Pulp-molding molded article and method for manufacturing the same
The pulp molded product addresses the limitations of paper containers by utilizing specific fiber compositions and a novel manufacturing process, achieving enhanced strength, flexibility, and surface properties, thereby improving product appeal and efficiency.
Patent Information
- Application Number
- JP2023074900
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing paper containers have a complex manufacturing process, limited shape flexibility, and low strength, which hinders their ability to showcase product appeal effectively.
A pulp molded product is developed with specific fiber diameter and length proportions, incorporating fine cellulose fibers and a paper strength agent, and a manufacturing method involving slurry deposition, dewatering, and hot pressing to achieve a density of 0.45-0.65 g/cm³ and a thickness of 1.2 mm or less, enhancing strength and shape flexibility.
The pulp molded product exhibits excellent strength, flexibility, and surface properties, allowing for efficient production and improved product appeal, while reducing manufacturing complexity and cost.
Smart Images

Figure 2024159117000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a pulp molded article. [Background technology]
[0002] In recent years, environmental problems related to an increase in waste and the like have been occurring frequently. In view of this, paper containers are being used to store toiletry products, beverages, foods, and the like, instead of plastic containers and metal containers. For example, as a paper container for liquids such as a milk container, there is a so-called gable-top paper container, which is made of paperboard coated on both sides with polyethylene resin and has a gable roof at the top. Such paper containers not only contribute to resource and energy conservation, but also contribute to environmental conservation by being easily recycled or incinerated when disposed of. Therefore, paper containers are widespread in various fields.
[0003] However, since the above-mentioned paper containers are formed by folding and pasting paperboard, the manufacturing process is complicated and the manufacturing costs are high. In addition, the above-mentioned paper containers have a low degree of freedom in terms of shape, and therefore have problems such as being unable to fully demonstrate the appeal of the product based on the shape of the container.
[0004] One of the means for increasing the degree of freedom in the shape of paper containers is pulp molding, which produces molded products from a slurry containing pulp and water. In pulp molding, the pulp in the slurry is generally deposited on a mold to form a pulp layer, which is then dehydrated and dried in an oven. The molded products obtained by this technique, i.e., pulp molded products, are excellent in heat resistance, cold resistance, moisture absorption and release, etc., which are characteristic physical properties of paper-based packaging materials, and have come to be widely used as paper tray containers for food, fixed cushioning materials for fruits, etc. (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-285188 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a technique that is advantageous for realizing a pulp molded product exhibiting excellent strength. [Means for solving the problem]
[0007] According to one aspect of the present invention, the pulp contains pulp having a fiber diameter of 4 μm or more, the ratio of fibers having a fiber length of 1 mm or less in the pulp is within a range of 33 to 55% by number, and the density is 0.45 g / cm 3 As a result, a pulp molded product is provided having a nitrogen content in the range of 2000 to 3000 μg / g as measured by a chemiluminescence method.
[0008] According to another aspect of the invention, the density is 0.65 g / m 3 The present invention provides a pulp molded article according to the above aspect, wherein the pulp molded article has a diameter of less than 1 / 2 mm.
[0009] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, having a minimum thickness of 1.2 mm or less.
[0010] According to yet another aspect of the present invention, there is provided a pulp molded product according to any one of the above aspects, further comprising fine cellulose fibers having a fiber diameter of 800 nm or less.
[0011] According to yet another aspect of the present invention, there is provided a pulp molded product according to the above aspect, in which the proportion of the fine cellulose fibers in the total amount of the pulp and the fine cellulose fibers is within the range of 1 to 9 mass %.
[0012] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
[0013] According to yet another aspect of the present invention, there is provided a pulp molded product according to any of the above aspects, wherein the pulp includes a first pulp having an average fiber diameter in the range of 15 to 22 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
[0014] According to yet another aspect of the present invention, there is provided the pulp molded product according to the above aspect, wherein the pulp further includes a second pulp having an average fiber diameter in the range of 22 to 40 μm.
[0015] According to yet another aspect of the present invention, there is provided the pulp molded product according to any one of the above aspects, wherein the proportion of the first pulp in the pulp is 50% by mass or more.
[0016] According to yet another aspect of the present invention, there is provided a pulp molded article according to any one of the above aspects, which is a container.
[0017] According to yet another aspect of the present invention, a slurry is prepared, the slurry comprising fibers containing pulp having a fiber diameter of 4 μm or more, a strength agent, and water, the ratio of fibers having a fiber length of 1 mm or less being within the range of 33 to 55%, the strength agent comprising one or more poly(meth)acrylamides each containing an acrylamide group, an anionic group, and a cationic group, the ratio of the strength agent based on a solid content to the total of the fibers and the strength agent being within the range of 2.1 to 5.2 mass%, depositing the fibers on a cutting mold having a three-dimensional shape to form a pulp layer, dehydrating the pulp layer to obtain an intermediate molded product, and sandwiching the undried intermediate molded product between a male mold and a female mold and heating it to a temperature within the range of 120 to 250° C. while applying a pressure within the range of 0.1 to 3.0 MPa to obtain a slurry having a density of 0.45 g / cm. 3and obtaining the above-mentioned pulp molded article.
[0018] According to yet another aspect of the present invention, the pulp molded product has a density of 0.65 g / m 3 The present invention provides a method for producing a molded pulp article according to the above aspect, which achieves less than 100%.
[0019] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to any one of the above aspects, which produces the pulp molded product having a minimum thickness of 1.2 mm or less.
[0020] According to yet another aspect of the present invention, there is provided the method for producing a pulp molded product according to any one of the above aspects, wherein the fibers further contain fine cellulose fibers having a fiber diameter of 800 nm or less.
[0021] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to the above aspect, in which the proportion of the fine cellulose fibers in the slurry relative to the total amount of the pulp and the fine cellulose fibers is within the range of 1 to 9 mass%.
[0022] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to any of the above aspects, in which the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
[0023] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to any of the above aspects, wherein the pulp includes a first pulp having an average fiber diameter in the range of 15 to 22 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
[0024] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to the above aspect, wherein the pulp further includes a second pulp having an average fiber diameter in the range of 22 to 40 μm.
[0025] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to any one of the above aspects, wherein a ratio of the first pulp in the pulp is 50 mass % or more.
[0026] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product relating to any of the above aspects, wherein depositing the fibers on the mold includes preparing a cover body as a hollow body having an opening, fixing the mold to the opening, immersing the mold fixed to the opening in the slurry, and reducing the pressure in the space enclosed by the cover body and the mold immersed in the slurry.
[0027] According to yet another aspect of the present invention, there is provided a method for producing a pulp molded product according to the above aspect, in which the mold is immersed in the slurry so that the mold is positioned above the cover body. Effect of the Invention
[0028] The present invention provides a technique that is advantageous for realizing a pulp molded product exhibiting excellent strength. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a perspective view showing a pulp molded product according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of FIG. [Diagram 3] FIG. 3 is a diagram showing a pulp layer forming process in pulp molding using the apparatus of FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates an example of a pulp layer formed on a mold. [Diagram 5] FIG. 5 is a diagram showing a dewatering process in pulp molding using the apparatus of FIG. [Figure 6] FIG. 6 is a diagram showing a conveying process of a pulp layer in pulp molding using the apparatus of FIG. [Figure 7] FIG. 7 is a diagram showing a hot press forming process in pulp molding using the apparatus of FIG. [Figure 8] FIG. 8 is a cross-sectional view that illustrates an example of a pulp molded product obtained by the heat pressing process. [Figure 9] FIG. 9 is a diagram showing a conveying process of a pulp molded product in pulp molding using the apparatus of FIG. [Figure 10] FIG. 10 is a diagram showing a state in which the transport process of FIG. 9 has been completed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.
[0031] The embodiments described below are merely examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of the present invention within the technical scope defined by the claims.
[0032] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.
[0033] <1> Pulp Molding FIG. 1 is a perspective view showing a pulp molded product according to one embodiment of the present invention. The pulp molded product MP2 shown in Fig. 1 is a container. This pulp molded product MP2 includes a bottom and a side wall, and is open at the top.
[0034] The bottom has a disk shape. The orthogonal projection of the bottom onto a plane perpendicular to the depth direction of the container may have a shape other than a circle, for example, a polygonal shape such as a square.
[0035] The side wall has a cylindrical shape extending upward from the edge of the bottom. The side wall expands in diameter from the bottom toward the opening. The inner and outer surfaces of the side wall may be perpendicular to the upper surface of the bottom. However, the pulp molded product MP2 in which the side wall expands in diameter from the bottom toward the opening is advantageous in realizing high releasability and is easy to stack.
[0036] The pulp molded product MP2 may have various shapes such as a cup shape, a bowl shape, a tray shape, a box shape, etc. The pulp molded product MP2 does not have to be a container as long as it is a three-dimensional molded product, i.e., a molded product having a three-dimensional shape, not a two-dimensional shape like a sheet.
[0037] The pulp molded product MP2 preferably has a minimum thickness of 1.2 mm or less. That is, the minimum thickness of the wall of the pulp molded product MP2, here the minimum thickness of the bottom and side walls, is preferably 1.2 mm or less. It is more preferable that the pulp molded product MP2 has a minimum thickness of 1.0 mm or less. A thick pulp molded product MP2 is bulky, especially when stacked. Also, if the thickness is increased, it becomes difficult to mold the pulp molded product MP2 into a complex shape. On the other hand, making the wall of the pulp molded product MP2 thin is advantageous in that drying during production can be completed in a short time.
[0038] The pulp molded product MP2 preferably has a minimum thickness of 0.4 mm or more, more preferably 0.7 mm or more. The pulp molded product MP2 has a thin wall, so that the thickness of the wall is likely to vary.
[0039] In addition, a pulp molded product having a shape in which multiple surfaces are connected generally has a greater thickness at the connection points of the surfaces than at other points. In the pulp molded product MP2, the thickness at the connection points between the bottom and the side walls is usually greater than at other points. The above "minimum thickness" specifies the thickness at points other than the connection points.
