Preparation method of composite cathode material

A dry mechanical mixing method forms a composite positive electrode material with a LATP coating on LMNO, addressing the complexity and performance risks of conventional coating methods by enhancing conductivity and cycle life while reducing costs.

JP2024160916AActive Publication Date: 2024-11-15ADVANCED LITHIUM ELECTROCHEMISTRY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023163963
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-09-26
Publication Date
2024-11-15
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

Conventional methods for coating solid electrolytes on lithium manganese nickel oxide/spinel (LMNO) materials to improve microstructure and conductivity are complex and risk impairing the performance of LMNO, leading to issues like reduced capacitance and cycle life due to electrolyte decomposition under high voltage.

Method used

A dry mechanical mixing method is used to process a precursor and solid electrolyte, forming a composite positive electrode material with a core layer of LiNi0.5Mn1.5O4 and a covering layer of lithium aluminum titanium phosphate (LATP) to enhance conductivity and protect the surface from electrolyte damage, while controlling the weight percentage of LATP to 0.2-1.0 wt.%, preferably 0.2-0.3 wt.%.

Benefits of technology

The method simplifies the manufacturing process, improves the performance of the positive electrode material, enhances rate and cycling performance, and reduces manufacturing costs by forming a protective coating that mitigates electrolyte damage, resulting in improved capacitance and extended cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160916000001_ABST
    Figure 2024160916000001_ABST
Patent Text Reader

Abstract

To provide a preparation method of composite cathode material, materializing a simple and quick preparation process and enabling effective improvement of cathode material.SOLUTION: A preparation method of a composite cathode material includes steps of (a) providing a nickel-manganese compound material, wherein the nickel-manganese compound material is NixMny(OH)2 or NixMnyO(x+y=1); (b) of providing a solid electrolyte material, and forming a composite material by mixing the nickel-manganese compound material with the solid electrolyte material by a mechanical mixing method, wherein a weight percent of the solid electrolyte material relative to the nickel-manganese compound material is 0.2 wt.% to 1.0 wt.%; and (c) of providing a Li source, mixing the Li source with the composite material, forming the composite cathode material by sintering them, wherein the composite cathode material comprises a core layer and a coated layer, the core layer is made of LiNi2xMn2yO4, and the coated layer is made of the solid electrolyte material.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cathode material for secondary batteries, in particular to a method for preparing a composite cathode material, in particular to a method for preparing a precursor and a solid electrolyte by dry mechanical mixing to form a cathode material and simultaneously complete the surface coating of the solid electrolyte, which has a simple and rapid preparation process and can effectively improve the performance of the cathode material. [Background technology]

[0002] In recent years, the performance requirements for electric vehicles (e.g., electric cars) and their energy storage devices have been increasing, and high performance is also required for the secondary batteries used in them. Among the many types of batteries, lithium manganese nickel oxide / spinel (LiMn 1.5 Ni 0.5 O4,LMNO) is known as a positive electrode material that can be charged at a high voltage (5V). The high potential allows the lithium manganese nickel oxide / spinel material to have a higher energy density compared to lithium cobalt oxide and lithium iron phosphate, making LMNO-based batteries widely usable for high energy and high rate applications.

[0003] However, the capacity of LMNO is affected by the decomposition of the electrolyte under high voltage, which can easily cause problems such as a decrease in capacitance, rate performance, and cycle life. Therefore, surface modification of LMNO has become an important challenge. In addition, in the conventional method of using LMNO in combination with a solid electrolyte, it is common to coat the solid electrolyte on the LMNO material to improve the microstructure of the LMNO surface, which can form a skeletal surface that can impart ion conduction and electrical conductivity to the LMNO surface, effectively alleviating the problem of poor cycle performance at high voltage and improving the conductive properties of LMNO. However, the conventional coating of LMNO on a solid electrolyte requires complicated procedures, and the coating of the solid electrolyte may also impair the performance of LMNO.

[0004] In view of the above, the present invention provides a method for preparing a composite positive electrode material to solve the problems encountered in the prior art, specifically, a precursor and a solid electrolyte are processed by dry mechanical mixing to form a positive electrode material, and at the same time, the surface coating of the solid electrolyte is completed, so that the preparation process is simple and fast, and the performance of the positive electrode material can be effectively improved. Summary of the Invention [Problem to be solved by the invention]

