Method of processing substrate, method of manufacturing semiconductor device, program, and substrate processing device
By forming a carbonitride film through multiple cycles of nitrogen modification, the method addresses impurity issues in existing carbonitride films, enhancing ashing and etching resistance.
Patent Information
- Application Number
- JP2023073800
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-27
AI Technical Summary
Impurities such as hydrogen bonded to carbon in carbonitride films affect the properties of the film, leading to reduced ashing and etching resistance.
A method involving multiple cycles of film formation and modification, where a first film is formed with nitrogen and hydrogen bonds, followed by a second modification using a more reactive nitrogen-based modifier to reduce the hydrogen content and maintain carbon concentration, forming a denser and more resistant second film.
The process improves the ashing and etching resistance of the film by reducing hydrogen and other impurities while maintaining desired carbon levels, resulting in a film with enhanced properties.
Smart Images

Figure 2024158536000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a program, and a substrate processing apparatus. [Background technology]
[0002] 2. Description of the Related Art As one step in the manufacturing process of a semiconductor device, a process of forming a carbonitride film on a substrate by supplying a plurality of types of process gases to the substrate is performed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-153825 A Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, when a carbonitride film is formed on a substrate, impurities such as hydrogen (H) bonded to carbon (C) may remain in the carbonitride film and affect the properties of the film.
[0005] The present disclosure provides a technique capable of improving the properties of a film formed on a substrate. [Means for solving the problem]
[0006] According to one aspect of the present disclosure, (a) performing a cycle including a step of supplying a substrate with a source material including a predetermined element, carbon, and hydrogen, and a step of supplying the substrate with a first modifier including nitrogen a predetermined number of times, thereby forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon on the substrate; (b) supplying a second modifier, which is a compound or a derivative thereof containing a nitrogen-hydrogen bond and a nitrogen-nitrogen bond in one molecule, different from the first modifier, to the substrate on which the first film has been formed, to modify the first film into a second film containing the predetermined element, carbon, and nitrogen and having a reduced content of hydrogen bonded to the carbon compared to the first film; The present invention provides a technique having the following features: Effect of the Invention
[0007] According to the present disclosure, it is possible to improve the characteristics of a film formed on a substrate. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace portion in vertical cross section. [Diagram 2] FIG. 2 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace portion in a cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 3 is a schematic configuration diagram of a controller of a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller. [Figure 4] FIG. 4 is a flow diagram showing a substrate processing process suitably used in one embodiment of the present disclosure. [Diagram 5] Fig. 5(A) is a diagram for explaining the state on the surface of a substrate when a first modifier is supplied onto the substrate on which raw material is adsorbed, and Fig. 5(B) is a diagram for explaining the state on the surface of a substrate when a second modifier is supplied onto the substrate on which raw material is adsorbed. [Figure 6] FIG. 6 is a flow diagram showing a modified example of a substrate processing process that is preferably used in one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described mainly with reference to Figures 1 to 5. Note that all of the drawings used in the following description are schematic, and the dimensional relationships of the elements, the ratios of the elements, etc. shown in the drawings do not necessarily match the actual ones. Furthermore, the dimensional relationships of the elements, the ratios of the elements, etc. between multiple drawings do not necessarily match.
[0010] (1) Configuration of the substrate processing device 1, the process furnace 202 has a heater 207 as a heating mechanism (temperature adjustment unit). The heater 207 is cylindrical and is installed vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) gas by heat.
[0011] A reaction tube 203 is disposed inside the heater 207 concentrically with the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A processing chamber 201 is formed in the cylindrical hollow portion of the reaction tube 203. The processing chamber 201 is configured to be capable of accommodating a wafer 200 as a substrate. Processing of the wafer 200 is performed in this processing chamber 201.
[0012] Nozzles 249a and 249b are provided in the processing chamber 201 so as to penetrate the lower sidewall of the reaction tube 203. Gas supply pipes 232a and 232b are connected to the nozzles 249a and 249b, respectively.
[0013] Gas supply pipes 232a and 232b are provided with mass flow controllers (MFCs) 241a and 241b, which are flow rate controllers (flow rate control parts), and valves 243a and 243b, which are on-off valves, in order from the upstream side of the gas flow. Gas supply pipe 232c is connected to the downstream side of valve 243a of gas supply pipe 232a. Gas supply pipes 232d and 232e are connected to the downstream side of valve 243b of gas supply pipe 232b. Gas supply pipes 232c, 232d, and 232e are provided with MFCs 241c, 241d, and 241e, and valves 243c, 243d, and 243e, in order from the upstream side of the gas flow.
[0014] As shown in FIG. 2, the nozzles 249a and 249b are provided in a circular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, from the lower part to the upper part of the inner wall of the reaction tube 203, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a and 249b are provided in a region horizontally surrounding the wafer arrangement region on the side of the wafer arrangement region where the wafers 200 are arranged, so as to extend along the wafer arrangement region. Gas supply holes 250a and 250b for supplying gas are provided on the side of the nozzles 249a and 249b, respectively. The gas supply holes 250a and 250b are each opened to face the center of the reaction tube 203, and can supply gas toward the wafers 200. A plurality of gas supply holes 250a and 250b are provided from the lower part to the upper part of the reaction tube 203.
[0015] A source gas containing a predetermined element, carbon (C), and hydrogen (H) is supplied from the gas supply pipe 232a into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a.
[0016] In this specification, the raw material gas refers to a raw material in a gaseous state, for example, a gas obtained by vaporizing a raw material that is in a liquid state at room temperature and normal pressure, a raw material that is in a gaseous state at room temperature and normal pressure, etc. When the word "raw material" is used in this specification, it may mean "a liquid raw material that is in a liquid state", "a raw material gas that is in a gaseous state", or both.
[0017] A first modifying agent containing nitrogen (N) is supplied from the gas supply pipe 232b through the MFC 241b, the valve 243b, and the nozzle 249b into the processing chamber 201. The first modifying agent may also be referred to as a first modifying gas or a first nitriding agent.
[0018] The term "agent" used in this specification includes at least one of a gaseous substance and a liquid substance. A liquid substance includes a mist substance. That is, a film-forming agent, a modifying agent, and an etching agent may include a gaseous substance, may include a liquid substance such as a mist substance, or may include both of them.
[0019] From the gas supply pipes 232c and 232d, an inert gas is supplied into the processing chamber 201 via the MFCs 241c and 241d, the valves 243c and 243d, the gas supply pipes 232a and 232b, and the nozzles 249a and 249b. The inert gas acts as a purge gas, a carrier gas, a dilution gas, etc.
[0020] A second modifying agent, which is different from the first modifying agent and has higher reactivity than the first modifying agent, is supplied from the gas supply pipe 232e through the MFC 241e, the valve 243e, the gas supply pipe 232b, and the nozzle 249b into the processing chamber 201. The second modifying agent may also be referred to as a second modifying gas or a second nitriding agent.
[0021] A raw material gas supply system (raw material supply system) that supplies a raw material gas is mainly composed of the gas supply pipe 232a, the MFC 241a, and the valve 243a. A first modifying agent supply system (first modifying gas supply system, first nitriding agent supply system) that supplies a first modifying agent is mainly composed of the gas supply pipe 232b, the MFC 241b, and the valve 243b. An inert gas supply system that supplies an inert gas is mainly composed of the gas supply pipes 232c, 232d, the MFCs 241c, 241d, and the valves 243c, 243d. A second modifying agent supply system (second modifying gas supply system, second nitriding agent supply system) that supplies a second modifying agent is mainly composed of the gas supply pipe 232e, the MFC 241e, and the valve 243e.
