Evaluation method of slag generating reaction

By observing the reaction between Fe oxide-containing powder and silicon dioxide-containing particles in a controlled environment, the slag formation reaction in flash-smelting furnaces is evaluated, enhancing matte recovery and stabilizing the slag production process.

JP2024159174APending Publication Date: 2024-11-08SUMITOMO METAL MINING CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023075005
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In flash-smelting furnaces, understanding the reaction behavior between copper concentrate and silica sand for optimal slag formation is challenging due to the difficulty in sampling and controlling conditions within the high-temperature furnace, which affects the separation of matte and slag.

Method used

A method involving the placement of Fe oxide-containing powder on silicon dioxide-containing particles, heating the sample in a controlled environment to observe the reaction behavior, and adjusting oxygen partial pressure to evaluate the slag formation reaction.

Benefits of technology

Enables detailed evaluation of the slag formation reaction, allowing for improved fluidity and settling of matte, thereby increasing the recovery of high-quality matte and stabilizing the slag production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159174000001
    Figure 2024159174000001
  • Figure 2024159174000002
    Figure 2024159174000002
  • Figure 2024159174000003
    Figure 2024159174000003
Patent Text Reader

Abstract

To provide an evaluation method of a slag generating reaction, capable of grasping a reaction behavior between Fe oxide-containing powder and silicon dioxide-containing particles, and being used for the evaluation of a reaction speed of a slag generating reaction between copper concentrate and silica sand generated in a flash smelting furnace.SOLUTION: An evaluation method of a slag generating reaction includes the steps of: making a sample in which Fe oxide-containing powder containing Fe oxide is installed on the surfaces of silicon dioxide-containing particles containing silica sand; installing in a heating furnace, a container on which the sample is mounted; supplying process gas to the heating furnace to adjust oxygen partial pressure in the heating furnace; and observing and recording a reaction behavior on a boundary surface between the silicon dioxide-containing particles and the Fe oxide-containing powder while heating the sample.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating a slag formation reaction. [Background technology]

[0002] Copper sulfide concentrate (copper concentrate) is a powdered solid sulfide, etc., which is supplied as a smelting raw material to a flash smelting furnace (hereinafter referred to as a flash furnace), which is a type of smelting furnace, and is separated into two types of solutions, mainly matte and slag.

[0003] In the flash smelting furnace, copper concentrate, silica sand containing silicon dioxide, and auxiliary fuel such as heavy oil are blown into the reaction shaft together with reactive gas such as oxygen-enriched air delivered separately from a concentrate burner installed at the top of the reaction tower (reaction shaft). In the reaction shaft, the copper concentrate reacts with the reactive gas to produce two types of solutions (matte and slag), which fall in the form of droplets through the reaction shaft and are collected in a settler. In the settler, the matte and slag are separated into layers due to the difference in their specific gravities, and a matte layer and a slag layer are formed in that order from the bottom side of the settler.

[0004] In order to effectively separate the matte and slag in the settler, it is necessary to increase the fluidity of the slag and promote the settling of the matte, but it is difficult to obtain an optimal slag composition using copper concentrate alone.

[0005] In view of this, for example, a method has been proposed in which, when processing matte from copper concentrate in a flash smelting furnace, a flux such as silica stone, limestone, iron ore, or the like is added as a melting material together with the copper concentrate, and a eutectic composition is utilized to obtain slag at a temperature lower than the melting point of the oxide (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6387865 Summary of the Invention [Problem to be solved by the invention]

[0007] In a flash smelting furnace, it is desirable to cause the copper concentrate and the silica sand to collide with each other in the reaction shaft and complete the slag-forming reaction that occurs between the copper concentrate and the silica sand before the copper concentrate and the silica sand reach the settler, so a method is required to grasp the reaction behavior of the copper concentrate and the flux in detail and to find the conditions under which the slag-forming reaction can be completed quickly. One method for grasping the reaction behavior of the copper concentrate and the flux in detail is to sample the copper concentrate, silica sand, or molten material falling from inside the flash smelting furnace during operation.

[0008] However, the flash furnace is a large, high-temperature furnace, and inspection hatches are only installed in limited locations, making it difficult to remove the samples that fall from the reaction shaft. In addition, it is difficult to grasp and control the oxygen partial pressure and temperature at the sampling point, so in order to obtain results under the desired conditions, the above steps must be repeated, which is difficult in reality.

