Hydrophilic film and optical element

A hydrophilic film with titanium and silica particles and a multilayered structure addresses the issue of hydrophilicity loss in lenses by enhancing durability and photocatalytic properties to maintain and restore hydrophilicity.

JP2024158887AInactive Publication Date: 2024-11-08NIDEC CORP(JP) +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023074502
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing hydrophilic lenses lose their hydrophilicity over time due to dirt adherence and are unable to restore this property effectively, especially in environments with insufficient ultraviolet light exposure.

Method used

A hydrophilic film comprising titanium and silica particles with specific surface roughness and particle sizes, along with a multilayered structure, enhances durability and photocatalytic properties to maintain hydrophilicity.

Benefits of technology

The film effectively suppresses scratches and maintains hydrophilicity for a prolonged period, even in environments with limited ultraviolet light, and can restore hydrophilicity when exposed to sunlight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158887000001_ABST
    Figure 2024158887000001_ABST
Patent Text Reader

Abstract

To provide a hydrophilic film capable of suppressing scratching and maintaining a function for recovering hydrophilicity when irradiated with ultraviolet light (sunlight), and an optical element.SOLUTION: A hydrophilic film 70 including a plurality of titanium particles and a plurality of silica particles and having a surface roughness of 2.0 nm or more and 7.5 nm or less includes a first layer 20 and a second layer 60 arranged on the first layer 20. The first layer 20 includes the plurality of titanium particles; the second layer 60 preferably includes the plurality of silica particles; the average particle size of the titanium particles is 15 nm or more and 100 nm or less; and the average particle size of the silica particles is 5 nm or more and 20 nm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a hydrophilic film and an optical member. [Background technology]

[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor weather. One solution to the problem of impaired visibility is to make the surface of the window glass hydrophilic. This makes it possible to turn the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.

[0003] However, organic dirt caused by automobile exhaust gases or factory smoke easily adheres to the surface of hydrophilic members, causing water droplets to adhere to the surface, significantly reducing visibility.

[0004] In view of this, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-77260 A Summary of the Invention [Problem to be solved by the invention]

[0006] When the hydrophilic lens of Patent Document 1 is used for a long period of time, if dirt accumulates and the hydrophilic function is reduced, the hydrophilicity may not be restored even when irradiated with ultraviolet light (sunlight). Specifically, when the hydrophilic lens of Patent Document 1 is used for a long period of time, the hydrophilic layer may be scratched, and the function of restoring hydrophilicity may be reduced. Furthermore, when the hydrophilic lens of Patent Document 1 is used in an environment where it is not sufficiently exposed to ultraviolet light (sunlight), such as in an environment with continuous cloudy or rainy weather or in an environment where it is installed in a place with almost no light, recovery of the hydrophilic function may not be possible in the first place.

[0007] The present disclosure has been made in consideration of the above-mentioned problems, and its purpose is to provide a hydrophilic film and optical component that can suppress scratching and maintain the function of recovering hydrophilicity when irradiated with ultraviolet light (sunlight). Another object is to provide a hydrophilic film and an optical member that can maintain the hydrophilic function for a longer period even when used in an environment where the film is not sufficiently irradiated with ultraviolet light (sunlight). [Means for solving the problem]

[0008] An exemplary hydrophilic film of the present disclosure includes a plurality of titanium particles and a plurality of silica particles, and has a surface roughness of 2.0 nm to 7.5 nm.

[0009] An exemplary optical member of the present disclosure includes the hydrophilic film and a translucent member that transmits visible light. The hydrophilic film is disposed on the translucent member. Effect of the Invention

[0010] According to the exemplary embodiment of the present disclosure, it is possible to suppress scratches, and maintain the function of recovering hydrophilicity when irradiated with ultraviolet light (sunlight). Furthermore, even in an environment where ultraviolet light (sunlight) is not irradiated, it is possible to maintain hydrophilicity for a longer period of time. [Brief description of the drawings]

[0011] [Figure 1]FIG. 1 is a schematic diagram showing an example of an optical unit according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an optical member according to the present embodiment. [Diagram 3] FIG. 3 shows an image taken with an atomic force microscope (AFM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. In the drawings, the same or corresponding parts are given the same reference symbols and the description will not be repeated. The dimensions, shapes, and size relationships between components in the drawings are not necessarily the same as the actual dimensions, shapes, and size relationships between components. In particular, the thickness ratios and curvatures of the reflection adjustment film, hydrophilic film, and translucent member in the drawings may differ significantly from the actual ones.

