Non-aqueous electrolyte storage element
By using a non-aqueous electrolyte with unsaturated cyclic carbonates and dioxolanes, the growth of metallic lithium dendrites is inhibited, enhancing coulombic efficiency and stability in non-aqueous electrolyte storage devices.
Patent Information
- Application Number
- JP2023074975
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Non-aqueous electrolyte storage devices, such as lithium-sulfur batteries, face challenges in achieving high coulombic efficiency due to the growth of metallic lithium dendrites, which lead to decreased efficiency and potential short circuits.
Incorporating a non-aqueous electrolyte containing unsaturated cyclic carbonates and dioxolanes within specific volume percentages, forming protective films on electrode surfaces to inhibit dendrite growth and suppress electrolyte decomposition.
The solution enhances coulombic efficiency by preventing dendrite formation and reducing electrolyte decomposition, resulting in improved energy density and stability.
Smart Images

Figure 2024159159000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous electrolyte electricity storage element. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. The non-aqueous electrolyte secondary batteries generally have a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring lithium ions between the electrodes. In addition, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used as non-aqueous electrolyte storage elements other than non-aqueous electrolyte secondary batteries.
[0003] Known nonaqueous electrolyte storage elements include lithium-sulfur batteries (Li-S batteries) and other nonaqueous electrolyte storage elements that use elemental sulfur as the positive electrode active material (see Patent Document 1). Elemental sulfur and metallic lithium have large theoretical capacities, and a nonaqueous electrolyte storage element that uses elemental sulfur as the positive electrode active material and metallic lithium as the negative electrode active material is expected to be a storage element with high energy density. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-95390 A Summary of the Invention [Problem to be solved by the invention]
[0005] In non-aqueous electrolyte energy storage devices such as lithium-sulfur batteries, high coulombic efficiency is desirable for achieving higher energy density.
[0006] An object of the present invention is to provide a nonaqueous electrolyte electricity storage element having high coulombic efficiency. [Means for solving the problem]
[0007] A nonaqueous electrolyte storage element according to one aspect of the present invention comprises a positive electrode containing elemental sulfur, a negative electrode containing metallic lithium, and a nonaqueous electrolyte containing a nonaqueous solvent containing carbonates and dioxolanes, wherein the carbonates include unsaturated cyclic carbonates, and the content of the dioxolanes in the nonaqueous solvent is 1% by volume or more and 40% by volume or less. Effect of the Invention
[0008] According to one aspect of the present invention, a nonaqueous electrolyte electricity storage element having high Coulombic efficiency can be provided. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing one embodiment of a nonaqueous electrolyte electricity storage element. [Diagram 2] FIG. 2 is a schematic diagram showing one embodiment of an electricity storage device formed by assembling a plurality of nonaqueous electrolyte electricity storage elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] First, an overview of the nonaqueous electrolyte electricity storage element disclosed in this specification will be described.
[0011] (1) A nonaqueous electrolyte storage element according to one aspect of the present invention comprises a positive electrode containing elemental sulfur, a negative electrode containing metallic lithium, and a nonaqueous electrolyte containing a nonaqueous solvent containing carbonates and dioxolanes, wherein the carbonates include unsaturated cyclic carbonates, and the content of the dioxolanes in the nonaqueous solvent is 1% by volume or more and 40% by volume or less.
[0012] The nonaqueous electrolyte storage element described in (1) above has a high Coulombic efficiency. The reason for this is unclear, but the following reason is presumed. In general, in a nonaqueous electrolyte storage element having a negative electrode containing metallic lithium, metallic lithium may be precipitated in a dendritic form on the surface of the negative electrode during charging (hereinafter, metallic lithium in a dendritic form is referred to as a "dendrite"). Since dendrites have a large surface area, when the dendrites grow, the decomposition reaction of the nonaqueous electrolyte is promoted, which may lead to a decrease in Coulombic efficiency. In addition, when the dendrites grow and come into contact with the positive electrode, a micro-short circuit may occur, which may lead to a decrease in Coulombic efficiency. In the case of a nonaqueous electrolyte storage element having a positive electrode containing elemental sulfur and a negative electrode containing metallic lithium, the growth of the dendrites on the surface of the negative electrode is thought to be promoted by the precipitation of a sulfur compound, which dissolves from the positive electrode into the nonaqueous electrolyte, on the surface of the negative electrode. In such a non-aqueous electrolyte storage element, when the non-aqueous electrolyte contains an unsaturated cyclic carbonate, the sulfur element reacts with the unsaturated cyclic carbonate during initial charging and discharging, forming a good coating on the positive electrode surface. When a good coating is formed on the positive electrode surface, the dissolution of sulfur compounds is suppressed, and the growth of dendrites is suppressed, resulting in an increase in Coulomb efficiency. In addition, when the non-aqueous electrolyte contains an unsaturated cyclic carbonate, a coating derived from the unsaturated cyclic carbonate is formed on the negative electrode surface. Furthermore, when the non-aqueous electrolyte contains a predetermined amount of dioxolanes, a coating derived from dioxolanes is formed on the negative electrode surface. It is presumed that these coatings on the negative electrode surface further suppress the decomposition reaction of the non-aqueous electrolyte on the negative electrode surface, thereby further increasing the Coulomb efficiency.
