Optical member, lens unit, and optical unit
A resin substrate with a yellowing canceling layer and multilayer antireflection film addresses the issue of yellowing in lens units, ensuring stable optical performance under harsh conditions.
Patent Information
- Application Number
- JP2023075797
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
AI Technical Summary
Existing lens units using resin substrates face issues with yellowing due to oxidation under harsh temperature conditions, particularly in environments subject to vibrations, leading to unsuppressed image color changes.
Incorporating a transparent resin substrate with a yellowing canceling layer that changes its optical properties over time to counteract the yellowing of the resin substrate, combined with a multilayer antireflection film to form a gas barrier and reduce oxygen permeation.
The solution effectively suppresses changes in image color due to resin substrate yellowing, maintaining stable optical properties under high-temperature conditions.
Smart Images

Figure 2024160606000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical member, a lens unit, and an optical unit. [Background technology]
[0002] Lens units used in vehicle-mounted cameras and sensors, as well as surveillance cameras, may use resin lenses with an anti-reflection film formed on a resin substrate for the purpose of reducing weight and cost. However, in applications where the lenses are used under severe temperature conditions, such as vehicle-mounted cameras and surveillance cameras, there is a problem that the resin substrate discolors (yellowing) due to oxidation. To solve this problem, Patent Document 1 places a resin lens in an enclosed space formed by a lens barrel and a glass element, and further forms an oxygen-permeation-preventing film between the resin substrate and the anti-reflection film, thereby suppressing the yellowing of the resin substrate due to oxygen. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-105194 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, it is difficult to completely maintain the sealed space of the lens unit. For example, when the lens unit is used in an environment where it is subjected to vibration, such as a lens unit for in-vehicle use, oxygen is more likely to enter the lens unit. Therefore, the technology of Patent Document 1 has a problem in that it cannot suppress yellowing of the resin substrate.
[0005] Therefore, an object of the present invention is to provide an optical member, a lens unit, and an optical unit that suppress changes in color of an image caused by yellowing of a resin substrate that occurs in a high-temperature environment. [Means for solving the problem]
[0006] In order to achieve the object of the present invention, the optical component of the present invention comprises a translucent resin substrate and a yellowing offset layer whose visible light transmittance changes in a direction opposite to the change in visible light transmittance of the resin substrate due to yellowing of the resin substrate, and is characterized in that the yellowing offset layer is provided on the resin substrate. Effect of the Invention
[0007] According to the present invention, it is possible to provide an optical member, a lens unit, and an optical unit that suppress changes in color of an image caused by yellowing of a resin substrate that occurs in a high-temperature environment. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a diagram showing an example of a configuration of an optical member according to the present invention. [Diagram 2] FIG. 11 is a diagram for explaining color matching functions. [Diagram 3] 3A and 3B are diagrams illustrating the configuration of an optical member according to Example 1 and the reflectance of the optical member. [Figure 4] FIG. 3 is a graph for explaining the extinction coefficient of the yellowing offset layer according to the first embodiment. [Diagram 5] FIG. 2 is a diagram showing the light absorption characteristics of the anti-reflection film and the yellowing offset layer according to Example 1. [Figure 6] 10A and 10B are diagrams illustrating the configuration of an optical member according to Example 2 and the reflectance of the optical member. [Figure 7] FIG. 11 is a graph for explaining the extinction coefficient of the yellowing offset layer according to Example 2. [Figure 8] FIG. 11 is a diagram showing the light absorption characteristics of the anti-reflection film and the yellowing offset layer according to Example 2. [Figure 9] 11A and 11B are diagrams illustrating the configuration of an optical member according to Example 3 and the reflectance of the optical member. [Figure 10] FIG. 11 is a graph for explaining the extinction coefficient of the yellowing offset layer according to Example 3. [Figure 11] FIG. 11 is a diagram showing the light absorption characteristics of the anti-reflection film and the yellowing offset layer according to Example 3. [Figure 12] 1A and 1B are diagrams showing a lens unit and an optical unit according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments will be described in detail with reference to the attached drawings. Note that the following embodiments do not limit the invention according to the claims. Although the embodiments describe a number of features, not all of these features are essential to the invention, and the features may be combined in any manner. Furthermore, in the attached drawings, the same reference numbers are used for the same or similar configurations, and duplicated descriptions are omitted.
[0010] Example 1 FIG. 1 is a diagram showing an example of the configuration of an optical member according to the present invention.
[0011] The optical member 6 includes an antireflection film 4 composed of at least one low refractive index layer 2 and one high refractive index layer 3 on a resin substrate 1, and a yellowing offset layer 5. The optical member 6 may include only the yellowing offset layer 5 on the resin substrate 1.
[0012] The yellowing offset layer 5 is a layer that changes its optical properties over time to offset the change in color of the resin substrate 1 that yellows due to heat. The yellowing offset layer 5 is made of metal incomplete oxides such as Al and Si. The yellowing offset layer 5 may be formed, for example, in the anti-reflection film 4 of FIG. 1, or may be formed between the resin substrate 1 and the anti-reflection film 4. Considering the optical properties of the optical member 6, the outermost layer of the optical member 6 is the low refractive index layer 2 that constitutes the anti-reflection film 4. In addition, although the yellowing offset layer 5 is composed of only one layer in FIG. 1, it is not limited thereto and may be composed of multiple layers.
[0013] (Resin substrate) The resin substrate 1 is a transparent resin substrate, and is formed of, for example, an olefin-based, polycarbonate-based, acrylic-based, styrene-based, polyester-based, polyurethane-based, etc. The resin substrate 1 may also be a substrate made of a heat- and light-curable resin such as a multifunctional reactive polymer having an aromatic dendrimer-like multi-branched structure, or, as necessary, an organic and inorganic hybrid material, such as a substrate having a silsesquioxane skeleton.