[0022] Any or all of the various supply systems described above may be configured as an integrated supply system 248 in which the valves 243a-243e and the MFCs 241a-241e are integrated. The integrated supply system 248 is connected to the gas supply pipes 232a-232e, and the supply operation of various gases into the gas supply pipes 232a-232e, i.e., the opening and closing operation of the valves 243a-243e and the flow rate adjustment operation by the MFCs 241a-241e, are controlled by a controller 121, which will be described later. The integrated supply system 248 is configured as an integrated or split type integrated unit, and can be attached and detached to and from the gas supply pipes 232a-232e, etc., in units of integrated units, and is configured so that maintenance, replacement, expansion, etc. of the integrated supply system 248 can be performed in units of integrated units.
[0023] An exhaust pipe 231 for exhausting the atmosphere in the processing chamber 201 is connected to the lower side wall of the reaction tube 203. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 is configured to be able to perform evacuation and stop evacuation in the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is in operation, and further, to adjust the pressure in the processing chamber 201 by adjusting the valve opening based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is in operation. An exhaust system is mainly configured by the exhaust pipe 231, the pressure sensor 245, and the APC valve 244. The vacuum pump 246 may be included in the exhaust system.
[0024] Below the reaction tube 203, a seal cap 219 is provided as a furnace port cover capable of airtightly closing the lower end opening of the reaction tube 203. The seal cap 219 is made of a metal material such as SUS and is formed in a disk shape. An O-ring 220 is provided on the upper surface of the seal cap 219 as a seal member that contacts the lower end of the reaction tube 203. Below the seal cap 219, a rotation mechanism 267 is provided for rotating the boat 217 described later. A rotation shaft 255 of the rotation mechanism 267 is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be vertically raised and lowered by a boat elevator 115 as a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transfer device (transfer mechanism) that transfers the wafers 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219.
[0025] The boat 217 as a substrate support is configured to support a plurality of wafers 200, for example 25 to 200, in multiple stages in a horizontal position and aligned vertically with their centers aligned, i.e., arranged at intervals. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, heat insulating plates 218 made of a heat-resistant material such as quartz or SiC are supported in multiple stages in a horizontal position.
[0026] A temperature sensor 263 serving as a temperature detector is installed in the reaction tube 203. By adjusting the power supply to the heater 207 based on temperature information detected by the temperature sensor 263, the temperature distribution in the process chamber 201 becomes a desired one. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.
[0027] As shown in FIG. 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122 configured as, for example, a touch panel is connected to the controller 121. An external storage device 123 can be connected to the controller 121. The substrate processing apparatus may be configured to include one control unit or multiple control units. That is, the control for performing the processing sequence described later may be performed using one control unit or multiple control units. The multiple control units may be configured as a control system connected to each other by a wired or wireless communication network, and the control for performing the processing sequence described later may be performed by the entire control system. In this specification, when the term "control section" is used, it may include one control section, or may include multiple control sections, or may include a control system made up of multiple control sections.
[0028] The storage device 121c is composed of, for example, a flash memory, an HDD (Hard Disk Drive), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe in which procedures and conditions of a substrate processing process described later are written, etc. are readably stored in the storage device 121c. The process recipe is a combination of procedures in a substrate processing process described later that is executed by the controller 121 to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. In addition, the process recipe is also simply referred to as a recipe. In this specification, when the word program is used, it may include only a recipe, only a control program, or both. The RAM 121b is configured as a memory area (work area) in which programs, data, etc. read by the CPU 121a are temporarily stored.
[0029] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241e, the valves 243a to 243e, the pressure sensor 245, the APC valve 244, the vacuum pump 246, the temperature sensor 263, the heater 207, the rotation mechanism 267, the boat elevator 115, and the like.
[0030] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to an input of an operation command from the input / output device 122, etc. The CPU 121a is configured to be capable of controlling the flow rate adjustment operation of various gases by the MFCs 241a-241e, the opening and closing operations of the valves 243a-243e, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotation mechanism 267, the lifting and lowering operation of the boat 217 by the boat elevator 115, etc., in accordance with the contents of the read recipe.
[0031] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 in a computer. The external storage device 123 includes, for example, a magnetic disk such as an HDD, an optical disk such as a CD, a magneto-optical disk such as an MO, and a semiconductor memory such as a USB memory. The storage device 121c and the external storage device 123 are configured as computer-readable recording media on which a program is recorded. Hereinafter, these are collectively referred to as recording media. When the term recording media is used in this specification, it may include only the storage device 121c alone, only the external storage device 123 alone, or both of them. The program may be provided to the computer using a communication means such as the Internet or a dedicated line, without using the external storage device 123.
[0032] (2) Substrate processing An example of performing, as one step of a semiconductor device manufacturing process using the processing furnace 202 of the above-mentioned substrate processing apparatus, a step of forming a first film containing predetermined elements, N, C, and H bonded to C on a wafer 200 having a silicon film (Si film) formed on its surface, and a step of modifying the first film into a second film containing predetermined elements, C, and N and having a reduced content of H bonded to C compared to the first film, will be described mainly with reference to Figures 4 and 5. In the following description, the operation of each part constituting the substrate processing apparatus is configured to be controllable by a controller 121.
[0033] The term "wafer" used in this specification may mean the wafer itself or a laminate of the wafer and a predetermined layer or film formed on its surface. The term "surface of a wafer" used in this specification may mean the surface of the wafer itself or the surface of a predetermined layer or the like formed on the wafer. When described in this specification, "forming a predetermined layer on a wafer" may mean forming a predetermined layer directly on the surface of the wafer itself or forming a predetermined layer on a layer or the like formed on the wafer. When used in this specification, the term "substrate" is synonymous with the term "wafer".
[0034] [First film formation process (also called film formation process)] (Wafer charging and boat loading, step S11) A plurality of wafers 200 are loaded (wafer charge) into the boat 217. Then, as shown in Fig. 1, the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115 and carried (boat load) into the processing chamber 201. In this state, the seal cap 219 seals the lower end of the reaction tube 203 via the O-ring 220.
[0035] (Pressure adjustment and temperature adjustment, step S12) The vacuum pump 246 evacuates (reduced pressure exhausts) the processing chamber 201 so that the pressure in the space in which the wafer 200 exists becomes a desired pressure (vacuum level). At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. The vacuum pump 246 is kept in a constantly operating state at least until the processing of the wafer 200 is completed. In addition, the wafer 200 in the processing chamber 201 is heated by the heater 207 so that the wafer 200 becomes a desired temperature. At this time, the power supply to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the processing chamber 201 has a desired temperature distribution. The heating of the processing chamber 201 by the heater 207 continues at least until the processing of the wafer 200 is completed. In addition, the rotation mechanism 267 starts to rotate the boat 217 and the wafer 200. The rotation mechanism 267 continues to rotate the boat 217 and the wafers 200 at least until the processing of the wafers 200 is completed.
[0036] (Preflow gas supply, step S13) First, a preflow gas is supplied to the wafer 200 in the processing chamber 201. As the preflow gas, a first modifying agent, which is a gas containing N, can be used. The details of the first modifying agent will be described later. This step is performed as a preflow for facilitating the adsorption of the source gas on the surface of the wafer 200 in step S15, which will be described later. Specifically, the valve 243b is opened to allow the first modifying agent to flow into the gas supply pipe 232b. The first modifying agent is adjusted in flow rate by the MFC 241b, supplied into the processing chamber 201 through the nozzle 249b, and exhausted from the exhaust pipe 231. At this time, the valve 243d is opened at the same time to allow an inert gas to flow into the gas supply pipe 232d. The inert gas is adjusted in flow rate by the MFC 241d, supplied into the processing chamber 201 together with the first modifying agent, and exhausted from the exhaust pipe 231.
