metal-containing component (B) is used in the mixing step, it is preferable to include a step of calcining the mixture obtained in the mixing step.

[0037] The method for producing an electrode material for water electrolysis of the present invention preferably includes a step of mixing at least one compound (A) selected from the group consisting of iron-containing oxides and iron-containing hydroxides and / or a raw material containing iron, with at least one metal-containing component (B) selected from the group consisting of nickel, cobalt, and oxides thereof and / or a raw material containing nickel or cobalt.

[0038] The raw material of the compound (A) that can be used in the above mixing step includes a compound containing an iron element. Examples of compounds containing iron element include iron nitrate (II), iron nitrate (III), iron chloride (II), iron chloride (III), iron sulfate (II), iron sulfate (III), iron acetate (II), basic iron acetate (III), iron carbonate (II), and other compounds, as well as hydrates of these compounds, and metallic iron.

[0039] As the raw material of the compound (A) that can be used in the mixing step, a compound containing a metal other than iron may be used together with the compound containing elemental iron. Examples of the compound containing a metal other than iron include nitrates, sulfates, carbonates, oxides, chlorides, hydroxides, acetates, and the like containing the metals represented by M above. When the metal other than iron in the raw material of compound (A) is calcium, examples of the metal include calcium carbonate, calcium chloride, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, and calcium acetate.

[0040] When the electrode material for water electrolysis of the present invention contains a composite oxide containing a metal other than iron as compound (A), it is preferable to use compound (A) obtained by calcining a mixture of at least one selected from the group consisting of iron oxide, iron hydroxide, and the above-mentioned compounds containing iron element and the above-mentioned compound containing a metal other than iron, nickel, and cobalt in the mixing step. The firing temperature in the above firing is preferably 300 to 1400°C. The firing time of the above firing is preferably 0.5 to 24 hours.

[0041] The raw material of the metal-containing component (B) that can be used in the mixing step may be a compound containing nickel and / or cobalt. Specifically, nickel nitrate (II), nickel sulfate (II), nickel chloride (II), nickel hydroxide (II), nickel acetate (II), nickel carbonate (II), basic nickel carbonate (II), and the like compounds and hydrates thereof, metallic nickel, etc.; cobalt acetate (II), cobalt nitrate (II), cobalt sulfate (II), cobalt chloride (II), cobalt hydroxide (II), cobalt carbonate (II), basic cobalt carbonate (II), and the like compounds and hydrates thereof, metallic cobalt, etc., and one or more of these can be used. Among these, nickel nitrate and cobalt acetate are preferred.

[0042] The step of mixing the compound (A) and / or the raw material of the compound (A) with the metal-containing component (B) and / or the raw material of the metal-containing component (B) may be dry mixing or wet mixing. When compound (A) and metal-containing component (B) are mixed, dry mixing is preferred. In the above mixing step, when the raw material of the compound (A) and / or the raw material of the metal-containing component (B) are used, the above mixing step is preferably wet mixing. As the solvent used in the wet mixing, water, alcohol, ketone, ether compound, etc. can be used, with water being preferred.

[0043] When a solvent is used in the mixing step, it is preferable to remove the solvent before the calcination step, so that the calcination step can be carried out efficiently. The method for removing the solvent is not particularly limited, but a method of evaporating the solvent is preferred, and a method of heating the mixture is preferred. The heating temperature is preferably 60 to 150°C, more preferably 80 to 120°C. The heating time is preferably from 5 to 30 hours, and more preferably from 10 to 20 hours.

[0044] In the step of firing the mixture obtained in the mixing step, the firing temperature is preferably 100 to 600°C, more preferably 200 to 600°C, and even more preferably 300 to 500°C. The firing time is preferably 10 to 480 minutes, and more preferably 30 to 240 minutes.

[0045] The firing can be carried out in an air atmosphere, a reducing atmosphere, an inert atmosphere, or a vacuum atmosphere. The reducing atmosphere can be an atmosphere containing more than 0 and 100 vol% or less of a reducing gas such as hydrogen in an inert gas such as helium, nitrogen, or argon. When metallic nickel and / or metallic cobalt is used as the metal-containing component (B) in the electrode material for water electrolysis of the present invention, it is preferable to carry out firing in a reducing atmosphere.

[0046] 3. Electrode for water electrolysis The electrode material for water electrolysis of the present invention can be suitably used for electrodes for water electrolysis. An electrode comprising the electrode material for water electrolysis of the present invention also constitutes the present invention. The water electrolysis electrode of the present invention is preferably used as an anode for water electrolysis.