[0040] The density of the pulp molded product MP2 is 0.45g / cm 3 The density of the pulp molded product MP2 is 1.20 g / cm 3 The density of the pulp molded product MP2 is preferably 0.45 to 0.90 g / cm 3 More preferably, the range is 0.45 to 0.70 g / cm 3 It is more preferable that the density of the pulp molded product MP2 is within the range of 0.65 g / cm3. 3 It may be less than.
[0041] When the density is low, it is difficult to achieve good strength. Pulp molded products MP2 with excessively high density usually have low flexibility and are prone to cracking.
[0042] The pulp molded product MP2 has a basis weight of 300 to 1000 g / cm 2 and preferably in the range of 300 to 650 g / cm 2 It is more preferable that the ratio is in the range of 1.
[0043] Here, the above-mentioned minimum thickness, density and basis weight are values obtained by the following method. That is, a square or rectangular test piece is cut out from a portion of the pulp molded product MP2 where the surface is not curved, and the dimensions, mass and thickness are measured. For example, 10 test pieces each having a strip shape with a width of 15 mm and a length of 145 mm are cut out from the pulp molded product MP2. Then, the width, length, thickness and mass of each test piece are measured. For example, a digital caliper is used to measure the width, length and thickness. For example, an electronic balance is used to measure the mass. Then, the thickness, density and basis weight of each test piece are calculated from the values obtained for each test piece. Then, the above-mentioned minimum density and basis weight are obtained by arithmetically averaging the values obtained for the 10 test pieces.
[0044] The pulp molded product MP2 contains pulp having a fiber diameter of 4 μm or more. According to one example, the fibers contained in the pulp molded product MP2 are made of pulp.
[0045] The fiber diameter of the pulp is preferably 7 μm or more. The fiber diameter of the pulp is preferably 100 μm or less, and more preferably 80 μm or less. The average fiber diameter of the pulp is preferably in the range of 15 to 40 μm, and more preferably in the range of 17 to 25 μm. Pulp suitable for the pulp molded product MP2 has a fiber diameter within the above range.
[0046] The fiber diameter of the pulp can be measured from an image obtained using a microscope such as an optical microscope. The average fiber diameter of the pulp can be obtained by arithmetically averaging the fiber diameters measured from the image.
[0047] The average fiber diameter of the pulp is preferably within a range of 15 to 40 μm. The pulp molded product MP2 may contain only one type of pulp as the pulp, or may contain multiple types of pulp. For example, the pulp molded product MP2 may contain only a first pulp as the pulp having an average fiber diameter within a range of 15 to 22 μm, or may contain the first pulp and a second pulp having an average fiber diameter within a range of 22 to 40 μm. The proportion of the first pulp in the pulp is preferably 50 mass% or more.
[0048] In the pulp molded product MP2, the proportion of pulp having a fiber length of 1 mm or less is in the range of 33 to 55% by number. This proportion is preferably in the range of 40 to 50%. In the production of the pulp molded product MP2, the paper strength agent described below adheres more easily to short fibers than to long fibers. Therefore, by increasing this proportion, the strength of the pulp molded product MP2 can be increased. However, if this proportion is excessively increased, it becomes difficult to release the pulp molded product MP2 from the mold. Note that the "fine cellulose fibers" described below are not included in the "pulp" referred to here.
[0049] The percentage of pulp having a fiber length of 1 mm or less is obtained by the following method. First, a 5g test piece is obtained from the pulp molded product MP2. Next, the test piece is finely shredded, and water is added so that the total mass is 500g, and the test piece is soaked overnight. Then, the test piece is stirred with a stirrer to disintegrate the pulp from each other. In this way, a dispersion containing pulp is obtained. Next, an appropriate amount is taken from the dispersion and further diluted with water to prepare an aqueous dispersion with a pulp solid content of 0.05% by mass.
[0050] Using the sample obtained in this way, fiber length is measured according to JIS P8226-2:2011 "Pulp - Fiber length measurement method by optical automatic analysis method - Part 2: Non-polarized method". The fiber length measurement is completed when 20,000 or more fibers with a fiber length of 0.2 mm or more are detected. From the frequency distribution of fiber lengths obtained from this fiber length measurement, the percentage of pulp with a fiber length of 1 mm or less is calculated.
[0051] The pulp molded product MP2 may further contain fine cellulose fibers. In this case, the fibers contained in the pulp molded product MP2 are preferably composed of pulp and fine cellulose fibers.
[0052] The fine cellulose fibers have a fiber diameter of 800 nm or less. Such fine fibers can contribute to improving the peel strength of the pulp molded product MP2.
[0053] The fiber diameter of the fine cellulose fibers is preferably 500 nm or less. Fine cellulose fibers having a small fiber diameter can fill the gaps between adjacent pulps without interfering with hydrogen bonding between the pulps. Therefore, in order to achieve excellent strength, it is preferable that the fine cellulose fibers have a small fiber diameter.
[0054] The fiber diameter of the fine cellulose fibers is preferably 10 nm or more, and more preferably 50 nm or more. A part of the fine cellulose fibers may be detached from the pulp layer together with water during the dehydration process in the production of the pulp molded product MP2. Fine cellulose fibers with a large fiber diameter are less likely to be detached. In addition, fine cellulose fibers with a large fiber diameter do not excessively increase the residual moisture content of the pulp layer immediately before the drying process in the production of the pulp molded product MP2. Therefore, fine cellulose fibers with a large fiber diameter are advantageous in completing the drying process in a short time in the production of the pulp molded product MP2.
[0055] The average fiber diameter of the fine cellulose fibers is preferably in the range of 50 to 500 nm, and more preferably in the range of 100 to 300 nm. The fine cellulose fibers suitable for the pulp molded product MP2 have a fiber diameter within the above range.
[0056] The fiber diameter of the fine cellulose fibers can be measured from an image obtained using a microscope such as a scanning electron microscope. The average fiber diameter of the fine cellulose fibers can be obtained by randomly selecting 20 fine cellulose fibers from the image and arithmetically averaging the fiber diameters measured for the selected fine cellulose fibers.
[0057] When the pulp molded product MP2 further contains fine cellulose fibers, the ratio of the fine cellulose fibers to the total amount of pulp and fine cellulose fibers is preferably in the range of 1 to 9 mass%, more preferably in the range of 3 to 5 mass%. If this ratio is reduced, the effect of improving the strength of the pulp molded product MP2 by adding the fine cellulose fibers is reduced. If this ratio is increased, the remaining moisture content of the pulp layer immediately before the drying step during the production of the pulp molded product MP2 increases, and therefore, the drying time during the production of the pulp molded product MP2 may become longer.
[0058] The nitrogen content of the pulp molded product MP2 is in the range of 2000 to 3000 μg / g as determined by a chemiluminescence method. This nitrogen content is preferably in the range of 2000 to 2500 μg / g. Increasing this nitrogen content improves the strength of the pulp molded product MP2. However, if the nitrogen content is too high, the adhesion of the pulp to the mold becomes excessive, making it difficult to manufacture the pulp molded product MP2.
[0059] Here, the nitrogen content of the pulp molded product MP2 measured by the chemiluminescence method is a value obtained by the following method. First, two test pieces are taken from the pulp molded product MP2 at arbitrary positions. Each test piece has a mass of 10 mg. Next, each test piece is measured by the chemiluminescence method specified in JIS K2609:1998 "Crude oil and petroleum products - Nitrogen analysis test method". For this measurement, for example, TN-2100H manufactured by Nitto Seiko Analytech Co., Ltd. can be used. The nitrogen content is obtained by arithmetically averaging the measured values thus obtained.
[0060] The pulp molded product MP2 has an ISO ring crush compressive strength in the range of, for example, 3.0 to 14.0 kN / m. The ISO ring crush compressive strength of the pulp molded product MP2 is preferably in the range of 3.0 to 6.0 kN / m, more preferably in the range of 3.0 to 4.5 kN / m.
[0061] Here, the ISO ring crush compressive strength of the pulp molded product MP2 is a value obtained by the method specified in JIS P8126:2015 "Compressive strength test method - Ring crush method". The compressive strength is determined by clamping a long and thin test piece bent into a cylindrical (ring-like) shape between parallel upper and lower compression plates, applying a compressive load to cause buckling, obtaining the maximum load, and dividing the obtained maximum load by the length of the test piece. In this test method, the long and thin test piece is prepared by cutting a strip-shaped test piece with a width of 15 mm and a length of 145 mm from the pulp molded product MP2.
[0062] The pulp molded product MP2 with a large ISO ring crush compressive strength is unlikely to buckle even when a large load is applied. However, if the ISO ring crush compressive strength of the pulp molded product MP2 is increased, it becomes more susceptible to breakage when an impact load is applied when dropped, etc.
[0063] <2> Pulp molding manufacturing equipment Next, a manufacturing apparatus that can be used to manufacture the pulp molded product MP2 will be described. FIG. 2 is a schematic diagram showing an example of a manufacturing apparatus that can be used to manufacture the pulp molded product of FIG.
[0064] The manufacturing apparatus 1 shown in FIG. 2 includes a support 10, a first station 20, a second station 30, and a third station 40.
[0065] The support 10 includes a frame and a rail installed on the upper portion thereof.
[0066] The first station includes a container 210 , a lifting device 220 , a cover body 230 , a mold 240 , a moving device 250 , a lifting device 260 , and an upper mold 270 .
[0067] The container 210 is placed within the frame of the support 10. The container 210 is open at the top. The container 210 contains a slurry S containing pulp, a paper strength agent, and water. The slurry S may further contain fine cellulose fibers.
[0068] The lifting device 220 is attached to the frame of the support 10 above the container 210. The lifting device 220 includes, for example, a hydraulic cylinder. The lifting device 220 supports a cover body 230. The lifting device 220 can raise and lower the cover body 230 at the position of the opening of the container 210.