[0009] One aspect of the present invention aims to provide a method for evaluating a slag formation reaction that can be used to understand the reaction behavior between an Fe oxide-containing powder and a silicon dioxide-containing particle and to evaluate the reaction rate of the slag formation reaction between copper concentrate and silica sand that occurs in a flash smelting furnace. [Means for solving the problem]

[0010] One aspect of the present invention is A step of preparing a sample in which an Fe oxide-containing powder containing Fe oxide is provided on a surface of a silicon dioxide-containing particle containing silicon dioxide; placing the container with the sample in a heating furnace; supplying a process gas into the heating furnace to adjust the oxygen partial pressure in the heating furnace; Observing and recording the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder while heating the sample; The present invention relates to a method for evaluating a slag formation reaction, comprising: Effect of the Invention

[0011] One embodiment of the method for evaluating a slag formation reaction according to the present invention can be used to grasp the reaction behavior between an Fe oxide-containing powder and a silicon dioxide-containing particle and to evaluate the reaction rate of a slag formation reaction between copper concentrate and silica sand that occurs in a flash smelting furnace. [Brief description of the drawings]

[0012] [Figure 1] 1 is a diagram showing a schematic configuration of a flash smelting furnace to which a method for evaluating a slag generation reaction according to an embodiment of the present invention is applied; [Diagram 2] FIG. 2 is a diagram illustrating an example of the configuration of an observation device. [Diagram 3] FIG. 2 is an explanatory diagram showing an example of the relationship between a predetermined temperature and the amount of reaction at the interface between an Fe oxide-containing powder and a silicon dioxide-containing particle. [Figure 4] Photographs showing the state of a sample before and after heating in a heating furnace. [Diagram 5] 1 is an image of the appearance of a sample during heating in an example observed with a microscope. [Figure 6] 1 is an image of the appearance of a sample of a comparative example when heated, observed with a microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described in detail. In order to facilitate understanding of the description, the same components in each drawing are given the same reference numerals, and duplicated descriptions will be omitted. In addition, the scale of each member in the drawings may differ from the actual scale. In this specification, "~" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified.

[0014] Before describing the method for evaluating a slag formation reaction according to the embodiment of the present invention, the configuration of a flash smelting furnace to which the method for evaluating a slag formation reaction according to the embodiment of the present invention is applied will be described.

[0015] <Self-melting furnace> Fig. 1 is a diagram showing a schematic configuration of a flash smelting furnace to which the evaluation method of the slag generation reaction according to the present embodiment is applied. As shown in Fig. 1, the flash smelting furnace 1 includes a reaction tower (reaction shaft) 10, a settler 20, and an exhaust flue 30. The flash smelting furnace 1 produces two types of solutions, slag and matte (copper content 60% to 65%), from copper concentrate (copper content 20% to 30%), which is a smelting raw material SP supplied to the reaction shaft 10, in the reaction shaft 10, and separates the slag and matte into layers in the settler 20 to recover matte with a high copper content.

[0016] The smelting raw material refers to valuable minerals containing the target metal to be extracted, useless minerals (gangue), etc., and includes copper concentrate, silica sand, etc. In this embodiment, a case where the smelting raw material contains copper concentrate and silica sand will be described.

[0017] Copper concentrate is copper ore having a particle size of, for example, 1 μm to 300 μm, and is a powdered solid sulfide (Cu-Fe-S) containing copper, iron, and sulfur. Copper concentrate is oxidized by oxygen-enriched air in the flash smelting furnace 1 and contains iron oxide (FeOx), which is an Fe oxide. The Fe oxide contained in the copper concentrate may have the form of FeO, Fe3O4, Fe2O3, etc.

[0018] Silica sand is a mineral whose main component is silicon dioxide (SiO2).

[0019] Matte is a mixture containing copper sulfide (Cu2S) and iron sulfide (FeS) as its main components, and is a solution containing a large amount of Cu.

[0020] Slag is a solution whose main component is silicate (2FeOx-SiO2) of iron oxide (FeOx), and contains a large amount of Fe.

[0021] The flash smelting furnace 1 may supply the smelting raw material SP, such as copper concentrate and the like, as well as fluxes such as silica stone, limestone, and iron ore as fluxes, into the reaction shaft 10 as melting materials.

[0022] The reaction shaft 10 is a hollow structure having a bottomed cylindrical top. The reaction shaft 10 is provided with a concentrate burner 11 at the top 10a. The number of the concentrate burners 11 may be one or more.

[0023] The concentrate burner 11 injects the smelting raw material SP, auxiliary fuel such as heavy oil, and a reaction gas RA such as oxygen-enriched air that is delivered separately into the reaction shaft 10 from the top 10a of the reaction shaft 10. The concentrate burner 11 can adjust the flow rate of the smelting raw material SP injected into the reaction shaft 10 by adjusting the flow rate of the reaction gas RA.

