Photosensitive insulating paste and electronic component
A balanced composition of glass frit and inorganic fillers in the photosensitive insulating paste addresses the issues of high dielectric constant and mismatched expansion coefficients, resulting in improved adhesion and increased coil wire count in inductor components.
Patent Information
- Application Number
- JP2023075785
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional photosensitive insulating pastes used for forming inductor components suffer from high dielectric constants, leading to increased thickness requirements and poor adhesion between the insulating layer and coil wiring, resulting in cracks and reduced coil wire count due to mismatched linear expansion coefficients.
A photosensitive insulating paste comprising a glass frit with SiO2 as the main component, a first inorganic filler with crystalline silicon oxide, and a second inorganic filler such as alumina, titania, or zirconia, balanced within specific volume ratios, along with a photoinitiator and solvent, to achieve a balanced resolution, dielectric constant, and linear expansion coefficient, enhancing adhesion and reducing crack formation.
The solution provides a photosensitive insulating paste that forms inductor components with improved adhesion, reduced dielectric constant, and increased coil wire count, thereby enhancing the reliability and inductance value of the inductor components.
Smart Images

Figure 2024160601000002 
Figure 2024160601000003 
Figure 2024160601000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a photosensitive insulating paste and an electronic component. [Background technology]
[0002] Conventionally, photosensitive insulating pastes have been used to form inductor components. For example, JP 2012-246176 A (Patent Document 1) describes a photosensitive insulating paste that contains 50% to 90% by mass of silicon oxide, bismuth oxide, boron oxide, aluminum oxide, and zirconium oxide as glass frit. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-246176 A Summary of the Invention [Problem to be solved by the invention]
[0004] The photosensitive insulating paste described in the above publication had high resolution. However, the difference between the linear expansion coefficient of the insulating layer formed from the photosensitive insulating paste and the linear expansion coefficient of the coil wiring became large, which resulted in the occurrence of cracks and the like. In addition, the dielectric constant of the insulating layer became high, which resulted in the need to increase the thickness of the insulating layer. In such cases, it was not easy to increase the number of coil wirings.
[0005] Therefore, an object of the present disclosure is to provide a photosensitive insulating paste having a good balance of resolution, dielectric constant, and linear expansion coefficient, and an electronic component using the photosensitive insulating paste. [Means for solving the problem]
[0006] In order to solve the above problems, a photosensitive insulating paste according to one embodiment of the present disclosure comprises: The composition includes a glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator, and a solvent; The glass frit contains SiO as a main component. 2 and B. 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; The first inorganic filler is a silicon oxide having crystallinity. The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; The first inorganic filler is contained in an amount of 10 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 30 volume % or less, relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler.
[0007] By including the glass frit, the first filler, and the second filler in the above ranges, a photosensitive insulating paste having a good balance of resolution, dielectric constant, and linear expansion coefficient can be formed.
[0008] In one embodiment of the photosensitive insulating paste, the softening point of the glass frit is 700°C or higher and lower than 900°C.
[0009] With the above configuration, the glass frit melts at a temperature lower than the sintering temperature of the metal material of the coil wiring contained in the inductor component, resulting in good adhesion between the base body formed from the photosensitive insulating paste containing the glass frit and the coil wiring.
[0010] In one embodiment of the photosensitive insulating paste, the first inorganic filler is contained in an amount of 20 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler.
[0011] By including the first inorganic filler and the second inorganic filler in the above ranges, the strength of the element body can be increased, and the difference in linear expansion coefficient between the element body and the metal material can be reduced, thereby improving the reliability of the inductor component. Also, the dielectric constant of the element body can be reduced. Therefore, the balance between the resolution, the dielectric constant, and the linear expansion coefficient is improved.
[0012] In one embodiment of the photosensitive insulating paste, the first inorganic filler is contained in an amount of 30 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 10 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler.
[0013] By including the first inorganic filler in the above range, the linear expansion coefficient of the element body formed from the photosensitive insulating paste is increased, the difference in linear expansion coefficient between the element body and the metal material can be reduced, and the occurrence of cracks can be suppressed. By including the second inorganic filler in the above range, the strength of the element body is increased. This further improves the reliability of the inductor component.
[0014] In one embodiment of the photosensitive insulating paste, the secondary component of the glass frit contains elemental phosphorus.
[0015] With the above-mentioned configuration, the melting point of the glass frit becomes relatively low and the linear expansion coefficient becomes large. This makes it possible to reduce the difference in linear expansion coefficient between the coil wiring and the element body. Furthermore, it is possible to suppress the occurrence of stress due to the difference in linear expansion coefficient, and thus the occurrence of cracks.
[0016] In one embodiment of the photosensitive insulating paste, the phosphorus element is contained in an amount of 0.1% by mass to 10% by mass.
[0017] The above-described configuration can reduce the difference in linear expansion coefficient between the coil wiring and the element body, and can further suppress the occurrence of stress due to the difference in linear expansion coefficient, thereby further suppressing the occurrence of cracks.
