Two-liquid type coating composition and method for using two-liquid type coating composition

The two-component paint system addresses separation issues in existing paints by using a dispersion liquid and mixture liquid with adjusted viscosities and specific gravities, along with a filler, resulting in a stable, crack-free coating film with enhanced strength and adhesion.

JP2024160773APending Publication Date: 2024-11-15KIKUSUI CHEM IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023076108
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing two-component paints using aqueous blast furnace slag suspensions and hydraulic reaction inducers often separate during storage due to differences in viscosity and specific gravity, leading to incomplete mixing and potential hard cake formation, which results in coating films with cracks.

Method used

A two-component paint system is developed with a dispersion liquid containing a latent hydraulic substance and a mixture liquid composed of an alkali compound, both with adjusted viscosities and specific gravities, along with a filler component to prevent separation and alleviate stress during curing, using components like blast furnace slag, titanium oxide, and alkali compounds.

Benefits of technology

The system ensures easy mixing and reduces cracking in the coating film by suppressing separation of latent hydraulic substances, enhancing film strength and adhesion, and providing a stable, crack-free surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160773000001
    Figure 2024160773000001
  • Figure 2024160773000002
    Figure 2024160773000002
  • Figure 2024160773000003
    Figure 2024160773000003
Patent Text Reader

Abstract

To provide a two-liquid type coating composition in which both a dispersion liquid and a mixture liquid are difficult to separate, and even if they are separated, they can be easily dispersed by re-stirring and the dispersion liquid and the mixture liquid can be easily mixed.SOLUTION: There is provided a two-liquid type coating composition composed of a dispersion liquid which viscosity is adjusted by dispersing a latent hydraulic material in water and a mixture liquid comprising an alkali compound and water which viscosity is adjusted, wherein the dispersion liquid has a viscosity in the range of 1500 to 35000 mPa s and the mixture liquid has a viscosity in the range of 500 to 10000 mPa s as measured by a Type B viscometer at 20 rpm at 23°C, the specific gravity of the dispersion liquid and the mixture liquid is in the range of 1.2 to 1.7 and thus both the dispersion liquid and the mixture liquid are difficult to separate, and even if they are separated, they can be easily dispersed by re-stirring and the dispersion liquid and the mixture liquid can be easily mixed.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a two-component paint to be applied to wall surfaces such as the interior and exterior walls of structures such as buildings, and particularly to a two-component paint using a latent hydraulic substance and an acrylic compound, and a method for using the same, and its fields of application are mainly in the fields of architecture and civil engineering. [Background technology]

[0002] Conventionally, there have been many types of paints that are applied to the interior and exterior walls of buildings and other structures, including those that use organic binders such as synthetic resin emulsions as their main component, and those that use inorganic binders such as cement. The coating films formed by these paints are used to improve the durability of wall surfaces and to enhance their design.

[0003] Among these, when the surface to be painted is concrete, a mixture of cement and synthetic resin emulsion or a mixture using inorganic binder such as cement may be used. Those using inorganic binders such as cement are often used due to the strength of the formed coating film, ease of use, ease of availability, etc. Among them, JP 2021-1260 A proposes a blast furnace slag-based paint.

[0004] This describes a blast furnace slag-based two-component paint, characterized in that the main component of the base material is a stabilized blast furnace slag aqueous suspension containing blast furnace slag, and the hydraulic reaction inducer is an alkaline liquid in which sodium silicate or sodium carbonate or potassium carbonate that induces the hydraulic reaction of the suspension is dissolved, and the base material and the hydraulic reaction inducer are packaged separately.

