Phenolic hydroxyl group-containing resin, curable composition, cured product, prepreg, circuit board, build-up film, semiconductor sealing material and semiconductor device
A phenolic hydroxyl group-containing resin with a modified fluorene structure addresses the high elastic modulus and dielectric property imbalance of existing phenolic resins, offering superior dielectric and mechanical performance at high temperatures.
Patent Information
- Application Number
- JP2023075273
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing phenolic resins with a biphenylaralkyl structure exhibit high crosslinking density and elastic modulus, making them unsuitable for applications requiring both excellent dielectric properties and low modulus of elasticity, especially at high temperatures.
A phenolic hydroxyl group-containing resin is developed with a modified fluorene structure, where the hydrogen atom at position 9 is replaced by an aralkyl group, achieving a balance of low dielectric loss tangent, low dielectric constant, and low elastic modulus.
The resin provides excellent dielectric properties and low elastic modulus in high temperature regions, enabling the production of materials with improved performance in electronic components.
Smart Images

Figure 2024159337000037 
Figure 2024159337000038 
Figure 2024159337000039
Abstract
Description
[Technical field]
[0001] The present invention relates to a phenolic hydroxyl group-containing resin, a curable composition, a cured product, a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device. [Background technology]
[0002] Epoxy resin compositions containing an epoxy resin and a curing agent therefor exhibit excellent heat resistance and insulating properties in the cured product, and are therefore widely used in electronic component applications such as semiconductors and multilayer printed circuit boards. However, against the backdrop of increasing signal speeds and frequencies in various electronic devices in recent years, it is becoming difficult to provide a resin composition that can form a cured product that exhibits a sufficiently low dielectric tangent while maintaining a sufficiently low dielectric constant. In response to this, biphenyl aralkyl resins have attracted attention as materials that provide excellent dielectric properties, and efforts are being made to use them as curing agents for epoxy resins or as raw materials for epoxy resins (for example, Patent Documents 1 to 5). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-301031 A [Patent Document 2] JP 2006-342176 A [Patent Document 3] JP 2007-308570 A [Patent Document 4] JP 2003-113225 A [Patent Document 5] JP 2010-229422 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, since a phenolic resin having a biphenylaralkyl structure forms a novolac-type resin based on the phenolic structure, a cured product using the same has a high crosslink density and usually has a high elastic modulus even in a high temperature range (e.g., 200 to 280°C), and there is room for improvement in terms of elastic modulus. There remains a need for resins that can combine excellent dielectric properties with a low modulus of elasticity at high temperatures. [Means for solving the problem]
[0005] As a result of extensive research aimed at solving the above-mentioned problems, the inventors have discovered that a phenolic hydroxyl group-containing resin having a structure in which the hydrogen atom at the 9th position of a fluorene structural unit is modified to an aralkyl can achieve both excellent dielectric properties (low dielectric constant and low dielectric tangent) and a low elastic modulus at high temperatures to a high degree, thereby completing the present invention.
[0006] The gist of the present invention is as follows. [1] A phenolic hydroxyl group-containing resin which is a reaction product of a fluorene compound (not having a substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1). [ka] (where: Ar is an aromatic ring group which may have a substituent. R1 is each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms; X is a leaving group. [2] The phenolic hydroxyl group-containing resin according to [1], wherein the amount of the fluorene compound is 0.01 to 0.99 mol per 1 mol of the compound represented by the general formula (1). [3] A phenolic hydroxyl group-containing resin represented by general formula (5): [ka] (where: Z is independently a group represented by the general formula (2A): [ka] or a structural unit represented by general formula (3A): [ka] It is a structural unit represented by Z' is independently a group represented by the general formula (2A'): [ka] or a structural unit represented by general formula (3A'): [ka] It is a structural unit represented by Ar each independently represents an aromatic ring group which may have a substituent, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer of 0 to 3, p is an average value greater than 0; R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer of 0 to 4, R 3’are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer of 0 to 4, However, the resin contains a structural unit represented by general formula (2A) and / or general formula (2A') and a structural unit represented by general formula (3A) and / or general formula (3A'). [4] The phenolic hydroxyl group-containing resin according to [3], which contains at least one of a compound represented by general formula (5-1) and a compound represented by general formula (5-2). [ka] (where: Ar, Z, R 1 , R 3’ and n' are as defined in [3].) [5] A phenolic hydroxyl group-containing resin according to any one of [1] to [4], having a hydroxyl group equivalent of 100 to 2000 g / eq. [6] The phenolic hydroxyl group-containing resin according to any one of [1] to [5], having a number average molecular weight of 100 to 10,000. [7] A curable composition comprising the phenolic hydroxyl group-containing resin according to any one of [1] to [6] and a curing agent. [8] A cured product of the curable composition of [7]. [9] A prepreg having a reinforcing substrate and a semi-cured product of the curable composition [7] impregnated into the reinforcing substrate.
[10] [9] A circuit board that is a laminate of prepreg and copper foil.
[11] A build-up film containing the curable composition of [7].
[12] A semiconductor encapsulant comprising the curable composition according to [7].
[13] A semiconductor device comprising the cured semiconductor encapsulant according to
[12] . Effect of the Invention
[0007] According to the present invention, it is possible to provide a phenolic hydroxyl group-containing resin that can achieve both excellent dielectric properties (low dielectric constant and low dielectric tangent) and a low modulus of elasticity in a high temperature range, and also to provide a curable composition containing the phenolic hydroxyl group-containing resin and a cured product thereof. Furthermore, by using the curable composition or the cured product thereof, it is possible to provide a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device that can achieve both excellent dielectric properties and a low modulus of elasticity in a high temperature range. [Brief description of the drawings]
[0008] [Figure 1] 1 shows the results of GPC measurement of the phenolic hydroxyl group-containing resin synthesized in Example 1. [Diagram 2] 1 shows the results of FD-MS measurement of the phenolic hydroxyl group-containing resin synthesized in Example 1. [Diagram 3] 1 shows the results of C13-NMR measurement of the phenolic hydroxyl group-containing resin synthesized in Example 1. [Figure 4] 1 shows the results of GPC measurement of the phenolic hydroxyl group-containing resin synthesized in Example 2. [Diagram 5] 1 shows the results of FD-MS measurement of the phenolic hydroxyl group-containing resin synthesized in Example 2. [Figure 6] 1 shows the results of C13-NMR measurement of the phenolic hydroxyl group-containing resin synthesized in Example 2. [Figure 7] 1 shows the results of GPC measurement of the phenolic hydroxyl group-containing resin synthesized in Example 3. [Figure 8] 1 shows the results of FD-MS measurement of the phenolic hydroxyl group-containing resin synthesized in Example 3. [Figure 9] 1 shows the results of C13-NMR measurement of the phenolic hydroxyl group-containing resin synthesized in Example 3. [Figure 10] 1 shows the results of GPC measurement of the phenolic hydroxyl group-containing resin synthesized in Example 4. [Figure 11] 1 shows the results of FD-MS measurement of the phenolic hydroxyl group-containing resin synthesized in Example 4. [Figure 12]1 shows the results of C13-NMR measurement of the phenolic hydroxyl group-containing resin synthesized in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the mode for carrying out the invention will be described in detail, however, the present invention is not limited to the following description and can be carried out in various modified forms within the scope of the gist thereof.
