Optical member, method of manufacturing the same, and optical device
By bonding a metal film to a resin base material using a primary bond and atomic layer deposition, the optical member's adhesion and durability are enhanced, addressing adhesion issues and maintaining optical performance.
Patent Information
- Application Number
- JP2023075799
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for forming antireflection films on resin-based optical members suffer from insufficient adhesion, leading to cracks and peeling, while increasing film thickness to improve adhesion compromises optical performance.
A resin-based optical member configuration involving a metal film bonded to the resin base material through a primary bond, primarily covalent or ionic, using the atomic layer deposition method to enhance adhesion and durability, with a transparent optical film formed on the metal film to maintain optical performance.
The solution increases durability by preventing cracks and peeling while maintaining optical performance, as demonstrated by reduced crack formation and yellowing under harsh conditions.
Smart Images

Figure 2024160608000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical member, a manufacturing method thereof, and an optical device, and in particular to a technique for laminating an optical film onto a resin substrate. [Background technology]
[0002] Optical films have been formed on optical components such as lenses and optical filters. For example, optical films having functions such as anti-reflection or infrared cut using the optical interference of a thin film are known. The optical film imparts a unique function to the optical component. In addition, by forming an anti-reflection film as the optical film, ghosts and flares of the optical component can be suppressed. Furthermore, by forming an infrared cut film as the optical film, it is possible to suppress unnecessary light (e.g., infrared light) from entering an imaging element when the optical component is incorporated into an optical device. In this way, in a photographing optical system, an optical component having an optical film formed thereon can be used to suppress image degradation.
[0003] In recent years, from the viewpoints of weight and cost, resin materials have come to be used as the base material of optical components. For example, Patent Document 1 discloses that when forming an anti-reflection film on a plastic substrate, a metal film is provided between the plastic substrate and the anti-reflection film by a vacuum deposition method in order to improve adhesion. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2003-270402 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method described in Patent Document 1, the adhesion of the antireflection coating is insufficient under severe conditions, and there is a possibility that cracks and peeling may occur. On the other hand, when the thickness of the metal film is increased in order to improve the adhesion of the antireflection coating, there is a problem that the optical performance such as transmittance is deteriorated.
[0006] An object of the present invention is to improve the durability of an optical member using a resin substrate while maintaining the optical performance. [Means for solving the problem]
[0007] An optical member according to an embodiment of the present invention has the following configuration. A resin substrate; A metal film formed on the resin substrate; an optical film that is formed on the metal film and has transparency to a specific wavelength, The resin substrate and the metal film are bonded together by a primary bond. Effect of the Invention
[0008] It is possible to improve the durability of an optical member using a resin substrate while maintaining the optical performance. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view of an optical member according to an embodiment. [Diagram 2] FIG. 4 is an enlarged view of a cemented lens and a cemented portion according to an embodiment. [Diagram 3] FIG. 4 is an enlarged view of a cemented lens and a cemented portion according to an embodiment. [Figure 4] 1A and 1B are a cross-sectional view and a graph showing optical characteristics of an optical member according to a first embodiment. [Diagram 5] 5A to 5C are a cross-sectional view and a graph showing optical characteristics of an optical member according to Example 2. [Figure 6] FIG. 1 is a diagram illustrating the configuration of an optical device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments will be described in detail with reference to the attached drawings. Note that the following embodiments do not limit the invention according to the claims. Although the embodiments describe a number of features, not all of these features are essential to the invention, and the features may be combined in any manner. Furthermore, in the attached drawings, the same reference numbers are used for the same or similar configurations, and duplicated descriptions are omitted.
[0011] An optical member according to one embodiment of the present invention includes a resin substrate, a metal film formed on the resin substrate, and an optical film having a specific wavelength transparency formed on the metal film. Here, the resin substrate and the metal film are bonded by a primary bond. FIG. 1 shows a cross-sectional view of an optical member according to one embodiment. The optical member 4 shown in FIG. 1 is composed of a metal film 2 formed on a resin substrate 1 and an optical film 3 formed on the metal film 2.
[0012] (Resin substrate) The type of the resin substrate 1 is not particularly limited, and various resin materials can be used. Examples of the material of the resin substrate 1 include polyester-based, olefin-based, polyether-based, acrylic-based, styrene-based, PET (polyethylene terephthalate), PES (polyethersulfone), polysulfone-based, PEN (polyethylene naphthalate), PC (polycarbonate), and polyimide-based resins. In addition, the material of the resin substrate 1 may be a heat- or light-curable resin, and for example, a polyfunctional reactive polymer having a multi-branched structure such as an aromatic dendrimer can be used.
[0013] The resin substrate 1 may also be a lens. The material of this lens is not particularly limited, but from the viewpoint of moldability and refractive index characteristics, olefin-based, PC-based, acrylic, styrene-based, polyester-based, or polyurethane-based resins can be used. The above-mentioned heat- or light-curable resins can also be used. In order to improve the performance of the lens, a material with a high refractive index and a small Abbe number, such as a PC-based or fluorene-containing polyester resin, can be used as the material of the resin substrate 1. However, the shape of the resin substrate 1 is not particularly limited. For example, the optical member 4 may be a filter such as an infrared cut filter or a UV cut filter, and in this case, the resin substrate 1 may be a planar substrate.
[0014] Resin substrates are flexible, light, and easy to process, but are prone to deformation or deterioration due to heat, compared to inorganic substrates such as glass. In order to suppress deformation or deterioration due to heat, the resin substrate 1 in one embodiment has high heat resistance (high glass transition temperature Tg), for example, the glass transition temperature Tg is 120° C. or higher or 140° C. or higher. In order to suppress deformation of the resin substrate 1 due to water absorption, an olefin-based material, particularly a cycloolefin-based material, can be used as the material for the resin substrate 1.
