Polyester film for battery current collector, film foil for battery current collector, and battery current collector

A specially designed polyester film for battery current collectors with controlled roughness and melting temperature, combined with a vapor-deposited metal layer, addresses curling and improves short-circuit response, effectively preventing runaway reactions.

JP2024158573APending Publication Date: 2024-11-08MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023073878
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing polyester films used in battery current collectors curl when a metal layer like copper or aluminum is applied by vapor deposition, and they have insufficient current interrupting functions during short circuits.

Method used

The polyester film for battery current collectors is designed with specific surface roughness and crystal melting temperature parameters, ensuring it has an arithmetic mean roughness of 90 nm or less, a crystal melting temperature of 258°C or less, and a shrinkage rate of 1% or less, with a metal layer applied by vapor deposition to prevent curling and enhance current interrupting capabilities.

Benefits of technology

The film effectively suppresses curling and enhances the current interrupting function during short circuits, contributing to stopping and preventing runaway reactions in batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158573000003
    Figure 2024158573000003
  • Figure 2024158573000004
    Figure 2024158573000004
  • Figure 2024158573000005
    Figure 2024158573000005
Patent Text Reader

Abstract

To provide a polyester film for a battery current collector, which can suppress curling even when a metal layer of copper, aluminum or the like is provided thereon by vapor deposition or the like.SOLUTION: A polyester film for a battery current collector has an arithmetic mean roughness (Ra) of 90 nm or less on at least one side, and a crystalline melting temperature (Tm) of 258°C or less as measured by differential scanning calorimetry (DSC).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film for a battery current collector, a film foil for a battery current collector, and a battery current collector. [Background technology]

[0002] Background Art Polyester films have traditionally been used in a variety of applications, including packaging, electronic components, electrical insulation, metal lamination, display components such as flexible displays, touch panels, anti-reflection, and shatterproofing of glass, due to their transparency, dimensional stability, mechanical properties, heat resistance, and chemical resistance.

[0003] In recent years, secondary batteries such as lithium ion batteries have been widely used in various products such as vehicles and portable devices. An electrode for such a secondary battery is formed, for example, by providing an electrode active material layer containing an electrode active material on the surface of an electrode current collector. This electrode current collector is a sheet-shaped conductive member and forms a part of the conductive path from the electrode active material layer to the electrode terminal. Electrode current collectors for secondary batteries are sometimes constructed with a laminated structure in which the surface of a resin substrate is covered with a thin metal film. Such laminated electrode current collectors have a current interrupting function in which the resin substrate melts and deforms, causing the thin metal film to break, when abnormal heat is generated due to an internal short circuit or the like, and therefore have the advantage of contributing to the prevention of the progression of abnormal heat generation (see Patent Document 1).

[0004] For example, Patent Document 2 discloses an electrode for a secondary battery and a film used therein, which have excellent heat resistance, improved battery capacity and life due to being made thinner, and are lighter than conventional products due to the use of a film as a substrate. Furthermore, Patent Document 3 discloses an electrode for a secondary battery and a film used therefor, which have excellent heat-resistant dimensional stability, improved battery capacity due to a thinner electrode material substrate, and are lighter than conventional products due to the use of a film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-311146 A [Patent Document 2] Japanese Patent Application Publication No. 10-40919 [Patent Document 3] Japanese Patent Application Publication No. 10-40920 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the inventors' investigations have revealed that the films of Patent Documents 2 and 3 have a problem in that the vapor-deposited films obtained curl when a metal layer of copper, aluminum, or the like is provided by vapor deposition or the like.The inventors' investigations have also revealed that the films of Patent Documents 2 and 3 may have insufficient current interruption function during a short circuit due to melting.

[0007] Therefore, the present invention has been made in consideration of the above-mentioned situation, and an object of the present invention is to provide a polyester film for battery current collectors that can suppress curling even when a metal layer of copper, aluminum, etc. is provided by vapor deposition or the like, and that can contribute to stopping and preventing runaway reactions by improving the current interruption function in the event of a short circuit due to melting. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above problems can be solved by the following configuration. The present invention has the following aspects.

[0009] [1] A polyester film for battery current collectors, having an arithmetic mean roughness (Ra) of 90 nm or less on at least one side and a crystalline melting temperature (Tm) of 258°C or less as measured by differential scanning calorimetry (DSC). [2] A polyester film for use in battery current collectors, having an arithmetic mean height (Sa) of 40 nm or less on at least one side and a crystalline melting temperature (Tm) of 258°C or less as measured by differential scanning calorimetry (DSC). [3] A polyester film for use in a battery current collector, having a maximum height roughness (Rz) of at least one surface of 470 nm or less and a crystalline melting temperature (Tm) of 258°C or less as measured by differential scanning calorimetry (DSC). [4] A polyester film for use in a battery current collector, having a maximum cross-sectional height (Rt) of at least one side of 1,400 nm or less and a crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) of 258°C or less. [5] A polyester film for use in a battery current collector, having a maximum cross-sectional height (St) of at least one side of 2,800 nm or less and a crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) of 258°C or less. [6] The polyester film for a battery current collector according to any one of the above [1] to [5], which has a shrinkage rate of 1% or less in both the longitudinal direction (MD) and the transverse direction (TD) when heat-treated at 120°C for 5 minutes. [7] The polyester film for a battery current collector according to any one of the above [1] to [6], which has a shrinkage rate of 2% or less in both the longitudinal direction (MD) and the transverse direction (TD) when heat-treated at 150°C for 15 minutes. [8] The polyester film for a battery current collector according to any one of the above [1] to [7], which contains a polyethylene naphthalate copolymer (A). [9] The polyester film for a battery current collector according to the above [8], wherein the content of the polyethylene naphthalate copolymer (A) in the polyester film is 50 mass % or more.

[10] The polyester film for a battery current collector according to the above [8] or [9], wherein the polyethylene naphthalate-based copolymer (A) contains naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol-ethylene oxide adduct and ethylene glycol as the diol component (a-2).

[11] The polyester film for a battery current collector according to the above

[10] , wherein the dicarboxylic acid component (a-1) contains 80 mol % or more of naphthalenedicarboxylic acid.

[12] The polyester film for a battery current collector according to the above

[10] or

[11] , wherein the diol component (a-2) contains a bisphenol-ethylene oxide adduct in an amount of 1 mol % or more and 49 mol % or less.

[13] The polyester film for a battery current collector according to any one of the above [1] to

[12] , which has a thickness of 1 μm or more and 12 μm or less.

[14] The polyester film for a battery current collector according to any one of the above [1] to

[13] , which has a coating layer.

[15] The polyester film for a battery current collector according to any one of the above [1] to

[14] , wherein the battery is a lithium ion battery.

[16] A film foil for a battery current collector, comprising the polyester film for a battery current collector according to any one of the above [1] to

[15] and a metal layer.

[17] The film foil for a battery current collector according to

[16] above, wherein the metal layer is made of copper or aluminum.