[0010] [term] In this specification, the term "reaction raw material" refers to a compound that is used to obtain a target compound by a chemical reaction such as synthesis or decomposition and that partially constitutes the chemical structure of the target compound, and excludes substances that play the role of chemical reaction assistants such as solvents and catalysts. In particular, in this specification, the term "reaction raw material" refers to a precursor for obtaining the target phenolic hydroxyl group-containing resin by a chemical reaction. The term "structural unit" as used herein refers to a (repeating) unit of a chemical structure formed during a reaction or polymerization, in other words, refers to a partial structure other than the structure of the chemical bonds involved in the reaction or polymerization in a product compound formed by a reaction or polymerization, i.e., a so-called residue.
[0011] The aliphatic hydrocarbon group in this specification may be any of linear, branched and cyclic types, and may have an unsaturated bond in the structure. Examples of the aliphatic hydrocarbon group include those having 1 to 20 carbon atoms. In this specification, the monovalent aliphatic hydrocarbon group includes an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, a cycloalkenyl group, and a cycloalkynyl group. The alkyl group in this specification may be either a straight-chain or branched type and includes those having 1 to 20 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a sec-pentyl group, a tert-pentyl group, a neopentyl group, an amyl group, a cyclopentyl group, a hexyl group, a heptyl group, an octyl group, a cumyl group, a nonyl group, a decyl group, an undecyl group, and a dodecyl group. The alkenyl group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as a vinyl group, an allyl group, a butenyl group, a butadienyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, and a dodecenyl group. The alkynyl group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as an ethynyl group, a propargyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, an octynyl group, a nonynyl group, a decynyl group, an undecynyl group, and a dodecynyl group. The cycloalkyl group in this specification may be a monocyclic group or a polycyclic group and includes those having 3 to 30 carbon atoms, such as a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, an adamantyl group, a methylcyclohexyl group, and an ethylcyclohexyl group. The cycloalkenyl group in this specification may be a monocyclic group or a polycyclic group, and examples of the cycloalkenyl group include those having 3 to 30 carbon atoms, such as a cyclohexenyl group, a methylcyclohexenyl group, and an ethylcyclohexenyl group. The cycloalkynyl group in this specification may be a monocyclic group or a polycyclic group, and examples of the cycloalkynyl group include those having 4 to 30 carbon atoms, such as a cyclohexynyl group, a methylcyclohexynyl group, and an ethylcyclohexynyl group. In this specification, the divalent aliphatic hydrocarbon group includes an alkylene group, an alkenylene group, an alkynylene group, a cycloalkylene group, a cycloalkenylene group, and a cycloalkynylene group. The alkylene group in this specification may be either a straight-chain or branched type and includes those having 1 to 20 carbon atoms, such as a methylene group, ethylene group, propylene group, butylene group, pentylene group, hexylene group, heptylene group, octylene group, nonylene group, decylene group, undecylene group, and dodecylene group. The alkenylene group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as a vinylene group, a propenylene group, a butenylene group, a butadienylene group, an octenylene group, a decenylene group, and a dodecenylene group. The alkynylene group in this specification may be either a straight-chain or branched type and includes those having 2 to 20 carbon atoms, such as an ethynylene group, a propynylene group, a butynylene group, a butazinylene group, a pentynylene group, a hexynylene group, a heptynylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, or a dodecynylene group. In the present specification, an alkoxy group has an alkyl-O- structure, and the above description of the alkyl group is applied to the alkyl portion in the structure, such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, a tert-butoxy group, an allyloxy group, etc. The cycloalkylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 3 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as the cycloalkyl group. The cycloalkenylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 3 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as cycloalkenyl groups. The cycloalkynylene group in this specification may be a monocyclic group or a polycyclic group, and can be one having 4 to 30 carbon atoms, such as a divalent group corresponding to the groups exemplified as cycloalkynyl groups. The aromatic ring in this specification is a hydrocarbon ring consisting of a single ring or condensed rings having aromaticity, and includes those having 6 to 20 carbon atoms, such as a benzene ring, a naphthalene ring, an indene ring, an anthracene ring, an adamantane ring, etc. The aromatic ring group is a residue of an aromatic ring. The aryl group in this specification is a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, a biphenyl group, or a phenanthryl group. In the present specification, the arylalkyl group is an alkyl group substituted with one or more, preferably one or two, particularly one, aryl group, and the above description of the aryl group and alkyl group applies to the aryl group and alkyl group, such as a benzyl group or a phenethyl group. Halogen atoms in this specification are fluorine, chlorine, bromine and iodine.
[0012] The number average molecular weight (Mn) and weight average molecular weight (Mw) in this specification are values measured using gel permeation chromatography (hereinafter abbreviated as "GPC") under the measurement conditions described in the examples described later. In this specification, the hydroxyl equivalent is a value measured by titration, which refers to the neutralization titration method in accordance with JIS K 0070.
[0013] [Reaction raw material for phenolic hydroxyl group-containing resin] The phenolic hydroxyl group-containing resin of the present invention is prepared using, as reaction raw materials, a fluorene compound (which does not have a substituent at the 9-position) (hereinafter, also simply referred to as a "fluorene compound"), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1).
[0014] <Fluorene compounds> The fluorene compound is not particularly limited as long as it does not have a substituent at the 9-position of the fluorene, and may be unsubstituted or substituted at a position other than the 9-position.
[0015] The fluorene compound may be a compound represented by the following general formula (2). [ka] (where: m is independently an integer of 0 to 4, R 2 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom.
[0016] The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, or a butyl group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, a naphthyl group, an indenyl group, or an indanyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine.
[0017] Each m is independently preferably an integer of 0 to 2, more preferably 0 or 1, and particularly preferably 0. The two m's may be the same or different, but are preferably the same. When both of m are 1 or more, R substituted on the two benzene rings constituting the fluorene skeleton 2 may be the same or different. When either or both of m is 2 or more, two or more R 2 may be the same or different.
[0018] A preferred example of the compound of the general formula (2) is fluorene. [ka]
[0019] The compound of formula (2) can be used alone or in combination of two or more kinds in any ratio.
[0020] <Phenol-containing hydroxyl group compounds> The phenolic hydroxyl group-containing compound is a compound having one phenolic hydroxyl group in the molecule.
[0021] An example of the phenolic hydroxyl group-containing compound is a compound represented by the following general formula (3). [ka] (where: n is an integer from 0 to 4, R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’’ may form a ring together with the carbon atom to which they are attached.
[0022] The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, or a butyl group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, or a naphthyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine. R 3 Among these, an alkyl group or an aryl group is preferable.
[0023] Or, two R's 3’’ may form a ring together with the carbon atom to which they are bonded. Examples of the ring include a hydrocarbon ring having 6 to 20 ring-constituting atoms, such as a benzene ring, a naphthalene ring, an anthracene ring, an adamantane ring, an indane ring, and an indene ring. These rings may have a substituent, and examples of the substituent include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom.
[0024] n'' is preferably 0, 1 or 2. If n'' is 2, then two R 3’’preferably form a benzene or naphthalene ring together with the carbon atom to which they are attached.
[0025] Preferred examples of the compound of formula (3) include the following compounds: [ka]
[0026] The compound of formula (3) can be used alone or in combination of two or more kinds in any ratio.
[0027] <Compound represented by general formula (1)> The compound represented by general formula (1) is a compound that can modify the hydrogen atom at the 9-position of the fluorene structural unit to an aralkyl, and can also react with a compound containing a phenolic hydroxyl group, and thus functions as a binder. [ka] (where: Ar is an aromatic ring group which may have a substituent. R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group.