[0014] The resin substrate 1 is more flexible, lighter, and easier to process than inorganic substrates such as glass. On the other hand, the resin substrate 1 is susceptible to changes in characteristics due to deformation caused by heat and the influence of moisture. The resin substrate 1 has high heat resistance (high glass transition temperature Tg) to prevent changes in characteristics. The glass transition temperature (Tg) of the resin substrate 1 is preferably 120° C. or higher, more preferably 140° C. or higher. Here, the glass transition temperature (Tg) of the resin substrate 1 is a temperature measured by differential scanning calorimetry (DSC) based on JIS K 7121.
[0015] Furthermore, the resin substrate 1 may be made of a resin material having low water absorption. The resin substrate 1 may be made of an olefin-based, particularly a cycloolefin-based, resin material.
[0016] The refractive index of the resin substrate 1 is preferably about 1.45 to 1.80, and more preferably about 1.50 to 1.65, at e-line (546.075 nm). In applications where the optical member 6 is used over a wide temperature range, such as in-vehicle cameras and surveillance cameras, a resin substrate 1 with small change in refractive index due to temperature is required. As for the change in refractive index of the resin substrate 1 due to temperature, at e-line, the difference between the refractive index at 0°C and the refractive index at 80°C is preferably 0.8% or less, and more preferably 0.6% or less.
[0017] The change in optical properties of the resin substrate 1 in a high-temperature environment (i.e., the yellowing index (ΔYI)) is preferably small. ΔYI is calculated from the difference between the yellowing index (YI) after 1500 hours at 120°C and the initial yellowing index (YI0). From the viewpoint of suppressing the change in optical properties, the ΔYI (corresponding to the second yellowing index) of the resin substrate 1 according to one embodiment is preferably 10 or less, more preferably 8 or less. On the other hand, the ΔYI of the resin substrate 1 according to one embodiment is preferably 2 or more, more preferably 4 or more. The ΔYI of the resin substrate 1 according to one embodiment is preferably 2 or more and 10 or less, more preferably 4 or more and 8 or less.
[0018] The resin substrate 1 has a transmittance of 80% or more in the visible light region of 400 to 700 nm, while the resin substrate 1 has a transmittance of 60% or more in the visible light region of 400 to 700 nm after 1500 hours at 120°C.
[0019] When a plurality of resin substrates 1 are used in the same unit, such as a lens unit, the plurality of resin substrates 1 may have different refractive indices or Abbe numbers in order to adjust optical characteristics such as aberration.
[0020] When the resin substrate 1 has a lens shape, the resin substrate 1 can be molded by, for example, injection molding. Specifically, a cavity including a lens portion, an outer periphery, a gate portion, etc., formed by butting a fixed mirror piece and a movable mirror piece together, is filled with resin material through the gate portion, and when the resin has solidified, the mold is opened and the resin substrate 1 is removed. Finally, the gate portion of the removed resin substrate 1 is cut off. With this method, aspheric lenses, which are difficult to process with glass, can be relatively easily manufactured. Note that molding of the resin substrate 1 is not limited to injection molding, and various known methods such as injection compression molding and cast polymerization can be used.
[0021] The resin substrate 1 is annealed before forming the anti-reflection film 4 and the yellowing offset layer 5 described below in order to release the internal stress generated during molding of the resin substrate 1 and to remove moisture adhering to the resin substrate 1. The annealing is carried out at a temperature of from 80° C. to the Tg (glass transition temperature) of the resin substrate 1 or lower, preferably for 0.5 to 24 hours, more preferably for 1 to 12 hours.
[0022] (Anti-reflective film) The anti-reflection film 4 is a multi-layer anti-reflection film in which layers with different refractive indices are laminated. The low refractive index layer is a layer made of MgF2 and SiO2. The intermediate refractive index layer is a layer made of Al2O3 and MgO. The high refractive index layer is a layer made of ZrO2, La2Ti2O7 (LaTiO3), Si3H4, Ta2O5, Nb2O5, TiO2, etc. The low refractive index layer, intermediate refractive index layer, and high refractive index layer are formed of materials that do not have significant light absorption in the visible light region of 400 to 700 nm.
[0023] In particular, the combination of a low refractive index layer made of SiO2 and a high refractive index layer made of TiO2 results in a large refractive index difference. The above combination is preferable in that it allows the number of layers in the anti-reflection coating 4 to be reduced when providing the anti-reflection coating 4 with the desired spectral characteristics. In FIG. 1, the first layer of the anti-reflection coating 4 is a high refractive index layer made of TiO2, but the first layer may be a low refractive index layer or an intermediate refractive index layer.
[0024] Here, the yellowing of the resin substrate 1 occurs when oxygen, water vapor, etc. act on the resin, causing the resin to oxidize. Therefore, the anti-reflective film 4 has a gas barrier function that suppresses the arrival of oxygen and water vapor at the resin substrate 1. The film density of the layer (thin film) constituting the anti-reflective film 4 is preferably high. For example, the thin film is formed by a film formation method that can obtain a high-density vapor deposition film even at a low temperature below the Tg of the resin substrate 1, such as a sputtering method, an ion-assisted method, or an ion plating method. On the other hand, if the film density of the thin film is too high, cracks may easily occur in the thin film. In order to prevent cracks in the thin film, for example, a single layer or multiple layers of thin films on the side closer to the resin substrate 1 are formed by a vacuum deposition method, which is one of the various film formation methods that is less likely to result in a high film density. In addition, a single layer or multiple layers of thin films on the side farther from the resin substrate 1 are formed with the addition of an ion-assisted method, an ion-plating method, or the like.