[0047] The electrode is not particularly limited as long as it contains the electrode material for water electrolysis of the present invention, but it is preferable that the electrode contains a conductive base material. The electrode preferably has the electrode material for water electrolysis on a conductive base material. Examples of the material for the conductive substrate include nickel, materials containing nickel as a main component, titanium, GC (glassy carbon), tantalum, zirconium, gold, silver, copper, palladium, platinum, cobalt, rhodium, and iridium.

[0048] 4.Water electrolysis cell The water electrolysis electrode of the present invention can be suitably used in a water electrolysis cell. A water electrolysis cell including the water electrolysis electrode of the present invention also constitutes the present invention. The water electrolysis cell preferably includes at least the water electrolysis electrode of the present invention as an anode, and a cathode electrically connected thereto.

[0049] 5. Hydrogen Production Methods The electrode material for water electrolysis of the present invention can be suitably used in a reaction for producing hydrogen by decomposing water. A method for producing hydrogen, comprising a step of decomposing water using the electrode material for water electrolysis of the present invention, also constitutes the present invention. EXAMPLES

[0050] In order to explain the present invention in detail, specific examples are given below, but the present invention is not limited to these examples. Unless otherwise specified, "%" means "% by weight." The methods for measuring each physical property are as follows.

[0051] <Measurement of volume resistance of catalyst> The powder volume resistivity was measured using a powder resistivity measurement system MCP-PD51 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) The powder resistivity measurement system is composed of a hydraulic powder press unit, a four-point probe, and a high-resistance measurement device (Loresta GX MCP-T700, manufactured by the same company). The volume resistivity (Ω·cm) was calculated according to the following procedure. 1) The sample powder was placed into a press jig (diameter 20 mm) equipped with a four-point probe on the bottom, and the jig was set in the pressurizing section of the powder resistivity measurement system. 2) After the powder press part was pressurized to 20 kN, the powder thickness was measured with a digital caliper and the resistance value was measured with a high resistance measuring device. 3) The volume resistivity (Ω cm) was calculated from the powder thickness and resistance value using the following formula. (Volume resistivity) = (Resistance value) x (Resistivity correction coefficient) x (Thickness)

[0052] <Specific surface area (BET-SSA) > In accordance with the provisions of JIS Z8830 (2013), the samples were heat-treated in a nitrogen atmosphere at 200°C for 60 minutes, and then the specific surface area (BET-SSA) was measured using a specific surface area measuring device (manufactured by Mountec Co., Ltd., product name "Macsorb HM-1220").

[0053] <Oxygen generation overvoltage and mass activity> The oxygen evolution overvoltage was measured by changing the potential from 1.2 V to 1.8 V by 10 mVs at room temperature with a 1 M potassium hydroxide solution saturated with oxygen at an electrode rotation speed of 1600 rpm. -1 The measurement was performed by sweeping at a rate of 1.0 V. The potassium hydroxide solution, which was the electrolyte, was saturated by bubbling oxygen for 1 hour before the measurement. The measurement was performed using the three-electrode method, with a platinum wire as the counter electrode and a mercury-mercury oxide electrode (Hg / HgO) as the reference electrode. The oxygen evolution overpotential was calculated by subtracting 1.23 V, which is the redox potential for oxygen evolution from water, from the voltage obtained at 10 mA. The mass activity was calculated as the current value per mg of catalyst by dividing the current value at 1.6 V during the above measurement by the amount of catalyst used.

[0054] <Example 1> 37.04g of iron oxide (III), 23.33g of calcium carbonate (manufactured by Sakai Chemical Industry Co., Ltd., product name "CWS"), 272.00g of 3mmΦ beads, and 120.75g of ion-exchanged water were wet-mixed for 30 minutes at 250 rpm using a planetary ball mill (manufactured by Fritsch, P-5). The beads were then removed and the mixture was heated and dried in a dryer set at 130°C to obtain a precursor powder. The obtained precursor powder was heated to 900°C in an air atmosphere and held for 4 hours, and then naturally cooled to room temperature to obtain a fired product. 54.00 g of the fired product was wet-ground in a planetary ball mill (Fritsch, P-5) at 250 rpm for 120 minutes, and then heated and dried at 130°C to obtain CaFe2O4 powder. 2.00 g of commercially available nickel oxide (II, III) manufactured by Wako Pure Chemical Industries, Ltd. and 2.00 g of the above CaFe2O4 powder were weighed and mixed in an agate mortar for 10 minutes to obtain Example 1 powder.