[0018] In order to solve the above problems, an electronic component according to one aspect of the present disclosure comprises: The body and A coil provided within the element and wound around an axis; Equipped with The coil has a plurality of coil wires, the element body includes a glass material, a first inorganic filler, and a second inorganic filler; The glass material contains SiO as a main component. 2 and B. 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; The first inorganic filler is a crystalline silicon oxide, The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; The first inorganic filler is contained in an amount of 10 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 30 volume % or less, relative to a total of 100 volume % of the glass material, the first inorganic filler, and the second inorganic filler.
[0019] By including the glass material, the first inorganic paste, and the second inorganic paste in the above ranges, it is possible to form an element body having a good balance of resolution, dielectric constant, and linear expansion coefficient.
[0020] In one embodiment of the electronic component, the ratio of the axial thickness of the coil wiring to the axial thickness of a portion of the element body between adjacent coil wirings is in the range of 1.0 to 3.0.
[0021] With the above configuration, the thickness of the portion between adjacent coil wirings in the element body is reduced, and as a result, the number of coil wirings can be increased, and the inductance value can be increased. If the above ratio is too small, the thickness of the portion between adjacent coil wirings in the element body is increased, the number of coil wirings is reduced, and the number of coil turns is reduced. As a result, the inductance value (L value) of the electronic component is reduced. If the ratio is too large, the thickness of the portion between adjacent coil wirings in the element body is too small, the distance between the coil wirings is reduced, and there is a risk that the stray capacitance will increase and the Q value will decrease.
[0022] Here, the axial thickness of the portion between adjacent coil wirings in the element body is the value of the shortest distance between adjacent coil wirings in a cross section that passes through the center of the element body and is perpendicular to the direction in which the coil wiring extends, and the axial thickness of the coil wiring is the maximum value of the coil wiring in the axial direction in a cross section that passes through the center of the element body and is perpendicular to the direction in which the coil wiring extends.
[0023] In one embodiment of the electronic component, the coil wiring has an average thickness in the axial direction of 3 μm or more and 15 μm or less.
[0024] With the above configuration, it is possible to suppress the DC electrical resistance (Rdc), increase the number of coil wires, and increase the inductance value. If the above average value becomes too small, the DC electrical resistance becomes large. If the above average value becomes too large, the number of coil wires becomes small, i.e., the number of turns of the coil becomes small, and the inductance value decreases.
[0025] In one aspect of the electronic component, the coil wiring has one or more turns.
[0026] The above configuration can improve the inductance value. In particular, by suppressing the dielectric constant of the element body, even if the coil wiring makes more than one turn and there are parts that run parallel to each other, it is possible to suppress an increase in stray capacitance, thereby improving the characteristics of the electronic component. Effect of the Invention
[0027] According to the present disclosure, it is possible to provide a photosensitive insulating paste having a good balance between resolution, dielectric constant, and linear expansion coefficient, and an electronic component using the photosensitive insulating paste. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a top perspective view illustrating an inductor component according to a first embodiment. [Diagram 2] FIG. 2 is an exploded perspective view of the inductor component of the first embodiment. [Diagram 3] 1 is an XY cross-sectional view of the inductor component of the first embodiment. FIG. [Figure 4A] 1A to 1C are explanatory diagrams illustrating a manufacturing method of an inductor component. [Figure 4B] 1A to 1C are explanatory diagrams illustrating a manufacturing method of an inductor component. [Figure 4C] 1A to 1C are explanatory diagrams illustrating a manufacturing method of an inductor component. [Figure 4D] 1A to 1C are explanatory diagrams illustrating a manufacturing method of an inductor component. [Figure 4E] 1A to 1C are explanatory diagrams illustrating a manufacturing method of an inductor component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, an electronic component according to one aspect of the present disclosure will be described in detail with reference to the illustrated embodiments. Note that the drawings include some schematic views and may not reflect actual dimensions or ratios. In addition, although an inductor component, which is an example of an electronic component, is described below, the electronic component may be an electronic component other than an inductor component.
[0030] (First embodiment) FIG. 1 is a top perspective view showing a schematic diagram of the inductor component of the first embodiment. FIG. 2 is an exploded perspective view of the inductor component. FIG. 3 is an XY cross-sectional view of the inductor component. In FIG. 1, an element body 10 is drawn transparently so that the structure can be easily understood, but it may be semi-transparent or opaque. In FIG. 3, via wiring is omitted so that the structure can be easily understood.
[0031] The inductor component 1 is electrically connected to wiring on a circuit board (not shown) via first and second external electrodes 30, 40. The inductor component 1 is used, for example, as an impedance matching coil (matching coil) for high-frequency circuits, and is used in electronic devices such as personal computers, DVD players, digital cameras, TVs, mobile phones, car electronics, and medical and industrial machinery. However, the uses of the inductor component 1 are not limited to this, and it can also be used, for example, in tuning circuits, filter circuits, and rectifying and smoothing circuits.