[0037] In addition, in order to prevent the first modifying agent from entering the nozzle 249a, the valve 243c is opened to allow an inert gas to flow into the gas supply pipe 232c. The inert gas is supplied into the processing chamber 201 via the gas supply pipe 232a and the nozzle 249a, and is exhausted from the exhaust pipe 231.
[0038] By supplying a gas containing, for example, a hydrogen nitride compound as a preflow gas to the wafer 200, the natural oxide layer on the wafer 200 is nitrided to form an NH termination on the wafer 200. This increases the density of the NH termination on the surface of the wafer 200, which serves as an adsorption site for the source material, and forms a uniform adsorption surface, thereby improving the film formation rate. A suitable example of the preflow gas used in this step will be described later.
[0039] As the inert gas, in addition to nitrogen (N2) gas, rare gases such as argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, etc. One or more of these can be used as the inert gas.
[0040] (Removal of residual gas, step S14) Next, residual gas in the processing chamber 201 is removed. Specifically, after the NH termination is formed on the surface of the wafer 200, the valve 243b is closed and the supply of the first modifying agent is stopped. At this time, the APC valve 244 is left open, and the processing chamber 201 is evacuated by the vacuum pump 246, and the first modifying agent and by-products remaining in the processing chamber 201, which have not reacted or have contributed to the formation of the NH termination, are removed from the processing chamber 201. At this time, the valves 243c and 243d are left open, and the supply of the inert gas into the processing chamber 201 is maintained. The inert gas acts as a purge gas.
[0041] Thereafter, the following steps S15 to S19 are executed in sequence.
[0042] (Source gas supply, step S15) In this step, the raw material gas is supplied into the processing chamber 201. Specifically, while the APC valve 244 is opened to a predetermined degree, the valve 243a is opened to allow the raw material gas to flow into the gas supply pipe 232a. The raw material gas is adjusted in flow rate by the MFC 241a, supplied into the processing chamber 201 from the gas supply hole 250a, and exhausted from the exhaust pipe 231. At this time, the raw material gas is supplied to the wafer 200. At the same time, the valve 243c is kept open to allow the inert gas to flow into the gas supply pipe 232c. The inert gas is adjusted in flow rate by the MFC 241c, supplied into the processing chamber 201 together with the raw material gas, and exhausted from the exhaust pipe 231.
[0043] In addition, in order to prevent the source gas from entering the nozzle 249b, the valve 243d is kept open to allow an inert gas to flow into the gas supply pipe 232d. The inert gas is supplied into the processing chamber 201 via the gas supply pipe 232b and the nozzle 249b, and is exhausted from the exhaust pipe 231.
[0044] The processing conditions for supplying the raw material gas in this step are as follows: Treatment temperature: 150 to 800°C, preferably 180 to 700°C, more preferably 400 to 700°C Treatment pressure: 1 to 2666 Pa, preferably 67 to 1333 Pa Raw material gas supply flow rate: 1 to 2000 sccm, preferably 10 to 1000 sccm Raw material gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds Inert gas supply flow rate: 100 to 10,000 sccm From the viewpoint of increasing the processing speed, it is particularly preferable to set the processing temperature to substantially the same temperature in each step of the first film formation process.
[0045] In this disclosure, the expression of a numerical range such as "150 to 800°C" means that the lower limit and the upper limit are included in the range. Thus, for example, "150 to 800°C" means "150°C or more and 800°C or less." The same applies to other numerical ranges. In this disclosure, the processing temperature means the temperature of the wafer 200 or the temperature inside the processing chamber 201, and the processing pressure means the pressure inside the processing chamber 201. Furthermore, the processing time means the time the processing continues. These also apply in the following explanations.
[0046] If the temperature of the wafer 200 is less than 150° C., the raw material is difficult to chemically adsorb onto the wafer 200, and a practical film formation rate may not be obtained. This can be solved by setting the temperature of the wafer 200 to 150° C. or higher. If the temperature of the wafer 200 is set to 180° C. or higher, the raw material can be sufficiently adsorbed onto the wafer 200, and a sufficient film formation rate can be obtained. If the temperature of the wafer 200 is set to 400° C. or higher, the raw material can be more sufficiently adsorbed onto the wafer 200, and a more sufficient film formation rate can be obtained.
[0047] If the temperature of the wafer 200 exceeds 800°C, the CVD reaction becomes stronger (gas phase reaction becomes dominant), which tends to deteriorate the film thickness uniformity and makes it difficult to control. By keeping the temperature of the wafer 200 at 800°C or less, the deterioration of the film thickness uniformity can be suppressed and it becomes possible to control it. By keeping the temperature of the wafer 200 at 700°C or less, the surface reaction becomes dominant, which makes it easier to ensure the film thickness uniformity and makes it easier to control it.
[0048] That is, by setting the temperature of the wafer 200 in this process to, for example, 150 to 800° C., the raw material can be adsorbed onto the wafer 200, improving the film formation rate and improving the film thickness uniformity. In addition, the occurrence of excessive gas phase reactions can be suppressed, and the generation of particles due to the reaction can be suppressed.
[0049] By supplying the raw material gas to the wafer 200, a first layer containing a predetermined element, C, and H, for example, having a thickness of less than one atomic layer to several atomic layers, is formed on the wafer 200 having an NH termination formed on the surface. That is, when a gas containing Si, C, and H as the predetermined elements is used as the raw material gas, the first layer contains H derived from the raw material in addition to Si-C bonds. H in the first layer forms bonds such as CH bonds and Si-H bonds. The Si-containing layer containing C and H is a layer containing Si-C bonds, Si-H bonds, and CH bonds. The Si-containing layer containing C and H may be a Si layer containing C and H, or an adsorption layer of the raw material gas, or may contain both.
[0050] The Si layer containing C and H is a general term that includes not only a continuous Si layer containing C and H, but also discontinuous Si layers and thin Si films containing C and H that are formed by overlapping these. A continuous Si layer containing C and H is sometimes called a thin Si film containing C and H. The Si that makes up the Si layer containing C and H includes Si whose bonds with C and H are not completely broken, as well as Si whose bonds with C and H are completely broken.
[0051] The adsorption layer of the source gas includes not only a continuous adsorption layer of the molecules of the source gas but also a discontinuous adsorption layer, i.e., the adsorption layer of the source gas includes an adsorption layer having a thickness of one molecular layer or less than one molecular layer, which is composed of the molecules constituting the source gas.
[0052] Here, a layer less than one atomic layer thick means an atomic layer that is formed discontinuously, and a layer one atomic layer thick means an atomic layer that is formed continuously. A layer less than one molecular layer thick means a molecular layer that is formed discontinuously, and a layer one molecular layer thick means a molecular layer that is formed continuously.
[0053] Under conditions where the source gas self-decomposes (e.g., thermally decomposes), for example, Si is deposited on the wafer 200 to form a Si layer containing C and H. Under conditions where the source gas does not self-decompose, the source gas is adsorbed onto the wafer 200 to form an adsorption layer of the source gas. Under either condition, at least some of the bonds in the source gas, such as Si-C bonds, Si-H bonds, and C-H bonds, are retained (maintained) without being broken, and are incorporated as they are into the Si-containing layer containing C and H.
[0054] The source gas may be a gas containing a predetermined element, C, and H. The gas containing the predetermined elements, C, and H may be, for example, a gas containing the predetermined elements Si, C, and H. The gas containing Si, C, and H may be, for example, a gas containing a compound containing a hydrocarbon group, i.e., a C-H bond, such as an alkylsilane gas or an alkylenesilane gas.