[0024] The average temperature inside the reaction shaft 10 is set to, for example, about 1300° C. In the reaction shaft 10, the copper concentrate is burned while falling inside the reaction shaft 10, and melted and oxidized, thereby producing two types of solutions (matte and slag) and sulfurous acid gas.

[0025] The settler 20 is provided below the reaction shaft 10, and one end of the settler 20 (left side in FIG. 1) is connected to the lower part of the reaction shaft 10. The settler 20 collects matte and slag generated in the reaction shaft 10 inside. In the settler 20, the matte and slag are separated into layers due to the difference in specific gravity between the matte and slag, and in the settler 20, a matte layer and a slag layer are formed in this order from the bottom side of the settler 20. The settler 20 has, on its side, one or more slag holes 21 as an outlet for removing slag, and one or more matte holes 22 as an outlet for removing matte.

[0026] The flue gas duct 30 is formed in a cylindrical shape, with one end connected to the top of the other end side (right side in Figure 1) of the settler 20 and the other end connected to the boiler 31, and supplies high-temperature sulfur dioxide gas generated in the reaction shaft 10 to the boiler 31.

[0027] The electric slag furnace 40 collects the slag discharged from the settler 20 through the slag hole 21, and separates and collects trace amounts of matte contained in the slag.

[0028] In the flash smelting furnace 1, copper concentrate is blown into the reaction shaft 10 from the top 10a of the reaction shaft 10 by the concentrate burner 11 together with silica sand, auxiliary fuel such as heavy oil, and reaction gas RA such as oxygen-enriched air delivered separately. The copper concentrate blown into the reaction shaft 10 is heated by the combustion heat of the fuel, the sensible heat of the reaction gas, and the radiant heat in the furnace wall of the reaction shaft 10, and the sulfur content in the raw material for smelting reacts with the reaction gas instantaneously and burns. The combustion heat generated by the combustion of the sulfur content in the raw material for smelting causes the dissolution and oxidation of the copper concentrate particles (copper concentrate particles) in the raw material for smelting, and two types of solutions (matte (Cu2S-FeS) and slag (FeOx-SiO2)) and sulfurous acid gas are generated mainly by the reactions shown in the following formulas (1) and (2). CuFeS2+O2→Cu2S-FeS+FeOx+SO2···(1) FeOx+SiO2→FeOx-SiO2···(2)

[0029] The matte and slag generated in the reaction shaft 10 fall in the form of droplets into the settler 20 and are collected in the settler 20. At this time, droplets consisting of matte and slag (matte and slag droplets) repeatedly collide in the reaction shaft 10, increasing their particle size as they fall. In the settler 20, the matte and slag are separated into layers due to the difference in their specific gravities, and a matte layer and a slag layer are formed in this order at the bottom of the settler 20.

[0030] An appropriate amount of matte in the settler 20 is extracted from the matte hole 22 in response to a request from a converter (not shown) to which the matte is to be transported, and the slag in the settler 20 is appropriately discharged from the slag hole 21. The slag discharged from the slag hole 21 is introduced into an electric slag furnace 40, where it is heated and maintained by heat transfer caused by the passage of electricity through an electrode 41. A portion of the matte in the flash furnace slag layer does not settle to the bottom of the settler 20 but is discharged together with the slag, and further settles to the bottom of the furnace during the residence time in the electric slag furnace 40, forming a matte layer and a slag layer in the electric slag furnace 40 as well. The matte in the electric slag furnace 40 is recovered, and only the slag containing a small amount of copper is discharged from a discharge port 42 to the outside of the furnace.

[0031] In this manner, in the flash smelting furnace 1, the copper concentrate is separated into slag and matte, and the copper content in the recovered matte is set to, for example, 60% to 65%.

[0032] In addition, high-temperature sulfur dioxide gas generated in the reaction shaft 10 is discharged through a settler 20 and an exhaust flue 30 and cooled in a boiler 31.

[0033] <Method for evaluating slag formation reaction> The evaluation method of the slag formation reaction according to the present embodiment will be described. The powder containing Fe oxide (Fe oxide-containing powder) and the particles containing silicon dioxide (silicon dioxide-containing particles) used in the evaluation method of the slag formation reaction according to the present embodiment are smelting raw materials supplied from the top of the reaction shaft 10 when matte and slag are produced by reacting with the reaction gas supplied into the reaction shaft 10. The Fe oxide-containing powder is regarded as a powder containing Fe oxide obtained by oxidizing the copper concentrate contained as the smelting raw material with oxygen-enriched air in the flash smelting furnace 1, and the silicon dioxide-containing particles are regarded as particles containing silicon dioxide contained in the silica sand contained as the smelting raw material.