[0005] As a result, the same effect as in the case of alumina cement could be obtained even when using blast furnace slag, and it was possible to obtain a liquid inorganic material consisting of a liquid suspension with blast furnace slag as the main component, and a blast furnace slag-based two-component or one-component water-based paint using this fluid suspension. This water-based paint hardens at room temperature and provides a coating film with high strength and excellent physical properties such as water resistance and weather resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-1260 Summary of the Invention [Problem to be solved by the invention]

[0007] However, when an aqueous suspension of blast furnace slag or a hydraulic reaction inducer is filled into a container and stored, depending on the storage conditions, separation may occur within the container, with substances with a higher specific gravity collecting at the bottom of the container. Even if the collected substances are stirred again, they may not be sufficiently mixed and may form lumps, forming a hard cake. In addition, the difference in viscosity between the dispersion liquid and the mixture liquid may make them difficult to mix, or the difference in specific gravity may make them difficult to mix.

[0008] The present disclosure provides a two-component paint in which both the dispersion and the mixture are difficult to separate, and even if they do separate, they can be easily dispersed by re-stirring, and the dispersion and the mixture are easily mixed. [Means for solving the problem]

[0009] This is a two-component paint consisting of a dispersion in which a latent hydraulic substance is dispersed in water and the viscosity is adjusted, and a mixed liquid which is made of an alkaline compound and water and has an adjusted viscosity. When the viscosity of the dispersion and the mixed liquid are measured with a B-type viscometer at 20 rpm and 23°C, the dispersion has a viscosity in the range of 1500 to 35000 mPa s, the mixed liquid has a viscosity in the range of 500 to 10000 mPa s, and the specific gravity of the dispersion and the mixed liquid is in the range of 1.2 to 1.7. This makes it difficult for the dispersion liquid and the mixture to separate, and even if they do separate, they can be easily dispersed by re-stirring, making it easy to mix the dispersion liquid and the mixture.

[0010] The admixture contains a filler component, and the particle size of the filler is in the range of 5 to 2000 μm and is larger than the particle size of the latent hydraulic substance. As a result, even in the case of a coating film formed from a two-component paint, separation of the relatively dense latent hydraulic substance in the uncured coating film is suppressed, resulting in less separation in the coating film, and the latent hydraulic substance interacts with the filler when the coating film hardens, mitigating the stress generated in the hardening reaction, reducing the occurrence of cracks on the surface and protecting the coated object.

[0011] Furthermore, by including titanium oxide in the mixture, the relatively thin coating film formed is less susceptible to cracking on the surface, and a relatively hard coating film is formed, making it possible to protect the coated object. A method for using a two-component paint composed of a dispersion and an admixture, in which the two-component paint in a mixed state of the dispersion and the admixture is used after adjusting the viscosity of the two-component paint in a mixed state of the dispersion and the admixture to a range of 150 to 350,000 mPa s when measured at 20 rpm and 23°C with a B-type viscometer, the solid content to a range of 30.0 to 80.0% by weight, and the latent hydraulic substance to a range of 10 to 40% by weight in the paint.

[0012] As a result, even in the case of a coating film formed in the range of 100 to 3000 μm, separation of the relatively dense latent hydraulic substance in the uncured coating film is suppressed, and separation in the coating film is reduced. When the coating film hardens, the latent hydraulic substance interacts with the filler, mitigating the stress generated in the hardening reaction, reducing the occurrence of cracks on the surface, and protecting the coated object. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present disclosure will be described. The present disclosure relates to a two-component paint comprising a dispersion in which a latent hydraulic substance is dispersed in water and the viscosity is adjusted, and a mixed liquid comprising an alkaline compound and water and the viscosity of which is adjusted, wherein, when the viscosity of the dispersion and the mixed liquid is measured with a B-type viscometer at 20 rpm and 23°C, the dispersion has a viscosity in the range of 1500 to 35000 mPa s, the mixed liquid has a viscosity in the range of 500 to 10000 mPa s, and the dispersion and the mixed liquid have a specific gravity in the range of 1.2 to 1.7.

[0014] First, a typical example of the latent hydraulic substance that is the main component of the dispersion liquid is blast furnace slag. This latent hydraulic substance hardens when stimulated by the alkalinity of an alkaline compound such as an alkaline solution. This is because the surface of the latent hydraulic substance soluble in an alkaline aqueous solution is destabilized by the alkaline compound described below, and as the moisture in the alkaline stimulant disappears, the active fillers approach each other and bond with each other.