[0055] Moreover, as the gas containing the predetermined element, C, and H, a gas containing the predetermined element, C, H, and a halogen element can be used. As the gas containing the predetermined element, C, H, and a halogen element, for example, a gas containing Si, C, H as the predetermined elements, and chlorine (Cl) as the halogen element can be used. As the gas containing Si, C, H, and Cl, for example, an alkylenehalosilane gas containing Si, an alkylene group, and a halogen group and having a chemical bond between Si and C (Si-C bond) or an alkylhalosilane gas containing Si, an alkyl group, and a halogen group and having a Si-C bond can be used.
[0056] Here, the alkylene group is represented by the general formula C n H 2n+2 It is a functional group formed by removing two hydrogen atoms from a chain saturated hydrocarbon (alkane) represented by the general formula C n H 2n The alkylene group includes a methylene group, an ethylene group, a propylene group, a butylene group, etc. An alkyl group is an assembly of atoms represented by the general formula C n H 2n+2It is a functional group formed by removing one H from a chain saturated hydrocarbon represented by the general formula C n H 2n+1 The alkyl group includes methyl, ethyl, propyl, and butyl groups. The halogen group includes chloro, fluoro, and bromo groups. In other words, the halogen group includes halogen elements such as chlorine (Cl), fluorine (F), and bromine (Br).
[0057] As the alkylenehalosilane gas, for example, a gas containing Si, a methylene group (-CH2-) as an alkylene group, and a chloro group (Cl) as a halogen group, i.e., a chlorosilane gas containing a methylene group, or a gas containing Si, an ethylene group (-C2H4-) as an alkylene group, and a chloro group (Cl) as a halogen group, i.e., a chlorosilane gas containing an ethylene group, can be used. As the chlorosilane gas containing a methylene group, for example, a methylenebis(trichlorosilane) gas, i.e., a bis(trichlorosilyl)methane ((SiCl3)2CH2, abbreviated as BTCSM) gas, etc. can be used. As the chlorosilane gas containing an ethylene group, for example, an ethylenebis(trichlorosilane) gas, i.e., a 1,2-bis(trichlorosilyl)ethane ((SiCl3)2C2H4, abbreviated as BTCSE) gas, etc. can be used.
[0058] As the alkylhalosilane gas, for example, a gas containing Si, a methyl group (-CH3) as an alkyl group, and a chloro group (Cl) as a halogen group, that is, a chlorosilane gas containing a methyl group, can be used. As the chlorosilane gas containing a methyl group, for example, 1,1,2,2-tetrachloro-1,2-dimethyldisilane ((CH3)2Si2Cl4, abbreviated as TCDMDS) gas, 1,2-dichloro-1,1,2,2-tetramethyldisilane ((CH3)4Si2Cl2, abbreviated as DCTMDS) gas, 1-monochloro-1,1,2,2,2-pentamethyldisilane ((CH3)5Si2Cl, abbreviated as MCPMDS) gas, etc. can be used. Unlike alkylene halosilane gases such as BTCSE gas and BTCSM gas, alkylhalosilane gases such as TCDMDS gas, DCTMDS gas, and MCPMDS gas are gases having Si-Si bonds, that is, they are source gases that contain specified elements and halogen elements and have chemical bonds between the specified elements.
[0059] Alkylenehalosilane gases such as BTCSM gas and BTCSE gas, and alkylhalosilane gases such as TCDMDS gas, DCTMDS gas, and MCPMDS gas can be said to be raw material gases that contain at least two Si atoms in one molecule, further contain Cl, and have Si-C bonds and C-H bonds. These gases act as both Si sources and C sources in this process. BTCSM gas, BTCSE gas, and the like can also be called alkylenechlorosilane gases. TCDMDS gas, DCTMDS gas, MCPMDS gas, and the like can also be called alkylchlorosilane gases.
[0060] When a gas containing a predetermined element, C, H, and a halogen element is used as the source gas, the first layer may contain a halogen element derived from the source gas as an impurity in addition to the predetermined element, C, and H. For example, when Cl is contained in the source gas as a halogen element, the first layer further contains bonds such as Si-Cl bonds.
[0061] (Removal of residual gas, step S16) Next, residual gas in the processing chamber 201 is removed. Specifically, after the first layer is formed, the valve 243a is closed and the supply of the source gas is stopped. At this time, the APC valve 244 is left open, and the processing chamber 201 is evacuated by the vacuum pump 246, and the source gas and by-products remaining in the processing chamber 201 that have not reacted or that have contributed to the formation of the first layer are removed from the processing chamber 201. At this time, the valves 243c and 243d are left open, and the supply of the inert gas into the processing chamber 201 is maintained. The inert gas acts as a purge gas.
[0062] (First modifier supply, step S17) Next, a first modifying agent is supplied to the wafer 200 in the processing chamber 201 . Specifically, similarly to step S13 described above, the valve 243b is opened, and the first modifying agent is caused to flow into the gas supply pipe 232b. The first modifying agent is adjusted in flow rate by the MFC 241b, supplied into the processing chamber 201 via the nozzle 249b, and exhausted from the exhaust pipe 231. At the same time, the valve 243d is kept open, and an inert gas is caused to flow into the gas supply pipe 232d. The inert gas is adjusted in flow rate by the MFC 241d, supplied into the processing chamber 201 together with the first modifying agent, and exhausted from the exhaust pipe 231.
[0063] In addition, in order to prevent the first modifying agent from entering the nozzle 249a, the valve 243c is kept open and an inert gas is allowed to flow through the gas supply pipe 232c. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232a and the nozzle 249a, and is exhausted from the exhaust pipe 231.
[0064] The processing conditions for supplying the first modifier in this step are as follows: Treatment pressure: 1 to 4000 Pa, preferably 10 to 1000 Pa First modifier supply flow rate: 0.1 to 20 slm, preferably 1 to 10 slm First modifier supply time: 1 to 120 seconds, preferably 10 to 60 seconds Inert gas supply flow rate: 0 to 10 slm Other process conditions may be the same as those used when supplying the source gas in the source gas supplying step.
[0065] As the first modifier, an N-containing gas can be used. As the N-containing gas, for example, nitrogen (N2) gas, ammonia (NH3) gas, diazane (N2H2) gas, hydrazine (N2H4) gas, N3H5 gas, or other hydrogen nitride gas can be used. As the N-containing gas, one or more of these can be used.
[0066] As described later, in this step, it is preferable to use a gas containing a hydrogen nitride compound that contains N and does not contain an N-N bond, which is a bond between N atoms, in one molecule, as the first modifier. As a gas containing a hydrogen nitride compound that contains N and does not contain an N-N bond, which is a bond between N atoms, in one molecule, for example, NH3 gas can be used.
[0067] The first modifier used in the above-mentioned preflow gas supply step S13 may be different from the first modifier used in this step. For example, the preflow gas supply step may use a gas containing a hydrogen nitride compound that contains N and has an N-N bond in one molecule, and the present step may use a gas containing a hydrogen nitride compound that contains N and does not have an N-N bond in one molecule. For example, the preflow gas supply step may supply a second modifier, which will be described later, as the preflow gas.
[0068] By supplying the first modifier containing N to the wafer 200, at least a part of the first layer formed on the wafer 200 is nitrided (modified). By modifying the first layer, a second layer is formed containing, for example, Si-C bonds, Si-N bonds, CN bonds, and impurities such as H and Cl remaining in the first layer. H in the second layer forms bonds such as C-H bonds, Si-H bonds, and NH bonds. That is, by using the first modifier, the first layer containing the specified elements, C, and H is modified to a second layer containing the specified elements, C, H, and N, and for example, a silicon carbonitride layer (SiCN layer) is formed.
[0069] Here, although some of H and Cl in the first layer are desorbed by supplying the first modifier, H and Cl exceeding the desired concentration remain in the second layer. When impurities such as H and Cl exceeding the desired concentration remain in the film, the film density decreases, and the ashing resistance may decrease.