[0013] The content of each component constituting the non-aqueous solvent is measured by liquid chromatography mass spectrometry (LC-MS) and gas chromatography mass spectrometry (GC-MS). Specifically, the measurement is performed as follows. The LC-MS and GC-MS measurements are performed consecutively under the same conditions. 1. Collection of non-aqueous electrolyte First, the nonaqueous electrolyte storage element is disassembled to remove the nonaqueous electrolyte. If the nonaqueous electrolyte cannot be removed, the nonaqueous electrolyte storage element is centrifuged to remove the nonaqueous electrolyte. If the nonaqueous electrolyte cannot be removed even after centrifugation, acetonitrile is injected into the nonaqueous electrolyte storage element as an extraction solvent, and the nonaqueous electrolyte diluted with acetonitrile is removed. 2.LC-MS The components of the collected non-aqueous electrolyte are analyzed by LC-MS. The LC-MS analysis is performed in the following order of qualitative analysis and quantitative analysis. The LC-MS analysis is performed using Waters' "Acquity H" and "Xevo G2-5QTof" instruments. Water is used as the eluent. (qualitative analysis) The measurement sample (non-aqueous electrolyte) is subjected to LC-MS analysis. If the peaks in the obtained liquid chromatogram cannot be separated, a GC-MS analysis, described below, is performed instead of the LC-MS analysis. If the peaks can be separated, the components contained in the measurement sample are predicted from the MS spectrum of each peak. A known sample of the predicted components (hereinafter referred to as "predicted components") is subjected to LC-MS analysis. The retention times and MS spectrum of the peaks corresponding to each predicted component of the measurement sample are compared with the retention times and MS spectrum of the peaks of a known sample of each predicted component, and if they match, the prediction is presumed to be correct. (Quantitative analysis) Quantitative analysis is performed using the calibration curve method. First, a known sample of the predicted component with a known concentration is measured by LC-MS, and a calibration curve is created by calculating the peak area. The calibration curve is calculated using the coefficient of determination (r 2 ) is created so that it is between 0.999 and 1. The amount of the predicted component in the measurement sample is calculated from the calibration curve and the area of the peak of the predicted component in the measurement sample. The above process is performed for all peaks detected in the LC-MS analysis of the measurement sample, and the amount of each predicted component is calculated. 3.GC-MS The GC-MS analysis is carried out in the following order: qualitative analysis and quantitative analysis. The GC-MS analysis equipment used is the Agilent 5975C. Argon is used as the carrier gas. (qualitative analysis) A measurement sample (non-aqueous electrolyte) is subjected to GC-MS analysis. The components contained in the sample are predicted from the MS spectrum of each peak in the obtained gas chromatogram. A known sample of the predicted components is subjected to GC-MS analysis. The retention time and MS spectrum of the peak corresponding to the prediction of the measurement sample are compared with the retention time and MS spectrum of the peak of a known sample of each predicted component, and if they match, the above prediction is presumed to be correct. (Quantitative analysis) The quantitative analysis is performed by the calibration curve method. The quantitative analysis by GC-MS is performed in the same manner as the quantitative analysis by LC-MS described above, and the content of each predicted component is determined. 4. Calculation of the content of each component The total content of each predicted component (i.e., each component) measured by LC-MS or GC-MS is regarded as the content of the non-aqueous solvent, and the content of each component in the non-aqueous solvent is calculated. Note that, when calculating the content (volume %) of each component in the non-aqueous solvent, the mass-based content of each component measured by LC-MS or GC-MS is converted to a volume at 20°C, and the total of the volumetrically converted contents of each component is regarded as the content of the non-aqueous solvent. In addition, when acetonitrile is used as the extraction solvent, acetonitrile is excluded from the calculation.