[18] The film foil for a battery current collector according to

[16] or

[17] above, wherein the metal layer is provided by any one of vapor deposition, plating, or sputtering.

[19] The film foil for a battery current collector according to any one of the above

[16] to

[18] , wherein the metal layer has a two-layer structure.

[20] 20. The film foil for a battery current collector according to claim 16, wherein the battery is a lithium ion battery.

[21] A battery current collector comprising an electrode layer on the metal layer of the film foil for a battery current collector according to any one of the above

[16] to

[20] .

[22] The battery current collector according to

[21] above, wherein the battery is a lithium ion battery. Effect of the Invention

[0010] According to the present invention, it is possible to provide a polyester film for battery current collectors, which can suppress curling even when a metal layer of copper, aluminum, or the like is provided by vapor deposition or the like, and can contribute to stopping and preventing runaway reactions by improving the current interruption function in the event of a short circuit due to melting. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a schematic structure of a film foil according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a metal layer according to an embodiment of the present invention having a two-layer structure. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic structure of a film foil in a case where the metal layer according to one embodiment of the present invention has a two-layer structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Next, an example of an embodiment of the present invention will be described, however, the present invention is not limited to the embodiment described below.

[0013] <<Polyester film>> The polyester film for battery current collector of the present invention (hereinafter also referred to as "the film") has a crystalline melting temperature (Tm) of 258°C or lower as determined by differential scanning calorimetry (DSC), and preferably satisfies at least one of the following requirements (1) to (5). It is sufficient to satisfy only one of these requirements, or a combination of a plurality of requirements may be satisfied. (1) The arithmetic mean roughness (Ra) of at least one surface is 90 nm or less. (2) The arithmetic mean height (Sa) of at least one surface is 40 nm or less. (3) The maximum height roughness (Rz) of at least one surface is 470 nm or less. (4) At least one surface has a maximum cross-sectional height (Rt) of 1400 nm or less. (5) At least one surface has a maximum cross-sectional height (St) of 2800 nm or less.

[0014] The film preferably has a shrinkage rate of 1% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 120° C. for 5 minutes.

[0015] The longitudinal direction (MD) of a film refers to the direction in which the film travels during the film production process, that is, the winding direction of a film roll, and is also called the machine direction or longitudinal direction. The width direction (TD) of a film refers to the direction parallel to the film surface and perpendicular to the longitudinal direction, that is, the direction parallel to the central axis of the roll of the film, and is also called the transverse direction.

[0016] The present film is not particularly limited as long as it satisfies the above-mentioned requirements, and the present film may have a single-layer structure or a laminated (multi-layer) structure. When the present film has a laminated structure, the present film may have a two-layer structure, a three-layer structure, or may have four or more layers as long as it does not deviate from the gist of the present invention. The number of layers to be laminated is not particularly limited, but is preferably 10 layers or less. If the number is 10 layers or less, the thickness of each layer is sufficient, so that the lamination property during film formation is sufficient, flow marks and the like are unlikely to occur, and the quality of the film is sufficiently maintained. When the present film has a laminated structure of two or more layers, three layers of two kinds or three layers of three kinds are preferable, and three layers of two kinds are more preferable.

[0017] The present film may be a non-stretched film (sheet) or a stretched film. Of these, a stretched film stretched in a uniaxial or biaxial direction is preferable. Of these, a biaxially stretched film is more preferable in terms of excellent balance of mechanical properties and flatness.

[0018] The present film preferably contains polyester as a main component resin, and when the present film has a laminated structure, the main component resin of each layer is preferably polyester. The term "main component resin" refers to the resin that is most abundant among the resins constituting each layer, and is, for example, a resin that accounts for 50% by mass or more, preferably 70% by mass or more, and more preferably 80% by mass or more (including 100% by mass) of the resins constituting each layer.

[0019] <Polyester> The polyester used as the raw material of the present film is not particularly limited, and may be a homopolyester or a copolymer polyester. Specific examples include polyesters obtained by polycondensation of a dicarboxylic acid component and a diol component.

[0020] Examples of the dicarboxylic acid component include naphthalenedicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, and 1,5-naphthalenedicarboxylic acid, aromatic dicarboxylic acids such as 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenonedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, and aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid.

[0021] Examples of the diol component include ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof).

[0022] Representative examples of polyesters include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate.

[0023] Examples of the copolymer polyester include a copolymer polyester containing a third component as a copolymerization component other than the compound that is the main component of the dicarboxylic acid component constituting the polyester and the compound that is the main component of the diol component.

[0024] In particular, from the viewpoint of easily adjusting the crystalline melting temperature (Tm) and the shrinkage rate to desired values, the present film preferably contains polyethylene naphthalate (hereinafter also referred to as "PEN") or a polyethylene naphthalate-based copolymer (A) (hereinafter also referred to as "PEN-based copolymer (A)") as the polyester, and more preferably contains a PEN-based copolymer (A). The content of the PEN or PEN-based copolymer (A) in the present film is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, and still more preferably 90 mass% or more (including 100 mass%) of the resin constituting the present film. In the case where the present film has a laminated structure, it is preferable that the content of PEN or the PEN-based copolymer (A) contained in each layer satisfies the above. Also, a mixture of PEN and the PEN-based copolymer (A) may be used.

[0025] The PEN copolymer (A) specifically includes a dicarboxylic acid component (a-1) and a diol component (a-2), and more specifically includes a naphthalene dicarboxylic acid such as 2,6-naphthalene dicarboxylic acid as the dicarboxylic acid component (a-1), and ethylene glycol as the diol component (a-2), and contains a copolymerization component in at least one of the dicarboxylic acid component (a-1) and the diol component (a-2).

[0026] The PEN copolymer (A) preferably contains 80 mol % or more of a naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid in the dicarboxylic acid component (a-1), more preferably 90 mol % or more, even more preferably 95 mol % or more of the dicarboxylic acid component (a-1), and even more preferably all (100 mol %) of the dicarboxylic acid component (a-1) is a naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid. By setting the content of naphthalenedicarboxylic acid in the dicarboxylic acid component (a-1) to 80 mol % or more, the shrinkage rate can be easily adjusted to fall within a desired range. Of the above naphthalenedicarboxylic acids, 2,6-naphthalenedicarboxylic acid is most preferred.

[0027] The PEN copolymer (A) preferably contains 51 mol% or more of ethylene glycol in the diol component (a-2), more preferably 60 mol% or more, even more preferably 70 mol% or more, particularly preferably 80 mol% or more, and particularly preferably 90 mol% or more. On the other hand, the ethylene glycol in the diol component (a-2) is preferably 99 mol% or less, more preferably 98 mol% or less, even more preferably 97 mol% or less, particularly preferably 96 mol% or less, and particularly preferably 95 mol% or less. By setting the content of ethylene glycol in the diol component (a-2) within this range, the crystalline melting temperature (Tm) can be easily adjusted to a desired range.

