Metal carbide-coating carbon material
A metal carbide-coated carbon material with controlled impurity concentrations and a tantalum carbide coating addresses gas generation issues in high-temperature semiconductor manufacturing, improving yield and reducing costs.
Patent Information
- Application Number
- JP2023075400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2043-05-01
AI Technical Summary
Existing metal carbide-coated carbon materials used in wide band gap semiconductor manufacturing fail to adequately suppress gas generation in high-temperature environments, leading to decreased yield and increased costs.
A metal carbide-coated carbon material with controlled concentrations of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur, within specific ranges, and a tantalum carbide coating film, applied via chemical vapor deposition, to minimize gas generation.
The solution effectively suppresses gas generation in high-temperature environments, enhancing the yield and reducing manufacturing costs of wide band gap semiconductor wafers by maintaining the integrity of the carbon base material.
Smart Images

Figure 2024160432000003 
Figure 2024160432000004 
Figure 2024160432000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal carbide-coated carbon material in which the surface of a carbon substrate is coated with a metal carbide coating film. [Background technology]
[0002] Wide band gap semiconductors such as SiC and GaN have high dielectric breakdown field strength and excellent heat resistance as well as low loss compared to Si semiconductors, and are therefore suitable for power semiconductors. On the other hand, the manufacturing cost of wide band gap semiconductor wafers is high compared to Si semiconductors. For this reason, there is a demand for reducing the manufacturing cost of wide band gap semiconductor wafers. The costs involved in the crystal growth process and epitaxial growth process of wide band gap semiconductors have a significant impact on the manufacturing cost of wide band gap semiconductor wafers, and there is a need to improve the yield of these processes in order to reduce the manufacturing cost of wide band gap semiconductor wafers.
[0003] There are several factors that can reduce the yield in the crystal growth process and epitaxial growth process of wide band gap semiconductors, one of which is the generation of gas from the carbon substrate used as the crucible, guide member, or susceptor. Gas is generated by sublimation of the carbon substrate itself or desorption of hydrocarbon gases adsorbed on the carbon substrate, and it is thought that the yield is reduced because the crystal orientation changes during crystal growth due to the gas.
[0004] As a countermeasure, a method of coating the carbon substrate with a metal carbide film can be mentioned. Metal carbides such as tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide have high melting points and excellent chemical stability, strength, toughness, and corrosion resistance. Therefore, by coating the carbon substrate with a metal carbide, the heat resistance, chemical stability, strength, toughness, and corrosion resistance of the carbon substrate can be improved, and gas generation can be suppressed.
[0005] It is also known that gas generation can be suppressed by subjecting the carbon substrate itself to high-purity treatment. In fact, Patent Document 1 uses a carbon substrate that has been highly purified, and Non-Patent Document 1 shows that the temperature-programmed desorbed gas from the carbon substrate can be reduced by subjecting the carbon substrate to high-purity treatment. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5502721 [Non-patent literature]
[0007] [Non-Patent Document 1] Toyo Tanso Co., Ltd. Special graphite products catalog, Internet: https: / / www.toyotanso.co.jp / Products / download / Summary of the Invention [Problem to be solved by the invention]
[0008] However, when the carbon substrate described in Patent Document 1 and the carbon substrate described in Non-Patent Document 1 were coated with a metal carbide film and used in a manufacturing apparatus for a wide band gap semiconductor, gas generation was not sufficiently suppressed in the crystal growth step and epitaxial growth step.
[0009] Therefore, an object of the present invention is to provide a metal carbide-coated carbon material that can suppress gas generation in a high-temperature environment. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that by setting the total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium and sulfur in the carbonized substrate of the metal carbide-coated carbon material to 10 ppm by mass or more and 10,000 ppm by mass or less, gas generation from the metal carbide-coated carbon material in a high-temperature environment can be suppressed, and have completed the present invention. The gist of the present invention is as follows. [1] A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film that coats at least a portion of the carbon substrate, the metal carbide constituting the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide; The carbon substrate contains at least one element selected from the group consisting of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur; The metal carbide-coated carbon material has a total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium and sulfur in the carbon substrate of 10 ppm by mass or more and 10,000 ppm by mass or less. [2] The metal carbide-coated carbon material according to the above [1], wherein the concentration of iron in the carbon substrate is 1 ppm by mass or more and 10,000 ppm by mass or less. [3] The metal carbide-coated carbon material according to the above [1] or [2], wherein the titanium concentration in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [4] The metal carbide-coated carbon material according to any one of the above [1] to [3], wherein the concentration of magnesium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [5] The metal carbide-coated carbon material according to any one of the above [1] to [4], wherein the concentration of silicon in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [6] The metal carbide-coated carbon material according to any one of the above [1] to [5], wherein the concentration of calcium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [7] The metal carbide-coated carbon material according to any one of the above [1] to [6], wherein the concentration of vanadium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [8] The metal carbide-coated carbon material according to any one of the above [1] to [7], wherein the sodium concentration in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less. [9] The metal carbide-coated carbon material according to any one of the above [1] to [8], wherein the concentration of potassium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
[10] The metal carbide-coated carbon material according to any one of the above [1] to [9], wherein the concentration of sulfur in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
[11] The metal carbide coated carbon material according to any one of the above [1] to
[10] , wherein the metal carbide coating film has a thickness of 10 μm or more and 100 μm or less.