[0034] In the method for evaluating the slag formation reaction according to the present embodiment, silicon dioxide-containing particles having Fe oxide-containing powder attached to their surfaces are used as samples to grasp the reaction behavior between the Fe oxide-containing powder and the silicon dioxide-containing particles in the samples. From this reaction behavior, the slag formation reaction in which copper concentrate and silica sand supplied as smelting raw materials from a concentrate burner 11 provided at the top 10a of a reaction shaft 10 fall toward a settler 20 and react with a reaction gas supplied into the reaction shaft 10 to generate matte and slag is indirectly evaluated in the flash smelting furnace 1 having the configuration shown in Fig. 1, and is used to evaluate the reaction rate of the slag formation reaction.

[0035] Matte is a type of slag produced from raw materials, and slag is a type of slag produced from raw materials. Slag is a type of slag produced from raw materials, and is a waste product produced when smelting copper. The slag-forming reaction is also called the slag-making reaction.

[0036] [Observation equipment] The method for evaluating the slag formation reaction according to this embodiment can be carried out by using a silicon dioxide-containing particle having Fe oxide-containing powder attached to its surface as a sample, and observing the reaction behavior at the interface between the silicon dioxide-containing particle of this sample and the Fe oxide-containing powder using an observation device.

[0037] An observation device used in the evaluation method for the slag production reaction according to this embodiment will be described. Fig. 2 is a diagram showing an example of the configuration of the observation device. As shown in Fig. 2, the observation device 100 has a heating furnace 110, a stage 120, a vacuum pump 130, a temperature regulator 140, a gas supply unit 150, an oxygen partial pressure measuring device 160, a microscope 170, a light source 180, a control unit 190, and a display unit 200. The observation device 100 heats a sample S placed in a container 101.

[0038] Sample S is a silicon dioxide-containing particle having an Fe oxide-containing powder attached to its surface. Details of Sample S will be described later.

[0039] The heating furnace 110 heats the sample S. The heating furnace 110 includes a holder 111 for placing the sample S, and heats the sample S in a state in which the sample S is placed in the holder 111. The heating furnace 110 is connected to a temperature regulator 140, and heats the inside of the heating furnace 110 and adjusts the heating temperature based on an electrical signal transmitted from the temperature regulator 140.

[0040] The heating furnace 110 may have an observation window 112 on its wall so that the internal condition can be observed from the outside.

[0041] The heating furnace 110 may be of any type as long as it can control the temperature and gas composition. For example, an infrared gold image furnace may be used.

[0042] The stage 120 is a support base on which the furnace 110 is placed, and the position of the furnace 110 may be adjusted by moving the furnace 110 approximately parallel to the installation surface of the stage 120 so that the sample S can be observed through the observation window 112. It is preferable to adjust the stage 120 so that the observation window 112 of the furnace 110 is positioned approximately at the center of the optical axis of the microscope 170 so that the sample S can be easily observed and recorded through the observation window 112.

[0043] The vacuum pump 130 is a pump for evacuating the inside of the furnace, and any type of pump can be used as long as it can evacuate the inside of the furnace.

[0044] The temperature regulator 140 controls heating and the heating temperature of the heating furnace 110. As the temperature regulator 140, a general temperature regulator may be used.

[0045] The gas supply unit 150 supplies into the furnace a process gas G used to adjust the oxygen partial pressure in the furnace.

[0046] As the process gas G, for example, an inert gas such as Ar gas, He gas, N2 gas, etc. may be used, or an inert gas with an adjusted oxygen partial pressure may be used. As the inert gas with an adjusted oxygen partial pressure, for example, a mixed gas in which an inert gas is mixed with CO gas and CO2 gas may be used. By supplying CO gas and CO2 gas to the inert gas and utilizing the equilibrium between CO and CO2, the oxygen partial pressure in the mixed gas can be adjusted.

[0047] As a method for adjusting the oxygen partial pressure in the furnace, other than the method using the process gas G, for example, a method of adjusting the oxygen partial pressure using an oxygen controller, etc. may be used.

[0048] The oxygen partial pressure measuring device 160 measures the oxygen partial pressure inside the heating furnace 110. As the oxygen partial pressure measuring device 160, a general oxygen partial pressure measuring device or the like may be used.

[0049] The microscope 170 is provided outside the heating furnace 110 and is placed at a position where the sample S can be observed from above the heating furnace 110 through the observation window 112.

[0050] The light source 180 is connected to the microscope 170 and can adjust the brightness when observing the sample S through the microscope 170.