[0015] In one embodiment, the difference between the refractive index of the resin substrate 1 at 0°C and the refractive index at 80°C for e-line is 0.8% or less, or 0.6% or less. Thus, the resin substrate 1 having a small change in refractive index due to temperature is suitable for applications in a wide range of operating temperatures, such as in-vehicle cameras or surveillance cameras. In one embodiment, the resin substrate 1 has a difference ΔYI between the yellowness index (YI: yellow index) after 1500 hours at 120°C and the initial YI, which is 10 or less, or 8 or less. Thus, the resin substrate 1 having a small change in optical properties due to high temperature, i.e., yellowing (ΔYI), is also suitable for applications in which the resin substrate 1 is installed in a high-temperature environment, such as in-vehicle cameras or surveillance cameras. In addition, in one embodiment, in order to increase the light transmittance of the optical member, the visible light wavelength transmittance of the resin substrate 1 is 80% or more, and the visible light wavelength transmittance after 1500 hours at 120°C is 60% or more. Here, the visible light wavelength refers to a wavelength of 400 to 700 nm.
[0016] The optical member according to the present embodiment may have multiple types of resin substrates 1. For example, when multiple substrates are used in the same optical device, such as a lens unit, optical properties such as aberration can be adjusted by using multiple resin substrates 1 with different refractive indices or Abbe numbers. The resin substrate 1 may be a cemented lens in which lenses of different resins are cemented together. A cemented lens is a lens in which lenses with different refractive indices are cemented together and integrated, and can be produced by cementing a convex surface and a concave surface with the same curvature. By using such a cemented lens, aberration correction can be improved.
[0017] When the resin substrate 1 is a cemented lens, each resin can form a primary bond with the metal film 2 regardless of the type of resin. In this way, even if the resin materials on the front and back of the lens are different, a strong bond can be obtained on both sides. Furthermore, the atomic layer deposition method (ALD method) described below has the characteristic of being able to form a conformal film, so that the metal film 2 can be formed so as to cover not only the main surfaces of the cemented lens but also the bonded part of the cemented lens. By forming the metal film 2 in this way, the bonding strength between the lenses in the cemented lens can be increased.
[0018] An optical adhesive can be used to bond the lenses together in the cemented lens. However, if the optical adhesive protrudes from the resin of the cemented lens, it becomes difficult to align the cemented lens with the optical axis when the cemented lens is placed in the optical system. For this reason, the optical adhesive is often applied so that it matches the end faces of the positioning surfaces of each resin that forms the cemented lens (i.e., the end faces of the resin and the end faces of the adhesive are aligned) or so that it is slightly concave with respect to the end faces of each resin (so that the adhesive does not protrude beyond the end faces of the resin). The metal film 2 formed by the ALD method has the property of being formed to follow even fine structures, so that it can cover the optical adhesive even if the optical adhesive is formed in this way. For example, as shown in FIG. 2, even if the optical adhesive 5 is formed concave with respect to the positioning surface 6 (i.e., the end face of the adhesive is located inside the end face of the resin), the metal film 2 is formed directly on the optical adhesive 5. For this reason, it is possible to effectively prevent water vapor and the like from entering the optical adhesive 5 and reducing the adhesive strength.
[0019] In this way, the metal film 2 formed by the ALD method can suppress the intrusion of water vapor or oxygen into the bonded portion, and is therefore effective in suppressing yellowing of the resin substrate. In order to more effectively suppress deterioration of the adhesive or yellowing of the resin substrate, an optical film, which will be described later, can also be formed by the ALD method so as to cover the bonded portion. Note that the effect of suppressing the decrease in adhesive strength of the optical adhesive in a cemented lens or the yellowing of the resin substrate due to oxygen or water vapor intrusion through the bonded portion can also be obtained by forming a film other than a metal film by the ALD method.
[0020] In FIG. 2, the ends of the resins to be bonded are aligned, but these ends do not necessarily need to be aligned. For example, one resin lens may be larger than the other resin lens as shown in FIG. 3. In such a case, the ALD method makes it possible to coat the area in the shadow of the larger resin lens around the bond between the resin lenses, so that it is easy to form the metal film 2 so as to cover the bond and the optical adhesive 5 even in such a case. As shown in FIG. 3, if the bond does not affect the alignment with the optical axis, the optical adhesive may protrude from the bond to an extent that does not affect the alignment. Note that the film obtained by the ALD method is a stack of monoatomic layers, so the film thickness is approximately uniform. Therefore, the influence of the variation in the thickness of the metal film 2 on the alignment is small.
[0021] The resin substrate 1 can be molded, for example, by injection molding. Specifically, a cavity including a lens portion, an outer periphery, and a gate portion, which is formed by butting a fixed mirror surface piece and a movable mirror surface piece, is filled with resin material through the gate portion, and when the resin solidifies, the mold is opened and the substrate is removed. Finally, the gate portion is cut off. In this manner, lenses having shapes that are difficult to process when using glass materials, such as aspherical lenses or high curvature lenses, can be relatively easily manufactured. Note that the molding method of the resin substrate 1 is not limited to injection molding, and various methods such as injection compression molding or cast polymerization can be used.
[0022] For the purpose of removing moisture adsorbed by the resin substrate 1 or releasing internal stress due to molding, the resin substrate 1 may be annealed before forming the metal film 2 and the optical film 3. The annealing is suitably performed at a temperature of about 80° C. or higher and about the Tg of the resin substrate 1 or lower, preferably about 15° C. lower than the Tg of the resin substrate, for 0.5 hours or more, more preferably 1 hour or higher and 24 hours or less, more preferably 12 hours or less.
[0023] (Metal Film) The metal film 2 is formed on the resin substrate 1. There is no particular limitation on the metal constituting the metal film 2, but a base metal can be used to reduce costs. Examples of metals constituting the metal film 2 include Al, Ni, Ti, Nb, Ta, W, and Hf. The metal film 2 may be formed of a molecular layer of one type of metal, or may be formed of molecular layers of multiple different types of metals.