[0028] The PEN copolymer (A) preferably contains 20 mol % or less, more preferably 10 mol % or less of a copolymerization component in the dicarboxylic acid component (a-1), and even more preferably, all of the dicarboxylic acid component (a-1) is a naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid, i.e., the copolymerization component is 0 mol %. The PEN copolymer (A) preferably contains 49 mol% or less of the copolymer component in the diol component (a-2), more preferably 40 mol% or less, even more preferably 30 mol% or less, particularly preferably 20 mol% or less, and particularly preferably 10 mol% or less. On the other hand, the copolymer component in the diol component (a-2) is preferably 1 mol% or more, more preferably 2 mol% or more, even more preferably 3 mol% or more, particularly preferably 4 mol% or more, and particularly preferably 5 mol% or more. By setting the content of the copolymerization component in the dicarboxylic acid component (a-1) and / or the diol component (a-2) within such range, the crystalline melting temperature (Tm) and the shrinkage rate can be easily adjusted to the desired range.

[0029] When the main component is 2,6-naphthalenedicarboxylic acid, examples of the copolymerization components added to the dicarboxylic acid component (a-1) include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 3,3'-diphenyl dicarboxylic acid, and 4,4'-diphenyl ether dicarboxylic acid; and aliphatic dicarboxylic acids such as cyclohexane dicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid. From the viewpoint of moldability, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred. These copolymerization components can be used alone or in combination of two or more.

[0030] Examples of copolymerization components added to the diol component (a-2) include diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof). From the viewpoint of maintaining film strength, bisphenols are more preferred, and as bisphenols, it is preferable to use bisphenol-ethylene oxide adducts, and it is particularly preferable to use bisphenol A-ethylene oxide adducts. These copolymerization components can be used alone or in combination of two or more.

[0031] That is, it is most preferable that the PEN copolymer (A) contains a naphthalene dicarboxylic acid such as 2,6-naphthalene dicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol-ethylene oxide adduct such as bisphenol A-ethylene oxide adduct and ethylene glycol as the diol component (a-2). In this PEN copolymer (A), the dicarboxylic acid component (a-1) contains a naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid in an amount of preferably 80 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and even more preferably 100 mol %. In addition, in this PEN copolymer (A), the diol component (a-2) contains a bisphenol-ethylene oxide adduct such as a bisphenol A-ethylene oxide adduct in an amount of preferably 1 mol% to 49 mol%, more preferably 2 mol% to 40 mol%, even more preferably 3 mol% to 30 mol%, particularly preferably 4 mol% to 20 mol%, and especially preferably 5 mol% to 10 mol%, and contains ethylene glycol in an amount of preferably 51 mol% to 99 mol%, more preferably 60 mol% to 98 mol%, even more preferably 70 mol% to 97 mol%, particularly preferably 80 mol% to 96 mol%, and especially preferably 90 mol% to 95 mol%.

[0032] In addition, when polyester is produced (polycondensed) using ethylene glycol as one of the raw materials, diethylene glycol is usually produced as a by-product from ethylene glycol. In this specification, this diethylene glycol is referred to as by-product diethylene glycol. The amount of diethylene glycol produced as a by-product from ethylene glycol varies depending on the type of polycondensation, but is about 5 mol% or less of ethylene glycol. In the present invention, 5 mol% or less of diethylene glycol is considered to be by-product diethylene glycol, and the by-product diethylene glycol is also included in ethylene glycol and is distinguished from a copolymerization component. On the other hand, depending on the content of diethylene glycol, more specifically, when diethylene glycol is contained in excess of 5 mol%, diethylene glycol is treated as a copolymerization component rather than as a by-product diethylene glycol.

[0033] In addition, when the present film has a multilayer structure, the type and content of the copolymerization component constituting the PEN-based copolymer (A) contained in any layer, preferably in each layer, may be the same as above, and the resin constituting each layer and the PEN-based copolymer (A) in each layer may be the same as or different from each other.

[0034] <Polymerization catalyst> The polycondensation catalyst used in polycondensing polyester is not particularly limited, and a conventionally known compound can be used, such as a titanium compound, a germanium compound, an antimony compound, a manganese compound, an aluminum compound, a magnesium compound, a calcium compound, etc. Among them, from the viewpoint of productivity, a titanium compound or an antimony compound is preferable.

[0035] <Particle> The present film may contain particles. By containing particles, the polyester film is given slipperiness and is prevented from being scratched during each process, resulting in good handleability. The type of particles contained in the present film is not particularly limited as long as it is a particle that can impart slipperiness, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, as well as crosslinked polymers such as crosslinked silicone resin particles, crosslinked acrylic resin particles, crosslinked styrene-acrylic resin particles, and crosslinked polyester particles, and organic particles such as calcium oxalate and ion exchange resins. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0036] The shape of the particles to be used is not particularly limited, and any of spherical, block, rod-like, flat, etc. may be used. There is also no particular limitation on the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination as necessary.

[0037] The average particle size of the particles used is usually 0.01 to 5 μm, preferably 0.03 to 4 μm, more preferably 0.05 to 3.5 μm, and even more preferably 0.1 to 3 μm. If the average particle size is within this range, the present film can achieve both ease of handling and transparency. In addition, when the particles are powder, the average particle size of the particles can be the particle size (d50) at an accumulated volume fraction of 50% in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device (e.g., Shimadzu Corporation's "SA-CP3 type"). The average particle size of the particles in the film, layer, or resin can be determined by observing 10 or more particles with a scanning electron microscope (SEM) to measure the diameters of the particles and calculating the average value. In this case, in the case of non-spherical particles, the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle.

[0038] When particles are incorporated into the present film, it is preferable to, for example, provide a surface layer and an intermediate layer and incorporate particles into the surface layer. In addition, when the film has a three-type, three-layer structure with different front and back designs, it is also possible to incorporate particles into at least one of the surface layers. The content of the particles depends on the average particle size, but is preferably 0.0003% by mass to 5% by mass in the layer containing the particles, more preferably 0.001% by mass to 3% by mass, even more preferably 0.01% by mass to 1% by mass, and even more preferably 0.05% by mass to 0.5% by mass. If the content is within this range, the film can have good slip properties and transparency.

[0039] The method of adding particles to the present film is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage of the polyester production, but it is preferable to add the particles after the esterification or transesterification reaction is completed.

[0040] <Other> In order to suppress the amount of precipitation of oligomer components, the film may be produced using a polyester having a low content of oligomer components as the raw material. As a method for producing a polyester having a low content of oligomer components, various known methods can be used, such as a method of performing solid phase polymerization after the production of a polyester. The amount of precipitation of oligomer components may be suppressed by forming the present film into a three or more layer structure and forming the surface layer of the present film from a polyester raw material having a low content of oligomer components. The polyester may also be obtained by carrying out the esterification or transesterification reaction, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0041] In addition to the above-mentioned particles, conventionally known ultraviolet absorbents, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the present film as required.