[0014] (2) In the nonaqueous electrolyte storage element described above in (1), the content of the unsaturated cyclic carbonate in the nonaqueous solvent may be 35% by volume or more.
[0015] The nonaqueous electrolyte electricity storage element described above in (2) has a higher Coulombic efficiency.
[0016] (3) In the nonaqueous electrolyte storage element according to (1) or (2) above, the content of the carbonate in the nonaqueous solvent may be 60% by volume or more and 99% by volume or less.
[0017] The nonaqueous electrolyte electricity storage element described above in (3) has a higher Coulombic efficiency.
[0018] A nonaqueous electrolyte electricity storage element, an electricity storage device, a method for manufacturing a nonaqueous electrolyte electricity storage element according to one embodiment of the present invention, and other embodiments will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0019] <Non-aqueous electrolyte electricity storage element> A nonaqueous electrolyte storage element (hereinafter, also simply referred to as "storage element") according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, a nonaqueous electrolyte, and a container that contains the electrode assembly and the nonaqueous electrolyte. The electrode assembly is usually of a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with a separator interposed therebetween, or of a wound type in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound. The nonaqueous electrolyte exists in a state that it is contained in the positive electrode, the negative electrode, and the separator. As an example of a nonaqueous electrolyte storage element, a nonaqueous electrolyte secondary battery (hereinafter, also simply referred to as "secondary battery") will be described.
[0020] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0021] The positive electrode substrate is conductive. Whether or not it has "conductivity" is determined by the volume resistivity being 10 or less, as measured in accordance with JIS-H-0505 (1975). -2 The threshold value is Ω·cm. The material of the positive electrode substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoints of potential resistance, high conductivity, and cost. The positive electrode substrate may be a foil, a vapor deposition film, a mesh, a porous material, etc., and a foil is preferred from the viewpoint of cost. Therefore, aluminum foil or an aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or an aluminum alloy include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).
[0022] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, the strength of the positive electrode substrate can be increased while increasing the energy density per volume of the nonaqueous electrolyte storage element. The "average thickness" refers to the average value of thicknesses measured at any five points.
[0023] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0024] The positive electrode active material layer contains elemental sulfur. The positive electrode active material layer contains optional components such as a conductive agent, a binder, a dispersant, a thickener, and a filler, as necessary. The positive electrode active material layer is usually formed from a positive electrode mixture containing elemental sulfur and other optional components.
[0025] The sulfur element is a component that functions as a positive electrode active material. The sulfur element contained in the positive electrode or the positive electrode active material layer may be simple sulfur or a sulfur compound. Examples of the sulfur compound include metal sulfides such as lithium sulfide, organic disulfide compounds, and organic sulfur compounds such as carbon sulfide compounds. As the sulfur element, one of these materials may be used alone, or two or more of them may be mixed and used. These materials may also be used in a composite form. The sulfur element has the advantages of a large theoretical capacity and low cost.
[0026] The sulfur element may be in the form of a complex with a conductive agent (a material having higher conductivity than simple sulfur or a sulfur compound). The complex may be in the form in which the sulfur element is supported on a conductive agent as a carrier, and specifically, may be a complex of the sulfur element and porous carbon (sulfur-porous carbon composite: SPC). The complex may be a complex of simple sulfur and porous carbon. The content of the sulfur element in the SPC (mass ratio of the sulfur element to the mass of the SPC) is preferably 50 mass% or more and 90 mass% or less, more preferably 60 mass% or more and 80 mass% or less. By setting the content of the sulfur element in the SPC to the above range, it is possible to achieve both large electric capacity and good conductivity.
[0027] The content of sulfur element in the positive electrode active material layer (mass ratio of sulfur element to the mass of the positive electrode active material layer) is preferably 40 mass% or more and 90 mass% or less, more preferably 50 mass% or more and 70 mass% or less. When SPC is used, the content of SPC in the positive electrode active material layer (mass ratio of SPC to the mass of the positive electrode active material layer) is preferably 60 mass% or more and 97 mass% or less, more preferably 70 mass% or more and 95 mass% or less. By setting the content of sulfur element or SPC within the above range, it is possible to achieve both large electric capacity and good conductivity, and to increase energy density, etc.