[0028] Ar is an aromatic ring group which may have a substituent. The aromatic ring group is not particularly limited, and is preferably a phenylene group, a naphthylene group, or an anthracenylene group. In the case of a phenylene group, it is preferable that the bonds are located at the 1- and 4-positions, in the case of a naphthylene group, it is preferable that the bonds are located at the 2- and 6-positions, and in the case of an anthracenylene group, it is preferable that the bonds are located at the 9- and 10-positions.
[0029] Examples of the substituent include an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, and a halogen atom. The aliphatic hydrocarbon group is preferably an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propylene group, or a butylene group. The aryl group is preferably a phenyl group, a tolyl group, a xylyl group, or a naphthyl group. The arylalkyl group is preferably a benzyl group, a phenethyl group, or a cumyl group. The alkoxy group is preferably a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The halogen atom is preferably fluorine, chlorine or bromine. Among them, the substituent is preferably an alkyl group, an aryl group, or the like.
[0030] X is a leaving group, and examples thereof include a hydroxyl group, a halogen atom, and an alkoxy group. The halogen atom is preferably chlorine, bromine or iodine. The alkoxy group is preferably an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, a propyloxy group, or a butoxy group. Among these, X is preferably a chlorine atom, a bromine atom, an iodine atom, a hydroxyl group, or a methoxy group. The two X's may be the same or different.
[0031] R 1 is a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms. The aliphatic hydrocarbon group having 1 to 4 carbon atoms is not particularly limited, and a methyl group, an ethyl group, a propyl group, a butyl group, and the like are preferred. R 1 Among them, hydrogen atom and methyl are preferable. 1 may be the same or different, but is preferably the same.
[0032] Preferred examples of the compound of formula (1) include the following: [ka]
[0033] [Method of producing phenolic hydroxyl group-containing resin] The phenolic hydroxyl group-containing resin of the present invention is a reaction product of the above-mentioned reaction raw materials, and specifically, can be produced as follows.
[0034] The amounts of the reaction raw materials, fluorene compound, phenolic hydroxyl group-containing compound and compound of general formula (1), used are as follows: From the viewpoint of introducing general formula (3), the amount of the compound of general formula (1) may be more than 1 mole relative to 1 mole of the fluorene compound, and is not particularly limited as long as it is more than 1 mole. For example, the amount of the fluorene compound used may be 0.01 moles or more, preferably 0.05 moles or more, and may be 0.99 moles or less, preferably 0.9 moles or less, relative to 1 mole of the compound of general formula (1). During the reaction, the fluorene compound and the compound of general formula (1) react in substantially their entirety, and therefore the molar ratio of the fluorene compound to the compound of general formula (1) used in the reaction is substantially the same as the molar ratio of the structural units derived from the fluorene compound to the structural units derived from the compound of general formula (1) in the obtained phenolic hydroxyl group-containing resin.
[0035] The amount of the phenolic hydroxyl group-containing compound used is not particularly limited, but may be an amount such that the amount of hydroxyl groups in the phenolic hydroxyl group-containing compound is 0.1 moles or more, preferably 0.02 moles or more, relative to the compound of general formula (1), and may be an amount such that the amount of hydroxyl groups in the phenolic hydroxyl group-containing compound is 10 moles or less, preferably 9.5 moles or less. Regarding the phenolic hydroxyl group-containing compound, some unreacted phenolic hydroxyl group-containing compound remains, but the amount of the reacted phenolic hydroxyl group-containing compound can be calculated from the hydroxyl group equivalent of the phenolic hydroxyl group-containing resin.
[0036] The phenolic hydroxyl group-containing resin can be produced, for example, by the following steps 1 and 2.
[0037] <Process 1> It is preferable to react the entire amount of the fluorene compound and the entire amount of the compound of general formula (1) in an organic solvent using an alkali catalyst at 10 to 100°C without adding a phenolic hydroxyl group-containing compound, or to react the entire amount of the fluorene compound and the entire amount of the compound of general formula (1) with a part or the entire amount of the phenolic hydroxyl group-containing compound in an organic solvent using an alkali catalyst at 10 to 100°C.
[0038] The amount of the phenolic hydroxyl group-containing compound used is not particularly limited, but it can be an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 0.1 mol or more, preferably 0.2 mol or more, and can be an amount in which the hydroxyl group of the phenolic hydroxyl group-containing compound is 10 mol or less, preferably 9.5 mol or less, relative to the general formula (1). By using such an amount, the generation of by-products can be suppressed.
[0039] Examples of organic solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aromatic hydrocarbon solvents such as toluene, xylene, mesitylene, and Solvesso; alcoholic solvents such as methanol, ethanol, 1-propyl alcohol, isopropyl alcohol, 1-butanol, sec-butanol, and tert-butanol; cellosolve solvents such as methyl cellosolve and ethyl cellosolve; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, and diethoxyethane; and aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, sulfolane, dimethylformamide, and dimethylacetamide. From the viewpoint of solubility, toluene, xylene, mesitylene, Solvesso, isopropyl alcohol, dimethyl sulfoxide, dimethylformamide, and dimethylacetamide are preferred. These organic solvents can be used alone or in combination of two or more at any ratio. The amount of the organic solvent used is not particularly limited, but is preferably 50 to 500% by mass based on the total amount of the compound of general formula (1) and the fluorene compound charged.
[0040] Examples of the alkali catalyst include lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium methoxy, sodium ethoxy, sodium tert-butoxy, potassium methoxy, potassium ethoxy, potassium tert-butoxy, triethylamine, pyridine, and dimethylaminopyridine. From the viewpoint of reactivity, sodium hydroxide or potassium hydroxide is preferred. The amount of the alkali catalyst used can be 10 to 1000 mol% based on the amount of the general formula (1) charged. These catalysts can be used as an aqueous solution of 1 to 50 mass%.
[0041] A phase transfer catalyst may be used in the reaction. Examples of the phase transfer catalyst include ammonium-based catalysts such as tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium, tetrabutylammonium iodide, tetrabutylammonium hydroxide, benzyltriethylammonium chloride, benzyltriethylammonium bromide, benzyltriethylammonium iodide, and benzyltriethylammonium hydroxide; phosphonium-based catalysts such as tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, and tetrabutylphosphonium hydroxide; and crown ether-based catalysts such as 12-crown-4-ether, 15-crown-5-ether, 18-crown-6-ether, and tribenzo-18-crown-6-ether. In terms of reactivity, tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltriethylammonium chloride, and benzyltriethylammonium iodide are preferred. The phase transfer catalyst may be used alone or in combination of two or more.
[0042] Additives may be used to promote the reaction. Examples of additives include halides such as lithium bromide, sodium bromide, potassium bromide, cesium bromide, lithium iodide, sodium iodide, potassium iodide, and cesium iodide. Among these, sodium iodide and potassium iodide are preferred. The additives may be used alone or in combination of two or more.
[0043] The reaction temperature can be from 10 to 100° C., and from the viewpoint of reactivity, is preferably from 20 to 80° C. The reaction time can be from 1 to 72 hours, and is preferably from 2 to 70 hours.