[0024] The metal film 2 is formed by metallic bonding between metals. Films formed by metallic bonding have excellent ductility and can be deformed relatively freely. In metallic bonding, metal atoms are bound by the Coulomb force between free electrons that are delocalized throughout the material, not just in the vicinity of a specific atomic nucleus, and the positively charged atomic nucleus of the metal. Because the free electrons have a wide range of movement, the bond is not easily broken even if the atomic nucleus moves. Therefore, even if the resin substrate 1 expands or contracts due to heat or water absorption, the metal film 2 easily deforms accordingly, and the occurrence of cracks or peeling can be suppressed.
[0025] The metal film 2 forms a layer (continuous film). In this way, the metal film 2 in contact with the resin substrate 1 is a layer, so that the intrusion of oxygen and water vapor into the resin substrate 1 can be suppressed. In this way, the intrusion of oxygen or water vapor from the interface between the resin substrate 1 and the metal film 2 can be suppressed, so that the yellowing of the resin substrate 1 can be suppressed. In addition, by forming the metal film 2 in this way, the occurrence of an interface where the resin substrate 1 and the first layer of the optical film come into contact with each other is suppressed, and the occurrence of cracks or peeling in this region is also suppressed. According to this configuration, it is possible to suppress the occurrence of absorption in the short wavelength region of visible light wavelengths in the optical member 4, which is caused by oxygen or water vapor in the atmosphere reaching the resin substrate 1 and oxidizing the resin substrate 1 due to the influence of the temperature band used.
[0026] Here, whether the metal film 2 is a continuous film, i.e., a layer, due to its thickness can be determined, for example, from the relationship between the sheet resistance Rs and the surface adhesion weight density t. Here, the film thickness can be determined based on the weight per area. In a semi-logarithmic graph with the logarithmic scale of the sheet resistance Rs on the vertical axis and the surface adhesion weight density t on the horizontal axis, when the metal film 2 is a layer, Rs=ρ / t holds regardless of the surface adhesion weight density t. Here, ρ indicates resistivity. That is, ln Rs=ln ρ-ln t holds, and in a narrow range of change in the surface adhesion weight density t, the change in ln t is very small, and the sheet resistance Rs is approximately parallel to the horizontal axis in the semi-logarithmic graph. On the other hand, when the metal film 2 does not form a layer, Rs is determined by the nucleus density, the dimensions of the nucleus, and the distance between the nuclei, and does not show film thickness dependency. Therefore, the sheet resistance Rs is a curve approximately parallel to the vertical axis in the semi-logarithmic graph.
[0027] As described above, the metal film 2 is formed on the resin substrate 1. In one embodiment, in order to protect the resin substrate 1 as described above, the metal film 2 completely covers the optical principal surface of the resin substrate 1. On the other hand, in one embodiment, the metal film 2 covers not only the optical principal surface of the resin substrate 1 but also the end of the resin substrate 1. The optical principal surface here refers to the surface into which light is incident when the optical member 4 is mounted in the optical system and the surface opposite thereto. By covering the resin substrate 1 up to the end with the metal film 2, it is possible to suppress the intrusion of oxygen or water vapor from the end of the resin substrate 1. According to this configuration, the yellowing of the resin substrate 1 can be more effectively suppressed. Furthermore, according to this configuration, the expansion caused by the resin substrate 1 absorbing moisture can be suppressed, so that cracks are less likely to occur.
[0028] The metal film 2 may not be a main element for achieving the optical characteristics of the optical member 4 (for example, low reflection characteristics when the optical film is an AR film). Therefore, the metal film 2 can be thinner than each thin film forming the optical film 3. More specifically, the metal film 2 may be thinner than the thinnest thin film among the thin films forming the optical film 3. Specifically, the thickness of the metal film 2 can be 5 nm or less. In particular, when the optical member 4 is required to have light transmittance, it is preferable that the light loss caused by forming the metal film 2, that is, the light absorption by the metal film 2, is small. From this viewpoint, the thickness of the metal film 2 is preferably 3 nm or less, more preferably 2 nm or less, and even more preferably 1 nm or less. In one embodiment, the metal film 2 is formed by the ALD method, and therefore has a thickness of at least one atomic layer. A continuous layer having such a thickness (a layer that covers the optical main surface of the resin substrate 1 without any breaks) can be formed by the ALD method described later.
[0029] In one embodiment, the metal film 2 is formed on both sides of the resin substrate, and has a light transmittance of 60% or more at 550 nm. Such an optical member 4 can be obtained, for example, by setting the thickness of the metal film 2 to about 3 nm or less. Even if the optical film is not an AR film, it is preferable that the light absorption of the metal film 2 in the light transmission region of the optical film 3 is small. For example, when the optical film 3 has a transmission region in the infrared region, the thickness of the metal film 2 can be selected so that the spectral transmittance of the optical member 4 in this transmission region (for example, the infrared region of 700 nm to 1200 nm) is 60% or more.
[0030] (linear combination) The metal film 2 is bonded to the resin substrate 1 by a primary bond. The primary bond is a chemical bonding force, generally including covalent, ionic, and metallic bonds. However, since there is no metallic bond between the resin substrate 1 and the metal film 2, the primary bond is substantially a covalent or ionic bond, and is preferably a covalent bond. The primary bond is distinguished from a mechanical bond such as an anchor effect and a secondary bond such as an intermolecular force. However, the metal film 2 and the resin substrate 1 may be bonded to each other by these bonds in addition to the primary bond. In one embodiment, the primary bond plays a major role in the bond between the metal film 2 and the resin substrate 1, that is, the metal film 2 is bonded to the resin substrate 1 mainly by a primary bond.
[0031] The bond between the resin substrate 1 and the metal film 2 can be evaluated by, for example, XPS (X-ray photoelectron spectroscopy). When the metal element constituting the metal film 2 is M and the carbon atom of the resin substrate 1 is C, the primary bond between the resin substrate 1 and the metal film 2 can be expressed as COM. Therefore, in the optical member 4, OM bonds and CO bonds resulting from the primary bonds are detected at the interface between the resin substrate 1 and the metal film 2. For example, when a region including the interface between the resin substrate 1 and the metal film 2 is measured by XPS, if an OM bond is detected, it can be evaluated that the resin substrate 1 and the metal film 2 are bonded by a primary bond.