[0013] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the light-transmitting member to the hydrophilic film. The "inside" of an optical member refers to the direction from the hydrophilic film to the light-transmitting member.

[0014] The optical member according to this embodiment is suitable as an optical member used in, for example, an optical unit including one or more optical members (particularly, an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit".

[0015] The optical member according to this embodiment may be used in an optical unit (particularly an optical unit used outdoors) including the optical member 100 and an optical lens. The optical lens transmits light with a wavelength of 400 nm or more and 700 nm or less. The optical member 100 is disposed on the opposite side of the optical lens in the traveling direction of light.

[0016] The static contact angle of the surface of the optical member 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be referred to simply as "contact angle." Note that the contact angle of the surface of the optical member according to this embodiment is a value measured in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0017] Moreover, the reflectance for light having a wavelength of 400 nm or more and 700 nm or less is 3% or less. The maximum reflectance of the optical member 100 for light having a wavelength of 400 nm or more and 700 nm or less is preferably 1.5% or less, more preferably 1.0% or less. The optical member 100 according to this embodiment can suppress the occurrence of image defects called ghost phenomenon and image defects called flare phenomenon as the above-mentioned maximum reflectance is lower. In particular, the occurrence of ghost phenomenon can be suppressed more effectively as the above-mentioned maximum reflectance is lower. When the above-mentioned maximum reflectance is 3.0% or less, the occurrence of ghost phenomenon can be suppressed. When the above-mentioned maximum reflectance is 1.0% or less, the occurrence of ghost phenomenon can be suppressed more effectively. Incidentally, light having a wavelength of 400 nm or more and 700 nm or less corresponds to light in the visible light region.

[0018] An example of the optical member 100 according to the present embodiment will be described below with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to the present embodiment. The optical member 100 is a light-transmitting The optical element includes a member 10, a hydrophilic film 70, and a reflection adjustment film 30.

[0019] <Translucent member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0020] The light-transmitting member 10 has a function as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 10 mm or more and 15 mm or less.

[0021] <Hydrophilic membrane> The hydrophilic film 70 covers the light-transmitting member 10. Specifically, the hydrophilic film 70 is disposed on the reflection adjustment film 30. The hydrophilic film 70 has hydrophilic properties.

[0022] The hydrophilic film 70 contains a plurality of titanium particles and a plurality of silica particles.

[0023] In detail, the hydrophilic film 70 includes a hydrophilic layer 20 and a coating layer 60. The hydrophilic layer 20 is an example of a "first layer." The coating layer 60 is an example of a "second layer."

[0024] <Hydrophilic layer> The thickness of the hydrophilic layer 20 is preferably 20 nm or more and 200 nm or less, more preferably 30 nm or more and 100 nm or less. If the thickness of the hydrophilic layer 20 is less than 20 nm, the function of restoring hydrophilicity tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, the transmittance of visible light tends to be insufficient.

[0025] In the present specification, the "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced over the surface to measure the step between areas with and without a layer (film). The step is measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."

[0026] The hydrophilic layer 20 contains a plurality of titanium particles. The titanium particles have a photocatalytic function. For example, when the optical member 100 is used for a long period of time, dirt adheres to the optical member 100, reducing the hydrophilic function. When the optical member 100 is irradiated with ultraviolet light (sunlight), the dirt is broken down and the hydrophilic function can be restored. The optical member 100 according to this embodiment is exposed to ultraviolet light of 1 mW / cm when the contact angle exceeds 30.0°. 2 It is preferable that the contact angle becomes 30.0° or less by irradiating the surface with light at 400 nm for 6 hours.

[0027] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferable.

[0028] The average particle size of the titanium particles is preferably 15 nm or more and 100 nm or less. Specifically, the titanium particles are, for example, primary or secondary particles of titanium dioxide. In particular, the hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide.