[0044] After the reaction is completed, the reaction mixture is separated into upper and lower layers as appropriate, and the lower layer, which is the aqueous layer, is removed to obtain the reaction product. At this time, water may be added as necessary to dissolve the insoluble salt and remove the lower layer. The aqueous layer may be basic, neutralized by neutralization, or acidic. Examples of neutralizing agents used for neutralization include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, sodium monophosphate, and ammonium chloride, and organic acids such as methanesulfonic acid, p-toluenesulfonic acid, and oxalic acid. These acid catalysts may be used alone or in combination of two or more.
[0045] <Process 2> In the case where no phenolic hydroxyl group compound is added or a portion of the compound is added in step 1, the entire amount or the remainder of the phenolic hydroxyl group-containing compound is added to the reaction product obtained in step 1, and the reaction is carried out in the presence of an acid catalyst at 60 to 250° C. In the case where the entire amount of the phenolic hydroxyl group compound is added in step 1, the reaction product obtained in step 1 is reacted in the presence of an acid catalyst at 60 to 250° C.
[0046] The phenolic hydroxyl group-containing compound used in step 2 may be the same as or different from the phenolic hydroxyl group-containing compound used in step 1.
[0047] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, organic acids such as methanesulfonic acid, p-toluenesulfonic acid, and oxalic acid, and Lewis acids such as boron trifluoride, aluminum chloride, and zinc chloride. From the viewpoint of solubility, p-toluenesulfonic acid and methanesulfonic acid are preferred. These acid catalysts may be used alone or in combination of two or more. The amount of the acid catalyst is not particularly limited, but is preferably 0.001 to 10% by mass based on the total amount of the reaction raw materials charged.
[0048] The reaction temperature is 60 to 250° C., and from the viewpoint of reactivity, is preferably 80 to 240° C. The reaction time can be 1 to 72 hours, and is preferably 2 to 70 hours.
[0049] After the reaction is completed, neutralization and washing are carried out, and unreacted reactants, organic solvents, etc. are distilled off under reduced pressure and heating conditions to obtain a phenolic hydroxyl group-containing resin.
[0050] The method for producing the phenolic hydroxyl group-containing resin of the present invention is not limited to the above. For example, instead of step 1, a fluorene compound and a compound of general formula (1) may be reacted in an organic solvent in the presence of a catalyst at 10 to 100°C, and then a part of the phenolic hydroxyl group-containing compound may be added and reacted at 10 to 100°C, after which the water layer is removed, a water washing treatment is performed, and the resulting reaction product may be subjected to step 2. In this case, the reaction product of step 1 may have a reactive group at the end, and the reactive group may be an ether reacted with a phenol, a halide, or a hydroxyl group depending on the type of compound used.
[0051] [Phenol-containing hydroxyl group-containing resin] The phenolic hydroxyl group-containing resin of the present invention is a reaction product of a fluorene compound, a phenolic hydroxyl group-containing compound, and a compound of general formula (1).
[0052] The fluorene compound represented by general formula (2), the phenolic hydroxyl group-containing compound represented by general formula (3), and the compound of general formula (1) can respectively produce a structural unit represented by general formula (2A) or general formula (2A'), a structural unit represented by general formula (3A) or general formula (3A'), and a structural unit represented by general formula (1A). [ka] (where: The definition, examples and preferred examples of m and m′ are the same as those of m in formula (2). R 2 and R 2’ The definition, examples and preferred examples of R in the general formula (2) are as follows:2 is the same as * represents a bond.) [ka] (where: n is an integer from 0 to 3, preferably 0, 1 or 2. n' is an integer of 0 to 4, preferably 0, 1 or 2; R 3 and R 3’ The definition, examples and preferred examples of are the same as those of R″ in general formula (3). * represents a bond.) [ka] (where: Ar and R 1 The definition, examples and preferred examples are the same as those of general formula (1), * represents a bond.)
[0053] The phenolic hydroxyl group-containing resin of the present invention may contain a structure in which the structural unit of general formula (1A) is bonded to the structural unit of general formula (2A) and / or (2A'). At least one molecular chain terminal of the phenolic hydroxyl group-containing resin of the present invention is preferably a structural unit of general formula (3A'), and both molecular chain terminals are preferably structural units of general formula (3A').
[0054] The phenolic hydroxyl group-containing resin of the present invention is composed of structural units of general formula (2A) and / or (2A'), structural units of general formula (3A) and / or (3A'), and structural units of general formula (1A), with the proviso that a bond of the structural unit of general formula (2A) may be bonded to a bond of the structural unit of general formula (1A). When a structural unit of general formula (2A') is present, the structural unit constitutes a molecular chain terminal. At least one of the molecular chain terminals is preferably a structural unit of general formula (3A), and more preferably both of the molecular chain terminals are structural units of general formula (3A).
[0055] Preferred examples of the compound of formula (1-1) include the following. [ka]
[0056] The phenolic hydroxyl group-containing resin of the present invention includes a phenolic hydroxyl group-containing resin represented by the following general formula (5). [ka] (where: Z is independently a group represented by the general formula (2A): [ka] or a structural unit represented by general formula (3A): [ka] It is a structural unit represented by Z' is independently a group represented by the general formula (2A'): [ka] or a structural unit represented by general formula (3A'): [ka] It is a structural unit represented by Ar each independently represents an aromatic ring group which may have a substituent, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer of 0 to 4, R 3are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer of 0 to 3, R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer of 0 to 4, R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer of 0 to 4, p is the average value and is a number greater than 0; However, the resin contains structural units represented by general formula (2A) and / or general formula (2A') and structural units represented by general formula (3A) and / or general formula (3A').
[0057] In the above, Ar, R 1 、 R 2 , R 3 , m, n, R 2’ , R 3’ , m', n' and p are the same as those mentioned above.
[0058] The phenolic hydroxyl group-containing resin of general formula (5) is a mixture of compounds in which p in the above general formula (5) is an integer of 0 or more (provided that not all of the compounds are compounds of general formula (5) in which p is 0), and preferably contains a compound containing both structural units represented by general formula (2A) and / or general formula (2A') and structural units represented by general formula (3A) and / or general formula (3A') in the molecule. In the resin, the total amount of the structural units of general formulae (2A) and (2A') is preferably 0.1 to 10 mol, and more preferably 0.5 to 9.5 mol, per 1 mol of the structural units of general formulae (3A) and (3A').
[0059] A preferred example is a phenolic hydroxyl group-containing resin represented by the following general formula (5-0). [ka] (In the formula, Ar, R 1 、 R 3’ , n' and p are the same as in general formula (5).
[0060] Here, Ar, R 1 、 R 3’ , n' and p are the same as those described above. 2 , m, R 3 Examples and preferred examples of n are the same as those mentioned above.
[0061] More preferred examples of the phenolic hydroxyl group-containing resin of the present invention include phenolic hydroxyl group-containing resins represented by the following general formula (5-0'). [ka] (where R 2 , m, R 3 , n, R 3’ and n' is as defined above; Ar' is [ka] and s is the average value, a number greater than 0; t is the average value, and is a number equal to or greater than 0; The order of the structural units bracketed by s and the structural units bracketed by t is not limited.
[0062] The phenolic hydroxyl group-containing resin of general formula (5) and the phenolic hydroxyl group-containing resin of general formula (5-0) can each be a mixture of compounds having a structural unit bounded by p with an integer of 0 or more, but not all of the compounds are compounds of general formula (5) in which p is 0. The phenolic hydroxyl group-containing resin of general formula (5) preferably contains at least one of a compound represented by general formula (5-1) and a compound represented by general formula (5-2). [ka] (where: Ar, Z, R 1 , R 3‘ and n' are as defined above; Z in general formula (5-1) and at least one Z in general formula (5-2) are structural units represented by general formula (2A).