[0028] The positive electrode active material layer may contain a positive electrode active material other than elemental sulfur, but the content of elemental sulfur in the entire positive electrode active material is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass.
[0029] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. The conductive agent in the positive electrode active material layer does not include a conductive agent that forms a complex with a sulfur element. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphite, non-graphitic carbon, graphene-based carbon, and the like. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. In addition, these materials may be used in a composite form. For example, a material in which carbon black and CNT are composited may be used. As the conductive agent in the positive electrode active material layer, carbon black is preferable from the viewpoints of electronic conductivity and coatability, and acetylene black is preferable among them. It is also preferable to use carbon black (preferably acetylene black) in combination with CNT.
[0030] The content of the conductive agent in the positive electrode active material layer (excluding the conductive agent in the complex of elemental sulfur and conductive agent) is preferably 0.5% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 15% by mass or less, and may be 10% by mass or less or 5% by mass or less. By setting the content of the conductive agent in the above range, the energy density of the nonaqueous electrolyte storage element can be increased.
[0031] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0032] The content of the binder in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, more preferably 2% by mass or more and 9% by mass or less, and may be 7% by mass or less or 5% by mass or less. By setting the content of the binder in the above range, the positive electrode active material, the composite, etc. can be stably held.
[0033] Examples of the dispersant include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the dispersant has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like. The content of the dispersant in the positive electrode active material layer is preferably 0.05% by mass or more and 5% by mass or less, and more preferably 0.1% by mass or more and 2% by mass or less. The polysaccharide polymer may function as a thickener or a binder.
[0034] Examples of the thickener include polyacrylic acid (PAA). The content of the thickener in the positive electrode active material layer is preferably 0.5% by mass to 5% by mass, more preferably 1% by mass to 3% by mass. Polyacrylic acid may function as a binder.
[0035] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof. The content of the filler in the positive electrode active material layer is preferably, for example, 0.1% by mass or more and 10% by mass or less. In one embodiment of the present invention, the positive electrode active material layer may not contain a filler.
[0036] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W, as components other than the sulfur element, other positive electrode active materials, conductive agents, binders, dispersants, thickeners, and fillers.
[0037] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.
[0038] The negative electrode substrate has electrical conductivity. Metals such as copper, nickel, stainless steel, and nickel-plated steel, or alloys thereof, and carbonaceous materials are used as the material of the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0039] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the nonaqueous electrolyte storage element.
[0040] The negative electrode active material layer contains metallic lithium. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a dispersant, a thickener, and a filler, as necessary. The optional components such as a conductive agent, a binder, a dispersant, a thickener, and a filler can be selected from the materials exemplified for the positive electrode. The negative electrode active material layer may not contain optional components such as a conductive agent, a binder, a dispersant, a thickener, and a filler. The negative electrode active material layer may be a layer of metallic lithium.
[0041] Metallic lithium is a component that functions as a negative electrode active material. Metallic lithium may be pure metallic lithium consisting essentially of lithium element, or may be a lithium alloy containing other metal elements. Examples of lithium alloys include lithium silver alloys, lithium zinc alloys, lithium calcium alloys, lithium aluminum alloys, lithium magnesium alloys, and lithium indium alloys. Lithium alloys may contain a plurality of metal elements other than lithium element.
[0042] The negative electrode active material layer may contain other negative electrode active materials than metallic lithium. However, the negative electrode active material layer is preferably a layer substantially composed of metallic lithium (pure metallic lithium or lithium alloy). The content of lithium element in the negative electrode active material layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 99% by mass or more. The upper limit of the content of lithium element in the negative electrode active material layer may be 100% by mass.
[0043] The negative electrode active material layer may be a non-porous layer (solid layer) or a porous layer, but is preferably a non-porous layer. The negative electrode active material layer may be, for example, a layer made of metallic lithium foil (pure metallic lithium foil or lithium alloy foil). The negative electrode active material layer may have metallic lithium at least in a charged state, and may or may not have metallic lithium in a discharged state, but is preferably a layer that exists in a discharged state, that is, a layer that exists in all states from a charged state to a discharged state. The average thickness of the negative electrode active material layer in a charged state is preferably 5 μm or more and 1,000 μm or less, more preferably 10 μm or more and 500 μm or less, and even more preferably 30 μm or more and 300 μm or less.