[0069] The cover body 230 is a hollow body having an opening at the top. A pump (not shown) is connected to the cover body 230.
[0070] The mold 240 is fixed to the opening of the cover body 230. Specifically, the mold 240 is fixed to the opening of the cover body 230 such that one surface of the mold 240 and a space adjacent to the mold 240 are surrounded by the mold 240 and the cover body 230.
[0071] The mold 240 is a mold that is liquid permeable. The mold 240 has a three-dimensional shape. That is, the mold 240 has one or more convex portions and / or one or more concave portions on the surface on which the pulp, etc. are accumulated. Specifically, the outer surface of the mold 240, i.e., the back surface of the surface adjacent to the above-mentioned space, has a shape corresponding to a pulp molded product. Here, the mold 240 is a male mold with a protruding upper surface.
[0072] The mold 240 includes, for example, a mold body having a number of through holes and an outer surface having a shape corresponding to the pulp molded product, and a mesh body arranged on and along the outer surface of the mold body.
[0073] The moving device 250 is movable between the first station 20 and the second station 30 along the rails of the support 10. The moving device 250 includes, for example, a motor as a power source. The moving device 250 is equipped with an elevator device 260, which can be transported between the first station 20 and the second station 30.
[0074] As described above, the lifting device 260 is attached to the moving device 250. The lifting device 260 includes, for example, a hydraulic cylinder. The lifting device 260 supports the upper mold 270. The lifting device 260 can raise and lower the upper mold 270.
[0075] The upper mold 270 is a holder that sandwiches a pulp layer, which will be described later, between itself and the mold 240 and holds the pulp layer by vacuum suction. The lower surface of the upper mold 270 has a shape corresponding to the outer surface of the mold 240. Here, the upper mold 270 is a female mold with a concave lower surface. The upper mold 270 has, for example, a large number of through holes, one end of which is open at the lower surface and the other end of which is connected to a pump.
[0076] The second station 30 is provided near the first station 20. The second station 30 includes a base 310, a lower mold 320, a moving device 330, a pressing device 340, and an upper mold 350.
[0077] The base 310 is placed within the frame of the support 10. On the base 310, a lower mold 320 is placed.
[0078] The lower mold 320 is a mold that is permeable to gas and / or liquid. The upper surface of the lower mold 320 has a shape corresponding to the outer surface of the mold 240. Here, the lower mold 320 is a male mold with a protruding upper surface. The lower mold 320 has, for example, a large number of through holes, and has a smooth surface that has a shape corresponding to the outer surface of the mold 240.
[0079] The moving device 330 is movable between the second station 30 and a fourth station (not shown) along the rails of the support 10. The moving device 330 includes, for example, a motor as a power source. When the moving device 330 is located at the second station 30, the movement of the moving device 330 in the up-down, left-right, and front-rear directions can be restricted by a locking mechanism. In addition, a pressing device 340 is attached to the moving device 330, and the pressing device 340 can be transported between the second station 30 and the fourth station.
[0080] As described above, the press device 340 is attached to the moving device 330. The press device 340 includes, for example, a hydraulic cylinder. The press device 340 supports the upper die 350. The press device 340 can raise and lower the upper die 350.
[0081] The upper mold 350 is a mold that is neither gas permeable nor liquid permeable. The lower surface of the upper mold 350 has a shape corresponding to the outer surface of the mold 240. Here, the upper mold 350 is a female mold with a concave lower surface. The upper mold 350 has a smooth surface that has a shape corresponding to the outer surface of the mold 240.
[0082] The second station 30 further includes a heater and a pump (neither of which are shown). The heater heats both the lower mold 320 and the upper mold 350. The pump is connected to the lower space of the lower mold 320.
[0083] The third station 40 is provided near the second station 30. The third station 40 includes a platform 410, a moving device 420, a lifting device 430, and a holder 440.
[0084] The base 410 is installed within the frame of the support 10. On the base 410, a pulp molded product is placed.
[0085] The moving device 420 is movable between the second station 30 and the third station 40 along the rails of the support 10. The moving device 420 includes, for example, a motor as a power source. The moving device 420 is provided with an elevator device 430, which can be transported between the second station 30 and the third station 40.
[0086] As described above, the lifting device 430 is attached to the moving device 420. The lifting device 430 includes, for example, a hydraulic cylinder. The lifting device 430 supports the holder 440. The lifting device 430 can raise and lower the holder 440.
[0087] The holder 440 is a holder that holds a pulp molded product (described later) by vacuum suction. The lower surface of the holder 440 has a shape corresponding to the outer surface of the mold 240. Here, the holder 440 has a concave lower surface. The holder 440 has, for example, a number of through holes that open at one end at the lower surface and are connected at the other end to a pump.
[0088] <3> Manufacturing method of pulp molded products In a manufacturing method according to one embodiment of the present invention, for example, a pulp molded product MP2 is manufactured using the above-mentioned manufacturing apparatus 1. This will be described with reference to FIGS.
[0089] FIG. 3 is a diagram showing a pulp layer forming step in pulp molding using the apparatus of FIG. 2. FIG. 4 is a cross-sectional view showing an example of a pulp layer formed on a mold. FIG. 5 is a diagram showing a dewatering step in pulp molding using the apparatus of FIG. 2. FIG. 6 is a diagram showing a pulp layer conveying step in pulp molding using the apparatus of FIG. 2. FIG. 7 is a diagram showing a heat press molding step in pulp molding using the apparatus of FIG. 2. FIG. 8 is a cross-sectional view showing an example of a pulp molded product obtained by the heat press step. FIG. 9 is a diagram showing a conveying step of a pulp molded product in pulp molding using the apparatus of FIG. 2. FIG. 10 is a diagram showing a state in which the conveying step of FIG. 9 has been completed.
[0090] In this method, first, a slurry S is prepared. As described above, the slurry S contains pulp, a strength agent, and water. The slurry S is a suspension having a high viscosity in which the pulp is dispersed in water and the strength agent is dissolved or dispersed in water. The slurry S may further contain fine cellulose fibers. Here, as an example, the slurry S contains pulp, fine cellulose fibers, a strength agent, and water.
[0091] The pulp contained in the slurry S has substantially the same characteristics as those described above for the pulp contained in the pulp molded product MP2.
[0092] There is no particular limitation on the type of pulp used in the slurry S. Examples of pulp include wood pulp, non-wood pulp, and waste paper, with wood pulp and non-wood pulp being preferred. From the viewpoint of environmental considerations such as forest conservation and utilization of unused resources, it is preferable to use non-wood pulp.
[0093] Pulps can be classified according to the difference in the preparation method. For example, examples of wood pulp include chemical pulps such as kraft pulp (KP), sulfite pulp (SP), and soda pulp (AP); semi-chemical pulps such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP); groundwood pulp (GP), and thermomechanical pulp (TMP). Among these, it is preferable to use chemical pulp. The pulp may be bleached pulp or unbleached pulp.
[0094] Wood pulp can be classified according to the raw material. Examples of wood pulp include coniferous pulp and hardwood pulp. Examples of coniferous pulp include pulp obtained from the fir and pine genus. Examples of hardwood pulp include pulp obtained from the acacia, eucalyptus, beech, and poplar genus (e.g., poplar).
[0095] Non-wood pulp is obtained from fibers extracted from the bark, stems, leaves, and leaf sheaths of plants. Specific examples include pulps obtained from cotton linters, cotton, linen, hemp, ramie, straw, esparto, Manila hemp, sisal, jute, flax, kenaf, bamboo, sugarcane, ganpi, mitsumata, kozo, and mulberry. Among these, bamboo and sugarcane pulps are preferred.
[0096] These pulps can be used alone or in combination of two or more kinds in any desired ratio.
[0097] Pulp has different fiber lengths and the like depending on its raw material and manufacturing method. For example, pulp made from sugarcane generally has a shorter average fiber length than pulp made from bamboo. The average fiber length of pulp can be adjusted by any method, for example, mechanical treatment such as beating or crushing. Thus, pulp having certain characteristics can be obtained, for example, by selecting an appropriate one from multiple types of pulp, or by appropriately combining two or more types of pulp. As the pulp, it is preferable to use non-wood pulp, and it is preferable to use pulp made from sugarcane, pulp made from bamboo, or a combination thereof.
[0098] The pulp content of the slurry S is preferably in the range of 0.01 to 3.0% by mass, more preferably in the range of 0.01 to 0.5% by mass. If the pulp content is low, it is difficult to achieve high productivity. If the pulp content is high, there is a possibility that the thickness of the pulp layer will vary widely.
[0099] The fine cellulose fibers that the slurry S may contain have substantially the same characteristics as those described above for the fine cellulose fibers contained in the pulp molded product MP2.
[0100] As the fine cellulose fibers, for example, those having an average fiber diameter in the range of 50 to 500 nm, those having an average fiber diameter less than 50 nm, those having an average fiber diameter greater than 500 nm, or a combination of two or more of them can be used. As the fine cellulose fibers or their dispersions having an average fiber diameter in the range of 50 to 500 nm, for example, the CELISH (registered trademark) series manufactured by Daicel Miraize Co., Ltd. or the EXILVA (registered trademark) series manufactured by Borregaard Co., Ltd. are listed. As the fine cellulose fibers or their dispersions having an average fiber diameter less than 50 nm, for example, BiNFi-s (registered trademark) manufactured by Sugino Machine Co., Ltd. and ELLEX (registered trademark)-☆ manufactured by Daio Paper Co., Ltd. are listed. As the fine cellulose fibers or their dispersions having an average fiber diameter greater than 500 nm, for example, the CELISH (registered trademark) series manufactured by Daicel Miraize Co., Ltd. are listed. As the fine cellulose fibers, it is preferable to use those having an average fiber diameter in the range of 50 to 500 nm.