[12] The metal carbide-coated carbon material according to any one of the above [1] to
[11] , wherein the metal carbide coating film has a surface having an arithmetic mean roughness Ra of 0.1 μm or more and 9.5 μm or less.
[13] The metal carbide coated carbon material according to any one of the above [1] to
[12] , wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less.
[14] The metal carbide coated carbon material according to any one of the above [1] to
[13] , wherein the metal carbide constituting the metal carbide coating film is tantalum carbide. Effect of the Invention
[0011] According to the present invention, it is possible to provide a metal carbide-coated carbon material capable of suppressing gas generation in a high-temperature environment. [Brief description of the drawings]
[0012] [Figure 1]1 is a schematic diagram of an external heat type reduced pressure CVD apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a set for a corrosion resistance test method according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram for explaining a method for measuring the adhesion strength of a metal carbide coating film according to the present embodiment. [Figure 4] 1 shows the results of a corrosion resistance test of the tantalum carbide-coated carbon materials of Examples 1 to 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The metal carbide-coated carbon material of the present invention will be described using a tantalum carbide-coated carbon material as an example.
[0014] [Tantalum carbide coated carbon material] A tantalum carbide-coated carbon material according to one embodiment of the present invention comprises a carbon substrate containing carbon as a main component, and a tantalum carbide coating film coating at least a portion of the carbon substrate, wherein the carbon substrate contains at least one element selected from the group consisting of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur, and the total concentration of the aluminum concentration, iron concentration, magnesium concentration, titanium concentration, silicon concentration, calcium concentration, vanadium concentration, nickel concentration, sodium concentration, potassium concentration, and sulfur concentration in the carbon substrate is 10 ppm by mass or more and 10,000 ppm by mass or less.
[0015] (Carbon substrate) The carbon substrate in the tantalum carbide-coated carbon material according to one embodiment of the present invention is a substrate mainly composed of carbon. The carbon substrate may further contain chlorine. Examples of the carbon substrate material include isotropic graphite, extruded graphite, pyrolytic graphite, and carbon fiber-reinforced carbon composite material (C / C composite). The shape and characteristics of the carbon substrate are not particularly limited, and the carbon substrate may be processed into any shape depending on the application.
[0016] <Total concentration of elements> The carbon substrate in the tantalum carbide-coated carbon material according to one embodiment of the present invention contains at least one element selected from the group consisting of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur. The total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur in the carbon substrate is 10 mass ppm or more and 10,000 mass ppm or less. If the total concentration of the above elements is greater than 10,000 mass ppm, the amount of gas generated from the carbon substrate in a high-temperature environment increases, and as a result, when the tantalum carbide-coated carbon material using the carbon substrate is used in a manufacturing device for a wide band gap semiconductor, the yield of the wide band gap semiconductor may decrease. In addition, even if the total concentration of the above elements is less than 10 mass ppm, the amount of gas generated from the carbon substrate in a high-temperature environment cannot be reduced much compared to when the total concentration of the above elements is 10 mass ppm. That is, the increase in the manufacturing cost of the carbon substrate caused by making the total concentration of the above elements smaller than 10 mass ppm may result in insufficient cost reduction in the manufacturing of the wide band gap semiconductor wafer. From this viewpoint, the total concentration of the above elements is preferably 15 mass ppm or more and 5000 mass ppm or less, more preferably 20 mass ppm or more and 1000 mass ppm or less. The concentration of the above elements in the carbon substrate can be measured by the method described in the Examples below. The total concentration of the above elements can be adjusted, for example, by heating the carbon substrate in halogen gas at about 2000°C to volatilize the above elements in the carbon substrate as low-boiling point halides. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Iron and Steel, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0017] <Iron concentration> The iron concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 1 mass ppm or more and 10000 mass ppm or less. When the iron concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the iron concentration is 1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the iron concentration can be suppressed. From this viewpoint, the iron concentration is more preferably 1 mass ppm or more and 4000 mass ppm or less, even more preferably 1 mass ppm or more and 1000 mass ppm or less, even more preferably 1 mass ppm or more and 100 mass ppm or less, and even more preferably 1 mass ppm or more and 50 mass ppm or less. The iron concentration in the carbon substrate can be measured by the method described in the Examples below. In addition, the iron concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000 ° C. to volatilize the iron in the carbon substrate as a low boiling point halide. Specifically, a method of removing impurities using chlorine is described in Reference Document 1 (Nagata, Kazuhiro, Tetsu-to-Haganen, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0018] <Titanium concentration> The titanium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less.When the titanium concentration is 10000 mass ppm or less, it can further suppress the generation of gas from the carbon substrate in a high temperature environment.In addition, when the titanium concentration is 0.1 mass ppm or more, it can suppress the increase in the cost of the carbon substrate caused by reducing the titanium concentration. From this viewpoint, the titanium concentration is more preferably 0.1 mass ppm or more and 2000 mass ppm or less, even more preferably 0.1 mass ppm or more and 1000 mass ppm or less, even more preferably 0.1 mass ppm or more and 500 mass ppm or less, even more preferably 0.1 mass ppm or more and 100 mass ppm or less, even more preferably 0.1 mass ppm or more and 50 mass ppm or less, even more preferably 0.1 mass ppm or more and 10 mass ppm or less, even more preferably 0.1 mass ppm or more and 5 mass ppm or less, even more preferably 0.1 mass ppm or more and 3 mass ppm or less. The titanium concentration in the carbon substrate can be measured by the method described in the examples below. The titanium concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000 ° C. to volatilize the titanium in the carbon substrate as a low-boiling point halide. Specifically, a method of removing impurities using chlorine is described in Reference Document 1 (Nagata, Kazuhiro, Tetsu-to-Haganen, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0019] <Magnesium