[0032] In addition, the ratio of OM bonds among all bonds containing M is P O-M , the ratio of CO bonds among all bonds containing C is P C-O In this case, P O-M / P C-O is preferably 0.1 or more, and more preferably 0.2 or more. O-M / P C-O is preferably 10.0 or less, and more preferably 5.0 or less. When the resin substrate 1 and the metal film 2 are bonded mainly by primary bonds, P O-M / P C-O can take such a range. Note that P O-MWhen the molecular skeleton of the resin base material 1 contains a C-O bond, it can be obtained by subtracting the C-O bond derived from the molecular skeleton.
[0033] The bond between the resin substrate 1 and the metal film 2 can also be evaluated by the adhesion strength. The adhesion strength can be evaluated, for example, by a micro-scratch method using an ultra-thin film scratch tester (CSR-2000: manufactured by Rhesca). In the micro-scratch method, a stylus attached to a phonograph needle-type sensor scratches a sample while increasing the load on the stylus, and obtains the load value at which the thin film peels off. The adhesion strength between the resin substrate 1 and the metal film 2 can be evaluated based on the load value obtained here. When the resin substrate 1 and the metal film 2 are bonded together by a primary bond, the load value is larger than when the metal film 2 is formed on the resin substrate 1 by the vacuum deposition method. When the resin substrate 1 and the metal film 2 are bonded together mainly by a primary bond, the load value is 120% or more, preferably 150% or more, compared to when the metal film 2 is formed on the resin substrate 1 by the vacuum deposition method. When the metal film 2 is formed on the resin substrate 1 by the vacuum deposition method, the resin substrate 1 and the metal film 2 are not bonded together mainly by a primary bond.
[0034] When the bond between the resin substrate 1 and the metal film 2 is evaluated as a primary bond by either the analysis by XPS or the evaluation by the micro-scratch method, it is considered that the bond between the resin substrate 1 and the metal film 2 is a primary bond. It is preferable that the bond between the resin substrate 1 and the metal film 2 is evaluated as a primary bond by both evaluations, since it is more strongly considered that the bond between the resin substrate 1 and the metal film 2 is a primary bond.
[0035] (Metal Film Forming Method) A method for forming the metal film 2 so as to be bonded to the resin substrate 1 by primary bonds includes the atomic layer deposition method (ALD method). Here, the ALD method will be explained. The ALD method is a vapor phase thin film formation method similar to CVD (Chemical Vapor Deposition). In CVD, two types of precursors are simultaneously introduced into a reaction chamber, and the reaction product is deposited on the substrate, whereas in ALD, only one type of precursor (first precursor) is introduced into the reaction chamber, and the first precursor that is not adsorbed to the substrate is discharged outside the chamber. After that, the first precursor adsorbed to the substrate is oxidized or reduced by the action of the second precursor, oxygen, plasma, or the like to form a layer. At this time, the substrate 1 and the layer to be formed are bound by primary bonds, that is, a primary bond (covalent bond or ionic bond) is formed between the resin substrate 1 and the metal film.
[0036] In addition, when forming the metal film 2 on the resin substrate 1, a hydroxyl group (OH group) is formed on the surface of the resin substrate 1 by plasma or ozone treatment before introducing the first precursor into the chamber. That is, when the carbon atom on the surface of the resin substrate 1 is C, a C-OH structure is formed on the surface of the resin substrate 1. When the metal species of the first precursor, which is the raw material of the metal film 2, is M, when the first precursor is introduced into the chamber, M is adsorbed on the surface of the resin substrate 1 so that OH of C-OH on the surface of the resin substrate 1 and M bond to form an M-OH bond. Then, the ligand of M or hydrogen of M-OH is released by the action of the second precursor, oxygen, plasma, etc. In this way, a primary bond represented by COM is formed between the resin substrate 1 and the metal film 2. In this way, the first layer of the metal film 2, which is the interface layer between the resin substrate 1 and the metal film 2, is mainly bonded by a covalent bond or an ionic bond. On the other hand, it is considered that the second and subsequent layers forming the metal film 2 form bonds between metals, that is, metallic bonds.
[0037] In the ALD method, the precursors are adsorbed on the entire exposed surface of the substrate, but the precursors do not react with each other. Therefore, a monoatomic layer is uniformly formed on the entire surface of the film formation area. In other words, the metal film 2 formed by the ALD method is a layer in which atomic layers are deposited. In other words, the ALD method can form a film with good shape conformability, and the film thickness control precision is also very high. In addition, the metal film 2 formed by the ALD method is easy to form a continuous layer even when the film thickness is thin, so it has higher gas barrier properties than metal films formed by other processes.
[0038] Here, the ALD method includes a thermal ALD method in which a reaction is accelerated by heat, and a PEALD (Plasma Enhanced Atomic Layer Deposition) method in which a reaction is accelerated by plasma. The most suitable method can be selected in consideration of the heat resistance of the resin substrate 1 and the precursor to be used.
[0039] Metal films that are not primarily bonded to a resin substrate can be formed by physical vapor deposition (hereinafter referred to as PVD) such as vacuum deposition or sputtering. It is known that there are three types of metal film formation processes by PVD: nucleus growth type, single layer growth type, and a combination of these. Here, the single layer growth type and the combination type occur only under certain special conditions. The former condition is, for example, when the substrate is smooth at the atomic level, when the substrate surface atomic lattice spacing and the metal film atomic lattice spacing have an equal or small integer ratio, or when the surface movement of metal atoms incident on the substrate is active (the substrate temperature is high). The latter condition is, for example, when a metal film is formed on a metal substrate under specific conditions. That is, when a film is formed on a resin substrate, the metal film basically grows by nucleus growth type.