[0029] The average particle size of the primary particles of titanium is preferably 5 nm or more and 20 nm or less, and more preferably 5 nm or more and 10 nm or less. If the average particle size of the primary titanium particles is more than 20 nm, sufficient transmittance to visible light cannot be obtained, or a uniform film cannot be formed.

[0030] In the present specification, the "average particle size of primary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 primary particles that can be observed in their entirety, the maximum and minimum diameters of each primary particle are measured, the average of the maximum and minimum diameters is defined as the particle size of the single primary particle, and the average of the particle diameters of each of the 50 primary particles is defined as the "average particle size of primary particles."

[0031] The average particle size of the secondary particles of the titanium particles is 15 nm to 100 nm, and preferably 20 nm to 60 nm. If the average particle size of the secondary particles of the titanium particles is less than 15 nm, the hydrophilicity of the hydrophilic layer 20 cannot be sufficiently restored. If the average particle size of the secondary particles of the titanium particles is more than 100 nm, sufficient transmittance for visible light cannot be obtained.

[0032] In this specification, the "average particle size of secondary particles" is determined by observing the hydrophilic layer 20 or the material of the hydrophilic layer 20 using a transmission electron microscope (TEM). Specifically, for any 50 secondary particles that can be observed in their entirety, the maximum and minimum diameters of each secondary particle are measured, the average of the maximum and minimum diameters is defined as the particle size of the one secondary particle, and the average of the particle diameters of each of the 50 secondary particles is defined as the "average particle size of secondary particles."

[0033] The content of titanium particles in the hydrophilic layer 20 is preferably 50% by mass or more and 70% by mass or less. By having the content of titanium particles of 50% by mass or more and 70% by mass or less, the hydrophilicity of the hydrophilic layer 20 can be more effectively restored and an increase in reflectance can be more effectively suppressed.

[0034] The hydrophilic layer 20 may further contain a binder, which further improves the abrasion resistance of the optical member 100. The binder preferably further contains tetraethoxysilane and silicon dioxide.

[0035] <Coating layer> The coating layer 60 is disposed on the hydrophilic layer 20. The coating layer 60 contains a plurality of silica particles.

[0036] Specifically, the coating layer 60 contains a plurality of primary silica particles. At least a portion of the hydrophilic layer 20 is partially or completely coated with the primary silica particles. As a result, the abrasion resistance of the optical member 100 is further improved, and the durability of maintaining hydrophilicity is improved. The coating layer 60 may further contain tetraethoxysilane.

[0037] The average particle size of the primary particles of silica is preferably 5 nm or more and 20 nm or less. If the average particle size of the primary particles of silica is less than 5 nm, the cost tends to increase. If the average particle size of the primary particles of silica is more than 20 nm, the transmittance of visible light tends to be insufficient.

[0038] The thickness of the coating layer 60 is preferably 5 nm or more and 20 nm or less. If the thickness of the coating layer 60 is less than 5 nm, sufficient durability tends not to be obtained. If the thickness of the coating layer 60 is more than 20 nm, the coating is easily scratched.

[0039] The surface roughness of the hydrophilic film 70 is 2.0 nm or more and 7.5 nm or less. If the surface roughness of the hydrophilic film 70 is less than 2.0 nm, the film is easily scratched. If the surface roughness of the hydrophilic film 70 is more than 7.5 nm, sufficient durability tends not to be obtained.

[0040] 1 and 2, in this embodiment, the surface roughness of the hydrophilic film 70 is 2.0 nm or more and 7.5 nm or less, so that the film has high durability and is less susceptible to scratches. As a result, even if the hydrophilicity is reduced, the function of recovering the hydrophilicity when irradiated with ultraviolet light (sunlight) can be maintained for a long period of time.

[0041] In addition, since the hydrophilic film 70 includes the hydrophilic layer 20 and the coating layer 60, it has higher durability and can recover its hydrophilicity more easily when irradiated with ultraviolet light (sunlight) even if its hydrophilicity is reduced. In addition, the hydrophilicity can be maintained for a longer period of time even in an environment where it is not irradiated with ultraviolet light (sunlight).

[0042] Furthermore, the average particle size of the titanium particles in the hydrophilic layer 20 is 15 nm or more and 100 nm or less, and the average particle size of the primary silica particles in the coating layer 60 is 5 nm or more and 20 nm or less, so that scratches can be better suppressed, and the hydrophilicity can be better restored when irradiated with ultraviolet light (sunlight).