[0042] The present film may contain resins other than polyester as long as the effects of the present invention are not impaired. Examples of other resins include polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, polyacetal resins, acrylic resins, ethylene vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polylactic acid resins, polybutylene succinate resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, and fluorine-based resins.

[0043] The thickness of the present film is preferably from 1 μm to 12 μm, more preferably from 1 μm to 10 μm, further preferably from 2 μm to 8 μm, and particularly preferably from 2 μm to 6 μm. By making the thickness 1 μm or more, the film strength is likely to be kept within a practical range. On the other hand, by making the thickness 12 μm or less, when it is used as a film foil for a lithium ion battery current collector, it can contribute to making the film foil, and in turn, the lithium ion battery current collector, thinner and lighter. The thickness can be adjusted by the film formation conditions. The thickness of this film was measured at five random locations on the surface with a 1 / 1000 mm dial gauge, and the average was taken as the thickness.

[0044] <Coating layer> The present film may have a coating layer formed by coating or the like. The coating layer may be formed by applying a resin composition for forming the coating layer to a polyester film, and optionally subjecting the applied resin composition to treatments such as drying, curing, and heat treatment, and at least heat treatment is preferably performed. The resin composition used in the coating layer is not particularly limited. The method for coating the resin composition is not particularly limited, and any conventionally known coating method such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, curtain coating, etc. can be used.

[0045] In addition, in-line coating and offline coating methods can also be used as a method for forming the coating layer. The method for heat-treating the coated resin composition is not particularly limited, and for example, when the resin layer is provided by offline coating, the heat treatment is usually performed at 80 to 200°C for 3 to 40 seconds, preferably at 100 to 180°C for 3 to 40 seconds. On the other hand, when the resin layer is provided by in-line coating, the heat treatment is usually performed at 70 to 280°C for 3 to 200 seconds. The heat treatment may be performed in two or more steps at different temperatures within the above temperature range. At least a part of the heat treatment may be performed by heating during stretching. In addition, drying and curing may be performed together by heating in the heat treatment.

[0046] The coating layer is preferably formed by in-line coating, which treats the film surface during the polyester film production process. In-line coating is a method of coating within the polyester film production process, specifically, a method of coating at any stage from melt extrusion of polyester to stretching, heat setting and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, and a film after heat setting and before winding up.

[0047] Although not limited to the following, for example, in the case of sequential biaxial stretching, a method in which a uniaxially stretched film stretched in the longitudinal direction (machine direction) is coated and then stretched in the transverse direction is particularly advantageous. According to such a method, film formation and resin layer formation can be carried out simultaneously, which is advantageous in terms of production costs, and since stretching is carried out after coating, the thickness of the resin layer can be changed by the stretching ratio, and thin film coating can be carried out more easily than with off-line coating films.

[0048] <Production method of polyester film> Next, a production example of the present film will be specifically described, but the production example is not limited to the following production example. For example, when producing a biaxially stretched film, a method is preferred in which the dried polyester pellets described above are extruded as a molten sheet from a die using a melt extrusion device such as an extruder, and then cooled and solidified with a cooling roll such as a rotating cooling drum to obtain an unstretched sheet. Here, the cooling is preferably performed to a temperature below the glass transition point of the polymer, for example, to obtain an unoriented sheet (unstretched sheet) in a substantially amorphous state. In addition, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and the cooling roll, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used.

[0049] Next, the obtained unstretched sheet is stretched in biaxial directions. In this case, the unstretched sheet is first stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3 to 6 times.

[0050] Then, the film is stretched in a direction perpendicular to the first-stage stretching direction. In this case, the stretching temperature is usually 70 to 170° C., preferably 75 to 160° C., and the stretch ratio is usually 3 to 7 times, preferably 3.5 to 6 times.

[0051] Then, the film is heat-treated under tension or relaxation of 30% or less at a temperature of usually 180 to 270°C, preferably 190 to 260°C, to obtain a biaxially stretched film. This heat treatment is also called a heat setting step. The heat treatment may be performed in two or more steps with different temperatures. After the heat treatment, the film may be cooled in a cooling zone. The cooling temperature is preferably higher than the glass transition temperature (Tg) of the polyester constituting the film, and more specifically, is preferably in the range of 100 to 160° C. This cooling may be performed in two or more steps at different temperatures. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0052] The present film can also be produced by a simultaneous biaxial stretching method, which involves simultaneously stretching and orienting the unstretched sheet in the machine direction (longitudinal direction) and width direction (transverse direction) under temperature control usually at 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is preferably 4 to 50 times, more preferably 7 to 35 times, and even more preferably 10 to 25 times in terms of area ratio. Then, the film is subsequently heat-treated under tension or under relaxation of 30% or less at a temperature of 170 to 250° C. to obtain a stretched and oriented film. Regarding the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0053] <Surface roughness and static friction coefficient of polyester film> The arithmetic mean roughness (Ra) of at least one surface of the present film is preferably 90 nm or less, more preferably 70 nm or less, even more preferably 50 nm or less, even more preferably 40 nm or less, particularly preferably 30 nm or less, and most preferably 25 nm or less. The arithmetic mean roughness (Ra) of at least one surface of the present film is preferably 1 nm or more, more preferably 3 nm or more, even more preferably 6 nm or more, even more preferably 10 nm or more, even more preferably 14 nm or more, even more preferably 17 nm or more, and even more preferably 22 nm or more.

[0054] The arithmetic mean height (Sa) of at least one surface of the present film is preferably 40 nm or less, more preferably 25 nm or less, even more preferably 20 nm or less, even more preferably 15 nm or less, even more preferably 10 nm or less, even more preferably 8 nm or less, particularly preferably 6 nm or less, and most preferably 4 nm or less. The arithmetic mean height (Sa) of at least one side of the present film is preferably 0.2 nm or more, more preferably 0.4 nm or more, even more preferably 0.7 nm or more, even more preferably 1 nm or more, even more preferably 1.5 nm or more, particularly preferably 2 nm or more, and most preferably 2.5 nm or more.

[0055] The maximum height roughness (Rz) of at least one surface of the present film is preferably 470 nm or less, more preferably 400 nm or less, even more preferably 350 nm or less, even more preferably 300 nm or less, particularly preferably 250 nm or less, and most preferably 200 nm or less. The maximum height roughness (Rz) of at least one surface of the present film is preferably 20 nm or more, more preferably 30 nm or more, even more preferably 40 nm or more, even more preferably 70 nm or more, particularly preferably 100 nm or more, and most preferably 140 nm or more.

[0056] The maximum cross-sectional height (Rt) of at least one surface of the present film is preferably 1400 nm or less, more preferably 1000 nm or less, even more preferably 800 nm or less, even more preferably 600 nm or less, particularly preferably 500 nm or less, and most preferably 400 nm or less. The maximum cross-sectional height (Rt) of at least one surface of the present film is preferably 50 nm or more, more preferably 80 nm or more, even more preferably 130 nm or more, even more preferably 180 nm or more, even more preferably 240 nm or more, particularly preferably 280 nm or more, and most preferably 320 nm or more.