[0025] The anti-reflective film 4 preferably has 4 to 12 layers, and more preferably 6 to 10 layers. The more the number of layers of the anti-reflective film 4 increases, the higher the gas barrier performance of the anti-reflective film 4 becomes. This is because, even if any of the layers constituting the anti-reflective film 4 has a defect, as long as there is no defect in the same region between the laminated layers, it is possible to prevent gases such as oxygen and water vapor from entering the resin substrate 1. In other words, when a minute film defect occurs in the layer forming the anti-reflective film 4, the more the number of layers of the anti-reflective film 4 increases, the easier it is to suppress yellowing of the resin substrate 1.
[0026] On the other hand, if the number of layers in the anti-reflection film 4 is too large, the film thickness becomes large and film stress makes the anti-reflection film 4 more susceptible to cracks. If a crack occurs in the anti-reflection film 4, oxygen, water vapor, and the like will reach the resin substrate 1 through the crack, accelerating the yellowing of the resin substrate 1.
[0027] The thickness of the anti-reflection film 4 (including the yellowing countermeasure layer 5) is preferably 200 nm to 600 nm, more preferably 250 nm to 500 nm. If the thickness of the anti-reflection film 4 is too thin, it becomes difficult to achieve sufficient low reflectance due to the interference effect of the thin film, and the gas barrier effect of the anti-reflection film 4 becomes small. On the other hand, if the thickness of the anti-reflection film 4 is too thick, cracks are likely to occur in the anti-reflection film 4.
[0028] Here, the low reflection region of the optical member 6 having the anti-reflection film 4 and the yellowing compensation layer 5 formed on the resin substrate 1 is a wavelength region in which the reflectance is 1.5% or less in the visible light region of 380 to 700 nm. The reflectance in the wavelength region before and after the low reflection region of the anti-reflection film 4 increases sharply. The low reflection region of the optical member 6 having only the anti-reflection film 4 on the resin substrate 1 shifts slightly to the long wavelength side due to aging. At this time, the reflectance on the short wavelength side of the visible light region increases sharply, so that the transmittance on the short wavelength side of the visible light region decreases, and the YI (yellowness index) of the optical member 6 increases. By setting the low reflection region from 380 nm, which is 20 nm shorter than 400 nm, the shortest wavelength of the visible light wavelength, the YI (yellowness index) of the optical member 6 can be suppressed from increasing even if the low reflection region of the anti-reflection film 4 shifts slightly to the long wavelength side due to aging.
[0029] (Yellowing prevention layer) The yellowing offset layer 5 changes the optical properties over time, for example, by oxidation of the yellowing offset layer 5, so as to offset the yellowing of the resin substrate 1 caused by oxidation due to heat. The yellowing of the resin substrate 1 is evaluated by YI0 (initial yellowness), YI (yellowness), and ΔYI (yellowing degree). As the yellowing of the resin substrate 1 progresses, the YI and ΔYI values increase. Here, the yellowing offset layer 5 has the function of decreasing YI and ΔYI as the yellowing of the resin substrate 1 progresses.
[0030] Here, we will explain YI (yellowness index) based on JIS K 7105. Figure 2 shows the spectral response characteristics of the three types of cones (L, M, S) in photoreceptor cells. Tristimulus values X, Y, and Z are obtained by multiplying the color matching functions xbar(λ), ybar(λ), and zbar(λ) by the relative spectral distribution of standard illuminant D65 and the transmittance spectrum of the substance to be measured. Then, YI (yellowness index) is calculated by substituting the obtained tristimulus values into Equation 1.
[0031] Here, YI (yellowness index) is the degree to which the hue moves away from colorless or white toward yellow, and is expressed as a positive value. In other words, when YI (yellowness index) is expressed as a negative value, it indicates that the hue moves from colorless or white toward blue. In this embodiment, YI (yellowness index) is calculated in a 2-degree visual field. Cx and Cz have coefficients shown in Equation 1.
[0032] ΔYI (yellowing index) is an index used to evaluate the deterioration of plastic (e.g., resin substrate 1) exposed to environments such as light and heat. According to Equation 2, ΔYI (yellowing index) is the difference between YI0 (initial yellowness) and YI (yellowing index after 1500 hours at 120°C). Here, the larger ΔYI is, the more advanced the yellowing is.
[0033] YI = 100(Cx X-Cz Z) / Y (Equation 1) Cx:1.2985 Cz:1.1335
[0034] ΔYI=YI-YI0 (formula 2) ΔYI: Yellowing, YI: Yellowing after 1500 hours at 120°C, YI0: Initial yellowing of the sample
[0035] The yellowing offset layer 5 reduces YI calculated by formula 1 over time. Specifically, the value of Z among the tristimulus values changes over time to become larger relative to X and Y. That is, the yellowing offset layer 5 changes to increase the transmittance (i.e., decrease the light absorption) in the light wavelength region of 400 to 500 nm where the relative spectral distribution of zbar is large.
[0036] The yellowing offset layer 5 is made of, for example, a metal oxide having an oxygen deficiency. When the oxygen of the metal oxide is deficient, light absorption occurs in the visible light region, so the metal oxide becomes opaque. On the other hand, when oxygen is replenished to the metal oxide (becoming a complete oxide), light absorption in the visible light region decreases, so the metal oxide becomes transparent. Among metal oxides, Al oxide has high gas barrier properties, so Al oxide can effectively suppress yellowing of the resin substrate 1. Thus, Al2Ox (x<3) is suitable as the yellowing offset layer 5. In addition, Si oxide has good adhesion to the resin substrate 1, so SiOy (1≦y<2) can be provided as the yellowing offset layer 5 between the resin substrate 1 and the anti-reflection film 4. This can also suppress cracks in the yellowing offset layer 5.