[0043] <Reflection adjustment film> The reflection adjustment film 30 is disposed under the hydrophilic layer 20. The reflection adjustment film 30 covers the light-transmitting member 10. The reflection adjustment film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The reflection adjustment film 30 suppresses reflection of light. Specifically, by including the reflection adjustment film 30, the optical member 100 suppresses light attempting to enter the light-transmitting member 10 from the reflection adjustment film 30 from being reflected by the surface on the reflection adjustment film 30 side.

[0044] The reflection adjustment film 30 has a multi-layer structure. Specifically, the reflection adjustment film 30 includes low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low-refractive index layers and high-refractive index layers are not limited as long as the combination allows the reflection adjustment film 30 to exhibit an anti-reflection effect. The refractive index of the low-refractive index layers is, for example, 1.80 or less. The refractive index of the high-refractive index layers is, for example, greater than 1.80. The layer located outermost among the low-refractive index layers and high-refractive index layers is the low-refractive index layer. The layer located innermost among the low-refractive index layers and high-refractive index layers is the low-refractive index layer.

[0045] The refractive index of the low refractive index layer may be less than that of the high refractive index layer. For example, the refractive index of the low refractive index layer is preferably 1.30 or more and 1.80 or less, more preferably 1.40 or more and 1.60 or less. By making the refractive index of the low refractive index layer 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.

[0046] The refractive index of the high refractive index layer may be greater than the refractive index of the low refractive index. For example, the refractive index of the high refractive index layer is preferably 1.80 or more and 3.00 or less, more preferably 2.00 or more and 2.80 or less. By having the refractive index of the high refractive index layer be 1.80 or more and 3.00 or less, the reflectance of the optical member 100 is further reduced. The high refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2 and Nb2O5, and more preferably contains Si3N4.

[0047] The refractive indices of the low refractive index layer and the high refractive index layer described above are merely examples and are not limited thereto. The refractive indices of the low refractive index layer and the high refractive index layer may be set to values ​​optimal for the refractive index of the light-transmitting member 10.

[0048] The thickness of the reflection adjustment film 30 is 5 times or more the thickness of the hydrophilic layer 20. The thickness of the reflection adjustment film 30 is preferably 100 times or less the thickness of the hydrophilic layer 20 from the viewpoint of productivity. The total film thickness of the reflection adjustment film 30 is preferably 20 nm or more and 2000 nm or less, more preferably 200 nm or more and 750 nm or less. If the total film thickness of the reflection adjustment film 30 is less than 20 nm, there is a tendency that sufficient anti-reflection effect cannot be obtained. If the total film thickness of the reflection adjustment film 30 exceeds 2000 nm, it takes a long time to form the film, and the productivity of the optical member 100 tends to decrease. In addition, if the total film thickness exceeds 2000 nm, there is a tendency that the production cost of the optical member 100 increases.

[0049] The thickness of one low refractive index layer is, for example, from 5.0 nm to 200.0 nm, and the thickness of one high refractive index layer is, for example, from 5.0 nm to 200.0 nm.

[0050] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.

[0051] <Method of manufacturing optical members> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a reflection adjustment film formation step, a coating step, and a drying step.

[0052] <Preparation steps> First, prepare a light-transmitting member 10. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0053] <Reflection adjustment film formation step> A low refractive index material is prepared. The low refractive index material preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2. The content of SiO2 in the low refractive index material is preferably 95 mass% or more. The method for forming the low refractive index material is preferably deposition or sputtering.

[0054] A high refractive index material is prepared. The high refractive index material preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4. The content of Si3N4 in the high refractive index material is preferably 95 mass% or more. The method for forming the high refractive index material is preferably deposition or sputtering.

[0055] The low refractive index layers and the high refractive index layers are alternately laminated. The total number of the low refractive index layers and the high refractive index layers is usually an odd number. However, the total number of the low refractive index layers and the high refractive index layers may be an even number.

[0056] <Application step> A hydrophilic material is applied. The hydrophilic material contains a plurality of titanium particles. The average particle size of the primary titanium particles is preferably 5 nm or more and 20 nm or less.