[0057] The maximum cross-sectional height (St) of at least one surface of the present film is preferably 2800 nm or less, more preferably 2000 nm or less, even more preferably 1500 nm or less, even more preferably 1000 nm or less, even more preferably 700 nm or less, particularly preferably 400 nm or less, and most preferably 200 nm or less. The maximum cross-sectional height (St) of at least one surface of the present film is preferably 20 nm or more, more preferably 50 nm or more, even more preferably 80 nm or more, even more preferably 100 nm or more, particularly preferably 130 nm or more, and most preferably 150 nm or more.

[0058] When the arithmetic mean roughness (Ra), arithmetic mean height (Sa), maximum height roughness (Rz), maximum cross-sectional height (Rt) or maximum cross-sectional height (St) of the present film is equal to or greater than the above lower limit, the surface of the present film is not too smooth and has an appropriate roughness, resulting in good slip properties, making it easier to obtain appropriate adhesion to the roll, and tending to have excellent roll runnability. In addition, if the arithmetic mean roughness (Ra) is equal to or less than the upper limit, there is an advantage that slippage, shifting, twisting, wrinkles, etc. are unlikely to occur on the transport roll during transport of the film when a metal layer is provided by deposition, sputtering, etc. In addition, since the energy applied by deposition, sputtering, etc. is likely to be uniform overall on the film surface, it is easy to control the film thickness to be more uniform, and it is also effective in suppressing curling of the film after deposition. In addition, partial heat shrinkage can also be suppressed, which in turn leads to the suppression of curling and wrinkles of the film after deposition.

[0059] When the present film has a laminate structure, it is preferable that the roughness of either the outermost or inner layer, more preferably both surfaces, is within the above range.

[0060] The arithmetic mean roughness (Ra), maximum height roughness (Rz), and maximum profile height (Rt) can be measured by a contact surface roughness meter in accordance with JIS B0601: 2013, according to the method described in the Examples. The arithmetic mean height (Sa) and maximum profile height (St) can be measured by a non-contact surface / layer cross-sectional shape measurement system, according to the method described in the Examples.

[0061] The surface roughness (Ra a , S a , Rz a , Rta , St. a ) and the surface roughness (Ra b , S b , Rz b , Rt b , St. b Specifically, it is preferable that the following condition (1) or (2) is satisfied. 1≦Sa a / Sa b <1.2···(1) 1≦St a / St b ≦8 (2) In the above formula, Sa a ≧Sa b And St a ≧St b It is.

[0062] S a / Sa b is more preferably 1.16 or less, even more preferably 1.13 or less, even more preferably 1.1 or less, particularly preferably 1.08 or less, and most preferably 1.06 or less. a / Sa b is more preferably 1.01 or greater, even more preferably 1.02 or greater, even more preferably 1.025 or greater, particularly preferably 1.03 or greater, and most preferably 1.035 or greater. St a / St b is more preferably 6 or less, even more preferably 4 or less, even more preferably 3 or less, even more preferably 2 or less, particularly preferably 1.7 or less, and most preferably 1.5 or less. a / St b is more preferably 1.03 or greater, even more preferably 1.07 or greater, even more preferably 1.1 or greater, even more preferably 1.14 or greater, particularly preferably 1.18 or greater, and most preferably 1.2 or greater.

[0063] In addition, the static friction coefficient between one side and the other side of the present film is preferably 0.76 or less, more preferably 0.7 or less, even more preferably 0.65 or less, even more preferably 0.6 or less, and particularly preferably 0.55 or less. The static friction coefficient between one surface and the other surface of the present film is preferably 0.2 or more, more preferably 0.3 or more, even more preferably 0.35 or more, and even more preferably 0.4 or more.

[0064] By having the surface roughness of the one surface and the other surface within the above range, by having the static friction coefficient of the one surface and the other surface within the above range, and further by having both the surface roughness and static friction coefficient of the one surface and the other surface within the above range, it is easier to obtain the same effect as described above, which is preferable. The static friction coefficient can be measured by the method described in the examples.

[0065] The method for adjusting the surface roughness Ra, Sa, Rz, Rt, St and the static friction coefficient is not particularly limited, and various methods such as transfer processing such as embossed roll transfer, embossed belt transfer, embossed film transfer, sandblasting, shot blasting, etching, engraving, surface crystallization, etc. can be used. A method of roughening the surface by casting a film-like molten resin on a cast roll is preferred because it is easy to continuously and uniformly form surface irregularities while extruding the molten resin into a film. In this case, the surface roughness of the resin film can be adjusted by adjusting the arithmetic mean roughness of the cast roll. It is also possible to appropriately adjust the particle size, shape, and content of the particles contained in the resin, or by adjusting the film-forming conditions such as the stretching temperature and stretching ratio. In addition, when a functional layer such as a coating layer or a release layer is separately provided by coating or the like, this can be achieved by appropriately adjusting the composition of the coating liquid used, the coating thickness, the coating conditions, the timing of coating (inline or offline, etc.), etc.

[0066] <Physical properties of polyester film> The shrinkage of the present film when heat-treated at 120°C for 5 minutes is preferably 1% or less in either the machine direction (MD) or the transverse direction (TD). If the shrinkage (120°C, 5 minutes) is 1% or less, sufficient dimensional stability during high-temperature treatment can be obtained. Examples of high-temperature treatment include a treatment for providing a metal layer, which will be described later. If the shrinkage during the provision of the metal layer is small, a decrease in adhesion with the metal layer and deformation of the film can be suppressed. From this viewpoint, the shrinkage rate (120°C, 5 min) is more preferably 0.7% or less in either the machine direction (MD) or the transverse direction (TD), further preferably 0.6% or less, and particularly preferably 0.5% or less. The lower limit of the shrinkage rate (120°C, 5 min) is not particularly limited, but is usually about -0.5%, preferably -0.3%. It is particularly preferable that the shrinkage rate (120° C., 5 minutes) is within the above range in both the machine direction (MD) and the transverse direction (TD).

[0067] From the viewpoint of improving dimensional stability during high-temperature treatment, the shrinkage rate of the present film when heat-treated at 150°C for 15 minutes is preferably 2% or less in either the longitudinal direction (MD) or the transverse direction (TD), more preferably 1.7% or less, even more preferably 1.6% or less, still more preferably 1.5% or less, and even more preferably 1.4% or less. The lower limit of the shrinkage rate (150°C, 15 minutes) is not particularly limited, but is usually about -0.5%, preferably -0.1%. It is particularly preferable that the shrinkage rate (150° C., 15 minutes) is within the above range in both the machine direction (MD) and the transverse direction (TD). From the same viewpoint, the shrinkage rate of the present film when heat-treated at 180° C. for 5 minutes is preferably 4% or less in both the machine direction (MD) and the transverse direction (TD), more preferably 3.5% or less, further preferably 3% or less, and particularly preferably 2.5% or less. The lower limit of the shrinkage rate (180° C., 5 minutes) is not particularly limited, but is usually about −0.5%, and preferably 0%. It is particularly preferable that the shrinkage rate (180° C., 5 minutes) is within the above range in both the machine direction (MD) and the transverse direction (TD).