[0037] In order to effectively offset the yellowing of the resin substrate 1, the ΔYI (corresponding to the first yellowing degree) of the yellowing offset layer 5 is preferably −7 or more and −0.05 or less, more preferably −3 or more and −0.1 or less. When the ΔYI of the yellowing offset layer 5 is a negative value, the yellowing offset layer 5 in the initial state needs to have a certain light absorption characteristic in the region of zbar(λ).
[0038] The extinction coefficient (k450) of the yellowing countermeasure layer 5 at a light wavelength of 450 nm is preferably 5.0×10 -4 More preferably, 1.0×10 -3 That is all. The higher the transmittance of the yellowing offset layer 5 in the visible light region, the more preferable. Of the above-mentioned tristimulus values, it is particularly preferable that the values of X and Y are as large as possible. It is better that the extinction coefficient at the light wavelengths corresponding to X and Y is small. When the extinction coefficient at a light wavelength of 550 nm is k550 and the extinction coefficient at a light wavelength of 600 nm is k600, it is preferable that k550 / k450 and k600 / k450 are each 0.8 or less, and more preferably 0.6 or less. In addition, the extinction coefficient of the present invention can be a value calculated or measured by a measurement method using a spectroscopic ellipsometer.
[0039] The yellowing offset layer 5 has at least one of a single layer and multiple layers. The yellowing offset layer 5 has an overall light absorption of preferably 0.5 to 10% at a light wavelength of 450 nm, more preferably 1 to 5%. In order to impart the above light absorption characteristics to the yellowing offset layer 5, the thickness of the yellowing offset layer 5 is preferably 8 to 200 nm, more preferably 20 to 150 nm. In order to impart the above light absorption characteristics to the yellowing offset layer 5, the number of layers and the extinction coefficient of the yellowing offset layer 5 can be appropriately adjusted.
[0040] Furthermore, when coating is applied to both sides of the resin substrate 1, the yellowing offset layer 5 may be formed on only one side of the resin substrate 1, or on both sides of the resin substrate 1. Furthermore, a plurality of different yellowing offset layers 5 may be formed on the resin substrate 1. For example, a film of SiOy (1≦y<2) may be formed in contact with the resin substrate 1, and a film of Al2Ox (x<3) may be formed on the SiOy (1≦y<2). As described above, the yellowing offset layer 5 can offset the yellowing of the resin substrate 1 and at the same time suppress cracks in the yellowing offset layer 5.
[0041] In particular, when the yellowing offset layer 5 is formed between the resin substrate 1 and the first layer of the anti-reflection film 4, it is preferable to form the yellowing offset layer 5 without applying ion assist or the like during the formation of the yellowing offset layer 5. For example, when the yellowing offset layer 5 is formed using ion assist or the like, the yellowing offset layer 5 becomes a dense, hard film. As a result, cracks are likely to occur in the yellowing offset layer 5 due to the difference in linear expansion coefficient between the resin substrate 1 and the formed yellowing offset layer 5.
[0042] When the yellowing offset layer 5 is formed between the resin substrate 1 and the anti-reflection film 4, it is preferable to form the layer so that the film density of the yellowing offset layer 5 increases continuously from the resin substrate 1 side. As described above, forming the yellowing offset layer 5 with a relatively low film density at the interface between the yellowing offset layer 5 and the resin substrate 1 is effective as a measure against cracks in the yellowing offset layer 5. However, it is preferable to form the yellowing offset layer 5 so that the film density of the yellowing offset layer 5 is high at a portion other than the interface between the yellowing offset layer 5 and the resin substrate 1 in terms of improving the gas barrier property.
[0043] In addition, at the interface where the difference between the film density of the yellowing offset layer 5 and the film density of the anti-reflection film 4 is large, the yellowing offset layer 5 is likely to crack. For this reason, the yellowing offset layer 5 is formed so that the film density of the yellowing offset layer 5 in contact with the resin substrate 1 gradually increases from the interface side between the resin substrate 1 and the yellowing offset layer 5 upward. This makes it possible to improve the crack resistance of the yellowing offset layer 5 while maintaining the gas barrier property for the resin substrate 1. Specifically, when the yellowing offset layer 5 is formed in contact with the resin substrate 1 using the ion-assisted method, the ion beam acceleration voltage and acceleration current are gradually increased. Also, the amount of argon, oxygen, etc. introduced during ion-assisted is adjusted. This makes it possible to continuously increase the film density of the yellowing offset layer 5 from the resin substrate 1 side.
[0044] Al2Ox (x<3) and SiOy (1≦y<2) can provide suitable gas barrier properties to the yellowing offsetting layer 5 depending on the film formation conditions. In order to effectively provide gas barrier properties to the yellowing offsetting layer 5, it is preferable to form the yellowing offsetting layer 5 in a process that increases the film density by an ion-assisted method or the like. However, if the yellowing offsetting layer 5 with high film density is formed in a layer close to the resin substrate 1, cracks are likely to occur in the yellowing offsetting layer 5. In other words, in order to provide the yellowing offsetting layer 5 with high gas barrier properties while suppressing the occurrence of cracks in the yellowing offsetting layer 5, it is preferable to form the yellowing offsetting layer 5 in a layer away from the resin substrate 1 by an ion-assisted method.
[0045] When the total number of anti-reflection films 4 and yellowing offsetting layers 5 is N, it is preferable to provide the yellowing offsetting layer 5 as the N / 2th layer or later, counting from the resin substrate 1 side, and it is more preferable to provide the yellowing offsetting layer 5 as the (N-1)th layer.