[0063] The phenolic hydroxyl resin of the present invention may contain a compound of general formula (6) as a part thereof. The compound of general formula (6) corresponds to the compound of general formula (5) above in which p is 0. [ka] (where: Ar, R 1 , R 3’ and n' are as defined above.
[0064] The number average molecular weight (Mn) of the phenolic hydroxyl group-containing resin may be in the range of 100 to 10,000, and preferably in the range of 200 to 8,000. The number average molecular weight (Mw) of the phenolic hydroxyl group-containing resin may be in the range of 100 to 50,000, and preferably in the range of 300 to 4,000. The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the phenolic hydroxyl group-containing resin can be in the range of 1-5, and is preferably 1-4.
[0065] The hydroxyl equivalent of the phenolic hydroxyl group-containing resin can be in the range of 100-2,000, and is preferably in the range of 200-1,800.
[0066] [Curable composition] The curable composition of the present invention can contain the phenolic hydroxyl group-containing resin of the present invention and a curing agent. By using the phenolic hydroxyl group-containing resin of the present invention, it is possible to develop excellent dielectric properties (low dielectric constant and low dielectric loss tangent) and a low elastic modulus in the high temperature range in the cured product obtained from the curable composition.
[0067] The curing composition may contain other phenolic hydroxyl group-containing compounds other than the phenolic hydroxyl group-containing resin of the present invention. Examples of other phenolic hydroxyl group-containing compounds include various bisphenol compounds, various novolak resins, and aralkylene group-containing phenolic resins. These may be used alone or in combination. The ratio of the phenolic hydroxyl group-containing resin of the present invention to the total of the phenolic hydroxyl group-containing resin of the present invention and other phenolic hydroxyl group-containing compounds is appropriately adjusted according to the desired cured product performance, etc., but is preferably 50 mass% or more, more preferably 80 mass% or more.
[0068] The curing agent is not particularly limited as long as it is a compound having a functional group capable of reacting with the phenolic hydroxyl group-containing resin of the present invention, and examples thereof include epoxy resins. The epoxy resin is not particularly limited, and a wide variety of resins can be used. Examples include various bisphenol-type epoxy resins, various novolac-type epoxy resins, and aralkylene group-containing epoxy resins. These may be used alone or in combination.
[0069] The compounding ratio of the phenolic hydroxyl group-containing resin and the curing agent is appropriately adjusted depending on the desired performance of the cured product, etc., but it is preferable that the reactive group in the curing agent is in the range of 0.5 to 1.5 moles per mole of the phenolic hydroxyl group in the phenolic hydroxyl group-containing resin. When using the other phenolic hydroxyl group-containing compounds described above, it is preferable that the reactive group in the curing agent is in the range of 0.5 to 1.5 moles per mole of the total of the phenolic hydroxyl groups in the curable composition.
[0070] When an epoxy resin is used as the curing agent, a curing accelerator may be used as necessary. Various types of curing accelerators can be used, including phosphorus compounds, tertiary amines, imidazoles, organic acid metal salts, Lewis acids, and amine complex salts. These may be used alone or in combination. Among them, phosphorus compounds such as triphenylphosphine or imidazoles are preferred from the viewpoint of excellent curability, heat resistance, electrical properties, and moisture resistance reliability. The amount of the curing accelerator added is preferably in the range of 0.01 to 10 parts by mass with respect to 100 parts by mass of the total mass (excluding the solvent) of the curable composition.
[0071] The curable composition may contain other resin components, such as active ester resins, maleimide resins, cyanate resins, unsaturated polyester resins, and polybutadiene resins.
[0072] The curable composition may contain various compounding agents such as a curing accelerator, a silane coupling agent, a release agent, a pigment, an emulsifier, a non-halogen-based flame retardant, an inorganic filler, a flame retardant (e.g., an inorganic phosphorus-based flame retardant, an organic phosphorus-based flame retardant, or a halogen-based flame retardant), and a solvent.
[0073] The curable composition can be obtained by uniformly mixing the phenolic hydroxyl group-containing resin of the present invention, a curing agent, and any optional components (eg, curing catalyst, compounding ingredients, etc.).
[0074] [Cured product] The cured product of the present invention can be obtained by curing the curable composition of the present invention. The curing method is not particularly limited, and a known method can be adopted. The cured product can be in the form of a laminate, a cast product, an adhesive layer, a coating film, a film, etc.
[0075] [Semiconductor encapsulation materials] The semiconductor encapsulant of the present invention may contain the curable composition of the present invention. Since the curable composition of the present invention contains the phenolic hydroxyl group-containing resin of the present invention, the semiconductor encapsulant containing the curable composition can exhibit excellent dielectric properties (low dielectric constant and low dielectric loss tangent) and a low elastic modulus in the high temperature range.
[0076] The semiconductor encapsulant may be prepared by adding an inorganic filler to the curable composition of the present invention. The inorganic filler is not particularly limited, and examples thereof include barium sulfate, barium titanate, amorphous silica, crystalline silica, Neuburg silica, fused silica, spherical silica, talc, clay, magnesium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, silicon nitride, and aluminum nitride. The amount of the inorganic filler may be 0.5 to 1200 parts by mass based on 100 parts by mass of the curable composition.
[0077] The semiconductor encapsulant may contain various compounding agents, including those described for the curable composition.
[0078] The semiconductor encapsulant can be obtained by mixing the curable composition of the present invention and, if necessary, compounding ingredients. For example, a method of thoroughly melt-mixing the composition using an extruder, kneader, roll, or the like until the composition becomes homogeneous can be mentioned.
[0079] [Semiconductor Devices] The semiconductor device of the present invention can include a cured product of the semiconductor encapsulant of the present invention. The semiconductor encapsulant used in the semiconductor device of the present invention contains a curable composition containing the phenolic hydroxyl group-containing resin of the present invention. Since the semiconductor device of the present invention includes a cured product of the semiconductor encapsulant, it exhibits excellent dielectric properties (low dielectric constant and low dielectric tangent) and a low elastic modulus in the high temperature range.
[0080] A semiconductor device can be obtained by heating and curing the semiconductor encapsulant of the present invention, for example, by casting or molding using a transfer molding machine, injection molding machine, or the like, and then heating and curing in a temperature range of room temperature (20°C) to 250°C.
[0081] [Prepreg] The prepreg of the present invention may have a reinforcing substrate and a semi-cured product of the curable composition of the present invention impregnated into the reinforcing substrate. The method for obtaining a prepreg from the curable composition is not particularly limited, and examples thereof include a method in which the curable composition is made into a varnish by blending an organic solvent described later into the curable composition, which is then impregnated into a reinforcing base material (e.g., paper, glass cloth, glass nonwoven fabric, aramid paper, aramid cloth, glass mat, glass roving cloth, etc.), and then heated at a heating temperature (preferably 50 to 170°C) according to the type of solvent used to semi-cure (or uncure) the curable composition. The mass ratio between the curable composition and the reinforcing base material used is not particularly limited, but it is preferable to adjust the resin content in the prepreg to 20 to 60 mass %.