[0101] When using fine cellulose fibers, the proportion of fine cellulose fibers in the total amount of pulp and fine cellulose fibers in the slurry S is preferably in the range of 1 to 9 mass%, and more preferably in the range of 3 to 5 mass%.
[0102] The strength agent is one or more poly(meth)acrylamides each containing (meth)acrylamide groups, anionic groups and cationic groups.
[0103] Here, the "(meth)acrylamide group" refers to at least one of an acrylamide group and a methacrylamide group. Also, "poly(meth)acrylamide" refers to a polymer containing acrylamide but not methacrylamide as a monomer, a polymer containing methacrylamide but not acrylamide as a monomer, or a polymer containing acrylamide and methacrylamide as monomers. Terms using similar notations, such as "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyl group", should be construed as abbreviations of multiple compounds or groups in the same manner as above.
[0104] The cationic group is, for example, a primary amine, a secondary amine, or a tertiary amine. The anionic group is, for example, a carboxyl group, a sulfo group, a nitrate salt, or a phosphate salt.
[0105] The acrylamide group and methacrylamide group can form hydrogen bonds with the carboxyl group of cellulose. The cationic group and anionic group can contribute to improving the affinity between the paper strength agent and water. And the cationic group can interact with the carboxyl group of cellulose in the slurry S.
[0106] The poly(meth)acrylamide is, for example, a copolymer obtained by copolymerizing monomer components including the first to third monomers. The first monomer is at least one of acrylamide and methacrylamide. According to one example, the first monomer is acrylamide.
[0107] The second monomer introduces a cationic group into the poly(meth)acrylamide. The second monomer is, for example, one or more of an unsaturated monomer having a secondary amino group, an unsaturated monomer having a tertiary amino group, and a quaternary salt of these unsaturated monomers.
[0108] The unsaturated monomer having a secondary amino group is, for example, diallylamine. The unsaturated monomer having a tertiary amino group is, for example, one or more of (meth)acrylates having a tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate; and (meth)acrylamides having a tertiary amino group, such as N,N-dimethylaminopropyl (meth)acrylamide and N,N-diethylaminopropyl (meth)acrylamide. The quaternary salts of these monomers are, for example, salts obtained by reacting the unsaturated monomer having a secondary amino group or the unsaturated monomer having a tertiary amino group with a quaternizing agent. The quaternary salt may be an inorganic acid salt such as hydrochloride and sulfate, or an organic acid salt such as acetate. The quaternizing agent is, for example, one or more of methyl chloride, benzyl chloride, dimethyl sulfate, and epichlorohydrin.
[0109] According to one example, the second monomer is N,N-dimethylaminoethyl methacrylate, N,N-dimethylaminoethyl methacrylate benzyl chloride, N,N-dimethylaminoethyl acrylate benzyl chloride, or N,N-dimethylaminopropylacrylamide.
[0110] The third monomer introduces an anionic group into the poly(meth)acrylamide. The third monomer is, for example, one or more of unsaturated monomers having a carboxyl group, such as (meth)acrylic acid, itaconic acid, itaconic anhydride, fumaric acid, and maleic acid; unsaturated monomers having a sulfonic acid group, such as vinyl sulfonic acid and methallylsulfonic acid; and salts thereof, such as alkali metal salts, such as sodium salts and potassium salts, or ammonium salts. According to one example, the third monomer is itaconic acid, acrylic acid, or sodium methallylsulfonate.
[0111] The poly(meth)acrylamide may have a branched structure. Examples of compounds that can be used to introduce a branched structure into poly(meth)acrylamide (hereinafter, sometimes referred to as a branch-introducing compound) include N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nt-butyl(meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethylacrylamide, N,N-diethyl(meth)acrylamide, and N,N-diisopropyl(meth)acrylamide; N,N N,N'-alkylenebis(meth)acrylamides such as N,N'-ethylenebis(meth)acrylamide, N,N'-alkylenebis(meth)acrylamides, triallyl isocyanurate, triallyl trimellitate, triallylamine, and triallyl(meth)acrylamide, and other crosslinkable unsaturated monomers containing a triallyl group, and (meth)acryloyl group-containing triazines such as 1,3,5-triacryloyl-1,3,5-triazine and 1,3,5-triacryloylhexahydro-1,3,5-triazine. According to one example, the compound used to introduce a branched structure into poly(meth)acrylamide is N,N-dimethylacrylamide or N,N'-methylenebisacrylamide.
[0112] The above-mentioned monomer components can further include other monomers. The other monomer components are, for example, one or more of aromatic unsaturated monomers such as styrene, α-methylstyrene, and vinyltoluene; alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate; vinyl carboxylates such as vinyl acetate and vinyl propionate; nitriles such as acrylonitrile; mercaptans such as 2-mercaptoethanol and n-dodecyl mercaptan; alcohols such as ethanol, isopropyl alcohol, and n-pentyl alcohol; aromatic compounds such as α-methylstyrene dimer, ethylbenzene, isopropylbenzene, and cumene; and carbon tetrachloride.
[0113] The ratio of the first monomer to the total of the monomer components and the branch-introducing compound is preferably within the range of 75 to 90 mol %. The ratio of the second monomer to the total of the monomer components and the branch-introducing compound is preferably within the range of 6 to 18 mol %. The ratio of the third monomer to the total of the monomer components and the branch-introducing compound is preferably within the range of 2.5 to 22 mol %. The ratio of the branch-introducing compound to the total of the monomer components and the branch-introducing compound is preferably about 0.1 mol %.
[0114] A polymerization initiator can be used for copolymerization of the first to third monomers. The polymerization initiator is, for example, one or more of persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; azo compounds such as 2,2'-azobis(2-amidinopropane) hydrochloride and 2,2'-azobis[2(2-imidazolin-2-yl)propane] hydrochloride; and hydrogen peroxide. According to one example, the polymerization initiator is ammonium persulfate. The amount of the polymerization initiator is preferably in the range of 0.001 to 5 parts by mass, more preferably in the range of 0.01 to 1 part by mass, relative to 100 parts by mass of the total of the monomer components and the branch-introducing compound.
[0115] As the paper strength agent, a commercially available product may be used. For example, the Polystron (registered trademark) series manufactured by Arakawa Chemical Industries, Ltd., the DS series or DH series manufactured by Seiko PMC Co., Ltd., or the Hermide (registered trademark) series manufactured by Harima Chemical Industries, Ltd. may be used as the paper strength agent.
[0116] The above-mentioned strength agent generates ionic interactions with cellulose in the slurry S and forms hydrogen bonds, and therefore has a particularly excellent effect in strengthening the bonds between fibers. Therefore, such strength agents can be used in small amounts to produce a pulp molded product MP2 with excellent strength.
[0117] The ratio of the strength agent to the total of the pulp, the fine cellulose fibers, and the strength agent on a solid content basis is preferably within the range of 2.1 to 5.2 mass%, more preferably within the range of 2.2 to 4.5 mass%.
[0118] The slurry S may further contain other additives. As the additives, organic low molecular weight materials, organic high molecular weight materials, inorganic materials, or combinations thereof may be used, and examples of such additives include agents that impart water resistance or oil resistance, and the agent may be selected according to the performance requirements of the pulp molded container.
[0119] The proportion of other additives in the total of pulp, fine cellulose fibers, paper strength agent, and other additives is preferably 3% by mass or less, and more preferably 1% by mass or less.
[0120] Next, the slurry S is supplied into the container 210. Then, as shown in FIG. 3, the cover body 230 is lowered by the lifting device 220 so that the upper surface of the mold 240 is positioned sufficiently below the liquid level of the slurry S. In this state, the pump is driven to reduce the pressure in the space surrounded by the cover body 230 and the mold 240. This causes a flow of the slurry S across the mold 240, and a mixture of pulp and fine cellulose fibers is deposited on the mold 240. In this manner, a pulp layer MP1 is formed on the mold 240, as shown in FIG. 4.
[0121] Next, while the pump is still running, as shown in FIG. 5, the lifting device 220 lifts the cover body 230 to position the lower part of the mold 240 sufficiently above the liquid level of the slurry S. This reduces the pressure and dewaters the pulp layer MP1. Next, the lifting device 260 is driven to lower the upper mold 270 until its lower surface comes into contact with the pulp layer MP1. Note that the pulp layer MP1 is not shown in FIG. 5. This dewatering process is performed without heating either the upper mold 270 or the mold 240.
[0122] The decompression time in the dehydration step is preferably within the range of 1 to 60 seconds, and more preferably within the range of 1 to 10 seconds.
[0123] The moisture content of the pulp layer MP1 immediately after dehydration is preferably in the range of 40 to 90% by mass, more preferably in the range of 50 to 70% by mass, and even more preferably in the range of 60 to 70% by mass. If the moisture content is low, the movement of the fibers in the in-plane direction in the pulp layer may be insufficient in the heat pressing process. If the moisture content is high, the movement of the fibers in the in-plane direction in the pulp layer may be excessive in the heat pressing process, or the shape retention of the pulp layer MP1 may be insufficient during the period from the end of the dehydration process to the start of the heat pressing process.
[0124] After the decompression and pressurization of the space are stopped, the pump is driven to adsorb and hold the pulp layer MP1 to the upper mold 270. Note that the suction by the pump and upper mold 270 does not cause further dehydration of the pulp layer MP1.
[0125] Next, with the pulp layer MP1 being adsorbed and held by the upper mold 270, the lifting device 260 is driven to lift the upper mold 270 as shown in Fig. 2. This causes the pulp layer MP1 to be peeled off from the mold 240.
[0126] Next, the moving devices 250 and 330 are driven to move the pressing device 340 and the upper mold 350 from the second station 30 to the fourth station, and the lifting device 260 and the upper mold 270 from the first station 20 to the second station 30, as shown in FIG. 6. Then, the lifting device 260 is driven to lower the upper mold 270 until the pulp layer MP1 contacts the lower mold 320. Then, the suction by the pump and the upper mold 270 is stopped, and the pulp layer MP1 is released from the upper mold 270. Next, the lifting device 260 is driven to raise the upper mold 270. In this way, the pulp layer MP1 is transferred from the first station 20 to the second station 30, and the pulp layer MP1 is placed on the lower mold 320.