[0046] (Method of manufacturing optical members) The optical member 6 is manufactured by forming the anti-reflection film 4 and the yellowing offset layer 5 on the resin substrate 1 by a vapor phase deposition method. Here, a method for manufacturing the optical member 6 using an ion-assisted vapor phase deposition method will be described, but the optical member 6 can also be manufactured by various known methods such as a sputtering method, an ion plating method, and a vacuum deposition method.
[0047] First, the residual stress of the resin substrate 1 when the resin substrate 1 is formed is removed by annealing (4 hours at 120°C). Next, the resin substrate 1 is washed. The resin substrate 1 is washed by ultrasonic cleaning. The cleaning liquid for the resin substrate 1 is, for example, an HFE (hydrofluoroether) solvent. If foreign matter adheres to the resin substrate 1 before the anti-reflection film 4 or the like is formed on the resin substrate 1, the place where the foreign matter adhered to the resin substrate 1 becomes a pinhole after the anti-reflection film 4 is formed on the resin substrate 1. Then, oxygen and water vapor reach the resin substrate 1 through the pinhole, and the effect of the anti-reflection film 4 or the like in preventing the yellowing of the resin substrate 1 is reduced. Therefore, it is preferable to remove the foreign matter on the resin substrate 1 by washing. After washing the resin substrate 1, annealing may be performed again to drive out the moisture adsorbed on the resin substrate 1, if necessary.
[0048] The resin substrate 1 is set in a film-forming jig, and the resin substrate 1 is attached to a deposition dome so that the film-forming surface of the resin substrate 1 faces the deposition source. Next, the deposition dome is placed in a deposition chamber and evacuated. The interior of the deposition chamber is vacuumed to a desired degree, for example, 1.0×10 -3 When the pressure drops to about Pa, the first layer of the anti-reflection coating 4 is deposited. Specifically, the starting material filled in the crucible is heated by an electron beam and evaporated onto the resin substrate 1. At this time, the evaporated components receive kinetic energy from argon or oxygen gas molecules irradiated by the ion gun. As a result, a dense film is formed on the resin substrate 1. In addition, taking into consideration damage to the resin substrate 1 and temperature rise during deposition, the ion beam acceleration voltage of the ion gun is preferably about 500 V and the acceleration current is preferably about 500 mA.
[0049] Here, before forming the first layer of the anti-reflection coating 4 on the resin substrate 1, ion beam cleaning may be performed in which the resin substrate 1 is irradiated with an ion beam in order to remove dirt and improve surface activity. By performing ion beam cleaning, it is possible to improve the adhesion between the resin substrate 1 and the first layer of the anti-reflection coating 4. When the first layer of the evaporated film formed on the resin substrate 1 reaches a desired film thickness, heating of the starting material by the electron beam is stopped, and a second layer of the anti-reflection coating 4 is formed on the resin substrate 1. Once the desired number of layers have been formed on the resin substrate 1, a yellowing offset layer 5 is formed on the resin substrate 1.
[0050] The yellowing offset layer 5 is, for example, an Al2Ox (x<3) layer. Specifically, Al2O3 is used as a starting material, and the starting material is heated by an electron beam and evaporated on the resin substrate 1. As in the case of forming the anti-reflection film 4, an ion gun or the like may be used to assist the evaporation components. When the use of an ion gun or the like to effectively absorb short wavelengths is not possible, and when the film density of the yellowing offset layer 5 is to be reduced, normal vacuum evaporation may be performed without using an ion gun or the like. In addition, the deposition rate and the amount of oxygen supplied may be adjusted as necessary. When the deposition of the yellowing offset layer 5 is completed, the remaining layers of the anti-reflection film 4 are formed on the resin substrate 1.
[0051] After the remaining layers of the anti-reflection coating 4 have been deposited, the chamber is vented, the pressure in the deposition chamber is returned to atmospheric pressure, and the optical member 6 is removed from the deposition chamber. The deposition dome rotates at a predetermined speed during deposition. This makes the film thickness uniform on the same circumference of the deposition dome, improving the reproducibility of the optical characteristics within a deposition lot. When depositing the anti-reflection coating 4 and the like on both sides of the resin substrate 1, the surface of the resin substrate 1 on which no film has been deposited is placed opposite the deposition source. Then, deposition is performed on the other side of the resin substrate 1 in the same manner as on the side of the resin substrate 1 on which deposition has already been performed.
[0052] In this embodiment, the starting materials are heated by electron beams in all the depositions of the anti-reflection film 4 and the yellowing offsetting layer 5, but this is not limiting and a resistance heating method or the like can be used depending on the starting materials. In addition, in the deposition of each layer of the anti-reflection film 4 and the yellowing offsetting layer 5, gases such as air, oxygen, and nitrogen can be introduced as necessary to adjust the chemical composition of each layer.
[0053] Example 1 FIG. 3 is a diagram showing the configuration of the optical member according to the first embodiment and the reflectance of the optical member.
[0054] The optical member 6 includes a resin substrate 1 formed of COP (cycloolefin polymer) E48R (product name: manufactured by Nippon Zeon) in a lens shape, an anti-reflection film 4 consisting of a high refractive index layer TiO2 and a low refractive index layer SiO2 on the resin substrate 1, and a yellowing compensation layer 5 consisting of Al2Ox. The total number of layers of the anti-reflection film 4 and the yellowing compensation layer 5 is 7. The total thickness of the anti-reflection film 4 and the yellowing compensation layer 5 is 234.6 nm. The anti-reflection film 4 and the yellowing compensation layer 5 were formed using an ion-assisted method. In the optical member 6 of Example 1, the same anti-reflection film 4 and the yellowing compensation layer 5 can be formed on both sides of the resin substrate 1. Note that FIG. 3 shows a case where the anti-reflection film 4 and the yellowing compensation layer 5 are formed on only one side of the resin substrate 1. In addition, the optical member 6 has a low reflection region with a reflectance of 1.5% or less at light wavelengths of 380 to 700 nm as shown in FIG. 3.