[0070] In addition, in this step, when a gas containing a highly reactive hydrogen nitride-based compound or a derivative thereof such as the second modifier described in detail later is used, excessive C may be desorbed from the first layer while the nitriding reaction proceeds until the N concentration in the first layer reaches the desired concentration. In other words, the C concentration in the second layer may not be maintained at the desired concentration. Therefore, it is preferable to use a gas containing a low-reactivity hydrogen nitride-based compound as the first modifier in this step. As the gas containing a low-reactivity hydrogen nitride-based compound, a gas containing a hydrogen nitride-based compound that contains N as described above and does not contain an N-N bond, which is a bond between N atoms in one molecule, may be used.
[0071] Furthermore, the first modifying agent is supplied after being activated by heat without plasma, because this allows the above-mentioned reaction to proceed more gently, and the second layer is formed more easily. When the second layer is formed, impurities such as Cl contained in the first layer form a gaseous substance containing at least Cl during the process of the modifying reaction of the first layer by the first modifying agent, and are discharged from the processing chamber 201. That is, the impurities such as Cl in the first layer are separated from the first layer by being extracted or desorbed from the first layer. As a result, the second layer contains fewer impurities such as Cl than the first layer.
[0072] (Removal of residual gas, step S18) Next, the residual gas in the processing chamber 201 is removed. Specifically, after the second layer is formed, the valve 243b is closed and the supply of the first modifying agent is stopped. At this time, the APC valve 244 is left open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the unreacted first modifying agent remaining in the processing chamber 201 or the first modifying agent after contributing to the formation of the second layer and by-products from the processing chamber 201. At this time, the valves 243c and 243d are left open to maintain the supply of the inert gas into the processing chamber 201. The inert gas acts as a purge gas.
[0073] (First predetermined number of times, step S19) The cycle of non-simultaneously performing the above-mentioned steps S15 to S18 is performed a first predetermined number of times (n times, n is an integer of 1 or more). This makes it possible to form a first film containing a predetermined element, N, C, and H bonded to C (i.e., C-H bonds) on the wafer 200. It is preferable that the above-mentioned cycle is performed multiple times until the first film has a desired thickness. As the first film, for example, a silicon carbonitride film (SiCN film) containing Si, N, C, and C-H bonds can be formed.
[0074] At this time, the thickness of the first film is, for example, 10 to 200 Å, preferably 10 to 100 Å. If the thickness of the first film is less than 10 Å, a film having desired properties may not be obtained. If the thickness of the first film is 10 Å or more, a film having desired properties may be obtained. If the thickness of the first film exceeds 200 Å, the modification effect by the modification process described later may not be sufficient over the entire thickness direction of the first film. If the thickness of the first film is 200 Å or less, the modification effect by the modification process described later can be applied over the entire thickness direction of the first film. If the thickness of the first film is 100 Å or less, the modification effect by the modification process described later can be applied more reliably over the entire thickness direction of the first film.
[0075] Here, the first film contains impurities such as H and Cl remaining from the first layer in addition to Si-C bonds, Si-N bonds, and CN bonds. H in the first film forms bonds such as CH bonds, Si-H bonds, and NH bonds. In this way, if CH bonds, Si-H bonds, and NH bonds remain in the film, the ashing resistance deteriorates. However, when the first film is subjected to a plasma treatment to remove impurities such as H and Cl in order to improve the ashing resistance, not only the impurities such as H and Cl but also C may escape from the film. Therefore, in this embodiment, in order to reduce impurities such as H and Cl while suppressing the escape of C from the film, the following modification process is performed after the above-mentioned film formation process.
[0076] In this embodiment, after the first film is formed by performing the above-mentioned film forming process (steps S12 to S19), the next modification process (steps S20 to S22) is performed without exposing the wafer 200 to an oxygen-containing atmosphere. If the wafer 200 is exposed to an oxygen-containing atmosphere after the first film is formed, an oxide layer may be formed on the surface of the first film. If an oxide layer is formed on the surface of the first film, the modification effect in the depth direction of the first film, which is the effect of reducing H and the like, in step S21 described later, may be hindered, and the modification effect may not be sufficiently obtained. That is, by performing the next second film forming process without exposing the wafer to an oxygen-containing atmosphere after performing the first film forming process, the modification effect in step S21 can be improved. That is, the next second film forming process is performed in a state where no oxide layer is formed on the surface of the first film.
[0077] The second film formation process is performed after the supply of the first modifying agent in step S17 in the first film formation process and the removal of residual gas in step S18 to purge the space in which the wafers 200 exist (also called inert gas purge). That is, the space in which the wafers 200 exist is purged after the film formation process and before the modification process. This makes it possible to remove impurities such as Cl to a certain extent before the modification process is performed.
[0078] [Second film formation process (also called modification process)] (Pressure adjustment and temperature adjustment, step S20) The processing chamber 201 is evacuated by the vacuum pump 246 so that the pressure inside the processing chamber 201 becomes a desired pressure. In addition, the wafer 200 inside the processing chamber 201 is heated by the heater 207 so that the wafer 200 becomes a desired temperature.
[0079] (Second modifier supply, step S21) Next, a second modifying agent is supplied to the wafer 200 on which the first film is formed. Specifically, the valve 243e is opened to allow the second modifying agent to flow into the gas supply pipe 232b. The second modifying agent is adjusted in flow rate by the MFC 241e, supplied into the processing chamber 201 via the nozzle 249b, and exhausted from the exhaust pipe 231. At the same time, the valve 243d is kept open to allow an inert gas to flow into the gas supply pipe 232d. The inert gas is adjusted in flow rate by the MFC 241d, supplied into the processing chamber 201 together with the second modifying agent, and exhausted from the exhaust pipe 231.
[0080] In addition, in order to prevent the second modifying agent from entering the nozzle 249a, the valve 243c is kept open to allow an inert gas to flow through the gas supply pipe 232c. The inert gas is supplied into the processing chamber 201 through the gas supply pipe 232a and the nozzle 249a, and is exhausted from the exhaust pipe 231.
[0081] The processing conditions for supplying the second modifier in this step are as follows: Treatment temperature: room temperature to 700°C, preferably 150 to 700°C, more preferably 150 to 400°C Treatment pressure: 1 to 2666 Pa, preferably 67 to 1333 Pa Second modifier supply flow rate: 1 to 2000 sccm, preferably 10 to 1000 sccm Second modifier supply time: 1 to 120 seconds, preferably 1 to 60 seconds Inert gas supply flow rate: 0 to 10,000 sccm However, from the viewpoint of increasing the processing speed, it is preferable that the processing temperature in this step is substantially the same as the processing temperature in the first film forming process.
[0082] If the temperature of the wafer 200 is below room temperature, the second modifier is hardly activated, and a sufficient modification effect may not be obtained when modifying the first film. By setting the temperature of the wafer 200 to room temperature or higher, the second modifier is activated and the modifying action can be exerted over the entire thickness direction of the first film. Furthermore, by setting the temperature of the wafer 200 to 150°C or higher, the activation of the second modifier is further promoted, and the modifying action can be more reliably exerted over the entire thickness direction of the first film.
[0083] If the temperature of the wafer 200 exceeds 700°C, the thermal decomposition of the second modifier may proceed excessively, and the modification effect on the first film may not be obtained. For example, if N2H4 is used as the second modifier, excessive thermal decomposition may result in the generation of less reactive NH3 from the second modifier instead of the highly reactive intermediate NH2, and the modification effect on the first film may not be obtained. Also, if the temperature of the wafer 200 exceeds 400°C, the thermal decomposition of the second modifier may proceed partially, and the modification effect on the first film may decrease for the same reason. The modification effect can be obtained by setting the temperature of the wafer to 700°C or less. Also, the modification effect can be obtained more reliably by setting the temperature of the wafer 200 to 400°C or less.