[0055] <Example 2> 28.82 g of nickel nitrate hexahydrate and 14 mL of ion-exchanged water were weighed and placed in an evaporating dish and stirred, and then 0.30 g of the CaFe2O4 powder obtained in Example 1 was weighed and placed in the evaporating dish and stirred. The mixture was heated on a hot stirrer set at 100-150°C to obtain a dry powder. The obtained dry powder was placed in an alumina boat, and heated to 400°C while passing a mixed gas containing 5 vol% hydrogen in nitrogen at 800 mL / min. The mixture was then kept at 400°C for 1 hour, and then naturally cooled to room temperature to obtain Example 2 powder.

[0056] <Example 3> The powder of Example 3 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 1.20 g, the amount of nickel nitrate hexahydrate added was 24.27 g, and the amount of ion-exchanged water added was 12 mL.

[0057] <Example 4> The powder of Example 4 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 3.00 g, the amount of nickel nitrate hexahydrate added was 22.14 g, and the amount of ion-exchanged water added was 9 mL.

[0058] <Example 5> The powder of Example 5 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 3.00 g, the amount of nickel nitrate hexahydrate added was 11.49 g, and the amount of ion-exchanged water added was 9 mL.

[0059] <Example 6> The powder of Example 6 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 5.00 g, the amount of nickel nitrate hexahydrate added was 7.98 g, and the amount of ion-exchanged water added was 15 mL.

[0060] <Example 7> The powder of Example 7 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 5.00 g, the amount of nickel nitrate hexahydrate added was 2.79 g, and the amount of ion-exchanged water added was 15 mL.

[0061] <Example 8> The powder of Example 8 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 5.00 g, the amount of nickel nitrate hexahydrate added was 1.33 g, and the amount of ion-exchanged water added was 15 mL.

[0062] <Example 9> The powder of Example 9 was obtained in the same manner as in Example 2, except that the amount of CaFe2O4 powder added was 5.00 g, the amount of nickel nitrate hexahydrate added was 0.26 g, and the amount of ion-exchanged water added was 15 mL.

[0063] <Example 10> The powder of Example 10 was obtained in the same manner as in Example 4, except that the amount of nickel nitrate hexahydrate was 22.14 g, the amount of cobalt acetate tetrahydrate was 9.71 g, and the amount of ion-exchanged water added was 30 mL.

[0064] <Example 11> 9.71 g of cobalt (II) acetate tetrahydrate and 30 mL of ion-exchanged water were weighed and placed in an evaporating dish and stirred, and then 3.00 g of the CaFe2O4 powder obtained in Example 1 was weighed and placed in the evaporating dish and stirred. The mixture was heated on a hot stirrer set at 100-150°C to obtain a dry powder. The obtained dry powder was placed in an alumina boat, heated to 400°C in an air atmosphere, held at 400°C for 4 hours, and then naturally cooled to room temperature to obtain Example 11 powder.

[0065] <Example 12> Example 12 powder was obtained in the same manner as in Example 4, except that the amount of nickel nitrate hexahydrate added was 11.49 g and the amount of iron (III) oxide was 3.00 g instead of 3.00 g of CaFe2O4 powder.

[0066] <Example 13> 11.10 g of calcium chloride was dissolved in 400 mL of ion-exchanged water to obtain solution A. 54.06 g of iron chloride hexahydrate was dissolved in 800 mL of ion-exchanged water to obtain solution B. Solution A and solution B were mixed, and 1 mol / L of potassium hydroxide aqueous solution was added until the pH became 13. The obtained precipitate was filtered and washed with ion-exchanged water. Then, it was heated and dried in a dryer set at 130°C to obtain a mixture of calcium hydroxide and iron hydroxide. 2.00 g of the obtained mixture and 2.00 g of commercially available nickel (II, III) oxide powder manufactured by Wako Pure Chemical Industries, Ltd. were weighed and mixed in an agate mortar for 10 minutes to obtain Example 13 powder.

[0067] <Comparative Example 1> 5.00 g of nickel nitrate hexahydrate was placed in an alumina boat, heated to 400°C in an air atmosphere, held for 4 hours, and then naturally cooled to room temperature to obtain a sintered powder. Next, the boat was heated to 400°C while flowing a mixed gas containing 5 vol% hydrogen in nitrogen at 800 mL / min, held at 400°C for 1 hour, and then naturally cooled to room temperature to obtain a powder for Comparative Example 1.