[0057] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0058] The content of the solvent in the hydrophilic material is preferably 50% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50% by mass or more and 99.9% by mass or less, coating can be easily performed.

[0059] The method of applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, or a combination of two or more of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, or dip spin coating.

[0060] <Drying step> The hydrophilic material is dried to produce the hydrophilic layer 20. The hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of a plurality of primary particles of photocatalyst particles. The average particle size of the secondary particles of the photocatalyst particles is 15 nm or more and 100 nm or less.

[0061] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.

[0062] <Coating material application step> A coating material is applied. The coating material contains a plurality of primary silica particles. The average particle size of the primary silica particles is 5 nm or more and 20 nm or less.

[0063] The coating material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0064] The content of the solvent in the coating material is preferably 50% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50% by mass or more and 99.9% by mass or less, the coating material can be easily applied.

[0065] The coating material is preferably applied by a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, or a combination of two or more of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, or dip spin coating.

[0066] The above describes the embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments, and can be implemented in various aspects without departing from the gist of the present disclosure. The drawings are mainly schematic illustrations of each component for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings are different from the actual ones due to the convenience of drawing. In addition, the material, shape, dimensions, etc. of each component shown in the above embodiments are only examples and are not particularly limited, and various modifications are possible within a range that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiment may be appropriately modified within a range that does not exceed the technical idea of ​​the present disclosure. In addition, the embodiments may be implemented in combination within a possible range.

[0067] The present technology can also adopt the following configuration.

[0068] (1) Multiple titanium particles; Multiple silica particles and A hydrophilic film comprising: The hydrophilic film has a surface roughness of 2.0 nm or more and 7.5 nm or less.

[0069] (2) A first layer; a second layer disposed on the first layer; Equipped with the first layer contains the plurality of titanium particles; The hydrophilic film according to (1), wherein the second layer contains the plurality of silica particles.

[0070] (3) the average particle size of the titanium particles is 15 nm or more and 100 nm or less; The hydrophilic film according to (1) or (2), wherein the average particle size of the silica particles is 5 nm or more and 20 nm or less.

[0071] (4) The first layer further contains a binder, The hydrophilic film according to (2), wherein the content of the titanium particles in the first layer is 50% by mass or more and 70% by mass or less.

[0072] (5) A hydrophilic film according to any one of (1) to (4), a transparent member that transmits visible light; Equipped with The hydrophilic film covers the light-transmitting member. EXAMPLES

[0073] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.

[0074] <Manufacturing of optical components> Optical members according to Examples 1 and 2, and optical members according to Comparative Examples 1 and 2 were manufactured.

[0075] <Example 1> <Preparation steps> A lens ("TAFD-5G" manufactured by HOYA Corporation, composition: glass, diameter 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was a convex surface (radius of curvature 12 mm) and the other surface was a concave surface (radius of curvature 3.07 mm).

[0076] <Reflection adjustment film formation step> A low refractive index material containing SiO2 and a high refractive index material containing Si3N4 were alternately laminated to form a reflection adjustment film having a total of 11 low refractive index layers and high refractive index layers.

[0077] <Application step> A hydrophilic material of Example 1 was prepared, containing 0.5 parts by mass of titanium dioxide particles, 0.5 parts by mass of silicon dioxide, 2 parts by mass of water, 76 parts by mass of isopropyl alcohol, 20 parts by mass of methanol, and 1 part by mass of nitric acid.

[0078] A hydrophilic material was applied onto the reflection adjustment film. Specifically, 60 μL of the hydrophilic material was dropped onto the optical axis of the light-transmitting member. Next, the light-transmitting member was rotated at a rotation speed of 5000 rpm using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.). At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.

[0079] <Drying step> A hydrophilic layer was formed by heat treatment at 90° C. for 30 minutes. The surface roughness of the hydrophilic layer was 7.56 nm.

[0080] <Coating material application step> A coating material containing 1 part by mass of silica particles (average particle size of primary particles: 5 nm), 99 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The coating material was applied onto the hydrophilic layer. Specifically, 60 μL of the coating material was dropped onto the optical axis of the light-transmitting member. Next, the light-transmitting member was rotated at a rotation speed of 5000 rpm using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.). At this time, the rotation axis was aligned with the optical axis of the light-transmitting member. A heat treatment was performed at 120° C. for 30 minutes to form a coating layer, and an optical member according to Example 1 was obtained. The surface roughness of the hydrophilic film was 2.50 nm. An image taken using an atomic force microscope (AFM) is shown in FIG. 3(a).