[0044] (Separator) The separator can be appropriately selected from known separators. For example, a separator consisting of only a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer, etc. can be used as the separator. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, a porous resin film is preferred from the viewpoint of strength, and a nonwoven fabric is preferred from the viewpoint of non-aqueous electrolyte retention. As the material of the substrate layer of the separator, polyolefins such as polyethylene and polypropylene are preferred from the viewpoint of shutdown function, and polyimide and aramid are preferred from the viewpoint of oxidation decomposition resistance. A material obtained by combining these resins may be used as the substrate layer of the separator.
[0045] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials with a mass loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ion crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the nonaqueous electrolyte storage element.
[0046] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0047] As the separator, a polymer gel composed of a polymer and a non-aqueous electrolyte may be used. Examples of the polymer include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of the polymer gel has an effect of suppressing leakage. As the separator, the above-mentioned porous resin film or nonwoven fabric may be used in combination with the polymer gel.
[0048] (Non-aqueous electrolyte) The nonaqueous electrolyte includes a nonaqueous solvent. As the nonaqueous electrolyte, a nonaqueous electrolyte solution including a nonaqueous solvent and an electrolyte salt dissolved in the nonaqueous solvent is preferably used. In one embodiment of the present invention, the nonaqueous electrolyte storage element may be a nonaqueous electrolyte storage element.
[0049] The non-aqueous solvent contains carbonates and dioxolanes.
[0050] The carbonates include unsaturated cyclic carbonates. The nonaqueous solvent contains an unsaturated cyclic carbonate, which can increase the Coulombic efficiency of the nonaqueous electrolyte storage element. The unsaturated cyclic carbonate is a cyclic carbonate having a carbon-carbon double bond or a carbon-carbon triple bond in the molecule. The carbon-carbon double bond also includes those that form an aromatic ring. The cyclic carbonate refers to a carbonate having a ring structure containing a carbonate group (-OC(=O)-O-). The unsaturated cyclic carbonate is preferably one having a carbon-carbon double bond in the molecule, and more preferably one having a carbon-carbon double bond in the molecule that does not form an aromatic ring. In the unsaturated cyclic carbonate, the carbon-carbon double bond or the carbon-carbon triple bond may be present in the ring structure or may be present outside the ring structure, but is preferably present in the ring structure. The unsaturated cyclic carbonate may be one in which some or all of the hydrogen atoms are substituted with halogen atoms.
[0051] Examples of the unsaturated cyclic carbonate include vinylene carbonate (VC), fluorovinylene carbonate, methylvinylene carbonate, fluoromethylvinylene carbonate, ethylvinylene carbonate, propylvinylene carbonate, butylvinylene carbonate, phenylvinylene carbonate, dimethylvinylene carbonate, diethylvinylene carbonate, dipropylvinylene carbonate, diphenylvinylene carbonate, trifluoromethylvinylene carbonate, vinylethylene carbonate, and styrene carbonate, and among these, VC is preferred. One or more of the unsaturated cyclic carbonates can be used.
[0052] The lower limit of the content of the unsaturated cyclic carbonate in the non-aqueous solvent is preferably 35% by volume, more preferably 40% by volume, and even more preferably 45% by volume. By having the content of the unsaturated cyclic carbonate be equal to or more than the lower limit, a sufficient amount of coating is formed on the positive electrode surface and the negative electrode surface, and the coulomb efficiency can be further increased. The upper limit of the content of the unsaturated cyclic carbonate in the non-aqueous solvent is preferably 65% by volume, more preferably 60% by volume, even more preferably 55% by volume, and even more preferably 50% by volume. The content of the unsaturated cyclic carbonate in the non-aqueous solvent may be equal to or more than any of the lower limits and equal to or less than any of the upper limits.
[0053] The lower limit of the content of the unsaturated cyclic carbonate in the carbonates is preferably 20% by volume, and may be 30%, 40%, or 50% by volume. The upper limit of the content of the unsaturated cyclic carbonate in the carbonates is preferably 80% by volume, and may be 70%, 60%, or 50% by volume. The content of the unsaturated cyclic carbonate in the carbonates may be any of the above lower limits or more and any of the above upper limits or less (however, the lower limit is less than the upper limit).
[0054] The carbonates may further contain other carbonates other than the unsaturated cyclic carbonate. The other carbonates include unsaturated chain carbonates and saturated carbonates, and saturated carbonates are preferred. The other carbonates may be those in which some or all of the hydrogen atoms are substituted with halogen atoms. The other carbonates may be used in one or more kinds.