[0084] By setting the temperature of the wafer 200 in this process to room temperature to 700°C, the second modifier or an intermediate thereof is reacted with H bonded to C, H bonded to Si, Cl bonded to Si, etc. in the first film, and it becomes easy to control the reactivity of the second modifier so as to desorb H, Cl, etc. while suppressing desorption of C.
[0085] In addition, by setting the temperature of the wafer 200 in this step lower than the temperature of the wafer 200 in the above-mentioned first film formation step, it is easy to adjust the degree of thermal decomposition and activation of the second modifier and control the reactivity of the second modifier and / or its intermediate. Therefore, it is easier to control the reactivity of the second modifier so as to desorb H bonded to C while suppressing desorption of C from the first film. In addition, by performing this step at a lower temperature, it is also possible to reduce the influence of the thermal history on the wafer 200 that occurs during this step. On the other hand, by setting the processing temperature to be substantially the same as the processing temperature in the first film formation step, the processing speed for the wafer 200 can be improved.
[0086] At this time, the partial pressure of the second modifier is set to be lower than the partial pressure of the first modifier in the above-mentioned step S17. Also, at this time, the flow rate of the second modifier may be set to be lower than the flow rate of the first modifier in the above-mentioned step S17. This makes it easier to control the reaction rate of the second modifier, which is more reactive than the first modifier.
[0087] Here, when the first film is modified using the plasma-excited second modifier, radicals and the like generated by plasma excitation have excessively high reactivity, and these radicals and the like cause not only H bonded to C in the film but also C bonded to a specific element or N to be desorbed. In the present disclosure, a second modifier that is more reactive than the first modifier is supplied to the wafer 200 in a non-plasma state. This allows H and the like bonded to C to be selectively desorbed while suppressing the desorption of C.
[0088] As the second modifier, a gas containing a hydrogen nitride compound or a derivative thereof that contains a bond between N and H (ie, an NH bond) and a bond between N atoms (ie, an NN bond) in one molecule can be used.
[0089] As the second modifier, for example, a gas containing at least one compound selected from among diazene (N2H2), hydrazine (N2H4), triazene (N3H3), triazane (N3H5), etc., which are hydrogen nitride compounds containing NH bonds and NN bonds in one molecule, can be used. In addition, as the second modifier, for example, a gas containing a derivative of a hydrogen nitride compound containing NH bonds and NN bonds in one molecule, such as monomethylhydrazine (CH3(NH)NH2), 1,1-dimethylhydrazine (asymmetric dimethylhydrazine) ((CH3)2-N-NH2), 1,2-dimethylhydrazine (tetramethylhydrazine) (N2(CH3)4), etc., can be used. As the second modifier, one or more of these can be used.
[0090] (Removal of residual gas, step S22) Next, residual gas in the processing chamber 201 is removed. Specifically, after the first film is modified to form the second film, the valve 243e is closed and the supply of the second modifying agent is stopped. At this time, the APC valve 244 is left open, and the processing chamber 201 is evacuated by the vacuum pump 246 to remove the unreacted second modifying agent remaining in the processing chamber 201 or the second modifying agent and by-products remaining after contributing to the modification of the first film from the processing chamber 201. At this time, the valves 243c and 243d are left open to maintain the supply of the inert gas into the processing chamber 201. The inert gas acts as a purge gas.
[0091] By supplying the second modifier to the wafer 200 without plasma, at least a part of the first film formed on the wafer 200 is nitrided (modified) and densified. By modifying the first film, a second film containing, for example, Si, C and N, i.e., a SiCN film, is formed on the wafer 200. The second modifier is supplied after being activated by heat without plasma, so that the above-mentioned reaction can proceed softly and the second film can be formed easily. When the second film is formed, impurities such as H and Cl contained in the first film constitute a gaseous substance containing at least H and Cl in this process, and are discharged from the processing chamber 201. That is, the first film is modified using a second modifier that is more reactive with CH bonds, Si-H bonds, NH bonds, etc. in the first film than the above-mentioned first modifier. As a result, the intermediate of the second modifier reacts with H and Cl in CH bonds, Si-H bonds, NH bonds, etc. in the first film, and H and Cl are desorbed from the first film. That is, impurities such as H and Cl are desorbed while maintaining the C concentration in the first film within a desired range. In other words, the first film on the wafer 200 can be modified to a second film containing a predetermined element, C, and N, with a reduced content of H bonded to C compared to the first film.
[0092] By reducing impurities such as H and Cl in the film in this way, the ashing resistance of the film can be improved. Also, by maintaining the C concentration in the film within a desired range, the etching resistance of the film can be improved. That is, by modifying the first film using the second modifier as described above, the first film can be modified into a second film that has both ashing resistance and etching resistance.
[0093] (Second predetermined number of times, step S23) In this step, if the number of cycles of steps S15 to S22 performed non-simultaneously is less than the second predetermined number (m times, m is an integer equal to or greater than 1), the pressure in the process chamber 201 and the wafer 200 in the process chamber 201 are adjusted to the desired pressure and temperature in the first film formation step (step S24) in the same manner as in step S12 described above, and the process returns to the process of step S15 described above. By performing the cycle including steps S15 to S22 the second predetermined number of times, a film having a desired film thickness and containing the predetermined elements, C, and N can be formed on the wafer 200. That is, in this embodiment, a cycle including the film formation step (excluding the preflow gas supply step) and the modification step is performed the second predetermined number of times to form a film having a desired film thickness and containing the predetermined elements, C, and N on the wafer 200. The preflow gas supply step may be performed not only once before this cycle as in this embodiment, but also for each cycle.
[0094] By performing steps S20 to S22 once for each of a number of cycles in which the above-mentioned steps S15 to S18 are performed non-simultaneously, the number of times steps S20 to S22 are performed can be reduced, thereby improving throughput.
[0095] Here, in this modification step (second film formation step), the first film is modified to a second film such that the amount of reduction in the content ratio of H contained in the first film is greater than the amount of reduction in the content ratio of C contained in the first film. That is, in this step, the first film is modified to a second film such that the amount of reduction in the content ratio of C in the first film is suppressed while the content ratio of H is reduced.
[0096] FIG. 5(A) is a diagram showing the state of the surface of wafer 200 when NH3 gas is supplied to the first film formed on wafer 200, and FIG. 5(B) is a diagram showing the state of the surface of wafer 200 when N2H4 gas is supplied to the first film formed on wafer 200.
[0097] As shown in FIG. 5(A), NH3 is composed only of NH bonds, which have a relatively large activation energy, and is therefore unlikely to be thermally decomposed into highly reactive intermediates. In addition, NH3 requires a large activation energy to react with the C-H bonds, Si-H bonds, and Si-Cl bonds remaining in the first film, and therefore is unlikely to cause a reaction that breaks these bonds. In other words, NH3 has a weak effect of removing these bonds in the first film. For example, the activation energy (Ea(H)) required for NH3 to react with the Si-H bonds contained in the first film and release H is 1.95, and the activation energy (Ea(Cl)) required for NH3 to react with the Si-Cl bonds and release Cl is 1.33.
[0098] On the other hand, as shown in FIG. 5(B), N2H4 contains N-N bonds with a relatively small activation energy, and is therefore easily thermally decomposed into the highly reactive intermediate NH2. In addition, the intermediate NH2 contains N with a dangling bond, and therefore requires a small activation energy to react with the C-H bonds, Si-H bonds, and Si-Cl bonds remaining in the first film, and is likely to cause a reaction that breaks these bonds. That is, N2H4 (its intermediate NH2) has a strong effect of removing these bonds in the first film. According to an example of the calculation results of a molecular simulation performed by the discloser, the activation energy (Ea(H)) required for NH2 to react with the Si-H bonds contained in the first film to remove H is 0.01, and the activation energy (Ea(Cl)) required for NH2 to react with the Si-Cl bonds contained in the first film to remove Cl is 0.16.