[0040] In the nucleus growth, some of the metal atoms incident on the surface of the resin substrate are reflected, and some are adsorbed by the substrate. As the adsorbed metal atoms move on the surface of the substrate, some of them are re-evaporated, and some form two-body particles with other metal atoms. By repeating this process, a cluster is formed, which is a combination of multiple metal atoms. The cluster repeatedly collides with metal atoms present on the substrate surface and releases single atoms, and becomes a stable nucleus (island) when the number of atoms constituting the cluster exceeds a certain critical value. The stable nucleus continues to grow and merges with adjacent stable nuclei to become a continuous film (layer). Here, the film thickness at which the stable nuclei become a continuous film is about 6 nm, depending on the substrate, film type, or film formation conditions. That is, when a metal film is formed as a layer on a resin substrate by PVD, the metal film has a thickness of about 6 nm or more. However, if a metal film with a thickness of about 6 nm is formed on both sides of the resin substrate, there is a high possibility that the light transmittance at 550 nm of the entire optical component will be less than 60%.
[0041] (optical film) The optical film 3 is formed on a metal film and has light transmittance at a specific wavelength. Having light transmittance means that the transmittance at a specific wavelength is 80% or more. The types of the optical film 3 include, for example, an AR film, an infrared cut film, an ultraviolet cut film, and an infrared pass film. In these films, the desired spectral characteristics can be obtained by optical interference of thin films with different refractive indexes. In this way, the optical film 3 can have a configuration in which multiple thin films are stacked. For example, the optical film 3 may have a stacked structure of thin films with multiple refractive indexes. The main optical characteristics of the optical member 4 are obtained by the optical film 3.
[0042] As an example, an AR film (anti-reflection film) will be described. In the AR film, low reflection in a desired wavelength region is realized by alternately laminating low refractive index layers and high refractive index layers. The outermost layer (anti-reflection layer) of the AR film can be a low refractive index layer. As the low refractive index layer and high refractive index layer used in the AR film, MgF2, SiO2, Al2O3, MgO, HfO2, ZrO2, La2Ti2O7 (LaTiO3), Si3N4, Ta2O5, Nb2O5, TiO2, etc. can be used.
[0043] In order to minimize the stress of the entire AR film, materials having stress in different directions can be selected for the low refractive index layer and the high refractive index layer. For example, as materials having opposing stresses and a large refractive index difference, SiO2 having compressive stress can be selected as the low refractive index material, and TiO2 having tensile stress can be selected as the high refractive index material. A large refractive index difference contributes to suppressing cracks because it can reduce the number of layers (film thickness) required to obtain the desired spectral characteristics.
[0044] At least one layer of the optical film 3 can be an Al2O3 layer. Since Al2O3 has high gas barrier properties, in an optical member 4 using a resin substrate 1, it is possible to suppress changes in optical properties (e.g., yellowing) that occur when the resin substrate 1 is oxidized due to the influence of oxygen or the like. A plurality of Al2O3 layers may be provided. In this case, in order to effectively utilize the gas barrier properties, the Al2O3 layer can be disposed in a location close to the substrate and in a location close to the surface, and in particular, can be disposed immediately below the antireflection layer, which is the first layer and the outermost layer of the AR film.
[0045] When the resin substrate 1 is used, the AR film is preferably composed of 4 layers or more, more preferably composed of 6 layers or more. On the other hand, the AR film is preferably composed of 12 layers or less, more preferably composed of 10 layers or less. The gas barrier performance of a laminate such as an AR film tends to increase as the number of layers increases. This is because even if there is a defect in the layer forming the laminate, gas such as oxygen or water vapor is unlikely to reach the resin substrate 1 if there is no defect in the same area in other layers. In other words, the more the number of layers, the easier it is to suppress deterioration such as yellowing of the resin substrate 1 even if a minute film defect occurs in the layer forming the AR film. On the other hand, if the number of layers is increased too much, the AR film is likely to crack due to film stress, especially when a resin substrate 1 having a curvature like a lens is used. The number of layers here refers to the number of layers of thin films that exhibit optical interference.
[0046] The thickness of the AR film is preferably 200 nm or more, more preferably 250 nm or more. On the other hand, it is preferably 600 nm or less, more preferably 500 nm or less. By increasing the film thickness, it becomes easier to obtain an anti-reflection effect due to the interference effect of the thin film, and the gas barrier effect of the AR film is improved. On the other hand, by decreasing the film thickness, cracks are less likely to occur.
[0047] In addition, the thickness of each of the low refractive index layers and the high refractive index layers, except for the outermost anti-reflection layer, is preferably 80 nm or less. By reducing the thickness of each layer, the stress of the layer can be reduced, and the occurrence of cracks or peeling can be suppressed, particularly when the layer is formed on a lens substrate. In order to prevent reflection, the outermost layer can be formed so that the optical thickness at the target wavelength λ is approximately λ / 4.
[0048] So far, the preferred conditions for forming an AR film on a lens substrate have been described. However, the preferred conditions can be selected appropriately according to the optical film to be formed. For example, when forming an optical film that requires a large number of layers and a film thickness to obtain optical properties, such as an infrared cut film or an infrared pass film, the number of layers and the film thickness can be determined to a degree that does not cause cracks.
[0049] The optical film 3 may be formed by the ALD method, as with the metal film 2. On the other hand, the optical film 3 may be formed by the CVD method or a PVD method such as a sputtering method, an ion plating method, or a vacuum deposition method. In applications where conformality is important, such as when a lens is used as the resin substrate 1, it is advantageous to form the optical film 3 by the ALD method. On the other hand, when productivity is important, the CVD method or the PVD method, which has a faster film formation speed than the ALD method, can be selected. In addition, the optical film 3 may be formed by using a plurality of methods as necessary, for example, a part of the AR film may be formed by the ALD film, and the remaining part may be formed by the CVD method or the PVD method.
[0050] So far, the case where each layer of the optical film 3 is composed of a single material has been described. On the other hand, the optical film 3 may be formed by stacking molecular layers at a level that does not cause optical interference, utilizing the characteristics of the ALD method. For example, by stacking molecular layers with different refractive indices, a layer with an intermediate refractive index can be formed. This method increases the degree of freedom in film design. In addition, by stacking molecular layers with opposite stress directions, a layer with very small film stress can be formed, and the occurrence of cracks in the optical film 3 can be suppressed.