[0055] The unsaturated chain carbonate is a chain carbonate having a carbon-carbon double bond or a carbon-carbon triple bond in the molecule. The chain carbonate refers to a carbonate that does not have a ring structure containing a carbonate group. The chain carbonate may have a ring structure that does not contain a carbonate group.
[0056] Examples of the unsaturated chain carbonate include methyl vinyl carbonate, divinyl carbonate, diphenyl carbonate, diallyl carbonate, and dibenzyl carbonate.
[0057] Saturated carbonates are carbonates that have neither a carbon-carbon double bond nor a carbon-carbon triple bond in the molecule. Examples of saturated carbonates include saturated cyclic carbonates and saturated chain carbonates.
[0058] Examples of the saturated cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), chloroethylene carbonate, fluoroethylene carbonate (FEC), and difluoroethylene carbonate (DFEC).
[0059] Examples of the saturated chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), 2,2,2-trifluoroethyl methyl carbonate (TFEMC), and bis(2,2,2-trifluoroethyl)carbonate (TFEC).
[0060] The saturated carbonate is preferably a halogenated saturated carbonate, and more preferably a fluorinated saturated carbonate. The fluorinated saturated carbonate may be a fluorinated saturated cyclic carbonate such as FEC or DFEC, or a fluorinated saturated chain carbonate such as TFEMC or TFEC. In one embodiment of the present invention, the non-aqueous solvent may contain a fluorinated saturated cyclic carbonate. In another embodiment of the present invention, the non-aqueous solvent may contain a fluorinated saturated chain carbonate.
[0061] The content of the saturated carbonate in the non-aqueous solvent is preferably from 10 vol % to 65 vol %, and more preferably from 20 vol % to 55 vol %.
[0062] The content of saturated carbonate in the carbonates is preferably 30% by volume or more and 80% by volume or less, and more preferably 40% by volume or more and 70% by volume or less.
[0063] The lower limit of the content of carbonates in the non-aqueous solvent (total content of unsaturated cyclic carbonate and any other carbonates) is preferably 60% by volume, more preferably 70% by volume, and may be 75% by volume, 80% by volume, or 85% by volume. When the content of carbonates in the non-aqueous solvent is equal to or more than the above lower limit, a sufficient amount of coating is formed on the positive electrode surface and the negative electrode surface, and the coulomb efficiency can be further improved. The upper limit of the content of carbonates in the non-aqueous solvent is preferably 99% by volume, more preferably 95% by volume, and may be 90% by volume, 85% by volume, or 80% by volume. The content of carbonates may be equal to or more than any of the above lower limits and equal to or less than any of the above upper limits (however, the lower limit is less than the upper limit).
[0064] Examples of dioxolanes include 1,3-dioxolanes, 1,2-dioxolanes, and compounds in which some or all of the hydrogen atoms of these are substituted with other atoms (e.g., halogen atoms, etc.) or groups (e.g., hydrocarbon groups, amino groups, etc.). As the dioxolanes, 1,3-dioxolanes is preferred. One or more dioxolanes can be used.
[0065] The lower limit of the content of dioxolanes in the non-aqueous solvent is 1 vol%, preferably 2 vol%, more preferably 3 vol%, and may be 5 vol%. The upper limit of the content of dioxolanes in the non-aqueous solvent is 40 vol%, preferably 30 vol%, and may be 20 vol%. By having the content of dioxolanes within the above range, the coulombic efficiency of the non-aqueous electrolyte storage element can be improved. The content of dioxolanes may be equal to or greater than any of the above lower limits and equal to or less than any of the above upper limits.
[0066] The non-aqueous solvent may further contain other non-aqueous solvents other than carbonates and dioxolanes. Examples of other non-aqueous solvents include ethers, amides, nitriles, etc. other than dioxolanes. However, the total content of carbonates and dioxolanes in the non-aqueous solvent is preferably 80% by volume or more and 100% by volume or less, more preferably 90% by volume or more and 100% by volume or less, even more preferably 99% by volume or more and 100% by volume or less, and even more preferably 100% by volume. In this way, the non-aqueous solvent is mainly composed of carbonates and dioxolanes, and thus the coulombic efficiency of the non-aqueous electrolyte storage element can be further increased.