[0127] Next, the moving devices 250 and 330 are driven to move the lifting device 260 and the upper mold 270 from the second station 30 to the first station 20 as shown in FIG. 2, and the pressing device 340 and the upper mold 350 are moved from the fourth station to the second station 30. Next, the pressing device 340 is driven to lower the upper mold 350 as shown in FIG. 7. Then, the pulp layer MP1 sandwiched between the upper mold 350 and the lower mold 320 is pressurized. At the same time, the heater is driven to heat the pulp layer MP1. Furthermore, at the same time, the pump is driven to suck and remove water and / or water vapor from the space sandwiched between the upper mold 350 and the lower mold 320. This adjusts the surface shape of the pulp layer MP1, and densifies and dries the pulp layer MP1. In this manner, the pulp molded product MP2 shown in FIG. 8 is obtained.
[0128] The moisture content of the pulp layer MP1 immediately before the start of the heat pressing step is substantially equal to the moisture content of the pulp layer MP1 immediately after the completion of the dewatering step.
[0129] In this heat pressing process, the pressing pressure is set to a range of 0.1 to 3.0 MPa. More preferably, the pressing pressure is set to a range of 0.2 to 1.2 MPa. If the pressing pressure is low, it is possible that a high-strength pulp molded product MP2 cannot be obtained. The pulp layer MP1 contains pulp and fine cellulose fibers with short fiber lengths. Such pulp and fine cellulose fibers are likely to move within the pulp layer MP1, particularly when the pressing pressure is excessively high. Therefore, if the pressing pressure is excessively high, the thickness of the pulp molded product MP2 is likely to vary.
[0130] In this heat pressing process, the heating temperature of the pulp layer MP1, i.e., the temperature of the upper mold 350 or the lower mold 320 heated by the heater, is in the range of 120 to 250°C. This temperature is more preferably in the range of 150 to 190°C. Since the pulp layer MP1 contains pulp with short fiber length and fine cellulose fibers, it is difficult for water vapor to escape to the outside. Therefore, if the heating temperature is low, it takes a long time to dry the pulp layer MP1. If the heating temperature is high, the shrinkage of the pulp layer MP1 due to drying becomes larger, which may result in larger distortion in the pulp molded product MP2.
[0131] The pressing time in the heat pressing step depends on the heating temperature, the shape of the molded product, etc., but is preferably within the range of 40 to 120 seconds, and more preferably within the range of 50 to 80 seconds.
[0132] Upon completing the above-mentioned hot pressing process, the press device 340 is driven so that the upper die 350 rises, and the pulp molded product MP2 is separated from the upper die 350.
[0133] Next, the moving devices 330 and 420 are driven to move the press device 340 and the upper mold 350 from the second station 30 to the fourth station, and the lifting device 430 and the holder 440 from the third station 40 to the second station 30, as shown in Fig. 9. Subsequently, the lifting device 430 is driven to lower the holder 440 until it comes into contact with the pulp molded product MP2. Air is ejected from inside the lower mold to release the pulp molded product MP2 from the lower mold, and then the pump is driven to adsorb and hold the pulp molded product MP2 on the holder 440. Next, the lifting device 430 is driven to lift the holder 440 while the pulp molded product MP2 is held by suction on the holder 440. Next, the moving devices 330 and 420 are driven to move the lifting device 430 and the holder 440 from the second station 30 to the third station 40, and move the press device 340 and the upper mold 350 from the fourth station to the second station 30, as shown in FIG. 10. Next, the suction by the pump and the holder 440 is stopped, and the pulp molded product MP2 is released from the holder 440. In this way, the pulp molded product MP2 is transferred from the second station 30 to the third station 40, and the pulp molded product MP2 is placed on the platform 410. In this manner, a pulp molded product MP2 is produced.
[0134] Thereafter, as necessary, the pulp molded product MP2 is subjected to post-treatment, such as printing with a pattern or plain printing, coating, or a combination thereof. The coating layer formed by the post-treatment is, for example, a layer containing a chemical that imparts water resistance or oil resistance, a layer filled with a material that imparts heat insulation, a layer foamed with a foaming agent, or a combination thereof. By performing the post-treatment, for example, it is possible to further improve the cosmetic properties of the pulp molded product MP2 or to impart new functions to the pulp molded product MP2.
[0135] According to the above method, a pulp molded article MP2 exhibiting excellent strength can be produced. For example, according to the above method, a pulp molded article MP2 exhibiting excellent strength even when it has a small thickness can be produced.
[0136] The pulp molded product MP2, which has a small wall thickness, is lightweight and has a small height when stacked, so that the pulp molded product MP2 can achieve high transportation efficiency.
[0137] The present inventors believe that the reason why the pulp molded article MP2 obtained by the above method exhibits excellent strength even when it has a small thickness is as follows.
[0138] The strength of pulp molded products is mainly provided by hydrogen bonds between the cellulose fibers contained in the pulp and entanglement of the fibers. If the wall thickness of a pulp molded product is reduced, the number of overlapping cellulose fibers in the thickness direction decreases, and the hydrogen bonds between the cellulose fibers and the entanglement of the fibers decrease, resulting in a decrease in strength.
[0139] In the above method, a strength agent is further added to the pulp slurry. The strength agent is one or more poly(meth)acrylamides each containing an acrylamide group, an anionic group, and a cationic group.
[0140] As described above, the acrylamide group can form hydrogen bonds with the carboxyl groups of cellulose, and the cationic group can form ionic interactions with the carboxyl groups of cellulose in the slurry S.
[0141] The cationic and anionic groups contribute to improving the affinity of the strength agent with water, and therefore these poly(meth)acrylamides can be uniformly dissolved in the pulp slurry. Furthermore, the strength agent is more easily fixed to short fibers than to long fibers. Here, the proportion of short fibers in the pulp is increased. Therefore, in the above method, a large amount of the strength agent is fixed to the short fibers, and the strength agent fixed to these short fibers strengthens the bonds between the short fibers and between the short fibers and long fibers.
[0142] Therefore, the pulp molded product MP2 obtained by the above method exhibits excellent strength even when it has a small thickness.
[0143] In the above method, when fine cellulose fibers are added to the pulp slurry, at least a part of the fine cellulose fibers penetrates into the gaps between the pulps in the pulp layer. In the pulp molded product MP2, the cellulose contained in a certain fine cellulose fiber can form hydrogen bonds with the cellulose contained in other fine cellulose fibers or the cellulose contained in the pulp. Therefore, the pulp molded product MP2 obtained by the above method when fine cellulose fibers are added to the pulp slurry exhibits excellent strength even when the thickness is smaller, or exhibits even greater strength even when the thickness is smaller.
[0144] Furthermore, according to the above method, since a paper strength agent is used, even when the product does not contain fine cellulose fibers or when the ratio of fine cellulose fibers to the total of pulp and fine cellulose fibers is small, a pulp molded product MP2 having excellent strength can be produced. Therefore, the residual moisture content of the pulp layer immediately before the drying step does not become excessively high, and therefore drying can be completed in a short time. In particular, when fine cellulose fibers having a large fiber diameter or average fiber diameter are used, drying can be completed in a shorter time. Therefore, improved production efficiency and energy savings can be expected.
[0145] Furthermore, by reducing the thickness of the walls of the pulp molded product MP2, the tact time for its manufacture can be shortened, i.e., a structure with thin walls can contribute to reducing the cost of the pulp molded product MP2.
[0146] Furthermore, the pulp molded product MP2 obtained by the above method has excellent surface properties, the reason for which will be explained below.
[0147] If drying is performed using an oven instead of the heat pressing process, the pulp layer will have large unevenness on the surface due to shrinkage. In addition, this method does not densify the pulp layer sufficiently, and therefore the pulp molded product will have high porosity. Therefore, in this case, it is not possible to produce a pulp molded product with excellent surface properties.
[0148] In addition, when drying is performed using an oven after the dehydration step, and the dried product is moistened as necessary and subjected to a heat press treatment, the height difference of the unevenness generated on the surface due to drying can be reduced by the subsequent moistening and heat press treatment. In addition, the porosity can be reduced by the moistening and heat press treatment. However, the height difference of the unevenness generated on the surface due to drying using an oven is very large, so it cannot be sufficiently reduced by the subsequent moistening and heat press treatment. In addition, even if moistening and heat press treatment are performed after drying, it is difficult to sufficiently reduce the porosity.
[0149] In the method described with reference to Figures 2 to 10, the pulp layer MP1 is dried in the heat pressing step. That is, in the above method, the heat pressing step is performed after the dehydration step without going through the drying step. Pulp and fine cellulose fibers each having the above-mentioned fiber diameter are used as the fibers.
[0150] Since no drying step is performed before the heat pressing step, the surface of the pulp layer MP1 does not have large unevenness with large height differences. In the heat pressing step, the upper mold 350 and the lower mold 320 prevent deformation of the pulp layer MP1 due to drying. In addition, since the heat pressing step is performed on the pulp layer MP1 that has a high moisture content and an average fiber length of the pulp within the above-mentioned range, the fibers can move appropriately in the in-plane direction within the pulp layer MP1. The pulp layer MP1 can be densified without causing thickness variations.
[0151] 2 to 10, a pulp-molded product MP2 with excellent surface properties can be manufactured. Specifically, a pulp-molded product MP2 is obtained that has a region on its surface where one or more of the arithmetic mean roughness Ra, the maximum height roughness Rz, and the average length RSm of the roughness curve element are small. Such a pulp-molded product MP2 has excellent cosmetic properties and is easy to form a printed layer or a coating layer on.