[0081] <Example 2> In the coating material application step of Example 1, instead of preparing a coating material containing 1 part by mass of silica particles (average particle size of primary particles: 5 nm), 98.8 parts by mass of water, and 0.2 parts by mass of ammonia, a coating material containing 0.5 parts by mass of silica particles (average particle size of primary particles: 5 nm), 93.3 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The surface roughness of the hydrophilic film was 4.08 nm. Also, an image taken using an atomic force microscope (AFM) is shown in FIG. 3(b).

[0082] <Comparative Example 1> The coating material application step of Example 1 was not performed. The surface roughness of the hydrophilic film was 7.6 nm. An image taken with an atomic force microscope (AFM) is shown in Figure 3(c).

[0083] <Comparative Example 2> In the coating material application step of Example 1, instead of preparing a coating material containing 1 part by mass of silica particles (average particle size of primary particles: 5 nm), 98.8 parts by mass of water, and 0.2 parts by mass of ammonia, a coating material containing 5 parts by mass of silica particles (average particle size of primary particles: 5 nm), 94.8 parts by mass of water, and 0.2 parts by mass of ammonia was prepared. The surface roughness of the hydrophilic film was 0.87 nm. Also, an image taken using an atomic force microscope (AFM) is shown in FIG. 3(d).

[0084] <Evaluation> The reflectance and scratch resistance were evaluated by the following methods for the optical members according to Examples 1 and 2 and the optical members according to Comparative Examples 1 and 2. The measurement results are shown in the following Table 1. All measurements were performed in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0085] <Wear test> An optical component was placed in pure water and rubbed 500 times with a scrubbing brush with a load of 300g on the surface. It was then observed with a laser microscope at 466 times magnification. The durability of the test piece was evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0086] 〇: No optical influence ×: Optical influence present

[0087] <Contact angle> Before using the optical member, the static contact angle with respect to pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). In addition, after the optical member was subjected to a thermal cycle test for 265 hours at -40°C for 30 minutes and 85°C for 30 minutes, the static contact angle with respect to pure water was measured using an automatic contact angle meter ("DMo-601" manufactured by Kyowa Interface Science Co., Ltd.). The evaluation results are shown in Table 1.

[0088] [Table 1]

[0089] The optical member according to Comparative Example 1 lost its hydrophilicity after 256 hours of thermal shock. The optical member according to Comparative Example 2 had poor abrasion resistance and was scratched, resulting in a deterioration of its optical properties. In contrast, the optical members according to Examples 1 and 2 were able to suppress scratches and maintain for a long period of time the function of recovering hydrophilicity when irradiated with ultraviolet light (sunlight). Furthermore, the hydrophilicity could be maintained for a longer period of time even in an environment where ultraviolet light (sunlight) was not irradiated. [Explanation of symbols]

[0090] 10...Translucent member 20...Hydrophilic layer 60...Covering layer 70...Hydrophilic membrane 100 Optical components

Claims

1. A plurality of titanium particles; Multiple silica particles and A hydrophilic film comprising: The hydrophilic film has a surface roughness of 2.0 nm or more and 7.5 nm or less.

2. A first layer; a second layer disposed on the first layer; Equipped with the first layer contains the plurality of titanium particles; The hydrophilic film according to claim 1 , wherein the second layer contains the plurality of silica particles.

3. The average particle size of the titanium particles is 15 nm or more and 100 nm or less, The hydrophilic film according to claim 2 , wherein the average particle size of the silica particles is 5 nm or more and 20 nm or less.

4. The first layer further comprises a binder, The hydrophilic film according to claim 2 , wherein the content of the titanium particles in the first layer is 50% by mass or more and 70% by mass or less.

5. The hydrophilic film according to any one of claims 1 to 4, a transparent member that transmits visible light; Equipped with The hydrophilic film covers the light-transmitting member.

Citation Information

Patent Citations

  • Hydrophilic lens

    JP2018077260A