[0051] The control unit 190 is connected to the microscope 170, and transmits the sample S observed by the microscope 170 as an image to the display unit 200. The control unit 190 may be a general personal computer or the like.

[0052] The display unit 200 is connected to the control unit 190, and displays an image sent from the control unit 190. As the display unit 200, a monitor or the like is used.

[0053] The evaluation method of the slag generation reaction according to this embodiment will be described. The evaluation method of the slag generation reaction according to this embodiment will be described when it is performed using the above-mentioned observation device 100. Note that the evaluation method of the slag generation reaction according to this embodiment is not limited to a particular device as long as it can evaluate the slag generation reaction without using the above-mentioned observation device 100.

[0054] A sample S is prepared in a container in which a powder containing Fe oxide (Fe oxide-containing powder) is placed on the surface of a silicon dioxide-containing particle containing silicon dioxide (sample preparation step).

[0055] Methods for applying the Fe oxide-containing powder to the surface of the silicon dioxide-containing particles include, for example, sprinkling the powder using a sieve or placing a small amount on the surface with a spoon.

[0056] The type of the container is not limited as long as it can withstand the heat in the heating furnace 110 and is made of a material in which the solubility of FeO-SiO2-based slag is small. The container is preferably made of platinum (Pt), Pt-Rh, or the like.

[0057] The container may be of any shape or size as long as it has a structure that prevents the slag produced after the reaction between the silicon dioxide-containing particles and the Fe oxide-containing powder from overflowing and can be installed in the furnace.

[0058] When placing the sample S in the container, silicon dioxide-containing particles having Fe oxide-containing powder applied thereon in advance may be placed in the container, or Fe oxide-containing powder may be applied to the surface of silicon dioxide-containing particles placed in the container.

[0059] The silicon dioxide-containing particles include silicon dioxide and may include other substances. The silicon dioxide-containing particles may be, for example, silica sand contained in the smelting raw material supplied into the reaction shaft 10. The composition of the silicon dioxide-containing particles is determined by chemical analysis, X-ray fluorescence analysis, etc. The silicon dioxide-containing particles may be, for example, naturally occurring sand, commercially available SiO2 reagent, etc.

[0060] The average particle size of the silicon dioxide-containing particles is preferably larger than that of the Fe oxide-containing powder, and is preferably, for example, 200 μm to 10 mm, so that the average particle size of the silicon dioxide-containing particles is approximately the same as that of the silica sand fed into the reaction shaft 10.

[0061] The average particle size refers to the volume average particle size based on the effective diameter. The average particle size is, for example, the particle size (median size) when the cumulative amount of the smallest particles accumulates to 50% by volume in a particle size distribution curve obtained by measuring the particle size distribution of silicon dioxide-containing particles using a laser diffraction / scattering method or a dynamic light scattering method. Hereinafter, the average particle sizes of other substances are defined in the same manner.

[0062] The Fe oxide-containing powder may be any material that directly contains Fe oxide or produces Fe oxide through oxidation, such as copper concentrate containing Fe oxide that is oxidized by oxygen-enriched air in the flash smelting furnace 1 as the smelting raw material supplied into the reaction shaft 10.

[0063] Copper concentrate contains, for example, Cu, Fe, S, CaO, MgO, SiO2, Al2O3, etc., and is composed of copper and iron sulfides (CuFeS2, Cu5FeS4, Cu9Fe9S 16 , FeS2, FeS), and Fe oxides (Fe2O3, Fe3O4, FeO). The Fe oxide-containing powder may be a substance other than copper concentrate that contains Fe oxide. Examples of substances other than copper concentrate that contain Fe oxide include Fe2O3 reagent, Fe3O4 reagent, FeO reagent, and slag. The composition of the Fe oxide-containing powder is determined by chemical analysis, fluorescent X-ray analysis, and the like.

[0064] The Fe oxide-containing powder may be sprinkled on the surface of the silicon dioxide-containing particles in such a manner that it does not accumulate thereon, so that the reaction interface can be easily observed.

[0065] The average particle size of the Fe oxide-containing powder is not particularly limited as long as it is smaller than that of the silicon dioxide-containing particles, but may be, for example, 1 μm to 200 μm.

[0066] Next, the container with the prepared sample S placed therein is placed in the holder 111 in the heating furnace 110 (placement step).

[0067] Next, the inside of the furnace in which the sample S is placed is evacuated using a vacuum pump 130, and then a process gas G with adjusted composition is supplied into the furnace from the gas supply unit 150 to replace the air in the furnace with the process gas G, and the oxygen partial pressure in the furnace is adjusted (oxygen partial pressure adjustment process).