[0152] The arithmetic mean roughness Ra is preferably in the range of 2 to 10 μm, more preferably in the range of 2.5 to 4.5 μm. The maximum height roughness Rz is preferably in the range of 10 to 60 μm, more preferably in the range of 15 to 30 μm. The average length RSm of the roughness curvilinear elements is preferably in the range of 90 to 300 μm, more preferably in the range of 90 to 150 μm, and even more preferably in the range of 90 to 130 μm.
[0153] Here, "arithmetic mean roughness Ra," "maximum height roughness Rz," and "average length of roughness curve element RSm" are surface texture parameters defined in JIS B0601: 2001. The surface texture parameters are measured using, for example, a Mitutoyo surface roughness measuring instrument SJ-210 (tip radius 2 μm, measuring force 0.75 mN) under the following conditions. Filter:Gasussian Cutoff λc: 0.25mm Cutoff λs: 8μm Measurement speed: 0.25mm / s Number of sections: 5 A plate-shaped piece is taken from the pulp molded product MP2, measurements are taken at any five points, and the average value is calculated.
[0154] The entire surface of the pulp molded product MP2 may have the above-mentioned surface properties, or only a portion of the surface may have the above-mentioned surface properties. For example, only the area including the portion where post-treatment such as printing is performed may have the above-mentioned surface properties, and the other areas may not have the above-mentioned surface properties. Alternatively, one side of the pulp molded product MP2 may have the above-mentioned surface properties, and the back side may not have the above-mentioned surface properties. Such a structure can be realized, for example, by making the surface properties of the part of the surface of the upper mold 350 and the lower mold 320 that contacts the pulp layer MP1 different from the other areas.
[0155] In addition, according to the method described with reference to Figures 2 to 10, a pulp molded product MP2 having a small standard deviation in basis weight can be manufactured. The standard deviation of the basis weight of the pulp molded product MP2 is preferably 30 g / m 2 More preferably, it is 15 g / m or less. 2 The lower limit of this standard deviation is zero, and according to one example, 2 g / m 2 It is.
[0156] Here, the standard deviation of the basis weight of the pulp molded product MP2 is a value obtained by the following method.
[0157] First, nine test pieces, each of which has a rectangular shape with a width of 15 mm and a length of 40 mm, are cut out from multiple regions located on a certain plane of the pulp molded product MP2. Next, the mass of these test pieces is measured. After that, the mass and area (600 mm2) of each test piece are recorded. 2 The basis weight is calculated from the basis weight thus obtained. The standard deviation is calculated from the basis weight thus obtained.
[0158] Next, nine test pieces are cut out from multiple regions located in another plane of the pulp molded product MP2 in the same manner as above. The masses of these test pieces are also measured, and the basis weights and their standard deviations are calculated.
[0159] If the pulp molded product MP2 has additional surfaces, test pieces are cut out, the masses are measured, and the basis weights and their standard deviations are calculated for each of the remaining surfaces in the same manner as above. The maximum value of these standard deviations is set as the standard deviation of the basis weight of the pulp molded product MP2.
[0160] The inventors believe that the reason why the method described with reference to Figures 2 to 10 (hereinafter referred to as the first method) makes it possible to produce pulp molded products MP2 with a small standard deviation of basis weight is as follows.
[0161] The pulp molded product can also be produced, for example, by the method described below (hereinafter referred to as the second method).
[0162] In the second method, first, a female mold is prepared as a mold. This mold includes a mold body having a large number of through holes and a recessed upper surface corresponding to a shape of a pulp molded product, and a mesh body provided on and along the inner surface of the mold body.
[0163] Next, the mold is placed so that its opening faces upward. A slurry containing pulp and water is then fed into the cavity of the mold to fill the mold. The slurry is then continued to be fed into the mold, and the pulp is deposited on the mesh. The slurry is fed into the mold so that the slurry in the mold is under pressure.
[0164] After a sufficient amount of pulp has accumulated on the mesh, the supply of the slurry into the mold is stopped. Then, the water remaining in the mold is discharged from the mold, for example, by injecting compressed air into the mold.
[0165] Next, the pulp layer is pressed between the cutting mold and the upper mold, which is a male mold, to dehydrate the pulp layer. This dehydration step is performed without heating either the upper mold or the cutting mold. The moisture content of the pulp layer immediately after dehydration is set to be the same as the moisture content of the pulp layer MP1 immediately after dehydration in the first method.
[0166] Next, the pulp layer is adsorbed and held by the upper mold, and in this state the upper mold is raised, whereby the pulp layer is peeled off from the mold.
[0167] Next, the upper mold, which is holding the pulp layer by suction, is moved to the position of the lower mold, which is a female mold. The upper mold is then lowered until the pulp layer comes into contact with the lower mold. After that, the suction is stopped and the pulp layer is released from the upper mold. In this way, the pulp layer is placed on the lower mold.
[0168] Next, the pulp layer is sandwiched between an upper mold and a lower mold for a hot press, and the pulp layer between them is pressurized. At the same time, the heater is driven to heat the pulp layer. At the same time, the pump is driven to suck and remove water and / or water vapor from the space sandwiched between the upper mold and the lower mold. In the second method, a pulp molded product is obtained as described above.
[0169] In the second method, during the period from when the supply of the slurry into the mold is started until the mold is completely filled with the slurry, a flow of the slurry circulating inside the mold may occur. This circulating flow can prevent the settling of the pulp. However, since the second method requires the mold to be filled with the slurry, the mold cannot be designed to allow water to be quickly discharged. Therefore, after the mold is completely filled with the slurry, even if the pressure of the slurry is increased, a circulating flow of the slurry sufficient to prevent the settling of the pulp does not occur, and the slurry in the mold causes the settling of the pulp.
[0170] As a result, the amount of pulp deposited on the sidewall of the mold is greater at the bottom than at the top. If the slurry is supplied until a sufficient amount of pulp is deposited on the top of the sidewall of the mold, an excessive amount of pulp will be deposited at the bottom of the mold. If excessive pulp is deposited, the amount of pulp deposited will vary greatly. For example, there may be a large difference in the amount of pulp deposited near the through holes provided in the mold body and at a position distant from them.
[0171] Thus, the second method causes a large variation in the amount of pulp deposition. During the hot press treatment, the fibers can move in the in-plane direction within the pulp layer, but the movement of each fiber is limited to a narrow range. In other words, the variation in the amount of pulp deposition is not eliminated by the movement of the fibers during the hot press treatment. Therefore, the second method cannot produce a pulp molded product with a small standard deviation in basis weight.
[0172] In contrast, in the first method, a mold 240 is placed on top of the cover body 230, and the composite body is immersed in a slurry S. The depth of the slurry S is much greater than the height of the mold 240. Therefore, even if pulp settles in the slurry S, the pulp concentration does not differ greatly between the upper position and the lower position of the mold 240. Therefore, according to the first method, pulp can be deposited approximately uniformly on the mold 240, and a pulp molded product MP2 with a small standard deviation of basis weight can be manufactured.
[0173] The pulp molded product MP2 has an opening and does not expand in the direction away from the opening. Here, the pulp molded product MP2 has an opening and tapers in the direction away from the opening. With this shape, the volume of the laminate formed by stacking multiple pulp molded products MP2 can be reduced.
[0174] In the first method, if the pulp layer MP1 is sandwiched between one of the upper mold 350 and the lower mold 320 and an elastic body and pressure is applied to the pulp layer MP1 instead of the upper mold 350 and the lower mold 320, the elastic body will deform, and a pulp molded product with excellent surface properties cannot be obtained.
[0175] In the second method, if one of the upper and lower dies used in the hot press treatment is made of an elastic material, it is not possible to obtain a pulp molded product with excellent surface properties. In addition, in this case, the standard deviation of the basis weight becomes large as described above.
[0176] The pulp molded product MP2 is, for example, a container. The pulp molded product MP2 may be an article other than a container. The pulp molded product MP2 may be a three-dimensional product, that is, a product having a three-dimensional shape, not a two-dimensional shape like a sheet.
[0177] 2 to 10 are provided to facilitate understanding of the manufacturing method of a pulp molded product according to one embodiment of the present invention. The above-mentioned method can also be implemented using manufacturing apparatuses having other structures. For example, in the manufacturing apparatus 1, the upper mold 270 and the upper mold 350 are female molds, and the mold 240 and the lower mold 320 are male molds. The upper mold 270 and the upper mold 350 may be male molds, and the mold 240 and the lower mold 320 may be female molds. In this way, various modifications are possible for the above-mentioned manufacturing apparatus 1 and manufacturing method. EXAMPLES
[0178] Specific examples of the present invention are described below, but the present invention is not limited to these specific examples.
[0179] <1> Test A <1.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples A1 to A4 and A9 are comparative examples.
[0180] (Example A1) A pulper was used to prepare a slurry consisting of pulp and water. The pulp content of the slurry was 0.3% by mass. Pulp P1 with an average fiber diameter of 17.4 μm and pulp P2 with an average fiber diameter of 24.3 μm were used as the pulp. The ratios of pulp P1 and pulp P2 to the solid content of the slurry were 70.0% by mass and 30.0% by mass, respectively.
[0181] Using this slurry, a pulp molded product was manufactured by the method described with reference to Figs. 2 to 10. In this case, a relatively large amount of pulp was piled up on the mold so as to obtain a pulp molded product with a large basis weight. The dewatering process was carried out so that the moisture content of the pulp layer immediately after dewatering was 65% by mass. The heat pressing process was carried out at a heating temperature of 180°C and a pressing pressure of 0.2 MPa. In the dewatering process and the heat pressing process, the clearance between the upper and lower dies was adjusted so as to obtain a pulp molded product with a wall thickness of 1.0 mm. In this manner, a container was manufactured as a pulp molded product.