[0015] This blast furnace slag is produced by reducing and melting iron ore with coke and removing it from the blast furnace together with the pig iron in a molten state at about 1500°C. After this, the slag is separated from the pig iron due to its difference in specific gravity. Depending on the method of cooling and solidifying, there are two types of blast furnace slag: slow-cooled slag and granulated slag. The particle size of this latent hydraulic substance is in the range of 1 to 50 μm, and it is a fine powder with high reactivity, which results in good hardening, easy formation of a coating film, and good initial water resistance. In addition, because it is white in color, it enhances the hiding power of the coating film and makes it easy to color the paint.

[0016] Its composition is CaO, SiO 2 ,Al 2 O 3 Its main component is , and its chemical composition is similar to that of cement. The dispersion is prepared by dispersing this latent hydraulic substance in water, and adjusting the viscosity of the dispersion by using a thickener or leveling agent to prevent the dispersed latent hydraulic substance from settling and separating.

[0017] The thickening agent and leveling agent are not particularly limited, and those generally used in paint formulations, such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl alcohol, and sodium polyacrylate, can be used. Among these, methyl cellulose and hydroxyethyl cellulose are preferred because they are likely to exhibit a thickening effect.

[0018] If necessary, a surfactant such as a dispersant or wetting agent may be used, and the addition of these improves the dispersibility of the latent hydraulic substance. When preparing this dispersion, foaming may occur, so it is preferable to use an antifoaming agent, which can suppress foaming that occurs when the dispersion is mixed with a mixture liquid described later.

[0019] Furthermore, various additives such as surfactants, preservatives, algae inhibitors, antifungal agents, pH adjusters, antifreeze agents, etc., which are generally used in paints, can be added to this dispersion as required. A dispersion can be obtained by dispersing this latent hydraulic substance in water, and the dispersion can be carried out by a mixer or other mixing machine.

[0020] The solids content of this dispersion is preferably in the range of 40 to 75% by weight. If it is less than 40% by weight, the solids content of the mixed two-component paint as a whole may be low, and cracks may occur in the formed coating film. If the content is more than 75% by weight, it becomes difficult to set the viscosity as described below, and mixing with the mixture liquid may become difficult.

[0021] The mixed liquid can be obtained by thickening a solution of an alkaline compound or the like, and can be obtained by mixing with a mixer or other mixer. The alkaline compound which is the main component of this admixture may be any compound which dissolves the latent hydraulic substance and can destabilize its surface, and which dissolves in water.

[0022] Alkaline compounds such as sodium hydroxide, potassium hydroxide, and sodium metasilicate are soluble in water and can be used to obtain an alkaline aqueous solution with a pH of 7 to 14 by dissolving substances that are alkaline and dissolve them in water. Furthermore, silica solutions such as colloidal silica that exhibit alkaline properties, water glass, lithium silicate, alumina sol, etc. may also be used and are preferably used.

[0023] By using these, they react with blast furnace slag to give strength to the coating film formed by the two-liquid paint and improve adhesion to the base. These alkaline stimulants may be used alone or in combination of two or more. Colloidal silica is a colloidal dispersion of fine amorphous silica particles in a solvent such as water, while water glass is a concentrated aqueous solution of sodium silicate that has high viscosity and is obtained by dissolving sodium silicate in water and heating it.

[0024] Lithium silicate is a type of alkali silicate that has superior heat resistance compared to organic binders, and alumina sol is a colloidal solution of alumina hydrate with water as a dispersion medium. Among these, colloidal silica, which is silica fine particles dispersed in water, is preferably used. This colloidal silica is preferably used because it can increase the ease of handling and surface strength, has good adhesion to the base, and can make the coating film hydrophilic, and forms a coating film with good hydrophilicity, which makes it less susceptible to stains such as those caused by raindrops.