[0099] That is, the activation energy of NH2, an intermediate generated by the decomposition of, for example, N2H4 as the second modifier, reacting with and desorbing H bonded to C contained in the first film is smaller than the activation energy of NH3, a first modifier, desorbing H bonded to C contained in the first film. That is, by reacting NH2, an intermediate of N2H4 that is more reactive than NH3, with H bonded to C in the first film, etc., it is possible to desorb H from the first film.
[0100] In addition, the activation energy of NH2 reacting with and desorbing Cl bonded to Si contained in the first film is smaller than the activation energy of NH3 desorbing Cl bonded to Si contained in the first film. In other words, Cl can be desorbed from the first film by reacting NH2, which is an intermediate of N2H4 and has a higher reactivity than NH3, with Cl bonded to Si in the first film.
[0101] That is, in this modification step, the first film is modified to a second film by modifying the first film using the second modifier so as to reduce the content ratio of H bonded to a predetermined element, H bonded to C, H bonded to N, etc. contained in the first film. That is, the content ratio (concentration) of, for example, H bonded to Si, H bonded to C, H bonded to N, etc. in the first film is reduced. Specifically, by supplying the second modifier, the above-mentioned intermediate generated from the second modifier is reacted with, for example, Si-H bonds, CH bonds, NH bonds, etc. contained in the first film, thereby H is desorbed from the first film. By reducing the content ratio of H in the film, the film properties such as ashing resistance can be improved.
[0102] In addition, in this process, the first film is modified to a second film so as to release halogen elements, such as Cl, contained in the first film. That is, the content ratio of Cl bonded to C, Cl bonded to Si, Cl bonded to N, etc. remaining in the first film is reduced. Specifically, by supplying the second modifier, the above-mentioned intermediate generated from the second modifier is reacted with C-Cl bonds, Si-Cl bonds, N-Cl bonds, etc. contained in the first film, thereby releasing Cl from the first film. By reducing the content ratio of halogen elements such as Cl in the film, it is possible to improve film properties such as ashing resistance.
[0103] Furthermore, the H concentration in the first film before the modification process is, for example, 20 to 30 atomic%, and the H concentration in the second film after the modification process is, for example, 0 to 10 atomic%. If the H concentration in the second film exceeds 10 atomic%, ashing resistance in a practical range may not be obtained. By making the H concentration in the second film 10 atomic% or less, the ashing resistance of the second film in plasma ashing using oxygen (O2) plasma or the like can be improved to a practical range.
[0104] Here, the C concentration in the second film after the modification step is maintained within a desired range in which etching resistance is maintained, for example, 5 to 30 atomic %, preferably 10 to 30 atomic %.
[0105] If the C concentration in the second film is less than 5 atomic %, the etching resistance may be significantly reduced. By making the C concentration in the second film 5 atomic % or more, the etching resistance can be improved when wet etching the second film using, for example, a diluted hydrogen fluoride (HF) aqueous solution. In addition, by making the C concentration in the second film 10 atomic % or more, the etching resistance of the second film can be improved to a practical range.
[0106] Furthermore, if the C concentration in the second film exceeds 30 atomic %, etching resistance in a practical range may not be obtained. By setting the C concentration in the second film to 30 atomic % or less, the etching resistance of the second film can be improved to a practical range.
[0107] That is, according to this embodiment, it is possible to modify both the C concentration and the H concentration in the film so that they are within the desired ranges described above, and it is possible to form a film that has both ashing resistance and etching resistance.
[0108] (Purge and return to atmospheric pressure, step S25) The valves 243c and 243d are opened, and the inert gas is supplied into the processing chamber 201 from the gas supply pipes 232c and 232d, respectively, and exhausted from the exhaust pipe 231. The inert gas acts as a purge gas. This purges the processing chamber 201, and gas and by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (purging). Thereafter, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).
[0109] (Boat unloading and wafer discharging, step S26) The seal cap 219 is lowered by the boat elevator 115 to open the bottom end of the reaction tube 203. Then, the processed wafers 200 supported by the boat 217 are unloaded from the bottom end of the reaction tube 203 to the outside of the reaction tube 203 (boat unloading). The processed wafers 200 are removed from the boat 217 (wafer discharging).
[0110] (3) Effects of this mode According to this aspect, one or more of the following effects can be obtained.
[0111] (a) The amount of impurities such as H and Cl contained in the film is reduced, making it possible to form a film with high film density and excellent ashing resistance. (b) While maintaining the C concentration in the film within a desired range, impurities such as H and Cl are reduced, making it possible to form a film with excellent etching resistance. (c) That is, the film formed on the wafer 200 can be modified to have both ashing resistance and etching resistance. (d) The above-mentioned effects can be obtained in the case of forming and modifying a CN-containing film other than a SiCN film.
[0112] <Other Aspects of the Disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.
[0113] (Modification) Next, a modification of the above-mentioned substrate processing process will be described with reference to FIG.
[0114] In this modification, a modification process is included in the film forming process described above. That is, steps S31 to S38, which perform the same processes as steps S11 to S18 described above, respectively, are followed by steps S39 and S40, which perform the same processes as steps S21 and S22 in the modification process described above, respectively. Then, in step S41, a cycle of steps S35 to S40 is performed a third predetermined number of times (p times, where p is an integer equal to or greater than 1).
[0115] By performing the second cycle a predetermined number of times, a third film of a desired thickness can be formed in which impurities such as H and Cl are reduced while maintaining the C concentration in a desired range, as in the case of the second film described above. That is, the same effects as those of the above-mentioned embodiment can be obtained in this modified example. In addition, in this modified example, a modification process is further performed to remove H, Cl, etc. while forming the first film formed on the surface of the wafer 200, thereby increasing the density of NH terminations on the surface of the wafer 200, which serve as adsorption sites for the source material, and improving the film formation rate, which is the formation speed of the first film. In addition, the processing time is shortened, and the throughput can be improved.
[0116] (Other Aspects) For example, in the above-mentioned embodiment, the predetermined element contained in the raw material gas is Si. However, the present disclosure is not limited to such an embodiment. For example, the predetermined element may be a metal element such as titanium (Ti), zirconium (Zr), hafnium (Hf), tantalum (Ta), niobium (Nb), aluminum (Al), molybdenum (Mo), tungsten (W), germanium (Ge), etc. In these cases, a metal-based carbonitride film such as a titanium carbonitride film (TiCN film), a zirconium carbonitride film (ZrCN film), a hafnium carbonitride film (HfCN film), a tantalum carbonitride film (TaCN film), a niobium carbonitride film (NbCN film), an aluminum carbonitride film (AlCN film), a molybdenum carbonitride film (MoCN film), a tungsten carbonitride film (WCN film), or a germanium carbonitride film (GeCN film) is formed. In these cases, the same effect as the above-mentioned embodiment can be obtained.
[0117] In the above embodiment, the film formation process is described using a case where a first film containing a predetermined element, N, C, and H bonded to C is formed on the wafer 200 having a Si film formed on its surface. However, the present disclosure is not limited to this, and can also be suitably used in a case where a first film is formed on the surface of the wafer 200 having an oxide film such as a silicon oxide film (SiO film) or a nitride film such as a silicon nitride film (SiN film) formed on its surface, or on the surface of the wafer 200 itself.