[0082] The semi-cured product of the curable composition can be obtained by adjusting the heating temperature and heating time to stop the curing reaction midway without completing it. The degree of curing of the semi-cured product can be, for example, 5% or more and 85% or less. Here, the cured product can have a higher degree of curing than the semi-cured product. The degree of curing of the semi-cured product can be calculated from the following formula by measuring the amount of heat generated during curing when the curable composition is heated and the amount of heat generated during curing of the semi-cured product by DSC. Degree of cure (%)=[1-(cure heat generation amount of semi-cured product / cure heat generation amount of curable composition)]×100
[0083] Examples of organic solvents used in the production of prepregs include methyl ethyl ketone, acetone, dimethylformamide, methyl isobutyl ketone, methoxypropanol, cyclohexanone, methyl cellosolve, ethyl diglycol acetate, propylene glycol monomethyl ether acetate, etc. The selection of the organic solvent and the amount used can be appropriately selected depending on the application, and for example, when producing a circuit board from a prepreg, polar solvents with a boiling point of 160° C. or less such as methyl ethyl ketone, acetone, dimethylformamide, etc. are preferred, and the amount used is preferably an amount such that the nonvolatile content is 40 to 80 mass%.
[0084] [Circuit board] The circuit board of the present invention is made of a laminate of the prepreg of the present invention and copper foil. The method for obtaining the circuit board is not particularly limited, and an example thereof is a method in which the prepreg of the present invention is laminated as necessary, copper foil is superimposed, and the laminate is heated and compressed at 170 to 300° C. under a pressure of 1 to 10 MPa for 10 minutes to 3 hours.
[0085] [Build-up film] The build-up film of the present invention may contain the curable composition of the present invention. The method for producing the build-up film is not particularly limited, and may be, for example, a method in which the curable composition of the present invention is applied onto a support film to form a curable composition layer to form an adhesive film for a multilayer printed wiring board.
[0086] The build-up film is required to soften under the temperature conditions for lamination in the vacuum lamination method (usually 70 to 140°C) and to exhibit fluidity (resin flow) that allows resin to fill via holes or through holes present in the circuit board at the same time as lamination of the circuit board. Therefore, it is preferable that the curable composition contains the above-mentioned components so as to exhibit such properties.
[0087] Here, the diameter of the through-holes in the multilayer printed wiring board is usually 0.1 to 0.5 mm, and the depth is usually 0.1 to 1.2 mm, and it is usually preferable to make it possible to fill the resin within this range. When both sides of the circuit board are laminated, it is preferable to fill about 1 / 2 of the through-holes.
[0088] Specifically, the adhesive film can be produced by preparing the curable composition in a varnish form, applying the varnish-like composition to the surface of the support film (Y), and then drying the organic solvent by heating or blowing hot air or the like to form a composition layer (X) made of the curable composition.
[0089] The thickness of the composition layer (X) formed is usually preferably equal to or greater than the thickness of the conductor layer. Since the thickness of the conductor layer of the circuit board is usually in the range of 5 to 70 μm, the thickness of the resin composition layer is preferably 10 to 100 μm.
[0090] The composition layer (X) may be protected with a protective film described below. By protecting the resin composition layer with a protective film, the surface of the resin composition layer can be prevented from being scratched or from being contaminated by dirt or the like.
[0091] Examples of the above-mentioned support film (Y) and protective film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate, polycarbonate, polyimide, and further release paper and metal foils such as copper foil and aluminum foil. The support film and protective film may be subjected to a release treatment in addition to a mud treatment and a corona treatment.
[0092] The thickness of the support film is not particularly limited, but is usually in the range of 10 to 150 μm, preferably 25 to 50 μm, and the thickness of the protective film is preferably 1 to 40 μm.
[0093] The above-mentioned support film (Y) is peeled off after laminating it onto the circuit board or after forming an insulating layer by heat curing. If the support film (Y) is peeled off after the adhesive film is heat cured, the adhesion of dust and the like during the curing process can be prevented. When peeling off after curing, the support film is usually subjected to a release treatment in advance.
[0094] [Application] The cured product obtained by the curable composition containing the phenolic hydroxyl group-containing resin of the present invention exhibits excellent dielectric properties (low dielectric constant and low dielectric tangent) and a low modulus of elasticity in the high temperature range, and therefore can be suitably used for heat-resistant or electronic components. In particular, it can be suitably used for prepregs, circuit boards, semiconductor encapsulants, semiconductor devices, build-up films, build-up boards, adhesives using conductive pastes, resist materials, and the like. It can also be suitably used as a matrix resin for fiber-reinforced resins, and is particularly suitable as a highly heat-resistant prepreg. In addition, the phenolic hydroxyl group-containing resin contained in the curable composition exhibits excellent solubility in various solvents, and can be made into a paint. The heat-resistant or electronic components thus obtained can be suitably used for various applications, including, but not limited to, industrial machine parts, general machine parts, automobile, railway, and vehicle parts, space and aviation-related parts, electronic and electrical parts, building materials, containers and packaging materials, daily necessities, sports and leisure goods, and housing members for wind power generation. EXAMPLES
[0095] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to the following description and can be practiced with various modifications within the scope of the gist. In the following, "parts" and "%" are based on mass unless otherwise specified.
[0096] The physical properties of the phenolic hydroxyl group-containing resin were evaluated as follows.
[0097] (1) GPC measurement The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of the phenolic hydroxyl group-containing resins obtained in the examples and comparative examples were calculated using the following measuring equipment and conditions. "Measuring device" Tosoh Corporation "HLC-8320 GPC" "Measurement conditions" Column: Tosoh Corporation guard column "HXL-L" + Tosoh Corporation "TSK-GEL G2000HXL" + Tosoh Corporation "TSK-GEL G2000HXL" + Tosoh Corporation "TSK-GEL G3000HXL" + Tosoh Corporation "TSK-GEL G4000HXL" Detector: RI (differential refractometer) Data processing: Tosoh Corporation's "GPC Workstation EcoSEC-WorkStation" Measurement conditions: Column temperature 40℃ Developing solvent: Tetrahydrofuran Flow rate 1.0ml / min Standard: In accordance with the measurement manual for the "GPC Workstation EcoSEC-WorkStation," the following monodisperse polystyrene with known molecular weight was used. (Polystyrene used) "A-500" manufactured by Tosoh Corporation "A-1000" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation "F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation "F-40" manufactured by Tosoh Corporation "F-80" manufactured by Tosoh Corporation "F-128" manufactured by Tosoh Corporation Sample: A tetrahydrofuran solution (1.0% by mass, calculated as resin solid content) of the phenolic hydroxyl group-containing resin obtained in Synthesis Example was filtered through a microfilter (50 μl).
[0098] (2) FD-MS measurement The FD-MS spectra of the phenolic hydroxyl group-containing resins obtained in the examples were measured using the following measuring device and conditions. Measurement equipment: JMS-T100GC AccuTOF Measurement conditions Measurement range: m / z=4.00~2000.00 Rate of change: 51.2mA / min Final current value: 45mA Cathode voltage: -10kV Recording interval: 0.07 seconds
[0099] (3) 13 C-NMR measurement Phenolic hydroxyl group-containing resin obtained in Example 13 C-NMR spectra were measured using the following measuring device and conditions. 13 C-NMR: “JNM-ECZ400S” manufactured by JEOL RESONANCE Resonance frequency: 100MHz Number of times: 4000 Solvent: Chloroform-d Sample concentration: 12% by mass Relaxation agent: Chromium(III) acetylacetonate
[0100] <Example 1: Synthesis of phenolic hydroxyl group-containing resin (A-1)> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 100.0 parts by mass of fluorene, 273.4 parts by mass of α,α'-dichloro-p-xylene (hereinafter abbreviated as PXDC), 147.0 parts by mass of phenol, 520.4 parts by mass of toluene, and 520.4 parts by mass of dimethyl sulfoxide (hereinafter abbreviated as DMSO) were charged, and the temperature was raised to 40°C to homogenize. Then, 269.4 parts by mass of 49% by mass of aqueous sodium hydroxide solution was added dropwise while paying attention to heat generation so that the temperature was 60°C or less. After the dropwise addition, the temperature was raised to 60°C, and the reaction was carried out at the same temperature for 8 hours, after which 383.9 parts by mass of water was added, the insoluble salt was dissolved, and the lower layer was removed by liquid separation. Then, the organic layer was neutralized with 6.88 parts by mass of an aqueous 89% by mass phosphoric acid solution, and then washed three times with 383.9 parts by mass of water.