[0068] The above shrinkage rates (120°C, 5 minutes), (150°C, 15 minutes) and (180°C, 5 minutes) can be adjusted by the type and content of polyester constituting the present film, the particle size and content of particles if particles are contained, the film formation conditions of the present film, etc. The shrinkage rates can be measured by the method described in the Examples.

[0069] In addition, the crystalline melting temperature (Tm) of the present film as measured by differential scanning calorimetry (DSC) is preferably 262°C or lower. If the crystalline melting temperature (Tm) is 262°C or lower, the temperature at which melting insulation begins to melt during a short circuit when the film is used in a battery (described later) is lowered, and therefore the halting and prevention of runaway reactions due to a short circuit can be started quickly. In other words, by lowering the temperature at which melting insulation begins to melt during a short circuit, the current interruption function during a short circuit due to melting can be improved. From this viewpoint, the crystalline melting temperature (Tm) is preferably 258° C. or lower, more preferably 256° C. or lower, even more preferably 254° C. or lower, and particularly preferably 252° C. or lower. On the other hand, from the viewpoint of formability and strength retention during high-temperature treatment, the crystalline melting temperature (Tm) is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 240° C. or higher.

[0070] The crystalline melting temperature (Tm) can be adjusted by the type and content of the polyester constituting the present film. The crystalline melting temperature (Tm) can be measured by the method described in the Examples.

[0071] <<Film foil>> The film foil for battery current collector of the present invention (hereinafter also referred to as "the present film foil") preferably has a metal layer on the surface of the present film. The metal layer may be provided on at least one side of the present film, but it is more preferable to provide the metal layer on both sides. More specifically, as shown in FIG. 1, the present film foil 1 preferably comprises a polyester film 11 and metal layers 12 on both sides thereof.

[0072] <Metal layer> The metal forming the metal layer is not particularly limited as long as it is a metal having electrical conductivity, and examples thereof include aluminum, nickel, gold, silver, copper, cadmium, titanium, etc. Among them, the metal layer is preferably made of copper or aluminum, from the viewpoint of being widely used, for example, as an electrode collector (positive electrode collector) used in the positive electrode of a lithium ion battery or an electrode collector (negative electrode collector) used in the negative electrode. Here, "made of" means that the metal layer contains copper or aluminum as a main component. The metal layer may contain an element other than a metal having electrical conductivity.

[0073] The metal layer is preferably provided by any one of vapor deposition, plating, and sputtering, and more specifically, a conventionally known method such as a vacuum vapor deposition method, an electroplating method, or a sputtering method can be used.

[0074] In particular, the metal layer preferably has a two-layer structure. As an example of such an embodiment, the metal layer 12 may have a two-layer structure of a metal layer 21 provided by vapor deposition or sputtering and a metal layer 22 provided by plating (see FIG. 2). In such a case, the present film foil 1 has, on both sides of the polyester film 11, the metal layer 21 provided by vapor deposition or sputtering and the metal layer 22 provided by plating, in this order (see FIG. 3). By using such a two-layer structure, it is possible to make the foil thinner and lighter than conventional metal foils while maintaining the same performance, and it is also possible to reduce costs compared to conventional metal foils.

[0075] <<Battery current collector>> The battery current collector of the present invention (hereinafter also referred to as "the current collector") preferably comprises an electrode layer on the metal layer. The electrode layer is formed by laminating a conventionally known electrode agent on the surface of the metal layer, and can be used as a battery electrode. Furthermore, by using this current collector, a battery such as a lithium ion battery can be produced by a conventionally known method.

[0076] <<Applications>> The present film and the present film foil can be used for battery current collectors, such as storage batteries, secondary batteries, and lithium ion batteries, and are preferably used for lithium ion batteries, and particularly preferably used for lithium ion secondary batteries. Therefore, the present current collector preferably has a configuration exemplified by electrode layer (positive electrode) / metal layer / polyester film / metal layer / electrode layer (positive electrode) for a positive electrode current collector, and electrode layer (negative electrode) / metal layer / polyester film / metal layer / electrode layer (negative electrode) for a negative electrode current collector. Because the present current collector has this configuration, it is possible to stop or prevent a runaway reaction caused by a short circuit, compared to conventional current collectors for lithium-ion batteries and the like that use metal foil, more specifically, electrode layer (positive electrode) / metal layer / electrode layer (positive electrode) or electrode layer (negative electrode) / metal layer / electrode layer (negative electrode), and yet it has the advantages of contributing to thinner, lighter material and reduced costs.

[0077] The reason why the present film, the present film foil, and the present current collector can contribute to stopping and preventing runaway reactions due to short circuits is because they have a current interrupting function at the short circuit site. The current interrupting function is achieved when the film melts and deforms in the event of abnormal heat generation, causing the thin metal film (metal layer) to break, or when the film base material (polyester film) melts and insulates the short circuit site. In particular, in the present invention, the crystalline melting temperature (Tm) of the polyester film is within a specific range, so that the starting temperature of molten insulation during a short circuit can be lowered, and molten insulation can contribute to stopping and preventing runaway reactions from an earlier stage. In addition, the reason why the present film, present film foil, and present current collector can contribute to thinner, lighter, and cost-saving devices is that, as mentioned above, the use of metal can be reduced by replacing part of the metal layer with polyester film.

[0078] <<Explanation of terms>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0079] The present invention will now be described in further detail with reference to examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.

[0080] <Evaluation method> (1) Intrinsic viscosity (IV) 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed out, dissolved in 100 mL of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and the viscosity was measured at 30 °C using a viscosity measuring device "VMS-022UPC·F10" (manufactured by Rigo Co., Ltd.).

[0081] (2) Average particle size The particle size at an accumulated volume fraction of 50% in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution analyzer (SA-CP3 type) manufactured by Shimadzu Corporation was taken as the average particle size d50.

[0082] (3) Crystal melting temperature (Tm) The crystal melting temperature (Tm) was measured when the temperature was raised from 20°C to 300°C at a rate of 10°C per minute using a PerkinElmer differential scanning calorimeter (DSC 8500) in accordance with JIS K7121 (2012). The extreme value of the maximum endothermic peak was taken as the crystal melting temperature (Tm). The analysis was performed by selecting the corresponding maximum endothermic peak range from "Peak area" in the "Analysis" menu of the built-in software.