[0032] The element body 10 is formed by laminating a plurality of insulating layers 11. The insulating layer 11 is obtained, for example, by applying a photosensitive insulating paste, repeating a process of drying as necessary a plurality of times to form a laminate, and then firing the laminate. The element body 10 is formed in a substantially rectangular parallelepiped shape. The surface of the element body 10 has a first side surface 13, a second side surface 14 opposite the first side surface, a first end surface 15, a second end surface 16 opposite the first end surface 15, a bottom surface 17 connected between the first end surface 15 and the second end surface 16, and a top surface 18 opposite the bottom surface 17. The first end surface 15, the second end surface 16, the bottom surface 17, and the top surface 18 are parallel to the lamination direction of the insulating layers 11. Here, "parallel" in this application is not limited to a strict parallel relationship, but also includes a substantial parallel relationship in consideration of a range of practical variations. In addition, in element body 10, due to firing or the like, the interfaces between the multiple insulating layers 11 may not be clear.
[0033] As shown in the drawings, for ease of explanation, the direction from first end face 15 to second end face 16 is defined as the X direction. The direction from second side face 14 to first side face 13 is defined as the Y direction. The direction from bottom face 17 to top face 18 is defined as the Z direction. The X direction, Y direction, and Z direction are perpendicular to each other, and when arranged in the order of X, Y, Z, they form a left-handed system.
[0034] The first external electrode 30 and the second external electrode 40 are composed of a conductive material such as Ag or Cu, and glass particles. The first external electrode 30 is L-shaped and provided across the first end face 15 and the bottom face 17. The second external electrode 40 is L-shaped and provided across the second end face 16 and the bottom face 17. In the first embodiment, the first external electrode 30 and the second external electrode 40 are L-shaped, but may have other shapes. For example, the first external electrode 30 and the second external electrode 40 may have a shape that is provided only on the bottom face. Alternatively, the first external electrode 30 may be provided on the first end face 15 of the body 10 and parts of the first side face 13, second side face 14, bottom face 17 and top face 18 adjacent to the first end face 15, and the second external electrode 40 may be provided on the second end face 16 and parts of the first side face 13, second side face 14, bottom face 17 and top face 18 adjacent to the second end face 16.
[0035] The coil 20 is made of, for example, the same conductive material and glass particles as the first and second external electrodes 30, 40. The coil 20 is wound in a spiral shape along the lamination direction of the insulating layers 11. A first end of the coil 20 is connected to the first external electrode 30, and a second end of the coil 20 is connected to the second external electrode 40. In this embodiment, the coil 20 and the first and second external electrodes 30, 40 are integrated and no clear boundary exists, but this is not limited thereto, and a boundary may exist by forming the coil and the external electrodes using different materials or different construction methods.
[0036] The coil 20 is formed in a substantially elliptical shape when viewed from the axial direction L, but is not limited to this shape. The shape of the coil 20 may be, for example, a circle, an ellipse, a rectangle, or another polygon. The axial direction L of the coil 20 refers to a direction parallel to the central axis of the spiral around which the coil 20 is wound. The axial direction L of the coil 20 and the lamination direction of the insulating layer 11 refer to the same direction (Y direction).
[0037] The coil 20 includes a plurality of coil wirings 25 wound on the insulating layer 11. The coil wirings 25 adjacent to each other in the stacking direction are electrically connected in series through via wirings 26 that penetrate the insulating layer 11 in the thickness direction. In this way, the plurality of coil wirings 25 are electrically connected in series to each other and form a spiral. Specifically, the coil 20 has a configuration in which a plurality of coil wirings 25, each having less than one turn, are stacked and electrically connected in series to each other, and the coil 20 has a helical shape. The number of turns of the coil 20 may be one or more turns, or a combination of less than one turn and more than one turn may be used.
[0038] Preferably, the ratio of the thickness D2 in the axial direction L of the coil wiring 25 to the thickness D1 in the axial direction L of the portion between adjacent coil wirings 25 in the element body 10 is in the range of 1.0 to 3.0. With the above configuration, the thickness D1 is small, and as a result, the number of coil wirings 25 can be increased and the inductance value can be increased. If the ratio is too small, the thickness D1 is large, the number of coil wirings 25 is reduced, and the number of turns of the coil 20 is reduced. As a result, the inductance value of the inductor component 1 is small. If the ratio is too large, the thickness D1 is too small, the distance between the coil wirings 25 is reduced, and there is a risk that the stray capacitance will increase and the Q value will decrease.
[0039] Here, thickness D1 is the value of the shortest distance between adjacent coil wirings 25 in a cross section that passes through the center of element body 10 and is perpendicular to the direction in which coil wiring 25 extends. Thickness D2 is the maximum value of coil wiring 25 in axial direction L in a cross section that passes through the center of element body 10 and is perpendicular to the direction in which coil wiring 25 extends.