[0067] As the electrolyte salt, a lithium salt is usually used. Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP), and lithium salts having halogenated hydrocarbon groups such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. As the lithium salt, imide salts such as LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) are preferred, imide salts having a halogenated hydrocarbon group are more preferred, imide salts having a fluorinated hydrocarbon group are even more preferred, and LiN(SO2CF3)2 is particularly preferred.
[0068] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm at 20°C and 1 atmosphere. 3 More than 2.5mol / dm 3 It is preferable that the value is 0.3 mol / dm or less. 3 More than 2.0mol / dm 3 More preferably, it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3More preferably, it is 0.7 mol / dm or less. 3 More than 1.5mol / dm 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the nonaqueous electrolyte can be increased.
[0069] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, and busulfan. Examples of the additives include sulfane, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.
[0070] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0071] The nonaqueous electrolyte may be a combination of a nonaqueous electrolyte solution and a solid electrolyte. The solid electrolyte may be selected from any material that has lithium ion conductivity and is solid at room temperature (e.g., 15°C to 25°C). Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, and polymer solid electrolytes.
[0072] The shape of the nonaqueous electrolyte storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery, a flat battery, a coin battery, and a button battery.
[0073] Fig. 1 shows a nonaqueous electrolyte storage element 1 as an example of a prismatic battery. The figure is a see-through view of the inside of the container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.
[0074] <Electricity storage device> The nonaqueous electrolyte storage element of the present embodiment can be mounted as an electricity storage unit (battery module) comprising a plurality of nonaqueous electrolyte storage elements assembled together in automobile power sources such as electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), etc., power sources for electronic devices such as personal computers and communication terminals, or power storage power sources, etc. In this case, the technology of the present invention may be applied to at least one of the nonaqueous electrolyte storage elements included in the electricity storage unit.
[0075] 2 shows an example of an electricity storage device 30 in which electricity storage units 20, each of which is an assembly of two or more electrically connected nonaqueous electrolyte electricity storage elements 1, are further assembled. The electricity storage device 30 may include a bus bar (not shown) that electrically connects two or more nonaqueous electrolyte electricity storage elements 1, a bus bar (not shown) that electrically connects two or more electricity storage units 20, and the like. The electricity storage unit 20 or the electricity storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more nonaqueous electrolyte electricity storage elements.
[0076] <Method of Manufacturing Nonaqueous Electrolyte Storage Element> The method for producing the nonaqueous electrolyte storage element of the present embodiment can be appropriately selected from known methods. The method for producing the nonaqueous electrolyte storage element of the present embodiment includes, for example, preparing an electrode body, preparing a nonaqueous electrolyte, and housing the electrode body and the nonaqueous electrolyte in a container. The preparation of the electrode body includes preparing a positive electrode and a negative electrode, and forming the electrode body by stacking or rolling the positive electrode and the negative electrode with a separator interposed therebetween.
[0077] The method of housing the non-aqueous electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution may be injected through an injection port formed in the container, and then the injection port may be sealed.
[0078] The manufacturing method may include performing initial charging and discharging on an undischarged nonaqueous electrolyte storage element. The initial charging and discharging starts with discharging. The number of times of charging and discharging in the initial charging and discharging is not particularly limited. Through the initial charging and discharging, a good coating is formed on the surfaces of the positive electrode and the negative electrode due to the decomposition of a part of the nonaqueous electrolyte, and a nonaqueous electrolyte storage element having high Coulombic efficiency is obtained.
[0079] <Other embodiments> The nonaqueous electrolyte storage element of the present invention is not limited to the above-described embodiment, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0080] In the above embodiment, the nonaqueous electrolyte storage element is used as a chargeable and dischargeable nonaqueous electrolyte secondary battery (e.g., a lithium-sulfur battery), but the type, shape, size, capacity, etc. of the nonaqueous electrolyte storage element are arbitrary. The present invention can also be applied to various secondary batteries, capacitors, etc.
[0081] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. EXAMPLES
[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0083] [Example 1] (Preparation of positive electrode) Elemental sulfur and microporous carbon were mixed in a mass ratio of 70:30. This mixture was placed in a sealed electric furnace. After argon flow for 1 hour, the temperature was increased to 150°C at a rate of 5°C / min and held for 5 hours, and then allowed to cool to 80°C, the temperature at which elemental sulfur solidifies. Thereafter, the temperature was increased again to 300°C at a rate of 5°C / min and held for 2 hours for heat treatment to produce a composite (sulfur-porous carbon composite: SPC). A positive electrode mixture paste containing the composite obtained above, acetylene black and carbon nanotubes as conductive agents, CMC as a dispersant, PAA as a thickener, and SBR as a binder in a mass ratio of 93:1.5:0.2:0.3:2.5:2.5, was applied to an aluminum positive electrode substrate and dried to prepare a positive electrode.