[0055] FIG. 4 is a diagram illustrating the extinction coefficient of the yellowing offset layer according to the first embodiment.
[0056] The extinction coefficients of the Al2Ox layer (yellowing countermeasure layer 5), k450, k550, and k600, are 7.96×10 -3 , 4.75×10 -3 , 3.95×10 -3 The values of k550 / k450 and k600 / k450 are 0.59 and 0.50, respectively.
[0057] Table 1 shows the initial YI0, YI, and ΔYI of Example 1 (optical member 6 having yellowing offset layer 5) and Comparative Example 1 (optical member 6 not having yellowing offset layer 5). ΔYI (=2.82) of Example 1 is smaller than ΔYI (=3.21) of Comparative Example 1. That is, yellowing is suppressed in the optical member 6 of Example 1.
[0058] [Table 1]
[0059] Fig. 5 is a diagram showing the light absorption characteristics of the antireflection film and the yellowing offset layer according to Example 1. Fig. 5 shows the initial light absorption characteristics and the light absorption characteristics after 1500 hours at 120°C of an optical member 6 having a glass substrate (B270i) on which the antireflection film 4 and the yellowing offset layer 5 are formed.
[0060] Here, since the SiO2 layer and TiO2 layer constituting the anti-reflection film 4 do not have significant light absorption in the visible light region, the light absorption of the optical member 6 is substantially due to the light absorption by the yellowing offsetting layer 5. After 1500 hours at 120°C (shown by the dashed line), the amount of light absorption is significantly reduced as the visible light wavelength becomes shorter compared to the initial value (shown by the solid line). This is because the ΔYI of the yellowing offsetting layer 5 is a negative value, and therefore the ΔYI of the resin substrate 1 can be offset by the amount of the ΔYI of the yellowing offsetting layer 5.
[0061] Example 2 FIG. 6 is a diagram illustrating the configuration of an optical member according to Example 2 and the reflectance of the optical member.
[0062] The optical member 6 includes a resin substrate 1 made of COP E48R (product name: manufactured by Zeon Corporation) molded into a lens shape, an anti-reflection film 4 made of a high refractive index layer TiO2 and a low refractive index layer SiO2 on the resin substrate 1, and two yellowing offset layers 5 made of SiOy and Al2Ox.
[0063] The total number of layers of the anti-reflection film 4 and the yellowing offset layer 5 is 8. The total thickness of the anti-reflection film 4 and the yellowing offset layer 5 is 474.8 nm. The SiOy of the yellowing offset layer 5 was formed so that the film density gradually increased from the resin substrate 1 side. Furthermore, the SiOy of the yellowing offset layer 5 was formed so that the chemical composition gradually approached SiO2. Specifically, ion assist was not used in the initial stage of the film formation of the yellowing offset layer 5, and ion assist was started during the film formation. Here, the yellowing offset layer 5 was formed so that the ion beam acceleration voltage, acceleration current, and supply gas amount were gradually increased. The anti-reflection film 4 and Al2Ox were formed by the ion-assisted method as in Example 1. Also, in Example 2, the same anti-reflection film 4 and yellowing offset layer 5 were formed on both sides of the resin substrate 1. Note that FIG. 6 shows a case where the anti-reflection film 4 and the yellowing offset layer 5 are formed only on one side of the resin substrate 1.
[0064] As shown in the graph on the right of FIG. 6, the optical member 6 has a low reflectance region with a reflectance of 1.5% or less in the light wavelength range of 380-700 nm.
[0065] 7 is a diagram for explaining the extinction coefficient of the yellowing offset layer according to Example 2. FIG 7 shows the extinction coefficient of SiOy in the yellowing offset layer 5.
[0066] The SiOy layer (yellowing countermeasure layer 5) is a layer whose film quality changes continuously. Here, the extinction coefficient of the SiOy layer is a value calculated from the light absorption characteristics of SiOy, assuming that the layer made of SiOy has a uniform composition. The extinction coefficients of the SiOy layer, k450, k550, and k600, are 9.99×10 -3 , 1.37×10 -3 , 1.18×10 -3 The values of k550 / k450 and k600 / k450 are 0.14 and 0.12, respectively. Note that the Al2Ox layer has the same extinction coefficient as in Example 1, so a description thereof will be omitted.
[0067] Table 2 shows YI0, YI, and ΔYI of Example 2 (optical member 6 having yellowing offset layer 5) and Comparative Example 2 (optical member 6 not having yellowing offset layer 5). ΔYI (=2.27) of Example 2 is smaller than ΔYI (=3.01) of Comparative Example 1. That is, yellowing is suppressed in the optical member 6 of Example 2.
[0068] [Table 2]
[0069] FIG. 8 is a diagram showing the light absorption characteristics of the antireflection film and the yellowing offset layer according to Example 2.
[0070] FIG. 8 shows the initial light absorption characteristic (shown by a solid line) of the optical member 6 in which the anti-reflection film 4 and the yellowing compensation layer 5 shown in Example 2 are formed on a glass substrate (B270i) and the light absorption characteristic (shown by a dashed line) after 1500 hours at 120°C. Here, the SiO2 layer and TiO2 layer of the anti-reflection film 4 in Example 2 do not have significant light absorption in the visible light region, as in Example 1, so the light absorption of the optical member 6 is substantially the light absorption by the yellowing compensation layer 5. The light absorption after 1500 hours at 120°C (shown by a dashed line) is significantly reduced compared to the initial light absorption amount (shown by a solid line) as the visible light wavelength becomes shorter. This is because the ΔYI of the yellowing compensation layer 5 has a negative value, and the ΔYI of the resin substrate 1 can be offset by the ΔYI of the yellowing compensation layer 5.