[0083] (4) Shrinkage rate A sample film of 1.5 cm x 15 cm was heat-treated for 5 minutes in a hot air oven maintained at a specified temperature (120°C, 150°C, 180°C) in an untensioned state, and the length of the sample film was measured before and after the treatment, and the elasticity was calculated using the following formula. The measurements were taken in both the machine direction (MD) and the width direction (TD) of the film. Shrinkage rate (%) = {(sample length before heat treatment) - (sample length after heat treatment)} ÷ (sample length before heat treatment) × 100

[0084] (5) Arithmetic mean roughness (Ra), maximum height roughness (Rz), maximum cross-sectional height (Rt) The surface of the film before copper deposition on which copper was to be deposited was measured in the longitudinal direction (MD) of the film using a contact surface roughness meter (Surf Coder SE3500) manufactured by Kosaka Laboratory Co., Ltd. under the conditions of stylus tip radius 0.5 mm, evaluation length arbitrary, arbitrary 2.5 mm, longitudinal magnification 20000, lateral magnification 20, cutoff value 0.08 mm, and measurement speed 0.1 mm / sec to determine the arithmetic mean roughness (Ra), maximum height roughness (Rz), and maximum cross-sectional height (Rt). The measurement was performed 12 times, and the average value of 10 points after dividing the maximum and minimum values ​​was taken as the measured value.

[0085] (6) Arithmetic mean height (Sa), maximum section height (St) The surface of the film before copper deposition on which copper was to be deposited was measured using a non-contact surface / layer cross-sectional shape measurement system (VertScan (registered trademark) R550GML) manufactured by Ryoka Systems Co., Ltd. under the conditions of 1.0x eyepiece magnification, 50x objective lens magnification, and measurement area 178μm length × 238μm width, and the arithmetic mean height (Sa) and maximum cross-sectional height (St) were obtained after fourth-order polynomial surface correction and median filter (3x3) processing. The measurement was performed 10 times and the average value was calculated.

[0086] (7) Curling of vapor-deposited film A biaxially oriented polyester film was attached to a 14 cm square mold using a vacuum deposition machine (MH59-0133) manufactured by Japan Vacuum Technology Co., Ltd., and one side of the film was vacuumed at a vacuum level of 2×10 -5 Copper was evaporated at a pressure of Torr or less for 30 seconds. In Example 1, both a deposition film evaporated on the coating solution A side and a deposition film evaporated on the coating solution B side were prepared. In Example 2, a film evaporated on the coating solution A side was prepared. A sample measuring 11 x 11 cm was cut from the obtained vapor-deposited film with the copper-deposited side facing down, and the degree of curling of the film was visually confirmed. ×: Large curls ○: The ends curl slightly ◎: No curl

[0087] (8) Coefficient of static friction A test piece measuring 15 x 160 mm was cut out from the film before copper deposition, and the static friction coefficient between one side of the test piece and the other side was measured. Specifically, one side of the test piece was kept in contact with the other side for 15 seconds before the start of the test, and then measurements were made in the machine direction (MD) under the following conditions. The sample was conditioned for at least 6 hours before the measurement. Equipment: Parallel movement friction tester (MCS-300) manufactured by Yokohama Systems Research Institute Co., Ltd. Slider: Total mass 104g (contact area is a square with a side of 12mm) Test speed: 20mm / min ·Temperature: 23℃±2℃ Relative humidity: 50%±10%

[0088] <Ingredients used> Raw material A: Dicarboxylic acid component (a-1): 2,6-naphthalenedicarboxylic acid = 100 mol%, diol component (a-2): ethylene glycol = 95 mol%, bisphenol A-ethylene oxide adduct = 5 mol% polyethylene naphthalate copolymer (A) (intrinsic viscosity = 0.62 dL / g) Raw material B: homopolyethylene naphthalate (intrinsic viscosity = 0.62 dL / g) Raw material C: homopolyethylene terephthalate (intrinsic viscosity = 0.65 dL / g) Raw material D: homopolyethylene terephthalate (intrinsic viscosity = 0.85 dL / g) Raw material E: homopolyethylene terephthalate (intrinsic viscosity = 0.63 dL / g) Raw material F: Masterbatch containing homopolyethylene terephthalate and 0.6% by mass of silica particles with an average particle size of 2.5 μm (intrinsic viscosity = 0.61 dL / g) Raw material G: Masterbatch containing homopolyethylene terephthalate and 0.9% by mass of silica particles with an average particle size of 3.5 μm (intrinsic viscosity = 0.70 dL / g) Raw material H: homopolyethylene terephthalate (intrinsic viscosity = 0.59 dL / g)

[0089] <Coating solution used> [Compound I] Aqueous dispersion of acrylic resin polymerized with the following composition Emulsion polymer of ethyl acrylate / n-butyl acrylate / methyl methacrylate / N-methylolacrylamide / acrylic acid = 65 / 21 / 10 / 2 / 2 (mass%) (emulsifier: anionic surfactant) [Compound II] Melamine compound: Hexamethoxymethylolmelamine [Compound III] Silica particles with an average particle size of 0.5 μm [Compound IV] Silica particles with an average particle size of 0.06 μm

[0090] [Table 1]

[0091] Example 1 Raw material C was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 37°C using an electrostatic adhesion method to obtain an unstretched sheet. The unstretched sheet was then stretched 3.8 times in the machine direction (MD) at 86°C using a roll stretching machine to obtain a uniaxially stretched film. Coating solution A having the composition shown in Table 1 was applied to one side (side A) of the uniaxially stretched film in an amount (after drying and stretching) of 0.10 g / m 2 On the opposite side (side B), coating solution B having the composition shown in Table 1 was applied in an amount (after drying and stretching) of 0.03 g / m 2 The film was then introduced into a tenter stretching machine, preheated at 90°C in the tenter, and stretched 4.2 times in the transverse direction (TD) at 115°C. Finally, the film was heat-set at 225°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 2.

[0092] Example 2 Raw material A was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 50°C using an electrostatic adhesion method to obtain an unstretched sheet. Next, the obtained unstretched sheet was stretched 3.8 times in the machine direction (MD) at 125°C using a roll stretching machine, and coating solution A was applied to one surface of the obtained uniaxially stretched sheet in the same manner as in Example 1 so that the amount (after drying and stretching) was 0.10 g / m 2 The film was then introduced into a tenter stretching machine, preheated at 120°C in the tenter, and stretched 4.7 times in the transverse direction (TD) at 130°C. Finally, the film was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 2.

[0093] (Reference example 1) Raw material B was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 50°C using an electrostatic adhesion method to obtain an unstretched sheet. Next, the obtained unstretched sheet was stretched 3.8 times in the machine direction (MD) at 130°C using a roll stretching machine, and coating solution A was applied to one surface of the obtained uniaxially stretched sheet in the same manner as in Example 1 so that the amount (after drying and stretching) was 0.10 g / m 2 Then, on the opposite side, coating solution A was applied so that the coating amount (after drying and stretching) was 0.10 g / m 2 The film was then introduced into a tenter stretching machine, preheated at 120°C in the tenter, and stretched 4.7 times in the transverse direction (TD) at 130°C. Finally, the film was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 2.