[0040] Preferably, the average value of the thickness in the axial direction L of the coil wiring 25 is 3 μm or more and 15 μm or less. With the above configuration, it is possible to suppress the DC electrical resistance (Rdc), increase the number of coil wirings 25, and increase the inductance value (L value). If the above average value becomes too small, the DC electrical resistance becomes large. If the above average value becomes too large, the number of coil wirings 25 becomes small, i.e., the number of turns of the coil 20 becomes small, and the inductance value decreases.
[0041] Preferably, the number of turns of coil wiring 25 is one or more. The above configuration can improve the inductance value of inductor component 1. In particular, by suppressing the dielectric constant of element body 10, even if coil wiring 25 has one or more turns and there are portions running in parallel, an increase in stray capacitance can be suppressed, and the characteristics of inductor component 1 can be improved.
[0042] (Photosensitive insulating paste and insulating layer 11) The photosensitive insulating paste and the insulating layer 11 will now be described.
[0043] The photosensitive insulating paste includes a glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator, and a solvent. The glass frit is mainly composed of SiO 2 and B. 2 O 3 and at least one of aluminum, sodium, and phosphorus as a secondary component. The first inorganic filler is a silicon oxide having crystallinity. The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment. The first inorganic filler is contained in an amount of 10 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 30 volume % or less, relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler.
[0044] The inventors' study revealed that a photosensitive insulating paste having a good balance of resolution, dielectric constant, and linear expansion coefficient can be formed by including the glass frit, the first inorganic filler, and the second inorganic filler in the above ranges. Specifically, by including the glass frit in the above ranges, a photosensitive insulating paste with high resolution can be obtained, and a high-precision inductor component 1 can be formed using this photosensitive insulating paste. If the glass frit content is high, the crack extension prevention effect of the filler contained in the element body 10 (insulating layer 11) formed from the photosensitive insulating paste cannot be obtained, the strength decreases, and cracks may occur in the element body 10. If the glass frit content is low, the glass frit cannot be densely sintered, and as a result, the element body 10 becomes brittle and easily breaks. If the first inorganic filler is included in the above ranges, it is possible to reduce the difference in linear expansion coefficient between the element body 10 and the metal material of the coil wiring 25 included in the inductor component 1 while densely sintering the element body 10, thereby suppressing the occurrence of cracks. Furthermore, it is possible to reduce the dielectric constant of the element body 10, and the electrical characteristics of the inductor component 1 can be improved. If the content of the first inorganic filler becomes too high, the content of the glass frit decreases and dense sintering is not possible, resulting in the element body 10 becoming brittle. If the content of the first filler becomes too low, the above-mentioned effects of reducing the linear expansion coefficient difference and dielectric constant cannot be obtained. By adding the second inorganic filler, the strength of the element body 10 can be increased, and the element body 10 can withstand the stress generated between the element body 10 and the coil wiring 25. As a result, by including the second inorganic filler in the above range, cracks are less likely to occur. If the content of the second inorganic filler becomes too high, the light transmittance of the photosensitive paste decreases, and the resolution deteriorates. Furthermore, in addition to the element body 10 becoming brittle and being difficult to densely sinter, the dielectric constant of the element body 10 increases, and the electrical characteristics of the inductor component 1 deteriorate. Furthermore, by including the glass frit, the first inorganic filler, and the second inorganic filler in the above ranges, the thickness of the element body 10 can be reduced and the number of coil wirings 25 can be increased, resulting in an increased inductance value of the inductor component 1.Furthermore, by including the glass frit, the first inorganic filler, and the second inorganic filler in the above ranges, the dielectric constant of element body 10 is reduced. This makes it possible to reduce the thickness of the portion between adjacent coil wirings 25 in element body 10 and increase the number of coil wirings 25, thereby increasing the inductance value of inductor component 1. As described above, by including the glass frit, the first filler, and the second filler in the above ranges, element body 10 can be formed with a good balance of resolution, dielectric constant, and linear expansion coefficient.
[0045] The glass frit may be borosilicate glass. In addition to borosilicate glass, other glass frits may be used, such as SiO 2 , B 2 O 3 , K 2 O, Li 2 O, CaO, ZnO, Bi 2 O 3 , P 2 O 5 and / or Al 2 O 3 Glasses containing, for example, SiO 2 -B 2 O 3 -K 2 O-based glass, SiO 2 -B 2 O 3 -Li 2 O-CaO glass, SiO 2 -B 2 O 3 -Li 2 O-CaO-ZnO glass, SiO 2 -B 2 O 3 -P 2 O 5 Glasses and Bi 2 O 3 -B 2 O 3 -SiO 2 -Al 2 O 3 These inorganic components may be a combination of two or more kinds.