[0051] The optical member 4 according to one embodiment of the present invention has the metal film 2 bonded to the resin substrate 1 by primary bonding, and thus has improved durability such as crack resistance and yellowing resistance as described above. In particular, the optical member 4 has improved durability in harsh environments. Durability in harsh environments can be confirmed, for example, by evaluating the cracking and yellowing index (ΔYI) that occurs after a high temperature test (120°C / 3000hr) or a high temperature and high humidity test (85°C 85% / 2000hr).
[0052] ΔYI can be calculated as follows. ΔYI is a value obtained by subtracting YI before the test from YI after the test, and YI before and after the test are calculated according to formula (1). In formula (1), X, Y, and Z are the total values obtained by multiplying the spectral data (T) by the relative output (S) of the D65 illuminant and the tristimulus values (x, y, z) of the standard observer, which are psychophysical quantities, for each wavelength (λ). YI is calculated with a 2-degree visual field, and Cx and Cz use the coefficients shown below. Spectral data (T) can be measured using a spectrophotometer (e.g., U-4100: manufactured by Hitachi High-Tech Corporation).
number
number
[0053] In the optical member 4 according to one embodiment of the present invention, which has a metal film 2 bonded to the resin substrate 1 by primary bonding, no cracks are observed, for example, after a high temperature test (120°C / 3000hr) and a high temperature / high humidity test (85°C / 85% / 2000hr). In particular, even if cracks are observed in an optical member having a metal film formed on a resin substrate by a vacuum deposition method and having a layer structure similar to that of the optical member 4, no cracks are observed in the optical member 4 according to one embodiment of the present invention after the same high temperature test or high temperature / high humidity test. According to one embodiment of the present invention, cracks are unlikely to occur in the optical member, which is believed to be due to the good adhesion of the metal film 2 to the resin substrate 1.
[0054] In addition, the optical member 4 according to one embodiment of the present invention, which has the metal film 2 bonded to the resin substrate 1 by primary bonding, has a low ΔYI, for example, 4 or less, after a high temperature test (120°C / 3000hr) and a high temperature and high humidity test (85°C 85% / 2000hr). In particular, even if an optical member having a metal film formed on a resin substrate by a vacuum deposition method and having a layer structure similar to that of the optical member 4 has a high ΔYI, for example, 9 or more, after a high temperature test (120°C / 3000hr) or a high temperature and high humidity test (85°C 85% / 2000hr), the optical member 4 according to one embodiment of the present invention has a lower ΔYI, for example, 4 or less, after the same high temperature test or high temperature and high humidity test. Thus, according to one embodiment of the present invention, yellowing of the optical member is suppressed, and this is believed to be due to the provision of a high-quality metal film 2 with few film defects.
[0055] Moreover, an optical member 4 according to another embodiment of the present invention includes a resin substrate 1, a metal film 2 having a thickness of 3 nm or less formed on the resin substrate 1, and an optical film 3 having a light-transmitting property at a specific wavelength formed on the metal film 2. Such an optical member 4 can be produced, for example, by providing the metal film 2, which is a continuous film, by the ALD method as described above. With such a configuration, it is possible to improve durability (for example, crack resistance and yellowing resistance in harsh environments) while maintaining the light transmittance of the optical member 4 as described above.
[0056] (Manufacturing method) A method for manufacturing an optical member 4 according to the present invention will be described. In the following, a case where the metal film 2 and the optical film 3, which is an AR film, are both formed by the ALD method will be described. However, the method for manufacturing the optical member 4 is not limited to the following method, and for example, the optical film 3 may be a film other than an AR film, or the AR film may be formed by another method. In the following, a case where the metal film 2 is Ni, the first layer of the AR film is an Al2O3 layer, and the subsequent layers are an alternating laminate of SiO2 and TiO2 will be described.
[0057] First, the resin substrate 1 is set in a film-forming jig and placed in a chamber. After the resin substrate 1 is placed in the reaction chamber, a vacuum pump is used to adjust the pressure in the chamber to a desired level. If necessary, a heater is used to adjust the temperature of the resin substrate 1 or the chamber. Here, as an annealing treatment, the resin substrate 1 may be held in the chamber for a certain period of time before the start of film formation.
[0058] When preparations for film formation are complete, sites on the resin substrate 1 where the first precursor of the metal film 2 can be adsorbed, such as OH groups, are provided. To provide the OH groups, for example, plasma or UV / O3 can be used. Alternatively, the OH groups may be adsorbed on the substrate by using water molecules as a precursor. Next, the first precursor (in this example, Ni(Cp)2: bis(cyclopentadienyl)nickel(II)), which is the source gas of the metal film 2 to be formed, is adsorbed on the substrate. At this time, the first precursor can be adsorbed at the locations where the OH groups formed on the resin substrate 1 are exposed, so the adsorbed first precursor forms a monolayer on the film formation surface regardless of the shape of the resin substrate 1.
[0059] Next, the excess first precursor that was not adsorbed on the deposition surface and the gas generated when the first precursor was adsorbed on the deposition surface are purged (removed). Then, the ligand is removed from the first precursor adsorbed on the resin substrate 1 using a second precursor that oxidizes or reduces the first precursor adsorbed on the deposition surface, or radical ozone plasma. In this way, a monomolecular film of Ni that constitutes the metal layer 2 is formed on the resin substrate 1.
[0060] Next, the first precursor is further adsorbed to the Ni film formed on the resin substrate 1. From the second time onwards, the formation of the metal layer 2 proceeds without necessarily providing a site for the first precursor to be adsorbed, such as an OH group. In this case, the first precursor is adsorbed to the film formation surface, i.e., the metal layer already formed on the resin substrate 1, while, for example, part of the ligand is desorbed. When the first precursor is sufficiently adsorbed to the already formed metal layer, the excess first precursor and the gas generated when the first precursor is adsorbed to the film formation surface are purged. Furthermore, the ligand is removed from the first precursor adsorbed to the film formation surface using a second precursor that oxidizes or reduces the first precursor adsorbed to the film formation surface, or radicals, ozone, plasma, etc. In this way, a further Ni film that constitutes the further metal film 2 is formed. From the second time onwards, it is considered that the Ni film forms a metallic bond with the already formed Ni film. By repeating this process, a metal film 2 having a desired film thickness can be formed.