[0068] The degree of vacuum and the oxygen partial pressure inside the furnace are not particularly limited and may be set to any appropriate value.

[0069] Next, the inside of the heating furnace 110 is heated using the temperature regulator 140, and the temperature of the sample S is raised to a predetermined temperature (e.g., 600°C to 1600°C), while observing and recording the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder contained in the sample S (reaction recording process).

[0070] The reaction behavior is observed through an observation window 112 provided in the heating furnace 110. In addition, the reaction behavior is preferably observed through a microscope 170 installed outside the furnace through the observation window 112.

[0071] The reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder contained in sample S shows the same reaction behavior as the reaction between the Fe oxide in the copper concentrate and the silica sand supplied as flux in the reaction shaft 10, and the Fe oxide in the copper concentrate reacts with the silica sand as follows. Note that the Fe oxide in the copper concentrate may include not only the Fe oxide originally contained in the copper concentrate, but also the Fe oxide generated by oxidation of the Fe sulfide in the copper concentrate in oxygen-enriched air. FeOx+SiO2→FeOx-SiO2(Slag)

[0072] By observing the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder contained in sample S, it is possible to evaluate the reaction behavior at the interface between the Fe oxide in the copper concentrate and the silica sand in the flash smelting furnace.

[0073] The observation may be carried out visually.

[0074] The recording may be performed by photographing the sample observed through the observation window 112 with a camera, or by attaching a microscope camera or the like to the microscope 170, and the recording method is not particularly limited.

[0075] The method for evaluating the slag generation reaction according to the present embodiment includes a sample preparation step, a sample placement step, an oxygen partial pressure adjustment step, and a reaction recording step. In the reaction recording step, the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder contained in the sample S is observed and recorded. The reaction behavior at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles is observed, recorded, and understood under substantially the same environment as the controlled temperature and atmosphere in the heating furnace 110, so that the slag generation behavior when the copper concentrate collides with the silica sand in the reaction shaft 10 can be understood. The reaction behavior at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles can be understood from the reaction amount at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles. An example of the relationship between a predetermined temperature and the reaction amount at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particle is shown in FIG. 3. The reaction amount is the reaction amount that contributes to the reaction between the Fe oxide-containing powder and the silicon dioxide-containing powder, and can be calculated from the following formula (1) when the reaction amount is Δm. Δm=k×exp(-Ea / (RT))×m (1) (In the formula, k is a frequency factor, Ea is the activation energy, and T is the temperature in the reaction shaft 10.)

[0076] As shown in Figure 3, as the temperature rises, the reaction amount at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles progresses from a state in which there is almost no reaction occurring at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles to a stage in which the reaction progresses significantly, and finally the entire reaction is completed. The reaction amount at a specified temperature can be predicted from the reaction curve shown in Figure 3, so the reaction rate of the slag-forming reaction between copper concentrate and silica sand can be predicted.

[0077] Therefore, the method for evaluating the slag formation reaction according to this embodiment can be used to evaluate the reaction rate of the slag formation reaction between copper concentrate and silica sand occurring in the reaction shaft 10 by understanding the reaction behavior between copper concentrate and silica sand.

[0078] Based on the evaluation results of the reaction rate of the slag formation reaction occurring in the reaction shaft 10, an operating method for completing the slag formation reaction early can be devised to increase the fluidity of the slag in the settler 20 and improve the specific gravity separation of the matte and slag, thereby increasing the recovery amount of the matte, which is the target product, in the settler.

[0079] In the method for evaluating a slag generation reaction according to the present embodiment, the average particle size of the silicon dioxide-containing particles can be made larger than the average particle size of the Fe oxide-containing powder, which allows a large amount of the Fe oxide-containing powder to be reliably placed on the surfaces of the silicon dioxide-containing particles, making it easier to observe the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder contained in the sample S.

[0080] In the method for evaluating a slag formation reaction according to the present embodiment, the average particle size of the silicon dioxide-containing particles can be set to 200 μm to 10 mm. This allows the size of the silicon dioxide-containing particles to be close to that of the silica sand supplied to the reaction shaft 10, so that the reaction state of the silica sand can be made closer to that in the actual operation of the flash smelting furnace 1. Therefore, the method for evaluating a slag formation reaction according to the present embodiment can more appropriately evaluate the reaction rate of the slag formation reaction between the copper concentrate and the silica sand that occurs in the reaction shaft 10 by understanding the reaction behavior between the copper concentrate and the silica sand.