[0046] The softening point of the glass frit is equal to or higher than 700° C. and lower than 900° C. With the above configuration, the glass frit melts at a temperature lower than the sintering temperature of the metal material of the coil wiring 25 included in the inductor component 1, improving adhesion between the element body 10 formed from the photosensitive insulating paste containing the glass frit and the coil wiring 25. The softening point is a value measured using a thermomechanical analyzer (TMA).
[0047] Examples of the first inorganic filler include quartz and silica, and quartz is preferably used. The above-mentioned composition increases the linear expansion coefficient, and the difference in linear expansion coefficient between the insulating layer 11 formed from the photosensitive insulating paste and the coil wiring 25 is further reduced. This makes it possible to suppress the occurrence of cracks between the insulating layer 11 and the coil wiring 25. Quartz is crystalline quartz, and the crystallinity of quartz is not particularly limited.
[0048] Preferably, the second inorganic filler is alumina.
[0049] The average particle size of each of the first inorganic filler and the second inorganic filler is, for example, 0.1 μm to 5.0 μm, specifically 0.3 μm to 3.0 μm. If the average particle size is too small, it becomes difficult to disperse the photosensitive insulating paste. If the average particle size is too large, the smoothness of the insulating layer 11 may decrease.
[0050] The alkali-soluble polymer includes, for example, an acrylic polymer having a carboxyl group in the side chain. The resin including an acrylic copolymer having a carboxyl group in the side chain can be produced, for example, by copolymerizing an unsaturated carboxylic acid and an ethylenically unsaturated compound.
[0051] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, vinylacetic acid, and anhydrides thereof. Examples of the ethylenically unsaturated compound include acrylic acid esters such as methyl acrylate and ethyl acrylate, methacrylic acid esters such as methyl methacrylate and ethyl methacrylate, and fumaric acid esters such as monoethyl fumarate.
[0052] As the acrylic copolymer having a carboxyl group in the side chain, one having an unsaturated bond of the following form introduced therein may be used. (1) An acrylic monomer having a functional group, such as an epoxy group, capable of reacting with the carboxyl group in the side chain of an acrylic copolymer is added to the carboxyl group. (2) The acrylic copolymer having epoxy groups introduced in place of the carboxyl groups in the side chains is reacted with an unsaturated monocarboxylic acid, and then a saturated or unsaturated polycarboxylic anhydride is introduced.
[0053] As the acrylic copolymer having a carboxyl group in the side chain, one having a weight average molecular weight (Mw) of 50,000 or less and an acid value of 30 or more and 150 or less may be used.
[0054] As the photosensitive monomer, dipentaerythritol monohydroxypentaacrylate can be used. In addition to dipentaerythritol monohydroxypentaacrylate, other photosensitive monomers include hexanediol triacrylate, tripropylene glycol triacrylate, trimethylolpropane triacrylate, EO-modified trimethylolpropane triacrylate, stearyl acrylate, tetrahydrofurfuryl acrylate, lauryl acrylate, 2-phenoxyethyl acrylate, isodecyl acrylate, isooctyl acrylate, tridecyl acrylate, caprolactone acrylate, ethoxylated nonylphenol acrylate, 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, diethylene glycol diacrylate, tetraethylene glycol diacrylate, triethylene glycol diacrylate, and ethoxylated bisphenol A. Diacrylate, propoxylated neopentyl glycol diacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, pentaerythritol triacrylate, propoxylated trimethylolpropane triacrylate, propoxylated glyceryl triacrylate, pentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, etc. can be used. In addition, compounds in which part or all of the acrylate in the molecule of the above compound is replaced with methacrylate can be used.
[0055] As the photopolymerization initiator, an acetophenone-based compound, a benzophenone-based compound, an acylphosphine-based compound, or an oxime ester-based compound can be used.
[0056] The solvent is not particularly limited, and examples of the solvent that can be used include ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monoethylhexyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, propylene glycol monophenyl ether, ethyl acetate, butyl acetate, pentyl acetate, hexyl acetate, and cyclohexanol acetate.
[0057] The photosensitive insulating paste may further contain an organic dye. An azo-based compound may be used as the organic dye. When the photosensitive insulating paste is used for photolithographic patterning, the organic dye functions as an ultraviolet absorbing agent for finely adjusting the ultraviolet transmittance.
[0058] Preferably, the first inorganic filler is contained at 20 volume % or more and 40 volume % or less, and the second inorganic filler is contained at 0 volume % or more and 20 volume % or less, relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler. By containing the first inorganic filler and the second inorganic filler in the above ranges, the strength of the element body 10 can be increased, and the difference in linear expansion coefficient between the element body 10 and the metal material is reduced, thereby improving the reliability of the inductor component 1. The dielectric constant of the element body 10 can also be reduced. This results in a better balance between the resolution, the dielectric constant, and the linear expansion coefficient.