[0094] Example 3 A mixed raw material consisting of raw materials E and F in a ratio of 77.5% by mass and 22.5% by mass, respectively, was fed into a twin-screw extruder and extruded at 300°C. An unstretched sheet was obtained by cooling and solidifying the raw material on a cooling roll set at 36°C using an electrostatic adhesion method. The unstretched sheet was then stretched 3.8 times in the machine direction (MD) at 87°C using a roll stretching machine. It was then preheated in a tenter at 82°C and stretched 4.1 times in the transverse direction (TD) at 108°C. Finally, it was heat-set at 227°C to obtain a biaxially stretched polyester film with a thickness of 6 μm. The evaluation results are shown in Table 2.

[0095] Comparative Example 1 A mixture of raw materials C, D, G, and H in proportions of 21 mass%, 12 mass%, 20 mass%, and 47 mass%, respectively, was fed into a twin-screw extruder and extruded at 300°C. An unstretched sheet was obtained by cooling and solidifying the mixture on a cooling roll set at 28°C using an electrostatic adhesion method. The unstretched sheet was then stretched 2.7 times in the machine direction (MD) at 100°C using a roll stretching machine, and then stretched twice in the machine direction (MD) at 87°C. It was then preheated at 78°C in a tenter, and stretched 4.2 times in the transverse direction (TD) at 115°C. Finally, it was heat-set at 226°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 2.

[0096] [Table 2]

[0097] In addition, the * in the table indicates that the same coating solution A as in Example 1 was used and applied under the same conditions, so the surface roughness is estimated to be similar to that of side A in Example 1.

[0098] As can be seen from the results in Table 1, the polyester films of the examples were capable of suppressing curling of the film after copper deposition. In addition, since the crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) was 258°C or lower, the films were capable of improving the current interruption function during a short circuit caused by melting, thereby contributing to the termination and prevention of runaway reactions. Therefore, the polyester films of the present invention can be suitably used as battery current collectors.

[0099] On the other hand, the polyester film of Comparative Example 1 did not have a specific surface roughness, and therefore curled after copper deposition. [Industrial Applicability]

[0100] The polyester film for battery current collector of the present invention can suppress curling even when a metal layer is provided, and can contribute to stopping and preventing runaway reactions by improving the current interruption function during a short circuit caused by melting. In addition, the battery current collector of the present invention, which is equipped with the film foil for battery current collectors of the present invention, is less likely to curl than battery current collectors using conventional metal foils, making it possible to stop and prevent runaway reactions caused by short circuits, and yet has the advantages of contributing to thinner, lighter weight, and cost reduction, and therefore has high industrial value. [Explanation of symbols]

[0101] 1 Film foil 11 Polyester film 12 metal layer 21 Metal layer (evaporation or sputtering) 22 Metal layer (plating)

Claims

1. A polyester film for a battery current collector, having an arithmetic mean roughness (Ra) of 90 nm or less on at least one side, and a crystalline melting temperature (Tm) of 258° C. or less as measured by differential scanning calorimetry (DSC).

2. A polyester film for a battery current collector, having an arithmetic mean height (Sa) of at least one surface of 40 nm or less and a crystalline melting temperature (Tm) of 258° C. or less as measured by differential scanning calorimetry (DSC).

3. A polyester film for a battery current collector, having a maximum height roughness (Rz) of 470 nm or less on at least one surface, and a crystalline melting temperature (Tm) of 258° C. or less as measured by differential scanning calorimetry (DSC).

4. A polyester film for a battery current collector, having a maximum cross-sectional height (Rt) of at least one surface of 1,400 nm or less and a crystalline melting temperature (Tm) of 258° C. or less as measured by differential scanning calorimetry (DSC).

5. A polyester film for a battery current collector, having a maximum cross-sectional height (St) of at least one surface of 2800 nm or less and a crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) of 258° C. or less.

6. The polyester film for battery current collector according to any one of claims 1 to 5, which has a shrinkage rate of 1% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 120°C for 5 minutes.

7. The polyester film for battery current collector according to any one of claims 1 to 5, which has a shrinkage rate of 2% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 150°C for 15 minutes.

8. The polyester film for a battery current collector according to any one of claims 1 to 5, comprising a polyethylene naphthalate-based copolymer (A).

9. The polyester film for a battery current collector according to claim 8 , wherein the content of the polyethylene naphthalate-based copolymer (A) in the polyester film is 50 mass % or more.

10. The polyethylene naphthalate copolymer (A) contains naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol-ethylene oxide adduct and ethylene glycol as the diol component (a-2). The polyester film for a battery current collector according to claim 8.

11. 11. The polyester film for a battery current collector according to claim 10, wherein the dicarboxylic acid component (a-1) contains 80 mol % or more of naphthalenedicarboxylic acid.

12. 11. The polyester film for a battery current collector according to claim 10, wherein the diol component (a-2) contains 1 mol % or more and 49 mol % or less of a bisphenol-ethylene oxide adduct.

13. The polyester film for a battery current collector according to any one of claims 1 to 5, having a thickness of 1 µm or more and 12 µm or less.

14. The polyester film for a battery current collector according to any one of claims 1 to 5, which has a coating layer.

15. The polyester film for a battery current collector according to any one of claims 1 to 5, wherein the battery is a lithium ion battery.

16. A film foil for a battery current collector, comprising the polyester film for a battery current collector according to any one of claims 1 to 5 and a metal layer.

17. The film foil for a battery current collector according to claim 16, wherein the metal layer is made of copper or aluminum.

18. The film foil for a battery current collector according to claim 16, wherein the metal layer is provided by any one of vapor deposition, plating, and sputtering.

19. The film foil for a battery current collector according to claim 16, wherein the metal layer has a two-layer structure.

20. 17. The film foil for a battery current collector according to claim 16, wherein the battery is a lithium ion battery.

21. A battery current collector comprising an electrode layer on the metal layer of the film foil for a battery current collector according to claim 16.

22. 22. The battery current collector of claim 21, wherein the battery is a lithium ion battery.

Citation Information

Patent Citations

  • Composite polymer film, manufacturing method thereof, metalized composite polymer film and application

    CN115447248A

  • Film for secondary battery electrode

    JP1998040920A

  • Flame-retardant polyester film for electric storage element electrode, electrode for electric storage element comprising the same, and electric storage element comprising the same

    JP2011174009A

  • Biaxially oriented polyester film

    JP2012107080A

  • Biaxially oriented polyester film for power storage element electrode

    JP2014220187A

Cited By

  • Films for metal lamination, film foils, film foils for battery current collectors, and battery current collectors

    JP7845590B2

  • JPWO2025225577A1

  • Film for metal lamination, film foil, film foil for battery current collector, and battery current collector

    WO2025225577A1