[0071] Example 3 FIG. 9 is a diagram illustrating the configuration of an optical member according to Example 3 and the reflectance of the optical member.
[0072] The optical member 6 includes a resin substrate 1 made of COP E48R (product name: manufactured by Zeon Corporation) molded into a lens shape, an anti-reflection film 4 made of a high refractive index layer TiO2 and a low refractive index layer SiO2 on the resin substrate 1, and two yellowing compensation layers 5 made of SiOy and Al2Ox. The total number of layers of the anti-reflection film 4 and the yellowing compensation layer 5 is eight. The total thickness of the anti-reflection film 4 and the yellowing compensation layer 5 is 242.1 nm.
[0073] Of the yellowing offsetting layers 5, the SiOy at the interface side with the resin substrate 1 was formed by vacuum deposition, and the seventh layer, Al2Ox, was formed by ion-assisted deposition. The SiOy was formed using SiO as a starting material without introducing oxygen during film formation. The anti-reflection film 4 was formed by the ion-assisted deposition method, as in Example 1. In Example 3, similar anti-reflection films 4 and yellowing offsetting layers 5 were formed on both sides of the resin substrate 1. FIG. 9 shows a case where the anti-reflection film 4 and yellowing offsetting layer 5 are formed on only one side of the resin substrate 1.
[0074] As shown in the graph on the right of FIG. 9, the optical member 6 has a low reflection region with a reflectance of 1.5% or less in the light wavelength range of 380 to 700 nm.
[0075] Fig. 10 is a diagram for explaining the extinction coefficient of the yellowing offset layer according to Example 2. Fig. 10 shows the extinction coefficient of SiOy in the yellowing offset layer 5.
[0076] The extinction coefficients of the SiOy layer (yellowing countermeasure layer 5), k450, k550, and k600, are 3.35×10 -2 , 8.61×10 -3 , 4.70×10 -3 The values of k550 / k450 and k600 / k450 are 0.26 and 0.14, respectively. Note that the extinction coefficient of the Al2Ox layer is the same as that of Example 1, so a description thereof will be omitted.
[0077] Table 3 shows YI0, YI and ΔYI of Example 3 (optical member 6 having yellowing offset layer 5) and Comparative Example 3 (optical member 6 not having yellowing offset layer 5). ΔYI (=2.53) of Example 3 is smaller than ΔYI (=3.19) of Comparative Example 3. That is, yellowing is suppressed in the optical member 6 of Example 3.
[0078] [Table 3]
[0079] FIG. 11 is a diagram showing the light absorption characteristics of the antireflection film and the yellowing offset layer according to Example 2.
[0080] FIG. 11 shows the initial light absorption characteristic (shown by a solid line) of the optical member 6 in which the anti-reflection film 4 and the yellowing compensation layer 5 shown in Example 3 are formed on a glass substrate (B270i) and the light absorption characteristic (shown by a dashed line) after 1500 hours at 120°C. Here, the SiO2 layer and TiO2 layer of the anti-reflection film 4 in Example 3 do not have significant light absorption in the visible light region, as in Example 1, so the light absorption of the optical member 6 is substantially the light absorption by the yellowing compensation layer 5. The light absorption after 1500 hours at 120°C (shown by a dashed line) is significantly reduced compared to the initial light absorption amount (shown by a solid line) as the visible light wavelength becomes shorter. This is because the ΔYI of the yellowing compensation layer 5 has a negative value, so that the ΔYI of the resin substrate 1 can be offset by the ΔYI of the yellowing compensation layer 5.
[0081] FIG. 12 is a diagram showing a lens unit and an optical unit according to the present invention.
[0082] The optical unit 21 includes a lens unit 20 including a lens barrel 11, lenses 13-16, and an aperture 17, a protective filter 12, a cover glass 18, and an image sensor 19. Light incident on the lens unit 20 is collected by the lenses 13-16 on the image sensor 19 including a CCD or CMOS sensor. The light collected on the image sensor 19 is converted into an electrical signal and imaged as necessary. At least one of the lenses 13-16 mounted on the lens unit 20 is the optical member 6 described in this embodiment. That is, an anti-reflection film 4 and a yellowing offset layer 5 are formed on a resin substrate 1 in at least one of the lenses 13-16 constituting the lens unit 20.
[0083] The diaphragm 17 has a function of preventing unnecessary light from entering the imaging element 19. The diaphragm 17 may be provided between the lenses, or only partially between the lenses. When the optical unit 21 is used under severe temperature conditions, such as in an in-vehicle camera or a surveillance camera, the diaphragm 17 is preferably a diaphragm made of a metal substrate. The metal diaphragm 17 is formed, for example, by blackening a metal substrate by anodization and forming a film having a light absorbing function on the metal substrate by deposition or the like.
[0084] The protective filter 12 is a filter provided to protect the lens unit 20 from ultraviolet rays and dirt, and has functions such as UV protection, water repellency, oil repellency, hydrophilicity, and hard coating. Furthermore, the protective filter 12 may have a function of cutting a part of light in the visible light range. As described above, the yellowing of the resin substrate 1 is a phenomenon in which light absorption occurs mainly in the short wavelength range of the visible light range (zbar range of the color matching function) due to changes over time. In order to reduce the variation in the transmittance of light incident on the imaging element 19 before and after the yellowing of the resin substrate 1, it is sufficient to limit the transmittance of light in this range in advance.