[0061] In this example, Ni(Cp)2 was used as the first precursor, but the first precursor is not limited to this. As the first precursor, for example, an organonickel complex such as Ni(dmamb)2, Ni(hfip)2, Ni(iPrMeCOCNtBu)2, Ni(acac)2, Ni(acac)2(tmeda), or Ni(Chex)(Cp) can be used. In the above example, Ni was used as the metal film 2, but when another metal is used, an organometallic complex corresponding to the metal can be used as the first precursor.
[0062] As the second precursor, for example, H2, NH3, O2, H2O, N2H4, or CH3OH can be used alone or in a suitable mixture. When introducing each precursor, a carrier gas, for example, an inert gas such as N2 or Ar, can be used.
[0063] After obtaining the metal film 2 with the desired thickness by repeating the above cycle, an AR film is formed as the optical film 3. First, OH groups, which are sites for adsorbing a first precursor (TMA: trimethylaluminum) for forming an Al2O3 layer, which is the first layer of the AR film, are provided on the metal film 2. In order to provide the OH groups, for example, plasma or UV / O3 may be used, or for example, water molecules may be used as the precursor.
[0064] Next, TMA is supplied into the reaction chamber. At this time, TMA bonds with OH groups on the metal film while releasing CH4. Next, the excess TMA and the generated CH4 are removed by purging. For purging, inert gas such as N2 or Ar can be used. Next, water molecules are supplied as the second precursor into the deposition chamber. Then, the unreleased methyl groups of the first precursor adsorbed on the metal film 2 are replaced with OH groups. After this, by further supplying the first precursor, TMA, is adsorbed to the OH groups while generating CH4 again. By repeating this cycle, an Al2O3 layer of the desired thickness is formed.
[0065] Next, the SiO2 layer is formed. The SiO2 layer can be formed in a film formation process similar to that of the Al2O3 layer described above, by using TDMAS (trisdimethylaminosilane) as the first precursor and water molecules as the second precursor.
[0066] After the SiO2 layer is formed to the desired thickness, the TiO2 layer is formed. The TiO2 layer can be formed in a process similar to that of the Al2O3 layer described above, for example, by using TDMAT (tetrakis(dimethylamino)titanium) as the first precursor and water molecules as the second precursor.
[0067] In the above example, TMA, TDMAS, and TDMAT are used as the first precursors for forming the Al2O3 layer, SiO2 layer, and TiO2 layer, respectively, but the first precursor is not limited to these. For example, aluminum trichloride, trimethylaluminum, triethylaluminum, chlorodimethylaluminum, aluminum ethoxide, aluminum isopropoxide, or aluminum secbutoxide can be used as the first precursor to form the Al2O3 layer. Also, silane tetrachloride, bisdiisopropylaminosilane, bisdiethylaminosilane, or the like can be used as the first precursor to form the SiO2 layer. Also, titanium tetrachloride, tetrakis(ethylmethylamido)titanium, or titanium isopropoxide bis(acetylacetonate) can be used as the first precursor to form the TiO2 layer.
[0068] (optical equipment) An optical device according to an embodiment includes an optical member 4 and an imaging element that captures an image of light that has passed through the optical member. Fig. 6 shows an optical device 21, which is an example of such an optical device. The optical device 21 includes a lens unit 20 that includes a lens barrel 11, lenses 13-16, and an aperture 17, and further includes a protective filter 12, a cover glass 18, and an imaging element 19. Light that enters the lens unit is focused by the lenses 13-16 on the imaging element 19, such as a CCD or CMOS sensor. The light focused on the imaging element 19 is converted into an electrical signal in the imaging element 19, and is visualized as necessary.
[0069] Here, at least one of the lenses 13-16 of the lens unit 20 is the optical member 4. That is, at least one of the lenses constituting the lens unit 20 has a structure in which at least a metal film 2 and an optical film 3 are formed on a resin base material 1. The lenses 13-16 mounted on the lens unit 20 can be a combination of various lenses such as glass lenses and resin lenses. When a glass lens is used, the lens 13, which is the furthest from the imaging element 19, is most likely to come into contact with oxygen and water vapor, and therefore a glass lens, which is less likely to deteriorate, can be used as the lens 13.
[0070] The diaphragm 17 has a function of preventing unnecessary light from entering the imaging element 19. The diaphragm 17 may be provided between each of the lenses 13 to 16, or may be provided only partially between the lenses 13 to 16. When the optical device 21 is used under severe temperature conditions such as an in-vehicle camera or a surveillance camera, the diaphragm 17 formed of a metal substrate can be used. As the material for such a metal diaphragm 17, for example, a metal plate blackened by anodization, or a metal plate on which a film having a light absorbing function is formed by vapor deposition or the like can be used.
[0071] The protective filter 12 is a filter for protecting the lens unit 20 from ultraviolet rays, dirt, or damage. The protective filter 12 can have functions such as UV cut, water repellency, oil repellency, hydrophilicity, or hard coating. Furthermore, the protective filter 12 may have a function of cutting off a part of the wavelengths in the visible region.
[0072] When a resin base material is used as the material of the lenses 13 to 16, light absorption may occur mainly in the short wavelength region of the visible region due to yellowing. In order to suppress the variation in transmittance before and after the yellowing of the resin base material, that is, the variation in the amount of light incident on the imaging element 19, the light transmission in this region can be limited in advance. For example, by cutting light wavelengths of about 450 nm or less that are significantly affected by yellowing, the variation in the light incident on the imaging element 19 before and after yellowing can be effectively reduced. Such a cutting function can be obtained by the light interference effect, for example, by laminating multiple layers of low refractive index layers and high refractive index layers alternately. It is not necessary to provide the protective filter 12. On the other hand, the lens 13 farthest from the imaging element 19 may have the function of the protective filter 12.