[0059] Preferably, the first inorganic filler is contained at 30 volume % or more and 40 volume % or less, and the second inorganic filler is contained at 10 volume % or more and 20 volume % or less, relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler. By containing the first inorganic filler in the above ranges, the linear expansion coefficient of the element body 10 formed from the photosensitive insulating paste is increased, and the difference in the linear expansion coefficient between the element body 10 and the metal material can be reduced, thereby suppressing the occurrence of cracks. By containing the second inorganic filler in the above ranges, the strength of the element body 10 is increased. This further improves the reliability of the inductor component 1.
[0060] In addition, the first inorganic filler may be contained in an amount of 10 volume % or more and 40 volume % or less and the second inorganic filler may be contained in an amount of 0 volume % relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler, or the first inorganic filler may be contained in an amount of 20 volume % or more and 40 volume % or less and the second inorganic filler may be contained in an amount of 0 volume %.
[0061] Preferably, the glass frit contains phosphorus as a minor component. With the above-mentioned configuration, the melting point of the glass frit becomes relatively low and the linear expansion coefficient becomes large. This makes it possible to reduce the difference in linear expansion coefficient between the coil wiring 25 and the element body 10. Furthermore, it is possible to suppress the occurrence of stress caused by the difference in linear expansion coefficient, and thus the occurrence of cracks.
[0062] Preferably, the glass frit contains 0.1 mass % to 10 mass % of phosphorus. The phosphorus content is measured using a wavelength dispersive X-ray fluorescence analyzer (WDX) or a high-frequency inductively coupled plasma (ICP) emission analyzer.
[0063] The insulating layer 11 includes a glass material, a first inorganic filler, and a second inorganic filler. The glass material contains SiO 2 as a main component. 2 and B. 2 O 3and at least one of aluminum, sodium, and phosphorus as a secondary component. The first inorganic filler is a silicon oxide having crystallinity. The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and inorganic oxide pigment. The first inorganic filler is included in an amount of 10 to 40 volume% and the second inorganic filler is included in an amount of 0 to 30 volume% relative to a total of 100 volume% of the glass material, the first inorganic filler, and the second inorganic filler. That is, the glass material is included in an amount of 30 to 90 volume%, the first inorganic filler is included in an amount of 10 to 40 volume%, and the second inorganic filler is included in an amount of 0 to 30 volume% relative to a total of 100 volume% of the glass material, the first inorganic filler, and the second inorganic filler. The main component refers to a component that is included in an amount of 60 volume% or more relative to 100 volume% of the glass material. The upper limit of the main component is not particularly limited, but is, for example, 99% by volume or less. The subcomponent refers to a component contained in an amount of 40% by volume or less relative to 100% by volume of the glass material. The lower limit of the subcomponent is not particularly limited, but is, for example, 0.1% by volume or more. The ratio of the glass material, the first inorganic filler, and the second inorganic filler contained in the insulating layer 11 is substantially the same as the ratio of the glass frit, the first inorganic filler, and the second inorganic filler contained in the photosensitive insulating paste. The glass material contained in the insulating layer 11 is obtained by firing the glass frit contained in the photosensitive insulating paste. The type and composition of the first inorganic filler and the second inorganic filler contained in the insulating layer 11 are the same as the type and composition of the first inorganic filler and the second inorganic filler contained in the photosensitive insulating paste.
[0064] As with the glass frit, first inorganic paste, and second inorganic paste of the photosensitive insulating paste, by including the glass material, first inorganic paste, and second inorganic paste in the above ranges, an insulating layer 11 (base body 10) can be formed that has a good balance of resolution, dielectric constant, and linear expansion coefficient.
[0065] (Manufacturing method) Next, a method for manufacturing the inductor component 1 will be described.
[0066] First, a negative photosensitive insulating paste and a conductive paste are prepared.
[0067] As shown in Fig. 4A, the outer insulating layer 11a is formed by applying a photosensitive insulating paste. The photosensitive insulating paste is applied by screen printing, for example. Fig. 4A to Fig. 4E are cross-sectional views in the XY direction.
[0068] As shown in Fig. 4B, a photosensitive insulating paste is applied to the outer insulating layer 11a to form a first insulating layer 11b. Thereafter, the first insulating layer 11b is exposed to light while a first portion 111 (shown by a two-dot chain line) of the first insulating layer 11b is shielded by a mask 110. As shown in Fig. 4C, the first portion 111 of the first insulating layer 11b is removed by development to form a groove 112 at a position corresponding to the first portion 111. As shown in Fig. 4D, the coil wiring 25 is formed in the groove 112.
[0069] 4E, second insulating layer 11c is formed by applying a photosensitive insulating paste onto first insulating layer 11b and coil wiring 25. The above steps are repeated multiple times to form a laminate, which is then fired to manufacture inductor component 1. EXAMPLES
[0070] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0071] (Examples 1 to 9, Comparative Examples 1 to 3) Phosphorus-containing borosilicate glass as the glass frit, quartz as the first inorganic filler, and alumina as the second inorganic filler were mixed in the ratios shown in Table 1 to form a photosensitive insulating paste.