concentration> The magnesium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the magnesium concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the magnesium concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the magnesium concentration can be suppressed. From this viewpoint, the magnesium concentration is more preferably 0.1 mass ppm or more and 100 mass ppm or less, even more preferably 0.1 mass ppm or more and 50 mass ppm or less, even more preferably 0.1 mass ppm or more and 20 mass ppm or less, even more preferably 0.1 mass ppm or more and 10 mass ppm or less, even more preferably 0.1 mass ppm or more and 5 mass ppm or less, and even more preferably 0.1 mass ppm or more and 2 mass ppm or less. The magnesium concentration in the carbon substrate can be measured by the method described in the examples below. The magnesium concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000° C. to volatilize the magnesium in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Haganen, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0020] <Silicon concentration> The silicon concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the silicon concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the silicon concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the silicon concentration can be suppressed. From this viewpoint, the silicon concentration is more preferably 0.1 mass ppm or more and 1000 mass ppm or less, still more preferably 0.1 mass ppm or more and 500 mass ppm or less, still more preferably 0.1 mass ppm or more and 200 mass ppm or less, still more preferably 0.1 mass ppm or more and 100 mass ppm or less, still more preferably 0.1 mass ppm or more and 50 mass ppm or less, and still more preferably 0.1 mass ppm or more and 30 mass ppm or less. The silicon concentration in the carbon substrate can be measured by the method described in the examples below. The silicon concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000° C. to volatilize the silicon in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Hagane, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0021] <Calcium concentration> The calcium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the calcium concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the calcium concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the calcium concentration can be suppressed. From this viewpoint, the calcium concentration is more preferably 0.1 mass ppm or more and 2000 mass ppm or less, even more preferably 0.1 mass ppm or more and 1000 mass ppm or less, even more preferably 0.1 mass ppm or more and 100 mass ppm or less, even more preferably 0.1 mass ppm or more and 50 mass ppm or less, and even more preferably 0.1 mass ppm or more and 10 mass ppm or less. The calcium concentration in the carbon substrate can be measured by the method described in the examples below. The calcium concentration can be adjusted, for example, by heating the carbon substrate in halogen gas at about 2000° C. to volatilize calcium in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Haganen, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0022] <Vanadium concentration> The vanadium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the vanadium concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the vanadium concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the vanadium concentration can be suppressed. From this viewpoint, the vanadium concentration is more preferably 0.1 mass ppm or more and 1000 mass ppm or less, still more preferably 0.1 mass ppm or more and 500 mass ppm or less, still more preferably 0.1 mass ppm or more and 100 mass ppm or less, still more preferably 0.1 mass ppm or more and 50 mass ppm or less, still more preferably 0.1 mass ppm or more and 10 mass ppm or less, and still more preferably 0.1 mass ppm or more and 5 mass ppm or less. The vanadium concentration in the carbon substrate can be measured by the method described in the examples below. The vanadium concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000° C. to volatilize the vanadium in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Hagane, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0023] <Sodium concentration> The sodium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the sodium concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the sodium concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the sodium concentration can be suppressed. From this viewpoint, the sodium concentration is more preferably 0.1 mass ppm or more and 100 mass ppm or less, even more preferably 0.1 mass ppm or more and 50 mass ppm or less, even more preferably 0.1 mass ppm or more and 20 mass ppm or less, and even more preferably 0.1 mass ppm or more and 5 mass ppm or less. The sodium concentration in the carbon substrate can be measured by the method described in the Examples below. In addition, the sodium concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000 ° C. to volatilize the sodium in the carbon substrate as a low boiling point halide. Specifically, a method of removing impurities using chlorine is described in Reference Document 1 (Nagata, Kazuhiro, Tetsu-to-Haganen, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0024] <Potassium concentration> The potassium concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the potassium concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the potassium concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the potassium concentration can be suppressed. From this viewpoint, the potassium concentration is more preferably 0.1 mass ppm or more and 100 mass ppm or less, still more preferably 0.1 mass ppm or more and 50 mass ppm or less, still more preferably 0.1 mass ppm or more and 20 mass ppm or less, still more preferably 0.1 mass ppm or more and 10 mass ppm or less, still more preferably 0.1 mass ppm or more and 5 mass ppm or less, still more preferably 0.1 mass ppm or more and 2 mass ppm or less, still more preferably 0.1 mass ppm or more and 1 mass ppm or less. The potassium concentration in the carbon substrate can be measured by the method described in the examples below. The potassium concentration can be adjusted, for example, by heating the carbon substrate in halogen gas at about 2000° C. to volatilize the potassium in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Iron and Steel, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0025] <Sulfur concentration> The sulfur concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the sulfur concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the sulfur concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the sulfur concentration can be suppressed. From this viewpoint, the sulfur concentration is more preferably 0.1 mass ppm or more and 100 mass ppm or less, still more preferably 0.1 mass ppm or more and 50 mass ppm or less, still more preferably 0.1 mass ppm or more and 20 mass ppm or less, still more preferably 0.1 mass ppm or more and 10 mass ppm or less, still more preferably 0.1 mass ppm or more and 5 mass ppm or less, still more preferably 0.1 mass ppm or more and 2 mass ppm or less, still more preferably 0.1 mass ppm or more and 1 mass ppm or less. The sulfur concentration in the carbon substrate can be measured by the method described in the examples below. The sulfur concentration can be adjusted, for example, by hydrogenating the carbon substrate and volatilizing the sulfur in the carbon substrate as hydrogen sulfide.