[0073] The cover glass 18 is provided to prevent foreign matter from adhering to the imaging element 19. The material of the cover glass 18 may be a glass material, or a quartz substrate or the like. The cover glass 18 may have a near-infrared cut function. When imaging light incident on the imaging element 19, if the imaging element 19 has sensitivity in the near-infrared region, a difference may occur between the color of the image and the color visible to the human eye. In such a case, an infrared cut film or the like can be formed on the cover glass 18 in order to suppress light in the near-infrared region from being incident on the imaging element 19. The infrared cut film can be realized by using the light interference effect, and can be provided by, for example, laminating multiple layers of low refractive index layers and high refractive index layers alternately. In addition, an infrared absorbing glass in which a material such as metal ions having absorption in the near-infrared region is kneaded may be used as the material of the cover glass 18.
[0074] To prevent the resin base material from yellowing, the inside of lens barrel 11 may be filled with an inert gas such as nitrogen or argon. Also, an oxygen scavenger such as iron may be placed inside lens barrel 11 so as not to enter the optical path. This configuration reduces the opportunities for the resin base material to come into contact with oxygen, and discoloration due to oxidation, such as yellowing, can be prevented.
[0075] 6 is configured with four lenses, there is no limit to the number of lenses, and it may be more or less than four. Note that the optical device 21 shown in Fig. 6 has an optical member 4 that is a lens, but it may also have an optical member 4 other than a lens, such as an infrared cut filter or a UV cut filter.
[0076] [Example 1] FIG. 4(A) shows a configuration diagram of an optical member according to Example 1, and FIG. 4(B) shows the spectral characteristics of the optical member according to Example 1. For the sake of explanation, FIG. 4 shows an optical film formed on one side of a resin substrate, but in reality, the same optical film is formed on the other side of the resin substrate. In Example 1, the substrate is a flat resin substrate (Φ=20 mm, t=2 mm) made of cycloolefin resin or a resin lens, and a Ni film is formed on the resin substrate 1 by the PEALD method, and an AR film is formed on the Ni film by the PEALD method as well. The thickness of the Ni film is 1 nm. The first layer of the AR film is an Al2O3 film, and the second and subsequent layers of the AR film are alternately laminated structures of TiO2 and SiO2.
[0077] According to the evaluation result of the transmittance of the optical member according to Example 1, the optical member maintains a transmittance of 80% or more in the visible light wavelength region. Also, according to the evaluation result of the reflectance of the optical member according to Example 1, the reflectance is 1.5% or less in the visible light wavelength region.
[0078] [Example 2] FIG. 5(A) shows the configuration of an optical member according to Example 2, and FIG. 5(B) shows the spectral characteristics of the optical member according to Example 2. In Example 2, the substrate is a cycloolefin-based flat resin substrate (Φ=20 mm, t=2 mm) or a resin lens, and a Ni film is formed on the resin substrate 1 by the ALD method, and an AR film is formed on the Ni film by the ion plating method. In this example, the ion plating method, which is one of the vacuum deposition methods that makes it easier to laminate different film materials compared to the ALD method, is used to form the AR film. The thickness of the Ni film is 1 nm. The AR film includes an alternating laminate structure of SiO2 and TiO2, an Al2O3 layer provided directly under the outermost layer for the purpose of improving gas barrier properties, and an MgF2 layer provided as the outermost layer to function as an anti-reflection layer and has a low refractive index and is advantageous for reducing reflection.
[0079] According to the evaluation result of the transmittance of the optical member according to Example 2, the optical member maintains a transmittance of 80% or more in the visible light wavelength region. Also, according to the evaluation result of the reflectance of the optical member according to Example 2, the reflectance is 1.0% or less in the visible light wavelength region.
[0080] The invention is not limited to the above-described embodiments, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are appended to apprise the public of the scope of the invention. [Explanation of symbols]
[0081] 1: resin substrate, 2: metal film, 3: optical film, 4: optical member, 5: optical adhesive, 6: positioning surface, 11: lens barrel, 12: protective filter, 13-16: lens, 17: aperture, 18: cover glass, 19: imaging element, 20: lens unit, 21: optical device
Claims
1. A resin substrate; A metal film formed on the resin substrate; an optical film that is formed on the metal film and has transparency to a specific wavelength, An optical member, characterized in that the resin base material and the metal film are bonded together by a primary bond.
2. When the metal element constituting the metal film is M and the carbon atom of the resin substrate is C, 2. The optical member according to claim 1, wherein the primary bond between the resin base material and the metal film is expressed by C-O-M.
3. The optical member according to claim 1 , wherein the metal film is a continuous film.
4. The optical film has a laminated structure of thin films having a plurality of refractive indices, The optical member according to claim 1 , wherein the metal film is thinner than the thinnest thin film among the thin films that form the optical film.
5. 2. The optical member according to claim 1, wherein the metal film has a thickness of 3 nm or less.
6. 2. The optical member according to claim 1, wherein the metal film is a film formed by depositing atomic layers.
7. the metal film is formed on both sides of the resin substrate, 2. The optical member according to claim 1, which has a light transmittance of 60% or more at 550 nm.
8. A resin substrate; A metal film having a thickness of 3 nm or less formed on the resin substrate; an optical film having transparency to a specific wavelength formed on the metal film; An optical member comprising:
9. 9. An optical device comprising: the optical member according to claim 1; and an imaging element that captures an image of light that has passed through the optical member.
10. A method for manufacturing an optical member, comprising the steps of: forming a metal film on a resin substrate by atomic layer deposition; forming an optical film having transparency to a specific wavelength on the metal film; A manufacturing method comprising the steps of:
Citation Information
Patent Citations
Method for manufacturing antireflection film having favorable adhesiveness
JP2003270402A