[0068] <Comparative Example 2> Commercially available cobalt oxide (II, III) manufactured by Wako Pure Chemical Industries, Ltd. was used as Comparative Example 2 powder.

[0069] <Comparative Example 3> The CaFe2O4 powder obtained in Example 1 was used as Comparative Example 3 powder.

[0070] <Comparative Example 4> Comparative Example 4 powder was obtained in the same manner as in Example 4, except that 22.14 g of nickel nitrate hexahydrate was replaced with 8.73 g of copper nitrate trihydrate.

[0071] <Comparative Example 5> 2.00 g of commercially available titanium powder manufactured by Wako Pure Chemical Industries, Ltd. and 2.00 g of the CaFe2O4 powder obtained in Example 1 were weighed and mixed in an agate mortar for 10 minutes to obtain a powder for Comparative Example 5.

[0072] The volume resistivity and specific surface area of ​​the powders of Examples 1 to 13 and Comparative Examples 1 to 5 obtained in the Examples and Comparative Examples were measured. The results are shown in Table 1.

[0073] <Preparation of electrodes> 5 mg of the powders of Examples 1 to 13 or Comparative Examples 1 to 5 obtained in the Examples and Comparative Examples, 7 μL of 5.0 wt% Nafion (registered trademark) solution, 900 μL of isopropyl alcohol, and 2100 μL of ultrapure water were weighed and subjected to ultrasonic dispersion treatment for 30 minutes. 7 μL of the obtained slurry was dropped onto a rotating disk electrode to obtain various electrodes. The obtained electrodes were used to measure the oxygen generating overvoltage and mass activity, and the results are shown in Table 1.

[0074] [Table 1]

[0075] The above results show that, compared to Comparative Example 1, which used only Ni as the metal-containing component (B), and Comparative Example 3, which used only CaFe2O4 as the compound (A), Examples 2 to 9, which contained CaFe2O4 and Ni, had low overpotential and high mass activity. Moreover, compared to Comparative Example 2 which contained only Co3O4 as the metal-containing component (B), Example 11 which contained CaFe2O4 and Co3O4 also showed a low overpotential and a high mass activity. Furthermore, it was shown that when NiO was used as the metal-containing component (B) in Example 1, the same effects as those of the examples using Ni were exhibited. It was shown that when Co was used as the metal-containing component (B) in Example 10, the same effects as those in Example 11 using Co3O4 were exhibited. Furthermore, in Examples 12 and 13, when iron oxide or iron hydroxide was used as compound (A), it was shown that the overpotential was reduced and the mass activity was improved. On the other hand, in Comparative Examples 4 and 5, when compound (A) was combined with copper or titanium, the overvoltage could not be reduced, and the mass activity was not improved. From the above, it has become clear that by combining at least one compound (A) selected from the group consisting of iron-containing oxides and iron-containing hydroxides with at least one metal-containing component (B) selected from the group consisting of nickel, cobalt, and oxides thereof, it is possible to achieve both a reduction in overvoltage and an improvement in catalytic activity, and to increase mass activity.

Claims

1. An electrode material for water electrolysis comprising: at least one compound (A) selected from the group consisting of iron-containing oxides and iron-containing hydroxides; and at least one metal-containing component (B) selected from the group consisting of nickel, cobalt, and oxides thereof.

2. 2. The electrode material for water electrolysis according to claim 1, wherein a content of the metal-containing component (B) is 0.5 to 95 mass% relative to 100 mass% in total of the compound (A) and the metal-containing component (B).

3. The electrode material for water electrolysis according to claim 1 or 2, wherein the electrode material for water electrolysis is an electrode material for alkaline water electrolysis.

4. An electrode comprising the electrode material for water electrolysis according to claim 1 or 2.

5. A water electrolysis cell comprising the electrode according to claim 4.

Citation Information

Patent Citations

  • Catalyst and anode

    JP2019112697A

  • Electrode catalyst, method for producing the same, and method for producing hydrogen

    JP2021070864A

  • Positive electrode for water electrolysis, electrolysis cell and method for producing positive electrode for water electrolysis

    WO2017047792A1

  • Positive electrode, positive electrode for water electrolysis, electrolysis cell, and method for producing hydrogen

    WO2018155503A1

Cited By

  • Catalyst for water electrolysis, membrane-electrode assembly, water electrolysis module, and water electrolyzer