[0025] The average particle size of the silica fine particles dispersed in this silica solution is preferably 4 to 100 nm, more preferably 6 to 50 nm, and most preferably 10 to 20 nm. When the content is within this range, the hydrophilicity can be easily adjusted, and the bonding strength between the silica fine particles is optimized.

[0026] If the average particle size of the silica particles is less than 4 nm, the bonding strength between the silica particles is too strong, which may cause shrinkage cracks in the coating film, whereas if it exceeds 100 nm, the bonding strength between the silica particles is weak, which may cause the coating film to be weak. The particle shape of the silica microparticles may be spherical, pearl necklace-like, needle-like, rod-like, etc., with spherical shapes being preferred, because when the silica microparticles dry to form a dry gel, the particles can form a close-packed structure, thereby improving the strength of the coating film formed by the coating material.

[0027] By thickening the solution of such an alkaline compound, the difference in viscosity from the viscosity-adjusted dispersion liquid is reduced, making it easier to mix, and making it possible to suppress settling and separation of the mixed two-component paint. The thickening of the solution of the alkaline compound is carried out using a thickening agent or a leveling agent, and is not particularly limited.

[0028] As with the above dispersion, the thickening agent and leveling agent may be any of those generally used in paint formulations, such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl alcohol, and sodium polyacrylate. Among these, methyl cellulose and hydroxyethyl cellulose are preferred because they are likely to exhibit a thickening effect.

[0029] If necessary, surfactants such as dispersants and wetting agents may be used, and adding these can improve the mixing with the dispersion liquid. Furthermore, defoamers may be used, and adding them can suppress the foaming that occurs when mixing with the dispersion liquid. It is preferable that this admixture contains a filler component, and it is more preferable that the particle size of the filler is in the range of 5 to 2000 μm, and that the particle size of the filler is larger than the particle size of the latent hydraulic substance.

[0030] By including this filler component, separation of latent hydraulic substances, which have a relatively high specific gravity, is suppressed in the uncured coating film, even in the case of a thick coating film formed with a two-component paint, and separation in the coating film is reduced. Furthermore, when the coating film hardens, the latent hydraulic substance interacts with the filler, alleviating the stress generated during the hardening reaction, reducing the occurrence of cracks on the surface and protecting the coated object.

[0031] If the particle size of the filler component is in the range of 5 to 2000 μm, which is larger than the particle size of the latent hydraulic substance, the filler becomes the skeleton when the coating film hardens, and the latent hydraulic substance exists among the filler particles, so that it is easy to interfere with the hardening of the entire coating film and the stress generated during the hardening reaction can be alleviated. More preferably, the particle size of the filler is in the range of 5 to 1000 μm. Within this range, the effect is better and cracks in the coating film are reduced.

[0032] The filler ingredients include zinc oxide, kaolin, talc, clay, calcium carbonate, diatomaceous earth, bentonite, white carbon, glass beads, aluminum hydroxide, magnesium hydroxide, and silica sand. Furthermore, it is preferable that the mixture contains titanium oxide, and since the particles of titanium oxide are relatively hard and nearly spherical in shape, the relatively thin coating film formed is less likely to crack on its surface, and a relatively hard coating film is formed, which can protect the coated object.

[0033] It is preferable that this content is in the range of 0.1 to 10.0% by weight in the mixed two-component paint. Within this range, a hard coating film can be formed with little cracking on the surface of the relatively thin coating film. Furthermore, various additives such as surfactants, preservatives, algae inhibitors, antifungal agents, pH adjusters, antifreeze agents, etc., which are generally used in paints, can be added to this mixture as necessary.

[0034] The solids content of this mixture is preferably in the range of 30 to 70% by weight. If it is less than 30% by weight, the solids content of the mixed two-component paint as a whole may be low, and cracks may occur in the formed coating film. If the content is more than 70% by weight, it becomes difficult to set the viscosity as described below, and mixing with the dispersion liquid may become difficult.