[0182] (Example A2) A pulp molded product was produced in the same manner as in Example A1, except for the following: In this example, a relatively small amount of pulp was deposited on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing steps, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0183] (Example A3) A pulp molded product was produced in the same manner as in Example A1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, a paper strength agent, and water. The ratio of pulp P1 and the ratio of pulp P2 in the solid content of the slurry were 69.3 mass% and 29.7 mass%, respectively. As the paper strength agent, DS4424 manufactured by Seiko PMC Co., Ltd. was used. This paper strength agent is an amphoteric water-soluble resin having an acrylamide group as a reactive group, as well as a cationic group and an anionic group. The ratio of the paper strength agent in the solid content of the slurry was 1.0 mass%.
[0184] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0185] (Example A4) Pulp molded products were produced in the same manner as in Example A3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.6 mass%, 29.4 mass%, and 2.0 mass%, respectively.
[0186] (Example A5) Pulp molded products were produced in the same manner as in Example A3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.4 mass%, 29.3 mass%, and 2.2 mass%, respectively.
[0187] (Example A6) Pulp molded products were produced in the same manner as in Example A3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.0 mass%, 29.1 mass%, and 2.9 mass%, respectively.
[0188] (Example A7) Pulp molded products were produced in the same manner as in Example A3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 67.3 mass%, 28.8 mass%, and 3.8 mass%, respectively.
[0189] (Example A8) Pulp molded products were produced in the same manner as in Example A3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 66.7 mass%, 28.6 mass%, and 4.8 mass%, respectively.
[0190] (Example A9) An attempt was made to manufacture a pulp molded product in the same manner as in Example A3, except that the ratios of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 66.0 mass%, 28.3 mass%, and 5.7 mass%, respectively. However, the pulp adhered strongly to the mold, and it was not possible to manufacture a pulp molded product.
[0191] <1.2> Evaluation The pulp molded products produced in Examples A1 to A8 were subjected to various measurements by the above-mentioned methods. In Example A9, the pulp was collected from the mold and the nitrogen content of the collected product was measured. The results are shown in Table 1 below.
[0192] [Table 1]
[0193] In Table 1, the evaluation of "releasability" is based on the following criteria. A: The mold can be released by blowing air and the surface condition is good. B: The mold could be released by blowing air, but peeling or cracks occurred on the surface. C: Demolding is impossible due to air ejection.
[0194] In Table 1, the values in the column labeled "RC strength retention" are relative values of the ISO ring crush compressive strength, with the value obtained for the pulp molded product of Example A1 taken as 100%. The "RC strength retention" was judged according to the following criteria. A: Strength retention is over 100%. B: Strength retention is 95% or more but less than 100%. C: Strength retention is less than 95%.
[0195] The "peel strength" was measured according to "Internal bond strength test method - Part 1: Z-axis tensile test method" described in JAPAN TAPPI 18-1. Specifically, first, a test piece having a square shape with one side of 25 mm was cut out from a pulp molded product. Next, double-sided adhesive tape was attached to both sides of the test piece, and the test piece was fixed to upper and lower jigs via the double-sided adhesive tape. For example, Scotch Tape (registered trademark) #400 manufactured by 3M was used as the double-sided adhesive tape. These jigs were pressed against each other with a load of 150 kgf, and this state was maintained for 20 seconds. This resulted in the sample piece being pressure-bonded to the jig. Thereafter, while fixing the position of the lower jig, the upper jig was raised at a speed of 20 mm / min to cause interlayer peeling of the test piece, and the maximum load at that time was obtained. The peel strength was taken as the average value of the maximum loads obtained by three measurements.
[0196] As shown in Table 1, the pulp molded products obtained in Examples A5 to A8 had smaller basis weights and wall thicknesses than the pulp molded product obtained in Example A1, but achieved ISO ring crush compression strengths equal to or greater than that of the pulp molded product obtained in Example A1. Also, the pulp molded products obtained in Examples A5 to A8 achieved higher peel strengths than the pulp molded product obtained in Example A1. Furthermore, Examples A5 to A8 achieved good releasability.
[0197] In contrast, in Examples A2 to A4, in which the amount of paper strength agent in the slurry was small, good releasability was achieved, but the pulp molded products obtained in these examples had low nitrogen contents in the pulp molded products and were inferior in ISO ring crush compressive strength. In particular, Examples A2 and A3 did not achieve peel strength as high as Examples A5 to A8.
[0198] In addition, in Example A9 in which the amount of the paper strength agent in the slurry was large, as described above, good releasability could not be achieved, and it was impossible to produce a pulp molded product.
[0199] <2> Test B As described below, in Test B, the proportion of pulp having fiber lengths of 1 mm or less was made smaller than in Test A.
[0200] <2.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples B1 to B4 are comparative examples.
[0201] (Example B1) Pulp molded products were produced in the same manner as in Example A1, except that the proportions of pulp P1 and pulp P2 in the solid content of the slurry were 85.0 mass % and 15.0 mass %, respectively.
[0202] (Example B2) A pulp molded product was produced in the same manner as in Example A1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, a paper strength agent, and water. The ratio of pulp P1 and the ratio of pulp P2 to the solid content of the slurry were 84.2 mass% and 14.9 mass%, respectively. As the paper strength agent, DS4424 manufactured by Seiko PMC Co., Ltd. was used. The ratio of the paper strength agent to the solid content of the slurry was 1.0 mass%.
[0203] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0204] (Example B3) A pulp molded product was produced in the same manner as in Example B2, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 81.7 mass%, 14.4 mass%, and 3.8 mass%, respectively.
[0205] (Example B4) A pulp molded product was produced in the same manner as in Example B2, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 81.0 mass%, 14.3 mass%, and 4.8 mass%, respectively.
[0206] <2.2> Evaluation Each of the pulp molded articles produced in Examples B1 to B4 was subjected to various measurements and evaluations similar to those performed in Test A. The results are shown in Table 2 below.
[0207] [Table 2]
[0208] As shown in Table 2, Examples B1 to B4 achieved good releasability. However, as shown in Tables 1 and 2, the pulp molded product obtained in Example B1 was inferior in ISO ring crush compressive strength compared to the pulp molded product obtained in Example A1. The pulp molded products obtained in Examples B2 to B4 were even inferior in ISO ring crush compressive strength compared to the pulp molded product obtained in Example B1. Also, Examples B1 to B4 did not achieve peel strength as high as Examples A5 to A8.
[0209] <3> Test C As described below, in Test C, the proportion of pulp having fiber lengths of 1 mm or less was increased compared to Test A.
[0210] <3.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples C1 and C2 are comparative examples.
[0211] (Example C1) An attempt was made to produce a pulp molded product in the same manner as in Example A1, except that the total amount of pulp contained in the slurry was changed to pulp P2. However, the pulp adhered strongly to the mold, and it was not possible to produce a pulp molded product.
[0212] (Example C2) An attempt was made to produce a pulp molded product in the same manner as in Example A1, except that the ratio of pulp P1 and the ratio of pulp P2 in the solid content of the slurry were 15.0 mass% and 85.0 mass%, respectively. However, the pulp adhered strongly to the mold, and it was not possible to produce a pulp molded product.
[0213] <3.2> Evaluation In the preparation of Examples C1 and C2, the pulp was collected from the mold and the nitrogen content of the collected material was measured, the results of which are shown in Table 3 below.
[0214] [Table 3]
[0215] As described above, in Examples C1 and C2, in which the proportion of pulp having a fiber length of 1 mm or less was high, good releasability could not be achieved, and it was impossible to produce a pulp molded product.
[0216] <4> Test D As described below, Test D had a reduced basis weight and press pressure compared to Test A.
[0217] <4.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples D1 to D3 are comparative examples.
[0218] (Example D1) A pulp molded product was produced in the same manner as in Example A1, except for the following points: In this example, a relatively small amount of pulp was piled on the mold so that a pulp molded product with a smaller basis weight was obtained, and the pressing pressure in the heat pressing step was set to 0.1 MPa.
[0219] (Example D2) A pulp molded product was produced in the same manner as in Example D1, except for the following: In this example, a relatively small amount of pulp was deposited on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and heat pressing steps, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0220] (Example D3) A pulp molded product was produced in the same manner as in Example D1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, a paper strength agent, and water. The ratio of pulp P1 and the ratio of pulp P2 to the solid content of the slurry were 66.7% by mass and 28.6% by mass, respectively. As the paper strength agent, DS4424 manufactured by Seiko PMC Co., Ltd. was used. The ratio of the paper strength agent to the solid content of the slurry was 4.8% by mass.
[0221] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0222] <4.2> Evaluation Each of the pulp molded articles produced in Examples D1 to D3 was subjected to various measurements and evaluations similar to those performed in Test A. The results are shown in Table 4 below.
[0223] [Table 4]
[0224] As shown in Table 4, Examples D1 to D3 achieved good releasability. However, as shown in Tables 1 and 4, the pulp molded product obtained in Example D1 was inferior in ISO ring crush compressive strength to the pulp molded product obtained in Example A1. The pulp molded products obtained in Examples D2 and D3 were even inferior in ISO ring crush compressive strength to the pulp molded product obtained in Example D1. Also, Examples D1 to D3 did not achieve peel strength as high as Examples A5 to A8.
[0225] <5> Test E Test E had an increased basis weight and press pressure compared to Test A, as described below.
[0226] <5.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples E1 to E3 are comparative examples.
[0227] (Example E1) A pulp molded product was produced in the same manner as in Example A1, except for the following points: In this example, a relatively large amount of pulp was piled on the mold so as to obtain a pulp molded product with a larger basis weight, and the pressing pressure in the heat pressing step was set to 0.4 MPa.
[0228] (Example E2) A pulp molded product was produced in the same manner as in Example E1, except for the following: In this example, a relatively small amount of pulp was deposited on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and heat pressing steps, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0229] (Example E3) A pulp molded product was produced in the same manner as in Example E1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, a paper strength agent, and water. The ratio of pulp P1 and the ratio of pulp P2 to the solid content of the slurry were 68.6 mass% and 29.4 mass%, respectively. As the paper strength agent, DS4424 manufactured by Seiko PMC Co., Ltd. was used. The ratio of the paper strength agent to the solid content of the slurry was 2.0 mass%.