[0085] According to the color matching function shown in Fig. 2, for example, by cutting light with a wavelength of about 450 nm or less, to which zbar has a high sensitivity, it is possible to effectively reduce the variation in the transmittance of light incident on the image sensor 19 before and after yellowing. Such a light cutting function is realized, for example, by laminating multiple layers of low refractive index layers and high refractive index layers alternately and utilizing the light interference effect. Note that the protective filter 12 does not necessarily need to be provided in the optical unit 21, and the function of the protective filter 12 may be imparted to the lens 13, which is the furthest from the image sensor 19.
[0086] The cover glass 18 is provided to prevent foreign matter from adhering to the imaging element 19, and is made of a quartz substrate in addition to a general glass material. The cover glass 18 may have a near-infrared cut function. When the light incident on the imaging element 19 is visualized (imaging), the color of the image may differ from the color visible to the human eye because it is affected by the sensitivity of the imaging element 19 in the near-infrared region. In this case, an infrared cut film or the like may be formed on the cover glass 18 to suppress the light in the near-infrared region from being incident on the imaging element 19. The infrared cut film can be provided, for example, by laminating multiple layers of low refractive index layers and high refractive index layers alternately and utilizing the light interference effect. In addition, instead of the cover glass 18, infrared absorbing glass into which metal ions having light absorption in the near-infrared region are kneaded may be used as necessary.
[0087] In order to prevent the resin substrate 1 from yellowing, the inside of the lens barrel 11 may be filled with an inert gas such as nitrogen or argon, or an oxygen scavenger made of iron or the like may be placed inside the lens barrel 11 so as not to block the optical path. This reduces the chance of the resin substrate 1 coming into contact with oxygen, and prevents discoloration of the resin substrate 1 due to oxidation, i.e., yellowing.
[0088] All of the lenses 13-16 mounted on the lens unit 20 may be resin lenses like the resin substrate 1, or glass lenses may be used for some of the lenses. When glass lenses are used as the lenses 13-16, it is preferable that the lens 13, which is the farthest from the imaging element 19 among the lenses constituting the lens unit 20, is a glass lens. This is because the lens 13, which is the farthest from the imaging element 19, is most likely to come into contact with oxygen and water vapor, and yellowing of the resin substrate 1 is most likely to progress.
[0089] 12 shows a configuration in which lens unit 20 has four lenses, but is not limited thereto, and lens unit 20 may have five or more lenses or three or less lenses. Furthermore, when optical members 6 of the present invention are used for all of lenses 13 to 16, the resin substrates 1 may be different for each lens, or may all be the same.
[0090] As described above, according to the present invention, it is possible to provide an optical member 6 having small changes in optical properties due to temperature by reducing changes in optical properties due to yellowing of the resin substrate 1 using the yellowing offset layer 5. Furthermore, the lens unit 20 and the optical unit 21 including the optical member 6 have small changes in optical properties due to temperature, and therefore can be used, for example, in vehicle-mounted cameras and surveillance cameras.
[0091] The invention is not limited to the above-described embodiments, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are appended to apprise the public of the scope of the invention. [Explanation of symbols]
[0092] 1. Resin substrate 2.Low refractive index layer 3. High refractive index layer 4.Anti-reflective coating 5.Yellowing prevention layer 6.Optical Components 11. Lens barrel 12.Protective Filters 13-16. Lenses 17. Aperture 18. Coverslip 19. Image sensor 20. Lens unit 21.Optical unit
Claims
1. A light-transmitting resin substrate; A yellowing compensation layer having a visible light transmittance that changes in a direction opposite to the change in the visible light transmittance of the resin substrate due to yellowing of the resin substrate, The yellowing offset layer is provided on the resin substrate. An optical member characterized by:
2. The resin substrate has a lens shape, Further provided on the resin substrate is an anti-reflection film composed of a plurality of layers each having a different refractive index. The optical member according to claim 1 .
3. The extinction coefficient of the yellowing countermeasure layer increases toward the short wavelength side of the visible light region, The ratio (k550 / k450) of the extinction coefficient k450 at a light wavelength of 450 nm to the extinction coefficient k550 at a light wavelength of 550 nm is 0.8 or less, The ratio (k600 / k450) of the extinction coefficient k450 at a light wavelength of 450 nm to the extinction coefficient k600 at a light wavelength of 600 nm is 0.8 or less; The optical member according to claim 1 .
4. The yellowing countermeasure layer contains an oxygen-deficient metal oxide. The optical member according to claim 1 .
5. The yellowing compensation layer is made of Al 2 Contains at least one of Ox (x<3) and SiOy (1≦y<2); The optical member according to claim 1 .
6. The yellowing offset layer is provided between the resin substrate and the anti-reflection film. The optical member according to claim 2 .
7. When the total number of layers of the anti-reflection film and the yellowing offsetting layer is N, at least one layer of the yellowing offsetting layer is provided above the N / 2 layer counted from the resin substrate side; The optical member according to claim 2 .
8. When the total number of layers is N, the yellowing offset layer is provided as the (N-1)th layer counted from the resin substrate side. The optical member according to claim 7 .
9. The film density of the yellowing offset layer provided between the resin substrate and the anti-reflection film increases as the film density increases from the interface between the resin substrate and the yellowing offset layer in the thickness direction of the yellowing offset layer.
7. The optical member according to claim 6.
10. A lens housing; A plurality of lenses housed in the lens housing; At least one lens of the plurality of lenses is the optical member according to any one of claims 1 to 9. A lens unit characterized by:
11. A lens unit according to claim 10; An imaging element; An optical unit characterized by:
Citation Information
Patent Citations
Lens unit
JP2016105194A