[0081] In the method for evaluating a slag formation reaction according to this embodiment, the reaction behavior at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles can be observed through the observation window 112 of the heating furnace 110. As a result, the method for evaluating a slag formation reaction according to this embodiment makes it easier to grasp the reaction behavior between the copper concentrate and the silica sand, and therefore the reaction rate of the slag formation reaction between the copper concentrate and the silica sand occurring in the reaction shaft 10 can be more appropriately evaluated.

[0082] In the method for evaluating a slag formation reaction according to this embodiment, the reaction behavior at the interface between the Fe oxide-containing powder and the silicon dioxide-containing particles can be observed through the observation window 112 of a microscope 170 installed outside the heating furnace. As a result, the method for evaluating a slag formation reaction according to this embodiment can grasp the reaction behavior between the copper concentrate and the silica sand in more detail, and therefore the reaction rate of the slag formation reaction between the copper concentrate and the silica sand occurring in the reaction shaft 10 can be more appropriately evaluated.

[0083] As described above, in the reaction shaft 10, the slag-forming reaction between the copper concentrate and the silica sand proceeds, and two types of solutions, slag and matte, are formed. The reaction status of the copper concentrate and the silica sand in the reaction shaft 10 greatly affects the capacity of the reaction shaft 10 and the copper extraction rate. For this reason, understanding the slag formation behavior and appropriately evaluating the reaction rate of the slag formation reaction are important for stabilizing the slag formation reaction and improving the copper extraction efficiency.

[0084] As described above, the method for evaluating the slag generation reaction according to this embodiment can be used to evaluate the reaction rate of the slag generation reaction occurring in the reaction shaft 10 from the observation and recording results during heating of the sample S. By using the method for evaluating the slag generation reaction according to this embodiment, the fluidity of the slag can be increased and the matte sedimentation can be promoted, thereby improving the yield of the matte. Therefore, the method can be effectively used for prior examination of equipment improvements for the flash smelting furnace 1, investigation of the effects of changes in the operating conditions of the flash smelting furnace 1, and the type of smelting raw material supplied to the flash smelting furnace 1, etc.

[0085] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES

[0086] The present embodiment will be described in more detail below with reference to examples, although the present embodiment is not limited to the following examples.

[0087] <Example> [Sample Preparation] Three SiO2 particles (purity: 99.99% or more, diameter: 2 mm, height: 2 mm) were placed on a platinum pan (diameter: 5.2 mm, height: 2.6 mm), and FeO powder (purity: 99.5%, particle size: 37 μm to 53 μm) was sprinkled on top to prepare a sample. The appearance of the sample before heating is shown in Figure 4(a).

[0088] [Check the reaction status] The reaction state of the sample placed in the platinum pan was observed using the observation device 100 shown in Fig. 2. The prepared sample was placed together with the platinum pan on a sample holder in the gold image furnace, and a lid with an observation window was attached to the gold image furnace to seal the device. The inside of the device was evacuated with a vacuum pump to reduce the pressure inside the device to 0.0293 Pa, and then the oxygen partial pressure was reduced to approximately 1 × 10 -7 Ar gas adjusted to 1 Pa was supplied to replace the gas in the device. Next, the temperature inside the furnace was raised to 1000°C at a rate of +200°C per minute using a temperature controller, and after reaching 1000°C, it was heated to 1450°C at a rate of +50°C per minute. The appearance of the sample during the temperature rise was observed with an optical microscope installed on the top of the Gold Image furnace, and recorded with an HDMI camera at 30 fps and a shutter speed of 1 / 345 sec.

[0089] The images of the appearance of the samples observed under a microscope when the temperatures in the furnace were 1100°C, 1200°C, 1202°C, 1204°C, 1300°C, and 1400°C are shown in Fig. 5. The appearance of the sample after heating to 1450°C is shown in Fig. 4(b).

[0090] As shown in Fig. 4(a), before heating, the FeO powder in the sample was not melted, and as shown in Fig. 5(a), even when heated to 1100°C, the FeO powder in the sample did not melt. As shown in Fig. 5(b) to Fig. 5(f), when the sample was heated to about 1202°C, the FeO powder in the sample began to melt, and when heated to about 1400°C, the FeO powder in the sample was almost melted. As shown in Fig. 4(b), after the sample was heated to about 1450°C, it was confirmed that the FeO powder in the sample had melted and spread over the surface of the SiO2 particles.

[0091] Therefore, by examining the reaction behavior between the FeO powder and SiO2 particles in the sample, it is possible to evaluate the temperature at which the liquid phase of the sample begins to form and the reaction rate between the FeO powder and SiO2 particles.