[0035] It is also possible to add a synthetic resin emulsion to either or both of this dispersion and mixture, which will provide good adhesion to the underlying coating, provide the coating with appropriate softness, and reduce cracks on the coating surface. The amount of the synthetic resin emulsion to be added depends on the type of synthetic resin, but is preferably in the range of 1 to 50% by weight in terms of the solid content of the synthetic resin emulsion relative to the solid content of the mixed two-component paint.

[0036] Within this range, the curing of the coating film is not affected, and the formed coating film can have an appropriate degree of softness. This synthetic resin emulsion may be any of those commonly used in the formulation of paints and coating materials, as long as it is well miscible with the alkaline compound.

[0037] This synthetic resin emulsion is a dispersion of synthetic resin in water, and examples of the synthetic resin include acrylic resin, styrene resin, urethane resin, silicone resin, fluororesin, epoxy resin, vinyl chloride resin, vinyl acetate resin, polyester resin, etc., either alone or in copolymer form. This synthetic resin emulsion is a general one that can be produced by a common polymerization technique such as emulsion polymerization, and includes synthetic resin emulsions produced from the synthetic resins described above.

[0038] Furthermore, it is possible to add an air-hardening binder such as slaked lime, or a pozzolanic reaction component such as fly ash or silica fume to either or both of the dispersion liquid and the admixture liquid. By adding these, it is possible to further improve the strength of the coating film. In addition, color pigments, fibers, water repellents, hydrophilizing agents, photocatalysts, etc. can be added to either the dispersion liquid or the mixture liquid, or both.

[0039] These color pigments include inorganic and organic pigments, and can be used to color general paints, such as titanium oxide, carbon black, oxide yellow, red oxide, cyanine blue, and cyanine green. Fibers include natural fibers such as pulp and cotton, as well as glass and mineral fibers. The addition of these fibers can mitigate the rapid drying that occurs after the mixed two-component paint is applied, prolong the alkaline wet state of the paint film, and slow the reaction hardening process, thereby improving the strength of the paint film.

[0040] In addition, shrinkage of the coating film can be suppressed, and cracks in the coating film can be reduced. Furthermore, by adding water repellents, hydrophilizing agents, photocatalysts, etc., it is possible to impart unique properties to the formed coating film.

[0041] The viscosity of the dispersion and mixture, when measured at 20 rpm and 23°C with a Brookfield viscometer, is in the range of 1500 to 35000 mPa·s for the dispersion and 500 to 10000 mPa·s for the mixture. When the viscosity of each is within this range, both the dispersion and the mixture are unlikely to separate, and even if they do separate, they can be easily dispersed by re-stirring. The viscosity difference within this range makes it easy to mix the dispersion and the mixture.

[0042] In addition, the difference in viscosity between the dispersion liquid and the mixture liquid is preferably 3000 mPa·s or less. With the difference in viscosity in this range, the mixture is easier to mix. If the viscosity of the dispersion is lower than 1500 mPa·s, the separation of latent hydraulic substances, which have a different specific gravity from water, cannot be prevented, and it is difficult to redisperse the separated and settled latent hydraulic substances.

[0043] If the viscosity is higher than 35,000 mPa·s, it is difficult to use, difficult to mix with a miscible liquid, and difficult to obtain a dispersion. If the viscosity of the mixture is lower than 500 mPa·s, it may be difficult to mix with the dispersion, and if it is higher than 10,000 mPa·s, it will be difficult to use and mix with the mixture, making it difficult to obtain a dispersion.

[0044] Since the specific gravities of the dispersion and mixture are in the range of 1.2 to 1.7, the dispersion and mixture are difficult to separate, and even if they do separate, they can be easily dispersed by re-stirring, and the dispersion and mixture are easy to mix. If the specific gravity is lower than 1.2, the proportion of water and air mixed in each liquid will be high, resulting in a low solids content, which can cause defects in the coating film that is formed.