[0072] The obtained photosensitive insulating paste was used to form the inductor component 1. In addition, the resolution, dielectric constant, and crack prevention effect were measured during the formation of the inductor component 1. The results are shown in Table 1.
[0073] (Resolution) The paste was printed with a thickness of 20 μm by screen printing, dried in a safety oven, exposed to light through a photomask with openings of various dimensions, and developed with an alkaline aqueous solution to form a wiring pattern. The width and thickness of the patterns that were produced without residue or missing patterns were measured, and the aspect ratio (thickness / width) was calculated. A: The resolution is 1.0 or more. ◯: Resolution is 0.5 or more and less than 1.0. ×: The resolution is less than 0.5.
[0074] (Dielectric constant) An insulating layer was formed from the photosensitive insulating paste, and the dielectric constant was measured using a signal analyzer (manufactured by Keysight Corporation). ◎: The dielectric constant is 6.0 or more. ◯: The dielectric constant is 6.0 or more and less than 7.0. ×: The dielectric constant is less than 7.0.
[0075] (Crack prevention effect) The crack prevention effect was measured as follows.
[0076] An inductor component made from insulating paste was fixed onto a substrate, and a test load (p)-displacement (h) plot was obtained when the nanoindenter's measuring indenter was pressed against the element part of the inductor component. The contact stiffness (S=dp / dh) as the load increased was calculated from the obtained test load (p)-displacement (h) data, and a contact stiffness (S)-test load (p) plot was created. Among the peaks showing a decrease in contact stiffness in the created plot, the peak at the lowest load was determined to be the first crack to have entered the element part of the component, and the load at that time was defined as the "crack initiation load." The nanoindenter device and measurement conditions are as follows. Equipment: Nanoindenter ENT-1100a (Elionix) Test load: 100gf Step interval: 20msec ◎: The load at which cracks occur is 70N or more. ◯: The crack generating load is 30N or more and less than 70N. ×: The load at which cracks occur is less than 30N.
[0077] [Table 1]
[0078] In Examples 1 to 4, a photosensitive insulating paste containing glass frit and a first inorganic filler was used. In Examples 1 to 4, the resolution, dielectric constant, and crack prevention effect of the photosensitive insulating paste were all good. In particular, by including 20 volume % or more and 40 volume % or less of the first inorganic filler, the dielectric constant became even better.
[0079] In Examples 5 to 9, a photosensitive insulating paste containing a glass frit, a first inorganic filler, and a second inorganic filler was used. In Examples 5 to 9, the resolution, dielectric constant, and crack prevention effect of the photosensitive insulating paste were all good. In particular, the crack prevention effect of Examples 5 to 9 was better than that of Examples 1 to 4. This is believed to be because the strength of the element body was improved by including the second inorganic filler. Also, in Examples 5 and 6, the resolution of the photosensitive insulating paste, the dielectric constant of the inductor component, and the crack prevention effect were all particularly good.
[0080] In Comparative Example 1, a photosensitive insulating paste containing only glass frit was used. In Comparative Example 1, the resolution and dielectric constant were good, but the crack prevention effect was evaluated as x. In Comparative Example 2, a photosensitive insulating paste containing 40% by volume of both the first inorganic filler and the second inorganic filler was used. However, the resolution, dielectric constant, and crack prevention effect were all evaluated as x. In Comparative Example 2, the content of the glass frit was reduced due to the increase in the content of the first inorganic filler and the second inorganic filler, and the formed insulating layer became brittle. In Comparative Example 3, the content of the glass frit was 20% by volume, the same as in Comparative Example 2, but the photosensitive insulating paste was formed with the first inorganic filler at 50% by volume and the second inorganic filler at 30% by volume. The resolution and dielectric constant were evaluated as good, but the crack prevention effect was evaluated as x. This is thought to be because the content of the glass frit was not within an appropriate range.
[0081] As described above, it has been found that by using a photosensitive insulating paste containing glass frit, a first inorganic filler, and a second inorganic filler in appropriate ranges, good results can be obtained in terms of resolution, dielectric constant, and crack prevention effect.
[0082] The present disclosure is not limited to the above-described embodiment, and the design can be changed without departing from the scope of the present disclosure. The shape of the core is not limited to the present embodiment, and the design can be changed. Furthermore, the number of coils is not limited to the present embodiment, and the design can be changed.