[0101] Next, 283.1 parts by mass of phenol and 10.4 parts by mass of p-toluenesulfonic acid monohydrate were charged, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 4.52 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while charging 812.8 parts by mass of methyl isobutyl ketone, and washed three times at the same temperature with 575.8 parts by mass of water. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, thereby obtaining a phenolic hydroxyl group-containing resin (A-1).
[0102] The GPC chart of the obtained phenolic hydroxyl group-containing resin (A-1) is shown in FIG. 13 The C-NMR chart is shown in Figure 2, and the FD-MS chart is shown in Figure 3. According to the GPC chart of FIG. 1, the Mn of the obtained phenolic hydroxyl group-containing resin (A) was 587, the Mw was 879, and the Mw / Mn was 1.497. 13 It was confirmed from the C-NMR chart that the reaction started from the 9-position of the fluorene, and from the FD-MS chart in Figure 3, m / z 558.3, 754.4, and 826.4, that the obtained phenolic hydroxyl group-containing resin (A) was the phenolic hydroxyl group-containing resin of the present invention. The hydroxyl group equivalent of the obtained phenolic hydroxyl group-containing resin (A-1) was 225g / eq, and the softening point was 56°C.
[0103] <Example 2: Synthesis of phenolic hydroxyl group-containing resin (A-2)> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 100.0 parts by mass of fluorene, 210.6 parts by mass of PXDC, 130.1 parts by mass of orthocresol, 440.7 parts by mass of toluene, and 440.7 parts by mass of DMSO were charged, and the temperature was raised to 40 ° C. to homogenize. Then, 297.7 parts by mass of 49% by mass of sodium hydroxide aqueous solution were added dropwise while paying attention to heat generation so that the temperature was 60 ° C. or less. After the dropwise addition, the temperature was raised to 60 ° C., and the reaction was carried out at the same temperature for 8 hours, after which 424.2 parts by mass of water was added, the insoluble salt was dissolved, and the lower layer was removed by liquid separation. Then, the organic layer was neutralized with 3.97 parts by mass of 89% by mass of phosphoric acid aqueous solution, and then washed three times with 424.2 parts by mass of water.
[0104] Next, 325.3 parts by mass of orthocresol and 8.81 parts by mass of p-toluenesulfonic acid monohydrate were charged, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 3.83 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while charging 661.1 parts by mass of toluene, and washed three times at the same temperature with 424.2 parts by mass of water. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, thereby obtaining a phenolic hydroxyl group-containing resin (A-2).
[0105] The GPC chart of the obtained phenolic hydroxyl group-containing resin (A-2) is shown in FIG. 13 The C-NMR chart is shown in FIG. 5, and the FD-MS chart is shown in FIG. 6. According to the GPC chart in FIG. 4, the Mn of the obtained phenolic hydroxyl group-containing resin (A-2) was 564, the Mw was 742, and the Mw / Mn was 1.315. 13It was confirmed from the C-NMR chart that the reaction started from the 9-position of the fluorene, and from the FD-MS chart in Figure 6, from m / z 586.4, 796.5, and 1064.7, that the obtained phenolic hydroxyl group-containing resin (A-2) was the phenolic hydroxyl group-containing resin of the present invention. The hydroxyl group equivalent of the obtained phenolic hydroxyl group-containing resin (A-2) was 254g / eq, and the softening point was 55°C.
[0106] <Example 3: Synthesis of phenolic hydroxyl group-containing resin (A-3)> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 75.0 parts by mass of fluorene, 158.0 parts by mass of PXDC, 110.3 parts by mass of 2,6-dimethylphenol, 343.2 parts by mass of toluene, and 343.2 parts by mass of DMSO were charged, and the temperature was raised to 40°C to homogenize. Then, 223.3 parts by mass of 49% by mass of aqueous sodium hydroxide solution was added dropwise while paying attention to heat generation so that the temperature was 60°C or less. After the dropwise addition, the temperature was raised to 60°C, and the reaction was carried out at the same temperature for 8 hours, after which 318.2 parts by mass of water was added, the insoluble salt was dissolved, and the lower layer was removed by liquid separation. Then, the organic layer was neutralized with 2.98 parts by mass of an aqueous 89% by mass phosphoric acid solution, and then washed three times with 318.2 parts by mass of water.
[0107] Next, 165.4 parts by mass of 2,6-dimethylphenol and 6.86 parts by mass of p-toluenesulfonic acid monohydrate were charged, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 2.98 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while charging 343.2 parts by mass of toluene, and washed three times at the same temperature with 318.2 parts by mass of water. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, thereby obtaining a phenolic hydroxyl group-containing resin (A-3).
[0108] The GPC chart of the obtained phenolic hydroxyl group-containing resin (A-3) is shown in FIG. 13The C-NMR chart is shown in Figure 8, and the FD-MS chart is shown in Figure 9. According to the GPC chart in Figure 7, the Mn of the obtained phenolic hydroxyl group-containing resin (A-3) is 699, the Mw is 1079, and the Mw / Mn is 1.544. 13 It was confirmed from the C-NMR chart that the reaction started from the 9-position of the fluorene, and from the FD-MS chart in Figure 9, m / z 614.4, 838.5, that the obtained phenolic hydroxyl group-containing resin (A-2) was the phenolic hydroxyl group-containing resin of the present invention. The hydroxyl group equivalent of the obtained phenolic hydroxyl group-containing resin (A-3) was 271 g / eq, and the softening point was 83°C.
[0109] <Example 4: Synthesis of phenolic hydroxyl group-containing resin (A-4)> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 75.0 parts by mass of fluorene, 158.0 parts by mass of PXDC, 130.1 parts by mass of β-naphthol, 363.1 parts by mass of toluene, and 363.1 parts by mass of DMSO were charged, and the temperature was raised to 40°C to homogenize. Then, 223.3 parts by mass of 49% by mass of aqueous sodium hydroxide solution was added dropwise while paying attention to heat generation so that the temperature was 60°C or less. After the dropwise addition, the temperature was raised to 60°C, and the reaction was carried out at the same temperature for 8 hours, after which 318.2 parts by mass of water was added, the insoluble salt was dissolved, and the lower layer was removed by liquid separation. Then, the organic layer was neutralized with 2.98 parts by mass of an aqueous 89% by mass phosphoric acid solution, and then washed three times with 318.2 parts by mass of water.