[0045] If it is heavier than 1.7, both the dispersion and the mixture are likely to separate, and the separated sediment may not be easily dispersed by re-stirring, and the dispersion and the mixture are difficult to mix. As described above, the dispersion and the admixture are composed, and by mixing them, a paint that can be hardened by the latent hydraulic substance and the alkaline compound can be obtained. In addition, the effect of the paint can be more fully exhibited by the filler component preferably contained in the admixture.

[0046] The mixing method is not particularly limited, and the mixture can be mixed using a mixer generally used in painting operations, such as a hand mixer. The viscosity of the two-component paint obtained by mixing this dispersion and admixture is preferably in the range of 150 to 100,000 mPa·s when measured with a B-type viscometer at 20 rpm and 23°C. If it is lower than 150 mPa·s, separation of the relatively dense latent hydraulic substance may not be suppressed.

[0047] If the viscosity is higher than 100,000 mPa·s, it is not possible to form a relatively thin and uniform coating film, and if the viscosity is outside this range, it is difficult to form a good coating film. When measured with a Viscotester, the range is 5 to 500 dPa·s. A Viscotester is a viscometer that allows for easier measurement than a B-type viscometer, and can be easily managed on-site.

[0048] Although there is no perfect correlation between values ​​measured with a Brookfield viscometer and values ​​measured with a Viscotester, the range of 5 to 500 dPa·s measured with a Viscotester is within the range of 150 to 100,000 mPa·s measured with a Brookfield viscometer, and is therefore a preferable range. This two-component paint hardens when stimulated by the latent hydraulic properties and the alkalinity of the alkaline compounds, and the reaction begins immediately after mixing, which can cause the viscosity of the paint to change.

[0049] The Viscotester can easily measure viscosity even at the painting site, so by measuring immediately before painting, painting work can be carried out more steadily. Furthermore, by allowing the coating work to be carried out stably, the coating film formed has fewer cracks on the surface and is capable of protecting the coated object.

[0050] When the mixed two-component paint contains the filler component and has a solid content in the range of 30.0 to 80.0% by weight, the occurrence of cracks on the surface of the coating film caused by the paint is reduced. If the solids content is less than 30.0% by weight, sufficient film formation may not occur and cracks may appear on the surface of the coating film. If the solids content is more than 80.0% by weight, there may be little liquid between the particles that make up the paint, which may result in the particles not being sufficiently wetted, resulting in poor coating workability.

[0051] The latent hydraulic substance is preferably contained in the mixed two-component paint in the range of 10 to 60% by weight. If it is more than 60% by weight, the coating film will have a strong bond and will likely crack, while if it is less than 10% by weight, the coating film will have poor strength and adhesion to the base. If the content is within the range of 10 to 60% by weight, the coating strength and adhesion to the substrate are good, and the coating is less likely to crack. If the content is within the range of 15 to 40% by weight, the coating is well balanced between cracking, strength, and adhesion.

[0052] Thus, it is preferable to use the two-component paint obtained by mixing the dispersion and the mixture after adjusting the viscosity of the paint to within the range of 150 to 100,000 mPa s when measured at 20 rpm and 23°C with a B-type viscometer, the solid content to within the range of 30.0 to 80.0% by weight, and the latent hydraulic substance to within the range of 10 to 60% by weight in the paint. This mixed two-component paint is applied to the base material to be coated, and after drying and curing, a coating film is formed, and the thickness of the coating film is preferably in the range of 100 to 3000 μm.

[0053] If the coating film formed is in the range of 100 to 3000 μm, separation of latent hydraulic substances, which have a relatively high specific gravity, in the uncured coating film is suppressed, and separation in the coating film is reduced. In addition, the latent hydraulic substance interacts with the filler when the coating is cured, thereby mitigating the stress generated during the curing reaction, reducing the occurrence of cracks on the surface and protecting the coated object.