[0083] The present disclosure includes the following aspects. <1> The composition includes a glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator, and a solvent; The glass frit contains SiO as a main component. 2 and B. 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; The first inorganic filler is a crystalline silicon oxide, The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; A photosensitive insulating paste comprising 10% by volume or more and 40% by volume or less of the first inorganic filler and 0% by volume or more and 30% by volume or less of the second inorganic filler, relative to a total of 100% by volume of the glass frit, the first inorganic filler, and the second inorganic filler. <2> The softening point of the glass frit is 700°C or more and less than 900°C. <1> 2. The photosensitive insulating paste according to claim 1 . <3> The first inorganic filler is contained in an amount of 20 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler. <1> or <2> 2. The photosensitive insulating paste according to claim 1 . <4> The first inorganic filler is contained in an amount of 30 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 10 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler. <1> from <3> 13. The photosensitive insulating paste according to any one of claims 1 to 12. <5> The subcomponent of the glass frit includes phosphorus element. <1> from <4> 13. The photosensitive insulating paste according to any one of claims 1 to 12. <6> The phosphorus element is contained in an amount of 0.1% by mass or more and 10% by mass or less. <5> 2. The photosensitive insulating paste according to claim 1 . <7> The body and A coil provided within the element and wound around an axis; Equipped with The coil has a plurality of coil wires, the element body includes a glass material, a first inorganic filler, and a second inorganic filler; The glass material contains SiO as a main component. 2and B. 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; The first inorganic filler is a crystalline silicon oxide, The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; An electronic component, wherein the first inorganic filler is contained in an amount of 10 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 30 volume % or less, relative to a total volume 100% of the glass material, the first inorganic filler, and the second inorganic filler. <8> a ratio of a thickness of the coil wiring in the axial direction to a thickness of a portion of the element body between adjacent coil wirings in the axial direction is in a range of 1.0 or more and 3.0 or less. <7> 2. An electronic component as described in claim 1. <9> The average thickness of the coil wiring in the axial direction is 3 μm or more and 15 μm or less. <7> or <8> 2. An electronic component as described in claim 1. <10> The number of turns of the coil wiring is one or more. <7> from <9> 13. An electronic component according to any one of claims 1 to 12. [Explanation of symbols]
[0084] 1. Inductor components 10 Base 13 First aspect 14 Second aspect 15 First end surface 16 Second end face 17 Bottom 18 Top 20 Coil 25 Coil wiring 26 Via wiring 30 1st external electrode 33 First external electrode conductor layer 40 2nd external electrode 43 Second external electrode conductor layer L axis direction D1 Thickness of the element between the coil wires D2 Coil Wiring Thickness
Claims
1. The composition includes a glass frit, a first inorganic filler, a second inorganic filler, an alkali-soluble polymer, a photosensitive monomer, a photopolymerization initiator, and a solvent; The glass frit contains SiO as a main component. 2 and B 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; the first inorganic filler is a crystalline silicon oxide, The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; a photosensitive insulating paste comprising: 10 volume % or more and 40 volume % or less of the first inorganic filler; and 0 volume % or more and 30 volume % or less of the second inorganic filler, relative to a total of 100 volume % of the glass frit, the first inorganic filler, and the second inorganic filler.
2. 2. The photosensitive insulating paste according to claim 1, wherein the softening point of the glass frit is 700° C. or more and less than 900° C.
3. 3. The photosensitive insulating paste according to claim 1, wherein the first inorganic filler is contained in an amount of 20 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler.
4. 3. The photosensitive insulating paste according to claim 1, wherein the first inorganic filler is contained in an amount of 30 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 10 volume % or more and 20 volume % or less, relative to a total volume 100% of the glass frit, the first inorganic filler, and the second inorganic filler.
5. 3. The photosensitive insulating paste according to claim 1, wherein the secondary component of the glass frit contains a phosphorus element.
6. The photosensitive insulating paste according to claim 5 , wherein the phosphorus element is contained in an amount of 0.1% by mass to 10% by mass.
7. The body and A coil provided within the element and wound around an axis; Equipped with The coil has a plurality of coil wires, the element body includes a glass material, a first inorganic filler, and a second inorganic filler; The glass material contains SiO as a main component. 2 and B 2 O 3 and containing at least one of an aluminum element, a sodium element, and a phosphorus element as a minor component; the first inorganic filler is a crystalline silicon oxide, The second inorganic filler includes at least one of alumina, titania, zirconia, ceria, forsterite, and an inorganic oxide pigment; an electronic component, wherein the first inorganic filler is contained in an amount of 10 volume % or more and 40 volume % or less, and the second inorganic filler is contained in an amount of 0 volume % or more and 30 volume % or less, relative to a total volume 100% of the glass material, the first inorganic filler, and the second inorganic filler.
8. 8. The electronic component according to claim 7, wherein a ratio of a thickness in the axial direction of the coil wiring to a thickness in the axial direction of a portion of the element body between adjacent coil wirings is in a range of 1.0 to 3.
0.
9. The electronic component according to claim 7 or 8, wherein an average thickness of the coil wiring in the axial direction is not less than 3 μm and not more than 15 μm.
10. The electronic component according to claim 7 , wherein the number of turns of the coil wiring is one or more.
Citation Information
Patent Citations
Glass ceramic composition
JP2000203878A
Photosensitive ceramic composition
JP2002162735A
Multilayer coil and its manufacturing method
JP2004296860A
Common mode filter and mounting structure thereof
JP2010177380A
Low dielectric constant (low k) dielectric composition for high frequency application
JP2019108263A