[0230] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0231] (Example E4) A pulp molded product was produced in the same manner as in Example E3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.4 mass%, 29.3 mass%, and 2.2 mass%, respectively.
[0232] (Example E5) A pulp molded product was produced in the same manner as in Example E3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.0 mass%, 29.1 mass%, and 2.9 mass%, respectively.
[0233] <5.2> Evaluation Each of the pulp molded articles produced in Examples E1 to E5 was subjected to various measurements and evaluations similar to those performed in Test A. The results are shown in Table 5 below.
[0234] [Table 5]
[0235] As shown in Tables 1 and 5, Example E1 achieved good releasability, and also achieved high ISO ring crush compressive strength and peel strength compared to Example A1. However, although Examples E2 and E3 achieved good releasability, the pulp molded products obtained in these examples had low nitrogen contents and were inferior in ISO ring crush compressive strength compared to the pulp molded product obtained in Example E1.
[0236] In contrast, the pulp molded products obtained in Examples E4 and E5 achieved ISO ring crush compressive strengths equal to or greater than that of the pulp molded product obtained in Example E1, despite having smaller basis weights and wall thicknesses than that of the pulp molded product obtained in Example E1. Also, the pulp molded products obtained in Examples E4 and E5 achieved greater peel strengths than that of the pulp molded product obtained in Example E1. Furthermore, Examples E4 and E5 achieved good releasability.
[0237] <6> Test F As described below, in Test F, the pressing pressure is increased compared to Test A. Also, in Test F, the basis weight is increased compared to Test A, or fine cellulose fibers are further contained in the slurry.
[0238] <6.1> Manufacturing of pulp molded products Pulp molded products were produced by the following method, in which Examples F1 to F3 and F5 are comparative examples.
[0239] (Example F1) A pulp molded product was produced in the same manner as in Example A1, except for the following points: In this example, a relatively large amount of pulp was piled on the mold so as to obtain a pulp molded product with a larger basis weight, and the pressing pressure in the heat pressing step was set to 1.2 MPa.
[0240] (Example F2) A pulp molded product was produced in the same manner as in Example F1, except for the following: In this example, a relatively small amount of pulp was deposited on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and heat pressing steps, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0241] (Example F3) A pulp molded product was produced in the same manner as in Example F1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, a paper strength agent, and water. The ratio of pulp P1 and the ratio of pulp P2 to the solid content of the slurry were 69.3 mass% and 29.7 mass%, respectively. As the paper strength agent, DS4424 manufactured by Seiko PMC Co., Ltd. was used. The ratio of the paper strength agent to the solid content of the slurry was 1.0 mass%.
[0242] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0243] (Example F4) Pulp molded products were produced in the same manner as in Example F3, except that the proportions of pulp P1, pulp P2, and strength agent in the solid content of the slurry were 68.4 mass%, 29.3 mass%, and 2.2 mass%, respectively.
[0244] (Example: F5) A pulp molded product was produced in the same manner as in Example F1, except for the following points. That is, in this example, a pulper was used to prepare a slurry consisting of pulp P1, pulp P2, fine cellulose fibers, a paper strength agent, and water. The ratio of pulp P1 and pulp P2 to the solid content of the slurry was 66.0 mass% and 28.3 mass%, respectively. The fine cellulose fibers used had an average fiber diameter of 100 nm. The ratio of the fine cellulose fibers to the solid content of the slurry was 3.8 mass%. DS4424 manufactured by Seiko PMC was used as the paper strength agent. The ratio of the paper strength agent to the solid content of the slurry was 1.9 mass%.
[0245] In this example, a relatively small amount of pulp was piled on the mold to obtain a pulp molded product with a smaller basis weight. In the dewatering and hot pressing processes, the clearance between the upper and lower dies was adjusted to obtain a pulp molded product with a wall thickness of 0.7 mm.
[0246] (Example F6) Pulp molded products were produced in the same manner as in Example F5, except that the proportions of pulp P1, pulp P2, fine cellulose fiber, and strength agent in the solid content of the slurry were 65.9 mass%, 28.2 mass%, 3.8 mass%, and 2.2 mass%, respectively.
[0247] <6.2> Evaluation Each of the pulp molded articles produced in Examples F1 to F6 was subjected to various measurements and evaluations similar to those performed in Test A. The results are shown in Table 6 below.
[0248] [Table 6]
[0249] As shown in Tables 1 and 6, Example F1 achieved good releasability, and also achieved high ISO ring crush compressive strength and peel strength compared to Example A1. However, although Examples F2, F3, and F5 achieved good releasability, the pulp molded products obtained in these examples had low nitrogen contents and were inferior in ISO ring crush compressive strength compared to the pulp molded product obtained in Example F1.
[0250] In contrast, the pulp molded products obtained in Examples F4 and F6 achieved ISO ring crush compressive strengths equal to or greater than that of the pulp molded product obtained in Example F1, despite having smaller basis weights and wall thicknesses than that of the pulp molded product obtained in Example F1. Also, the pulp molded products obtained in Examples F4 and F6 achieved greater peel strengths than that of the pulp molded product obtained in Example F1. Furthermore, Examples F4 and F6 achieved good releasability. [Explanation of symbols]
[0251] Reference Signs List 1... manufacturing apparatus, 10... support, 20... first station, 30... second station, 40... third station, 210... container, 220... lifting device, 230... cover body, 240... mold, 250... moving device, 260... lifting device, 270... upper mold, 310... table, 320... lower mold, 330... moving device, 340... press device, 350... upper mold, 410... table, 420... moving device, 430... lifting device, 440... holder, MP1... pulp layer, MP2... pulp molded product, S... slurry.
Claims
1. The pulp contains pulp having a fiber diameter of 4 μm or more, the ratio of fibers having a fiber length of 1 mm or less is within the range of 33 to 55% by number, and the density is 0.45 g / cm 3 The pulp molded product has a nitrogen content measured by a chemiluminescence method within a range of 2000 to 3000 μg / g.
2. Density 0.65g / m 3 The pulp molded product according to claim 1, wherein the pulp molded product has a viscosity of less than 1000 s.p.m.
3. 2. The pulp molded product according to claim 1, having a minimum thickness of 1.2 mm or less.
4. 2. The pulp molded product according to claim 1, further comprising fine cellulose fibers having a fiber diameter of 800 nm or less.
5. 5. The pulp molded product according to claim 4, wherein the proportion of the fine cellulose fibers in the total amount of the pulp and the fine cellulose fibers is within a range of 1 to 9 mass %.
6. 5. The pulp molded product according to claim 4, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
7. 5. The pulp molded product according to claim 4, wherein the pulp includes a first pulp having an average fiber diameter in the range of 15 to 22 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
8. 8. The pulp molded product according to claim 7, wherein the pulp further comprises a second pulp having an average fiber diameter in the range of 22 to 40 μm.
9. The pulp molded product according to claim 7 , wherein the proportion of the first pulp in the pulp is 50% by mass or more.
10. 2. The pulp molded article according to claim 1, which is a container.
11. preparing a slurry containing fibers containing pulp having a fiber diameter of 4 μm or more, a strength agent, and water, the proportion of fibers having a fiber length of 1 mm or less in the range of 33 to 55% by number, the strength agent containing one or more poly(meth)acrylamides each containing an acrylamide group, an anionic group, and a cationic group, and the proportion of the strength agent in the total of the fibers and the strength agent on a solid content basis is in the range of 2.1 to 5.2 mass%; depositing the fibers on a three-dimensional mold to form a pulp layer; dehydrating the pulp layer to obtain an intermediate molded product; The undried intermediate molded product is sandwiched between a male mold and a female mold and heated to a temperature in the range of 120 to 250° C. while being pressed at a pressure in the range of 0.1 to 3.0 MPa to obtain a molded product having a density of 0.45 g / cm. 3 To obtain the above pulp molded product, A method for producing a pulp molded product comprising the steps of:
12. The pulp molded product has a density of 0.65 g / m 3 The method for producing a molded pulp product according to claim 11, wherein the molded pulp product obtained is less than 100% by weight.
13. The method for producing a pulp molded product according to claim 11, wherein the pulp molded product has a minimum thickness of 1.2 mm or less.
14. The method for producing a pulp molded product according to claim 11, wherein the fibers further contain fine cellulose fibers having a fiber diameter of 800 nm or less.
15. 15. The method for producing a pulp molded product according to claim 14, wherein the ratio of the fine cellulose fibers to the total amount of the pulp and the fine cellulose fibers in the slurry is within a range of 1 to 9 mass %.
16. 15. The method for producing a pulp molded product according to claim 14, wherein the pulp has an average fiber diameter in the range of 15 to 40 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
17. 15. The method for producing a pulp molded product according to claim 14, wherein the pulp includes a first pulp having an average fiber diameter in the range of 15 to 22 μm, and the fine cellulose fibers have an average fiber diameter in the range of 50 to 500 nm.
18. The method for producing a pulp molded product according to claim 17, wherein the pulp further includes a second pulp having an average fiber diameter in the range of 22 to 40 μm.
19. The method for producing a pulp molded product according to claim 17, wherein the proportion of the first pulp in the pulp is 50 mass% or more.
20. The deposition of the fibers on the mold comprises: Preparing a cover body as a hollow body having an opening; Fixing the mold to the opening; Immersing the mold fixed to the opening in the slurry; reducing the pressure in a space surrounded by the cover body and the mold immersed in the slurry; The method for producing the pulp molded product according to claim 11, comprising:
21. The method for producing a pulp molded product according to claim 20, wherein the mold is immersed in the slurry so that the mold is positioned above the cover body.
Citation Information
Patent Citations
Pulp mold tray
JP2008285188A