[0054] If the thickness of this coating film is less than 100 μm, the base may not be covered sufficiently, and the coated object may not be protected completely. If it is thicker than 3000μm, the weight of the coating will be too heavy, making it difficult to apply efficiently on vertical surfaces, and paint dripping during the curing and drying process may occur, making it difficult to obtain a clean coating. Also, the coating thickness may become uneven, causing cracks due to differences in thickness.

[0055] A more preferable film thickness is in the range of 200 to 1000 μm. Within this range, the performance of the coating film formed by the mixed two-component paint can be fully exhibited, and the occurrence of cracks on the surface can be reduced. The mixed two-component paint can be applied using painting tools commonly used in painting work, such as a spray, a painting roller or a brush.

[0056] In the case of line painting, which is carried out in advance on painted exterior wall panels or other board materials using painting machines in a factory or the like, painting can be carried out using a reciprocating type spray, roll coater, curtain flow coater or the like. This base coating can be applied to a variety of substrates, including the concrete, mortar, ALC panels, siding boards, extruded panels, gypsum boards, slate, ceramic, plastic, wood, stone, and tiles that make up the walls of buildings.

[0057] It is preferable that the pH of the base is within the range of 7 to 14. This is because, in the mixed two-component paint, if the pH of the base is within the range of 7 to 14, the reaction curing at the interface with the base is likely to proceed, adhesion is good, and sufficient strength can be obtained as a whole coating film. Substrates with a pH in the range of 7 to 14 include concrete, mortar, ALC panels, siding boards, extrusion molded boards, slates, etc., which are mainly made of cement. A pH of 8 or higher is preferable.

[0058] Furthermore, it is also possible to apply an alkali-imparting agent to the base, adjust the pH of the base to a range of 7 to 14, and then apply the mixed two-liquid paint, which is preferably performed since it is possible to adjust the pH of the base. Such a method is often performed when the pH of the base is 6 or less. In this way, the applied alkali-imparting agent easily promotes reaction and hardening at the interface with the base, resulting in good adhesion and sufficient strength for the entire coating film.

[0059] The alkalinity imparting agent is similar to the above-mentioned alkaline compounds, and can be obtained by dissolving in water a substance that is soluble in water and exhibits alkalinity, such as sodium hydroxide or potassium hydroxide. Furthermore, silica solutions such as colloidal silica that exhibit alkaline properties, water glass, lithium silicate, alumina sol, etc. may also be used and are preferably used.

[0060] Furthermore, solutions of nitrites such as calcium nitrite and lithium nitrite, which are used for the purpose of preventing rust on concrete, are also preferably used. After a coating film is formed from the mixed two-liquid coating material, it is preferable to further coat the surface of the coating film with an alkali imparting agent.

[0061] By applying an alkali imparting agent to the coating film, the drying of the coating film is slowed down and the hardening progresses, which makes the coating film surface denser and increases its strength and hardness. This also improves the abrasion resistance of the coating film surface, resulting in excellent durability. Furthermore, in the case where the alkalinity imparting agent is colloidal silica in which fine particles of amorphous silica are dispersed in a colloidal state in a solvent such as water, the colloidal silica particles are scattered on the coating film surface, which makes the coating film surface hydrophilic, making it difficult for dirt to adhere to the coating film surface and making any dirt that does adhere easy to remove.

[0062] The two-component paint having the above-described structure and a method for using the two-component paint will now be described using more specific embodiments. First, the raw materials shown in Table 1 were uniformly stirred with a dissolver to prepare a dispersion. Blast furnace slag with an average particle size of 5 μm was used as the latent hydraulic material.

[0063] The filler used was calcium carbonate with an average particle size of 10 μm. The particle size was the D50 value calculated from the volume-based particle size distribution measured by laser diffraction. Hydroxyethyl cellulose was used as a thickener, and a dispersant and an antifoaming agent were also added.