[0110] Next, 195.2 parts by mass of β-naphthol and 7.26 parts by mass of p-toluenesulfonic acid monohydrate were charged, and the mixture was heated to 160°C while azeotroping the water and the solvent, and reacted at the same temperature for 3 hours. After the reaction was completed, the mixture was cooled, and the organic layer was neutralized with 3.15 parts by mass of a 49% by mass aqueous solution of sodium hydroxide, and cooled to 80°C while charging 544.6 parts by mass of toluene, and washed three times with 435.7 parts by mass of isopropyl alcohol and 318.2 parts by mass of water. The obtained organic layer was heated and distilled under reduced pressure to remove all volatile matter, thereby obtaining a phenolic hydroxyl group-containing resin (A-4).
[0111] The GPC chart of the obtained phenolic hydroxyl group-containing resin (A-4) is shown in FIG. 13 The C-NMR chart is shown in Fig. 11, and the FD-MS chart is shown in Fig. 12. According to the GPC chart in Fig. 9, the Mn of the obtained phenolic hydroxyl group-containing resin (A-4) was 366, the Mw was 746, and the Mw / Mn was 2.037. 13 The C-NMR chart confirmed that the reaction started from the 9-position of fluorene, and the FD-MS chart in Figure 6 confirmed that the resulting phenolic hydroxyl group-containing resin (A-2) was the phenolic hydroxyl group-containing resin of the present invention from m / z 658.4, 904.5, and 1172.7. The hydroxyl group equivalent of the resulting phenolic hydroxyl group-containing resin (A-3) was 337g / eq, and the softening point was 81°C.
[0112] A cured product was prepared from the synthesized phenolic hydroxyl group-containing resin, and the physical properties were evaluated as follows. The results are shown in Table 1. (1) Measurement of dielectric constant and dielectric tangent In accordance with JIS-C-6481, the dielectric constant and dielectric loss tangent of the test pieces at 1 GHz and 10 GHz were measured using an impedance material analyzer "HP4291B" manufactured by Agilent Technologies Inc. after they had been dried and then stored indoors at 23°C and 50% humidity for 24 hours. (2) Measurement method for hot elastic modulus The storage modulus at 260° C. was measured as the hot modulus using a viscoelasticity measuring device (DMA: solid viscoelasticity measuring device RSAII manufactured by Rheometrics, rectangular tension method; frequency 1 Hz, heating rate 3° C. / min).
[0113] <Examples 5 to 8 and Comparative Example 1> (1) Preparation of test specimens In the mass ratio shown in Table 1, cresol novolak epoxy resin (DIC Corporation, EPICLON N-655-EXP-S, epoxy equivalent 204 g / eq) and the phenolic hydroxyl group-containing resin (A) of Example 1, the phenolic hydroxyl group-containing resin (B) of Example 2, or the biphenyl aralkyl phenol resin (Meiwa Kasei Co., Ltd., MEHC-7851SS, hydroxyl group equivalent: 212 g / eq) were heated and melted at 130 to 150 ° C., homogenized, and then a catalyst (triphenylphosphine, hereinafter abbreviated as TPP) was added to obtain a resin composition. The obtained resin composition was pressed in a 150 ° C. press for 10 minutes, cured and molded, and then further heated at 175 ° C. for 5 hours to obtain a test piece. The physical properties of the obtained test piece were measured. The results are shown in Table 1.
[0114] [Table 1]
[0115] From the results shown in Table 1, it can be seen that excellent dielectric properties (low dielectric constant and low dielectric loss tangent) can be obtained and the elastic modulus can be reduced in the high temperature range by using the phenolic hydroxyl group-containing resins of Examples 1 to 4. It can be seen that the phenolic hydroxyl group-containing resin of Example 2 is also excellent in the elastic modulus when heated. [Industrial Applicability]
[0116] According to the present invention, it is possible to provide a phenolic hydroxyl group-containing resin that can achieve both excellent dielectric properties (low dielectric constant and low dielectric dissipation factor) and a low modulus of elasticity at high temperatures, and also to provide a curable composition containing the phenolic hydroxyl group-containing resin and a cured product thereof. Furthermore, by using the curable composition or the cured product thereof, it is possible to provide a prepreg, a circuit board, a build-up film, a semiconductor encapsulant, and a semiconductor device that can achieve both excellent dielectric properties (low dielectric constant and low dielectric dissipation factor) and a low modulus of elasticity at high temperatures.
Claims
1. A phenolic hydroxyl group-containing resin which is a reaction product of a fluorene compound (not having a substituent at the 9-position), a phenolic hydroxyl group-containing compound, and a compound represented by general formula (1): 【Chemistry 1】 (where: Ar is an aromatic ring group which may have a substituent, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, X is a leaving group.
2. 2. The phenolic hydroxyl group-containing resin according to claim 1, wherein the fluorene compound is present in an amount of 0.01 to 0.99 moles per mole of the compound represented by the general formula (1).
3. A phenolic hydroxyl group-containing resin represented by general formula (5): 【Chemistry 2】 (where: Z is independently a group represented by general formula (2A): 【Chemistry 3】 or a structural unit represented by general formula (3A): 【Chemistry 4】 It is a structural unit represented by Z' is independently a group represented by general formula (2A'): 【Chemistry 5】 or a structural unit represented by general formula (3A'): 【Chemistry 6】 It is a structural unit represented by Each Ar is independently an aromatic ring group which may have a substituent, R 1 each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 4 carbon atoms, R 2 each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m is independently an integer from 0 to 4; R 3 are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3 may form a ring together with the carbon atom to which they are attached, n is independently an integer from 0 to 3; p is an average value greater than 0; R 2’ each independently represents an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, m' is independently an integer from 0 to 4; R 3’ are each independently an aliphatic hydrocarbon group, an aryl group, an arylalkyl group, an alkoxy group, or a halogen atom, or two R 3’ may form a ring together with the carbon atom to which they are attached, Each n' is independently an integer from 0 to 4; However, the resin contains a structural unit represented by general formula (2A) and / or general formula (2A') and a structural unit represented by general formula (3A) and / or general formula (3A').
4. The phenolic hydroxyl group-containing resin according to claim 3, comprising at least one of a compound represented by general formula (5-1) and a compound represented by general formula (5-2): 【Chemistry 7】 (where: Ar, Z, R 1 , R 3’ and n' have the same meaning as in claim 3.
5. 4. The phenolic hydroxyl group-containing resin according to claim 1, wherein the hydroxyl group equivalent is 100 to 2000 g / eq.
6. 4. The phenolic hydroxyl group-containing resin according to claim 1, having a number average molecular weight of 100 to 10,000.
7. A curable composition comprising the phenolic hydroxyl group-containing resin according to claim 1 or 3 and a curing agent.
8. A cured product of the curable composition according to claim 7.
9. A prepreg comprising a reinforcing substrate and a semi-cured product of the curable composition according to claim 7 impregnated into the reinforcing substrate.
10. A circuit board which is a laminate of the prepreg according to claim 9 and copper foil.
11. A build-up film comprising the curable composition according to claim 7.
12. A semiconductor encapsulant comprising the curable composition according to claim 7.
13. A semiconductor device comprising the cured product of the semiconductor encapsulation material according to claim 12.
Citation Information
Patent Citations
Phenolaralkyl resin, epoxy resin composition and cured material thereof
JP2003113225A
Phenolic resin, epoxy resin and method for preparation thereof, and resin composition
JP2003301031A
Phenolic compound
JP2006342176A
Epoxy resin composition and cured product thereof
JP2007308570A
Phenolaralkyl resin, epoxy resin composition and cured material thereof
JP2010229422A