[0026] <Aluminum concentration> The aluminum concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the aluminum concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the aluminum concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the aluminum concentration can be suppressed. From this viewpoint, the aluminum concentration is more preferably 0.1 mass ppm or more and 1000 mass ppm or less, even more preferably 0.1 mass ppm or more and 100 ppm or less, even more preferably 0.1 mass ppm or more and 50 ppm or less, even more preferably 0.1 mass ppm or more and 20 mass ppm or less, and even more preferably 0.1 mass ppm or more and 5 ppm or less. The aluminum concentration in the carbon substrate can be measured by the method described in the examples below. The aluminum concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000° C. to volatilize the aluminum in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Hagane, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0027] <Nickel concentration> The nickel concentration in the carbon substrate in the tantalum carbide coated carbon material of one embodiment of the present invention is preferably 0.1 mass ppm or more and 10000 mass ppm or less. When the nickel concentration is 10000 mass ppm or less, the generation of gas from the carbon substrate in a high temperature environment can be further suppressed. In addition, when the nickel concentration is 0.1 mass ppm or more, the increase in the cost of the carbon substrate caused by reducing the nickel concentration can be suppressed. From this viewpoint, the nickel concentration is more preferably 0.1 mass ppm or more and 1000 mass ppm or less, even more preferably 0.1 mass ppm or more and 100 ppm or less, even more preferably 0.1 mass ppm or more and 50 ppm or less, even more preferably 0.1 mass ppm or more and 20 mass ppm or less, and even more preferably 0.1 mass ppm or more and 5 ppm or less. The nickel concentration in the carbon substrate can be measured by the method described in the examples below. The nickel concentration can be adjusted, for example, by heating the carbon substrate in a halogen gas at about 2000° C. to volatilize the nickel in the carbon substrate as a low-boiling halide. Specifically, a method of removing impurities using chlorine is described in Reference 1 (Kazuhiro Nagata, Tetsu-to-Hagane, Vol. 73, No. 9, pp. 1077-1081 (1987)).
[0028] <Arithmetic surface roughness Ra> The arithmetic mean roughness Ra of the surface of the carbon substrate affects the semiconductor single crystal growth and epitaxial growth. The larger the arithmetic mean roughness Ra of the surface of the carbon substrate, the greater the peel strength between the carbon substrate and the tantalum carbide coating film, which is preferable. On the other hand, if the arithmetic mean roughness Ra of the surface of the carbon substrate is too large, the specific surface area increases, which may cause cracks and peeling, and the product life may be shortened when used as a member for semiconductor single crystal growth and epitaxial growth. Therefore, from the viewpoint of the product life of the tantalum carbide-coated carbon material, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 10.0 μm or less. Considering the occurrence rate of cracks and peeling between the carbon substrate and the tantalum carbide coating film, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 0.1 μm or more and 10.0 μm or less, and more preferably 2.0 μm or more and 6.0 μm or less. In this way, the peel strength between the carbon substrate and the tantalum carbide coating film can be increased, and the product life can be extended when used as a member for semiconductor single crystal growth and epitaxial growth. The arithmetic mean roughness Ra of the surface of the carbon substrate is a value measured based on JIS B 0633:2001 (ISO 4288:1996).
[0029] <Linear thermal expansion coefficient> The linear thermal expansion coefficient of the carbon substrate is preferably 3.5×10 -6 / ℃ or more 8.2×10 -6 / ℃ or less. The linear thermal expansion coefficient of the carbon substrate is 3.5×10 -6 / ℃ or more 8.2×10 -6 When the linear thermal expansion coefficient of the carbon substrate is less than 0.5.0×10 / °C, the occurrence of microcracks in the tantalum carbide coating film can be further suppressed. From this viewpoint, the linear thermal expansion coefficient of the carbon substrate is more preferably less than 0.5.0×10 / °C. -6 ~7.5×10 -6 / ℃. The linear thermal expansion coefficient of the tantalum carbide coating is approximately 6.3×10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate can be measured in accordance with JIS R 1618.
[0030] (Tantalum carbide coating) The tantalum carbide coating film is a film mainly composed of tantalum carbide. The tantalum carbide coating film may cover a part of the carbon substrate, or may cover the entire carbon substrate. The tantalum carbide coating film may contain a small amount of atoms other than carbon and tantalum, as long as the effect of the present invention is not impaired. For example, the tantalum carbide coating film may contain impurity elements or doping elements other than carbon and tantalum at a concentration of 10000 mass ppm or less.