[0064] [Table 1]

[0065] The viscosity of each dispersion liquid prepared was measured at 20 rpm and 23° C. using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.) Storage stability was evaluated by leaving each dispersion liquid prepared at 50° C. for one week and checking the state of precipitation and aggregation. If more than 10% of the volume of the dispersion had settled and aggregated, or if the settled and aggregated particles could not be redispersed with a dissolver, the rating was ×; if some settled and aggregated but could be redispersed with a dissolver, the rating was ○; and if there was no settled or aggregated particles at all, the rating was ◎.

[0066] Next, the raw materials shown in Table 2 were uniformly stirred with a dissolver to prepare a mixed liquid. Colloidal silica with a pH of 11 was used as the alkaline compound. The color pigment was titanium oxide with an average particle size of 0.3 μm, the filler was calcium carbonate with an average particle size of 10 μm, the thickener was hydroxyethyl cellulose, and a dispersant and an antifoaming agent were also added.

[0067] [Table 2]

[0068] The viscosity of each mixture was measured at 20 rpm and 23° C. using a B-type viscometer, similar to the dispersion. Storage stability was also evaluated by storing each mixture at 50° C. for one week and checking the state of precipitation and aggregation. If more than 10% of the volume of the mixture had settled and aggregated, or if the settled and aggregated material could not be redispersed with a dissolver, the mixture was marked with an ×; if some settled and aggregated material had but could be redispersed with a dissolver, the mixture was marked with an ○; and if there was no settled or aggregated material at all, the mixture was marked with an ◎.

[0069] A two-component paint was prepared by mixing the dispersion and mixture, which had good storage stability, in a ratio of 1:1. To mix, 250g each of the dispersion and mixture were placed in a 500ml sealed container and mixed by shaking by hand for 1 minute. The viscosity of each two-component paint prepared was measured using a Brookfield viscometer at 20 rpm and 23°C. The mixing condition was also visually confirmed by the appearance of the paint and by the coating film formed using a film applicator that leaves a gap of 150 μm.

[0070] If the paint looked marbled, it was rated as ×; if the paint looked uniform but the coating film formed with the film applicator looked marbled, it was rated as ○; and if the coating film formed with the film applicator looked uniform, it was rated as ◎. The two-component paints with the mixing conditions other than × were applied to a mortar board with a paint roller to a coating thickness of about 200 μm, and the appearance of the coating formed was visually checked. If there were no cracks, it was rated as ○. The results are shown in Table 3.

[0071] [Table 3]

[0072] The combination of dispersion D with mixture A and mixture B was difficult to mix, possibly due to the large difference in viscosity between the dispersion and mixture.

Claims

1. Latent hydraulic substances are dispersed in water to form a dispersion with adjusted viscosity. A mixture of an alkaline compound and water with adjusted viscosity. A two-component paint comprising: The viscosity of the dispersion and mixture was measured at 20 rpm and 23°C using a Brookfield viscometer. The dispersion has a viscosity in the range of 1500 to 35000 mPa·s, and the mixture has a viscosity in the range of 500 to 10000 mPa·s, A two-component paint in which the specific gravity of the dispersion and mixture is in the range of 1.2 to 1.

7.

2. 2. The two-component paint according to claim 1, wherein the admixture contains a filler component, the particle size of the filler being in the range of 5 to 2000 μm and larger than the particle size of the latent hydraulic substance.

3. 3. The two-component paint according to claim 1 or 2, further comprising titanium oxide in the admixture.

4. A method for using a two-component paint comprising the dispersion and mixture according to claim 1, comprising the steps of: The viscosity of the two-component paint in the state where the dispersion and the mixture are mixed is in the range of 150 to 100,000 mPa·s when measured at 20 rpm and 23°C with a B-type viscometer. The solid content is in the range of 30.0 to 80.0% by weight. A method for using a two-component paint after adjusting the content of latent hydraulic substance in the paint to the range of 10 to 60% by weight.

5. A method for using the two-component paint according to claim 4, comprising the steps of: A method for using a two-component paint, in which a two-component paint in a mixed state of a dispersion and a mixture is applied to a substrate having a pH in the range of 7 to 14.