[0084] (Preparation of the negative electrode) A pure metallic lithium foil was prepared as the negative electrode.
[0085] (Preparation of non-aqueous electrolyte) A non-aqueous solvent consisting of vinylene carbonate (VC), fluoroethylene carbonate (FEC), and 1,3-dioxolane (DOL) mixed in a volume ratio of 45:45:10 was added as an electrolyte salt at a concentration of 1.0 mol / dm 3 A non-aqueous electrolyte was prepared by adding the above-mentioned components in an amount of 0.1 to 100% by weight.
[0086] (Assembly of non-aqueous electrolyte storage element) A microporous polyethylene film was prepared as the separator. The positive electrode, negative electrode, separator, and nonaqueous electrolyte were used to obtain a nonaqueous electrolyte storage element of Example 1.
[0087] [Examples 2 to 5, Comparative Examples 1 to 3] The nonaqueous electrolyte storage elements of Examples 2 to 5 and Comparative Examples 1 to 3 were obtained in the same manner as in Example 1, except that the types and volume ratios of the nonaqueous solvents used in the preparation of the nonaqueous electrolytes were as shown in Table 1. The nonaqueous solvents used were as follows: VC: Vinylene carbonate FEC: Fluoroethylene carbonate TFEMC: 2,2,2-trifluoroethyl methyl carbonate DOL: 1,3-dioxolane DOA: 1,4-dioxane
[0088] [evaluation] (Charge-discharge cycle test) First, each of the obtained nonaqueous electrolyte storage elements was discharged at a constant current of 0.1 C to 1.0 V. Thereafter, the battery was charged at a constant current of 0.1C up to 3.0V. Next, the battery was discharged at a constant current of 0.1C up to 1.0V. This charging and discharging process constitutes one cycle, and this charging and discharging cycle was repeated 8 times. A 10-minute pause was provided after each charging and discharging. The charging, discharging, and pause were all performed in a thermostatic chamber at 25°C. The coulombic efficiency for each cycle was calculated, and the average value of the coulombic efficiency for 8 cycles was calculated. The results are shown in Table 1.
[0089] [Table 1]
[0090] As shown in Table 1, the nonaqueous electrolyte storage elements of Examples 1 to 5, in which the nonaqueous solvent contained a predetermined amount of dioxolanes together with an unsaturated cyclic carbonate, all had high Coulombic efficiencies (average value) of 87% or more. In contrast, the nonaqueous electrolyte storage elements of Comparative Example 1, in which the nonaqueous solvent contained no dioxolanes, Comparative Example 2, in which the nonaqueous solvent contained DOA instead of dioxolanes, and Comparative Example 3, in which the content of dioxolanes in the nonaqueous solvent was greater than the predetermined amount, all had low Coulombic efficiencies. [Industrial Applicability]
[0091] The present invention can be applied to nonaqueous electrolyte electricity storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles. [Explanation of symbols]
[0092] 1. Non-aqueous electrolyte storage element 2 Electrode body 3 containers 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy Storage Unit 30 Energy storage device
Claims
1. A positive electrode containing elemental sulfur; a negative electrode including metallic lithium; A non-aqueous electrolyte including a non-aqueous solvent containing carbonates and dioxolanes. Equipped with The carbonates include unsaturated cyclic carbonates, The nonaqueous electrolyte electricity storage element has a dioxolane content of 1% by volume or more and 40% by volume or less in the nonaqueous solvent.
2. 2. The nonaqueous electrolyte storage element according to claim 1, wherein the content of the unsaturated cyclic carbonate in the nonaqueous solvent is 35% by volume or more.
3. 3. The nonaqueous electrolyte storage element according to claim 1, wherein the content of the carbonate in the nonaqueous solvent is 60% by volume or more and 99% by volume or less.
Citation Information
Patent Citations
Mesoporous carbon composite material and secondary battery using the same
JP2010095390A
Cited By
Amine functionalized silica catalyst for preparation of organic carbonate and other applications thereof
WO2026099899A1
Lithium-ion secondary battery
WO2026100689A1
Lithium-ion secondary battery
WO2026100690A1