[0031] <Film thickness> If the thickness of the tantalum carbide coating film is too thin, the gas generated from the carbon substrate may pass through the tantalum carbide coating film and adversely affect the semiconductor single crystal. On the other hand, if the thickness of the tantalum carbide coating film is too thick, the film formation time is extended, and the film formation cost increases. Considering these factors together, the thickness of the metal carbide coating film is preferably 10 μm or more and 100 μm or less, and more preferably 20 μm or more and 50 μm or less. The thickness of the tantalum carbide coating film is a value measured based on the cross-sectional observation of the tantalum carbide coating film by a scanning electron microscope (SEM). Specifically, the thickness of the cross-section of the tantalum carbide coating film was measured at five arbitrary points from the image of the cross-section of the tantalum carbide coating film taken by a scanning electron microscope (SEM), and the average value was taken as the thickness of the tantalum carbide coating film.
[0032] <Arithmetic surface roughness Ra> The arithmetic mean roughness Ra of the surface of the tantalum carbide coating film is preferably 0.1 μm or more and 9.5 μm or less, and more preferably 2.0 μm or more and 5.5 μm or less. If the value of the arithmetic mean roughness Ra of the surface of the tantalum carbide coating film is large, it may cause cracks and peeling as in the case of the carbon substrate, and may shorten the product life when used as a member for semiconductor single crystal growth and epitaxial growth. The arithmetic mean roughness Ra of the surface of the tantalum carbide coating film immediately after film formation varies depending on the arithmetic mean roughness Ra of the surface of the carbon substrate, and tends to be slightly smaller than the arithmetic mean roughness Ra of the carbon substrate surface. The arithmetic mean roughness Ra of the surface of the tantalum carbide coating film can also be controlled by performing polishing, etc., but since this increases the number of manufacturing steps, it is preferable to select the arithmetic mean roughness Ra of the surface of the carbon substrate according to the desired arithmetic mean roughness Ra of the surface of the tantalum carbide coating film. The arithmetic mean roughness Ra here is a value measured based on JIS B0633:2001 (ISO 4288:1996).
[0033] <Method of manufacturing tantalum carbide coated carbon material> The tantalum carbide coated carbon material according to one embodiment of the present invention can be produced by forming a tantalum carbide layer on the surface of a carbon substrate. The tantalum carbide coating film can be formed on the surface of the carbon substrate by, for example, a chemical vapor deposition (CVD) method, a sintering method, a carbonization method, or the like. Among these, the CVD method is preferred as a method for forming a tantalum carbide coating film, since it can form a uniform and dense tantalum carbide coating film.
[0034] Further, the CVD method includes a thermal CVD method, a photo-CVD method, a plasma CVD method, and the like, and for example, a thermal CVD method can be used to form a tantalum carbide layer. The thermal CVD method has advantages such as a relatively simple apparatus configuration and no damage to the carbon substrate by plasma. For example, an externally heated low-pressure CVD apparatus 10 as shown in FIG. 1 can be used to form a tantalum carbide coating film by the thermal CVD method. In the externally heated low-pressure CVD apparatus 10, a carbon substrate 14 is supported by a support means 15 in a reaction chamber 12 equipped with a heater 13, a raw material supply unit 16, an exhaust unit 17, and the like.
[0035] A method for producing a tantalum carbide-coated carbon material according to one embodiment of the present invention will be described with reference to FIG. First, the carbon substrate 14 is placed in the reaction chamber 12 of the externally heated low-pressure CVD apparatus 10. The carbon substrate 14 is supported by a supporting means 15 having three supporting portions each having a pointed tip.
[0036] Next, the reaction chamber 12 is heated. For example, the reaction chamber 12 is heated under conditions of an atmospheric pressure of 10 to 1000 Pa and a temperature of 800 to 2200°C.
[0037] Next, a tantalum carbide coating film is formed on the surface of the carbon substrate 14. As a raw material gas, methane (CH 4 ) and hydrogen (H 2 ) gas and tantalum pentachloride (TaCl 5 ) and a tantalum halide gas such as tantalum carbide are supplied to the reaction chamber 12. The tantalum halide gas can be generated, for example, by a method of heating and vaporizing a tantalum halide, or a method of reacting tantalum metal with a halogen gas. Then, the raw material gas supplied from the raw material supply unit 16 is subjected to a thermal CVD reaction at a high temperature and reduced pressure of a temperature of 800 to 2200°C and a pressure of 1 to 1000 Pa, to form a tantalum carbide coating film on the carbon substrate 14.
[0038] The tantalum carbide-coated carbon material according to the embodiment of the present invention is an example of the metal carbide-coated carbon material according to the present invention, and the metal carbide-coated carbon material according to the present invention is not limited to the tantalum carbide-coated carbon material according to the embodiment of the present invention. In the metal carbide-coated carbon material according to the present invention, the metal carbide constituting the metal carbide coating film that coats the carbon substrate is not limited to tantalum carbide. For example, carbides such as niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide can be used as the metal carbide constituting the metal carbide coating film that coats the carbon substrate. In addition, a combination of two or more metal carbides selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide may be used as the metal carbide constituting the metal carbide coating film that coats the carbon substrate. Among tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide, tantalum carbide is preferred because it has the highest melting point and is excellent in chemical stability, strength and corrosion resistance. EXAMPLES
[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0040] The metal carbide coated carbon materials of Examples 1 to 14 and Comparative Examples 1 to 4 were produced as follows. Example 1 First, isotropic graphite doped with aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared. The isotropic graphite was processed into a cylindrical shape with an outer diameter of 40 mm, an inner diameter of 30 mm, and a height of 30 mm, which was used as the carbon substrate 14. The arithmetic mean roughness Ra of the surface of this carbon substrate was 6.0 μm, and the linear thermal expansion coefficient of the carbon substrate 14 was 7.0×10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate was measured using a thermomechanical analyzer (TMA7300) manufactured by Hitachi High-Tech Corporation, and the thermal expansion coefficient in the temperature range from 200°C to 1200°C was used.