[0092] <Comparative Example> [Sample Preparation] A test similar to that in the example was carried out using a total of 20 mg of FeO powder and SiO2 powder. A sample was prepared by mixing 14.1 mg of FeO powder (purity: 99.5%, particle size: 37 μm to 53 μm) and 5.9 mg of SiO2 powder (purity: 99.9%, 20 μm to 37 μm) with a spoon. The sample was placed in a platinum pan (diameter 5.2 mm, height 2.6 mm) and heated to 10 kg / cm 2 It was compressed with a force of . [Check the reaction status] The sample was heated in the same manner as in the Example, except that the pressure inside the apparatus was reduced to 0.0248 Pa, and the appearance of the sample was observed under a microscope when the temperatures inside the furnace were 1100° C., 1120° C., 1140° C., 1150° C., 1160° C., 1170° C., 1180° C., 1190° C., and 1200° C. The images observed at each of these temperatures are shown in FIG. 6.

[0093] As shown in Figure 6, the reaction behavior of FeO powder and SiO2 powder can be observed, but it was confirmed that it was difficult to clearly confirm the temperature at which the formation of a liquid phase began in the initial stage of the reaction.

[0094] Therefore, in the comparative sample, the temperature at which the liquid phase begins to form cannot be clearly identified, and the reaction behavior between the FeO powder and the SiO2 powder in the sample is difficult to confirm, making it difficult to evaluate the reaction rate.

[0095] The aspects of the embodiment of the present invention are as follows, for example. <1> A step of preparing a sample in which an Fe oxide-containing powder containing Fe oxide is placed on the surface of a silicon dioxide-containing particle containing silica sand; placing the container with the sample in a heating furnace; supplying a process gas into the heating furnace to adjust the oxygen partial pressure in the heating furnace; Observing and recording the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder while heating the sample; A method for evaluating a slag formation reaction comprising: <2> The average particle size of the silicon dioxide-containing particles is larger than the average particle size of the Fe oxide-containing powder. <1> The method for evaluating a slag formation reaction according to claim 1. <3> The average particle size of the silicon dioxide-containing particles is 200 μm to 10 mm. <1> or <2> The method for evaluating a slag formation reaction according to claim 1. <4> The heating furnace has an observation window, The reaction behavior is observed through the observation window. <1> ~ <3> The method for evaluating a slag formation reaction according to any one of the above. <5> A microscope is installed outside the heating furnace, The reaction behavior is observed through the observation window with the microscope. <4> The method for evaluating a slag formation reaction according to claim 1. <6> The Fe oxide-containing powder and the silicon dioxide-containing particles are smelting raw materials supplied from the top of the reaction tower when they react with the reaction gas supplied into the reaction tower to generate matte and slag. <1> ~ <5> The method for evaluating a slag formation reaction according to any one of the above. [Explanation of symbols]

[0096] 1 Flash-melting furnace 10 Reaction tower (reaction shaft) 11 Concentrate burner 20 Settler 30 Flue flue 40 Electric smelting furnace 100 Observation equipment 110 Heating Furnace 120 Stages 130 Vacuum Pump 140 Temperature controller 150 Gas supply unit 160 Oxygen Pressure Measuring Device 170 Microscope 180 light source 190 Control section 200 Display S Sample

Claims

1. A step of preparing a sample in which an Fe oxide-containing powder containing Fe oxide is placed on the surface of a silicon dioxide-containing particle containing silica sand; placing the container with the sample in a heating furnace; supplying a process gas into the heating furnace to adjust the oxygen partial pressure in the heating furnace; Observing and recording the reaction behavior at the interface between the silicon dioxide-containing particles and the Fe oxide-containing powder while heating the sample; A method for evaluating a slag formation reaction comprising:

2. 2. The method for evaluating a slag formation reaction according to claim 1, wherein the average particle size of the silicon dioxide-containing particles is larger than the average particle size of the Fe oxide-containing powder.

3. 2. The method for evaluating a slag formation reaction according to claim 1, wherein the average particle size of the silicon dioxide-containing particles is 200 μm to 10 mm.

4. The heating furnace has an observation window, The method for evaluating a slag formation reaction according to claim 1 , wherein the reaction behavior is observed through the observation window.

5. A microscope is installed outside the heating furnace, The method for evaluating a slag formation reaction according to claim 4, wherein the reaction behavior is observed with the microscope through the observation window.

6. The method for evaluating a slag formation reaction according to claim 1, wherein the Fe oxide-containing powder and the silicon dioxide-containing particles are smelting raw materials supplied from the top of the reaction tower when they react with a reaction gas supplied into the reaction tower to generate matte and slag.

Citation Information

Patent Citations

  • Picture reader and recorder