[0118] In the above embodiment, the first film forming process and the modification process are performed consecutively (in-situ) in the same processing chamber 201. The present disclosure is not limited to this, and the first film forming process and the modification process may be performed separately (ex-situ) in different processing chambers (processing containers). In this case, the same effects as those of the above embodiment can be obtained. When these processes are performed in-situ, contamination of the substrate and changes in the surface state of the substrate that may occur due to the substrate being carried out of the processing chamber between processes or carried in from outside the processing chamber can be suppressed. When these processes are performed in-situ, the transition time between processes can be shortened. On the other hand, when these processes are performed ex-situ, the processes can be performed in parallel in different processing chambers, and the productivity can be increased accordingly.
[0119] It is preferable that the recipes used for the substrate processing are prepared individually according to the processing contents and stored in the storage device 121c via an electric communication line or the external storage device 123. Then, when starting the substrate processing, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the processing contents from among the multiple recipes stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using a single substrate processing device. In addition, it is possible to reduce the burden on the operator and quickly start the substrate processing while avoiding operational errors.
[0120] The above-mentioned recipes may not only be newly created, but may also be prepared by modifying an existing recipe that has already been installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe has been recorded. In addition, an existing recipe that has already been installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus.
[0121] In the above-mentioned embodiment, an example of processing a film using a batch-type substrate processing apparatus that processes multiple substrates at a time has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is processed using a single-wafer type substrate processing apparatus that processes one or several substrates at a time. In addition, in the above-mentioned embodiment, an example of processing a film using a substrate processing apparatus having a hot-wall type processing furnace has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is processed using a substrate processing apparatus having a cold-wall type processing furnace.
[0122] When using these substrate processing apparatuses, the film formation process can be performed under the same processing procedures and processing conditions as in the above embodiment, and the same effects as in the above embodiment can be obtained.
[0123] The above-mentioned aspects and modifications may be used in appropriate combination. The processing procedures and processing conditions in this case may be the same as those of the above-mentioned aspects and modifications. [Explanation of symbols]
[0124] 200 wafers (substrates)
Claims
1. (a) performing a cycle including a step of supplying a substrate with a source material including a predetermined element, carbon, and hydrogen, and a step of supplying the substrate with a first modifier including nitrogen a predetermined number of times, thereby forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon on the substrate; (b) supplying a second modifier, which is a compound or a derivative thereof containing a nitrogen-hydrogen bond and a nitrogen-nitrogen bond in one molecule, different from the first modifier, to the substrate on which the first film has been formed, to modify the first film into a second film containing the predetermined element, carbon, and nitrogen and having a reduced content of hydrogen bonded to the carbon compared to the first film; A substrate processing method comprising the steps of:
2. 2. The method of claim 1, wherein after (a), (b) begins without exposing the substrate to an oxygen-containing atmosphere.
3. 2. The substrate processing method according to claim 1, wherein in step (b), the first film is modified so as to reduce a content ratio of the carbon-hydrogen bonds over the entire first film in a thickness direction.
4. 2. The substrate processing method of claim 1, wherein in (b), the first film is modified to the second film such that a reduction in a content ratio of hydrogen contained in the first film is greater than a reduction in a content ratio of carbon contained in the first film.
5. 10. The method of claim 1, wherein the cycle is performed multiple times until the first film has a desired thickness.
6. 2. The substrate processing method according to claim 1, wherein in (b), the second modifier is supplied to the substrate in a non-plasma state.
7. The substrate processing method according to claim 1 , wherein the first modifier does not contain a nitrogen-nitrogen bond in one molecule.
8. The substrate processing method according to claim 7 , wherein the first modifier is a hydrogen nitride compound.
9. 2. The substrate processing method according to claim 1, wherein in step (b), an intermediate containing nitrogen having a dangling bond in one molecule generated from the second modifier is reacted with hydrogen bonded to the carbon contained in the first film, thereby desorbing the hydrogen from the first film.
10. 2. The substrate processing method according to claim 1, wherein an activation energy of an intermediate produced by decomposition of the second modifier to desorb hydrogen bonded to the carbon contained in the first film is smaller than an activation energy of the first modifier to desorb hydrogen bonded to the carbon contained in the first film.
11. 11. The substrate processing method according to claim 1, wherein the second modifier includes at least one compound or derivative of diazene, hydrazine, triazene, triazane, monomethylhydrazine, 1,1-dimethylhydrazine, and 1,2-dimethylhydrazine.
12. The substrate processing method according to any one of claims 1 to 10, wherein the raw material includes a compound including the specified element, carbon, hydrogen, and a halogen element in one molecule, and in (b), the first film is modified to the second film so as to release the halogen element contained in the first film.
13. The substrate processing method according to any one of claims 1 to 10, wherein in (b), the first film is modified to the second film so as to reduce a content ratio of hydrogen bonded to the specified element contained in the first film.
14. 11. The substrate processing method according to claim 1, wherein a partial pressure of the second modifier in (b) is lower than a partial pressure of the first modifier in (a).
15. 11. The substrate processing method according to claim 1, wherein the temperature of the substrate in (b) is lower than the temperature of the substrate in (a).
16. The substrate processing method according to any one of claims 1 to 10, further comprising the step of purging a space in which the substrate exists after (a) and before (b).
17. The predetermined number of times is one time, The substrate processing method according to any one of claims 1 to 10, wherein the second cycle including (a) and (b) is performed a plurality of times.
18. (a) performing a cycle including a step of supplying a substrate with a source material including a predetermined element, carbon, and hydrogen, and a step of supplying the substrate with a first modifier including nitrogen a predetermined number of times, thereby forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon on the substrate; (b) supplying a second modifier, which is a compound or a derivative thereof containing a nitrogen-hydrogen bond and a nitrogen-nitrogen bond in one molecule, different from the first modifier, to the substrate on which the first film has been formed, to modify the first film into a second film containing the predetermined element, carbon, and nitrogen and having a reduced content of hydrogen bonded to the carbon compared to the first film; A method for manufacturing a semiconductor device having the above structure.
19. (a) performing a cycle including a step of supplying a substrate with a source material including a predetermined element, carbon, and hydrogen, and a step of supplying the substrate with a first modifier including nitrogen a predetermined number of times, thereby forming a first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to the carbon on the substrate; (b) supplying a second modifier, which is a compound or a derivative thereof containing a nitrogen-hydrogen bond and a nitrogen-nitrogen bond in one molecule, different from the first modifier, to the substrate on which the first film has been formed, to modify the first film into a second film containing the predetermined element, carbon, and nitrogen and having a reduced content of hydrogen bonded to the carbon compared to the first film; A program for causing a computer to execute the above in a substrate processing apparatus.
20. a source supply system for supplying a source containing a predetermined element, carbon, and hydrogen to the substrate; a first modifier supply system that supplies a first modifier containing nitrogen to the substrate; a second modifier supply system that supplies a second modifier, which is different from the first modifier and is a compound or a derivative thereof that contains a nitrogen-hydrogen bond and a nitrogen-nitrogen bond in one molecule, to the substrate; (a) performing a cycle including a process of supplying the raw material to the substrate and a process of supplying the first modifier to the substrate a predetermined number of times to form a first film on the substrate, the first film including the predetermined element, nitrogen, carbon, and hydrogen bonded to carbon; (b) a control unit configured to be able to control the raw material supply system, the first modifier supply system, and the second modifier supply system to execute a process of modifying the first film into a second film containing the predetermined element, carbon, and nitrogen and having a reduced content of hydrogen bonded to the carbon compared to the first film, by supplying the second modifier to the substrate on which the first film has been formed; The substrate processing apparatus includes:
Citation Information
Patent Citations
Semiconductor device manufacturing method, substrate processing apparatus and program
JP2016131210A
Formation of flat surfaces in III-nitride materials
JP2019515860A
Densification of silicon carbide films using remote plasma processing
JP2020502797A
Substrate processing method and substrate processing device
JP2022065560A
Production method for semiconductor device, substrate treatment method, substrate treatment device, and program
WO2022201217A1