[0041] Next, as shown in Fig. 1, the carbon substrate 14 was placed in the reaction chamber 12 of the externally heated reduced pressure CVD apparatus 10. The carbon substrate 14 was supported by a support means 15 having three supporting parts each having a pointed tip. At this time, the tips of the supporting parts were in contact with the outer surface of the carbon substrate 14 in the case of a truncated cone-shaped carbon substrate 14, the outer surface of the carbon substrate 14 in the case of a bottomed cylindrical shape, the lower surface in the case of a disk shape, and the outer surface in the case of a cylindrical shape.
[0042] Next, methane (CH 4 ) gas at a flow rate of 0.25 SLM as the carrier gas, argon (Ar) gas at a flow rate of 1.0 SLM, and hydrogen (H 2 Tantalum pentachloride (TaCl) gas was heated to a temperature of 220°C at a flow rate of 0.125 SLM and vaporized. 5 ) were supplied at a flow rate of 0.25 SLM and reacted under conditions of an atmospheric pressure of 100 Pa and a temperature of 1250° C. inside the reaction chamber 12 to form a tantalum carbide coating film on the entire surface of the carbon substrate 14.
[0043] The carbon substrate 14 coated with the tantalum carbide coating film was removed from the reaction chamber 12, completing a cylinder made of a tantalum carbide-coated carbon material.
[0044] (Examples 2 to 5) Isotropic graphite with different doping amounts of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared. Except for that, a cylinder was produced in the same manner as in Example 1, and the evaluation was performed.
[0045] Example 6 Hydrogen (H 2 ) gas flow rate to 0.15 SLM, and tantalum pentachloride (TaCl 5 A cylinder was produced in the same manner as in Example 1, except that the flow rate of the gaseous phase oxidizer 10) was changed to 0.3 SLM and the film formation time was shortened to a film thickness of 10 μm, and then the cylinder was evaluated.
[0046] Example 7 Hydrogen (H 2A cylinder was produced in the same manner as in Example 1, except that the flow rate of the SiO 2 gas was changed to 0.15 SLM and the film formation time was extended to a film thickness of 50 μm, and then the cylinder was evaluated.
[0047] Example 8 A cylinder was produced in the same manner as in Example 1, except that the surface of the carbon substrate 14 was polished to have an arithmetic mean roughness Ra of the surface of the carbon substrate 14 of 0.1 μm, and the cylinder was evaluated.
[0048] Example 9 A cylinder was produced in the same manner as in Example 1, except that the surface of the carbon substrate 14 was subjected to sandblasting treatment by projecting an abrasive onto the surface thereof, and the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was set to 10 μm, and the cylinder was evaluated.
[0049] Example 10 Metal chlorides are tantalum pentachloride (TaCl 5 ) to niobium pentachloride (NbCl 5 ) and supplied at a flow rate of 0.25 SLM, a cylinder was produced in the same manner as in Example 1, and the evaluation was carried out.
[0050] Example 11 Metal chlorides are tantalum pentachloride (TaCl 5 ) to hafnium tetrachloride (HfCl 4 ) and supplied at a flow rate of 0.25 SLM, a cylinder was produced in the same manner as in Example 1, and the evaluation was carried out.
[0051] Example 12 Metal chlorides are tantalum pentachloride (TaCl 5 ) to zirconium tetrachloride (ZrCl 4 ) and supplied at a flow rate of 0.25 SLM, a cylinder was produced in the same manner as in Example 1, and the evaluation was carried out.
[0052] (Example 13) Metal chlorides are tantalum pentachloride (TaCl 5 ) to tungsten pentachloride (WCl 5) and supplied at a flow rate of 0.25 SLM, a cylinder was produced in the same manner as in Example 1, and the evaluation was carried out.
[0053] Example 14 Tantalum pentachloride (TaCl 5 ) and niobium pentachloride (NbCl 5 ) mixture (TaCl 5 :NbCl 5 A cylinder was produced in the same manner as in Example 1, except that the mixture was supplied with 0.25 SLM of toluene (O2=100:1), and the evaluation was carried out.
[0054] Comparative Example 1 Isotropic graphite with different doping amounts of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared and hydrogen (H 2 ) gas flow rate to 0 SLM, and tantalum pentachloride (TaCl 5 A cylinder was produced in the same manner as in Example 1, except that the flow rate of the liquid suction was changed to 0.5 SLM, and the cylinder was evaluated.
[0055] Comparative Example 2 Isotropic graphite with different doping amounts of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared, and a cylinder was produced in the same manner as in Example 1, except that the film formation time was shortened and the film thickness of the tantalum carbide coating film was changed to 2 μm, and then the cylinder was evaluated.
[0056] Comparative Example 3 Isotropic graphite with different doping amounts of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared, and a cylinder was produced in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was set to 32 μm, and the evaluation was performed. The results are shown in Table 1.
[0057] Comparative Example 4 Isotropic graphite with different doping amounts of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur was prepared, and a cylinder was produced in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon substrate 14 was set to 0.05 μm, and the evaluation was performed. The results are shown in Table 1.
[0058] The cylinders of Examples 1 to 14 and Comparative Examples 1 to 4 were subjected to the following evaluations. [Thickness of metal carbide coating] The thickness of the metal carbide coating film was measured by observing the cross section of the metal carbide coating film using a scanning electron microscope (SEM).
[0059] [Arithmetic mean surface roughness Ra] Using a Surftest SJ-210 manufactured by Mitutoyo Corporation, the arithmetic mean roughness Ra of the surface of the carbon substrate and the surface of the metal carbide coating film formed on the surface of the carbon substrate was measured.
[0060] [Elemental concentration in carbon substrate] <Measurement of sulfur concentration> The sulfur concentration in the carbon substrate was measured using a trace sulfur analyzer (manufactured by Nitto Seiko Analytech Co., Ltd., product name "TS-100"). (1) Sample preparation method After the film formation, the metal carbide-coated carbon material was cut out, and the metal carbide coating film was peeled off to leave only the carbon substrate. This was then wrapped in a Teflon (registered trademark) sheet and roughly crushed with a hammer. The coarse powder was then transferred to B 4 The mixture was pulverized in a mortar to prepare a measurement sample. (2) Measurement of sulfur concentration A 10 mg measurement sample was combusted at 1000°C in an oxygen atmosphere, and the generated SOx was analyzed to calculate the sulfur concentration in the carbon substrate.
[0061] <Concentration of elements other than sulfur> The tantalum carbide coating film was peeled off from the metal carbide-coated carbon material, and the metal concentration of the underlying carbon substrate was measured using an ICP-MS analyzer (inductively coupled plasma mass spectrometer) (900°C pyrolysis / gas analysis) (manufactured by Agilent Technologies, product name "Agilent 7900") to measure the concentration of elements other than sulfur in the carbon substrate. (1) How to prepare the measurement sample The metal carbide-coated carbon material was cut out, and the metal carbide coating film was peeled off to leave only the carbon substrate. This was then wrapped in a Teflon (registered trademark) sheet and roughly crushed with a hammer. The coarse powder was then transferred to B 4 Finely pulverized in a mortar C. A little over 0.1 g of this fine powder was weighed into a microwave decomposition container and decomposed according to the following decomposition recipe. Note that between steps, the container was air-cooled until the temperature dropped to 40°C. (Disassembly recipe) STEP.1:HNO 3 :5 mL + H 2 SO 4 :2.5 mL(80℃*2min, 60℃*3min, 220℃*20min, 230℃*30min) STEP.2: Add HClO 4 :0.5 mL (240℃*25min, 240℃*25min) The resulting solution was transferred to a 30 mL crucible and heated to dryness at 380° C. After drying, the metal residue was dissolved in a small amount of nitric acid, cooled, and then the solution was adjusted to 10 mL with a small amount of hydrofluoric acid and pure water to prepare a measurement solution. (2) Measurement of concentration Using an ICP-MS analyzer, the concentrations of elements in the carbon substrate were measured from the obtained measurement solution under the following conditions. (Measurement conditions) Alkaline and alkaline earth metals: Cool Plasma (RF power:600W) Other elements than those mentioned above: Hot Plasma (RF power:1500W)
[0062] [Method for measuring the amount of corrosion of carbon substrate] A cross-sectional view of the corrosion resistance test device is shown in Figure 2. A cylindrical metal carbide-coated carbon material 21 with an outer diameter of 40 mm, an inner diameter of 30 mm, and a height of 30 mm was prepared. This was covered with a heat insulating material 22 and set in a quartz tube 23. The temperature was raised to 2300°C by high-frequency induction heating, held for 2 hours after reaching that temperature, and then lowered over a period of 2 hours. The temperature of the heating element was measured with a radiation thermometer. Simultaneously with the start of heating, nitrogen was introduced at a flow rate of 1.0 SLM, and this was continued until the temperature began to decrease. The weight of the metal carbide-coated carbon material was measured before and after heating. The weight change (mg) of the metal carbide-coated carbon material was calculated by (weight after heating−weight before heating)×100.
[0063] The measurement temperature range of thermal desorption spectrometry (TDS) is up to 1500°C, and it is not possible to investigate gas generation in high-temperature environments of 1600 to 2300°C during the crystal growth process or epitaxial growth process of wide band gap semiconductors. Therefore, the gas generation in high-temperature environments was indirectly measured by measuring the weight change of the carbon substrate. In other words, if the weight change of the carbon substrate is large, the amount of gas generated in high-temperature environments is also large. Previous research has shown that when a carbon substrate is heated to around 2200°C, it reacts with nitrogen to generate gases such as cyanide and dicyanide, which results in the corrosion of the carbon substrate. Reference 2 (GJ TENNENHOUSE, JA MANGELS, JOURNAL OF MATERIALS SCIENCE LETTERS, 1, 1982, 282-284.) also states that N 2 It is said that cyanide is produced by the reaction of cyanide with carbon. In addition, looking at the above-mentioned Non-Patent Document 1, the results of TDS reach saturation at 1500°C, and it is considered that the outgassing of hydrocarbons and the like adsorbed on the carbon substrate itself does not have much of an effect in a high-temperature environment of 1600 to 2300°C. Therefore, the weight change at 2300°C is 2 It is believed that the difference in weight change is due to the reaction of the carbon with the metal contained in the base material, which acts as a catalyst for this reaction.
[0064] [Method for measuring the adhesion strength of metal carbide coating film] The adhesion strength of the metal carbide coating film was measured using a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus") by adhering the metal carbide coating film 41 and a pin 46 with adhesive 45, pressing down with a pressing jig 44 and pulling the pin 46, as shown in Fig. 3, to measure the stress at which the metal carbide coating film 41 peeled off. Five measurements were taken, and the average of the five calculations was regarded as the adhesion strength of the metal carbide coating film.
[0065] The production conditions for Examples 1 to 14 and Comparative Examples 1 to 4 are shown in Table 1. [Table 1]
[0066] The evaluation results of Examples 1 to 4 and Comparative Example 1 are shown in FIG. 4, and the evaluation results of Examples 1 to 14 and Comparative Examples 1 to 4 are shown in Table 2. [Table 2]
[0067] Comparing the results of Examples 1 to 14 with the results of Comparative Examples 1 to 4, when the total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium and sulfur in the carbon substrate was 10 ppm by mass or more and 10,000 ppm by mass or less, the weight change of the metal carbide-coated carbon material was suppressed.
[0068] The results of the weight change and the number of uses per corrosion resistance test (2 h) for the results of Examples 1 to 4 and Comparative Example 1 are plotted in FIG. 4. Comparing these, when the total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur in the carbon substrate is 10 mass ppm or more and 10,000 mass ppm or less, the weight loss per test hardly changes as the number of tests increases. On the other hand, in the case of a composition such as Comparative Example 1, it was shown that the weight loss increases as the number of tests increases.
[0069] Comparing the results of Example 1, Example 6, and Example 7 with the results of Comparative Example 2, when the total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur in the carbon substrate is 10 mass ppm or more and 10000 mass ppm or less, and the thickness of the tantalum carbide coating film is 10 μm or more and 100 μm or less, the weight change of the metal carbide-coated carbon material is further suppressed. When the thickness of the tantalum carbide coating film is less than 10 μm, the weight loss amount is large. In addition, when the thickness of the tantalum carbide coating film exceeds 100 μm, the film formation time increases, which is not preferable because the film formation cost increases. Therefore, it is preferable that the thickness of the tantalum carbide coating film is in the range of 10 μm or more and 100 μm or less.
[0070] Comparing the results of Example 1, Example 8, and Example 9 with the results of Comparative Example 3 and Comparative Example 4, when the total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur in the carbon substrate is 10 mass ppm or more and 10,000 mass ppm or less, and the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less, or the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less, the weight change of the metal carbide coated carbon material is further suppressed. When the arithmetic mean roughness Ra of the surface of the carbon substrate is larger than 10 μm, the weight loss amount is large. When the arithmetic mean roughness Ra of the surface of the carbon substrate is smaller than 0.1 μm, the weight loss amount is also large.
[0071] Comparing the results of Example 1 and Examples 10 to 14, when the metal carbide coating film was a tantalum carbide coating film, the weight change of the metal carbide-coated carbon material was further suppressed. [Explanation of symbols]
[0072] 10. Externally heated low-pressure CVD equipment 11 Top Chamber 12 Reaction chamber 13. Heater 14 Carbon Substrate 15 Support means 16 Raw material supply department 17 Exhaust section 20. Schematic diagram of corrosion resistance test equipment set 21 Metal carbide coated carbon material 22 Insulation 23 Quartz tube 24 Coil 41 Metal carbide coating film 42 Carbon Substrate 44 Holding jig 45 Adhesive 46 pin
Claims
1. A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film that coats at least a portion of the carbon substrate, the metal carbide constituting the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide; The carbon substrate contains at least one element selected from the group consisting of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium, and sulfur; The metal carbide-coated carbon material has a total concentration of aluminum, iron, magnesium, titanium, silicon, calcium, vanadium, nickel, sodium, potassium and sulfur in the carbon substrate of 10 ppm by mass or more and 10,000 ppm by mass or less.
2. 2. The metal carbide coated carbon material according to claim 1, wherein the iron concentration in the carbon substrate is 1 ppm by mass or more and 10,000 ppm by mass or less.
3. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of titanium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
4. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of magnesium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
5. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of silicon in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
6. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of calcium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
7. 2. The metal carbide coated carbon material according to claim 1, wherein the vanadium concentration in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
8. 2. The metal carbide coated carbon material according to claim 1, wherein the sodium concentration in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
9. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of potassium in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
10. 2. The metal carbide coated carbon material according to claim 1, wherein the concentration of sulfur in the carbon substrate is 0.1 ppm by mass or more and 10,000 ppm by mass or less.
11. 2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide coating film has a thickness of 10 μm or more and 100 μm or less.
12. 2. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less.
13. 2. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less.
14. 2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide constituting the metal carbide coating film is tantalum carbide.
Citation Information
Patent Citations
Crucible for burning ceramics
JP1994122578A
Carbon composite material for reducing atmosphere furnace and production method therefor
JP2007308369A
Tantalum carbide-covered carbon material and process for producing the same
JP2008308701A
Tantalum carbide-coated carbon material and method for manufacturing the same
JP2011153070A
Tantalum carbide coating carbon material and method of manufacturing the same, and member for semiconductor single-crystal manufacturing apparatus
JP2019099453A