[0005] The objective of the present invention is to provide a method for preparing a composite positive electrode material. Specifically, the precursor and the solid electrolyte are treated by the dry mechanical fusion method to form the positive electrode material, and the surface coating of the solid electrolyte is completed at the same time. This makes the preparation process simple and quick, and can effectively improve the performance of the positive electrode material. 1.3 Al 0.3 Ti 1.7 Regarding the coating of the (PO4)3,LATP) solid electrolyte, the present invention uses a dry mechanical mixing method to coat Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 The nickel manganese compound material of O and the solid electrolyte material are mixed first, then a lithium source is added and mixed, and sintered to form a composite positive electrode material having a core layer and a coating layer. The inner core layer is LiNi 0.5 Mn 1.5O4, and the outer coating layer is made of a solid electrolyte material. The lithium aluminum titanium phosphate (LATP) solid electrolyte has excellent inherent ion conductivity properties, so when the lithium aluminum titanium phosphate (LATP) coats the surface of the lithium nickel manganese oxide positive electrode material LMNO to form a composite positive electrode material, it helps to improve the rate performance and cycle performance of the lithium nickel manganese oxide positive electrode material LMNO, and the lithium aluminum titanium phosphate (LATP) coating layer can also provide a protective function to delay the damage caused by the electrolyte to the material surface. In addition, to obtain the optimal solid electrolyte coating effect, Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 The weight percentage of the solid electrolyte material to the nickel manganese compound material such as O is controlled to 0.2 wt.% to 1.0 wt.%, preferably 0.2 wt.% to 0.3 wt.%. That is, in the present invention, by simply adding a small amount of lithium aluminum titanium phosphate LATP solid electrolyte, a coating layer that improves the rate performance of the lithium nickel manganese oxide positive electrode material LMNO can be formed, and the manufacturing cost can be further reduced.

[0006] Another object of the present invention is to provide a method for preparing a composite cathode material. Rather than directly coating the lithium aluminum titanium phosphate (LATP) on the lithium nickel manganese oxide cathode material LMNO, the present invention uses a mechanical method, for example, a mechanofusion method, to mix the lithium aluminum titanium phosphate (LATP) into the pre-treatment material of the lithium nickel manganese oxide cathode material LMNO to form the lithium nickel manganese oxide cathode material LMNO, so that Mn 3+ The production of Mn is further reduced. 3+It can prevent the lithium manganese oxide (LMNO) from dissolving from the positive electrode material and reducing and depositing on the negative electrode, which causes electrical deterioration during cycling. The operating temperature of the mixing process is, for example, 25°C to 45°C, and the rotation speed is 700 rpm to 3500 rpm, and the mixing time is 5 minutes to 30 minutes in stages. By controlling the mixing method, operating temperature, rotation speed and time of the lithium aluminum titanium phosphate (LATP) and the pretreatment material, the structural defects of the solid electrolyte coating layer caused by high temperature or excessive friction between particles can be prevented, and at the same time, the lithium nickel manganese oxide positive electrode material LMNO can exhibit low impedance and good charge and discharge performance due to the coating layer of the LATP solid electrolyte. [Means for solving the problem]

[0007] In order to achieve the above object, the present invention provides a nickel manganese compound material, the nickel manganese compound material comprising: x Mn y (OH)2 or Ni x Mn y O, and x+y=1; providing a solid electrolyte material, mixing the nickel manganese compound material and the solid electrolyte material by a mechanical mixing manner to form a composite material, the weight percentage of the solid electrolyte material to the nickel manganese compound material is 0.2 wt.%-1.0 wt.%; providing a lithium source, mixing the lithium source and the composite material, and sintering to form the composite positive electrode material, the composite positive electrode material comprising a core layer and a coating layer, the core layer being LiNi 2x Mn 2y and step (c) comprising: O4, said coating layer covering said core layer, said coating layer comprising said solid electrolyte material. Preferably, the nickel manganese compound material is Ni 0.25 Mn 0.75(OH)2, and in step (b), after being mixed by a mechanical method, a first heat treatment process is carried out, the temperature range of the first heat treatment process is 300°C to 850°C, the treatment time of the first heat treatment process is 5 hours to 7 hours, and the temperature rise rate of the first heat treatment process is 2.5°C / min. Preferably, the nickel manganese compound material is Ni 0.25 Mn 0.75 O, step (a) includes a pre-oxidation process, the temperature range of the pre-oxidation process is 300°C to 850°C, the treatment time of the pre-oxidation process is 5 hours to 7 hours, and the temperature rise rate of the pre-oxidation process is 2.5°C / min. Preferably, in step (b), after mixing by mechanical means, a first heat treatment process is carried out, the temperature range of the first heat treatment process is 300°C to 750°C, the treatment time of the first heat treatment process is 5 hours to 7 hours, and the heating rate of the first heat treatment process is 2.5°C / min. Preferably, in step (b), the process of mechanically mixing the nickel manganese compound material and the solid electrolyte includes mixing at a rotation speed of 700 rpm for 5 minutes, mixing at a rotation speed of 1400 rpm for 5 minutes, mixing at a rotation speed of 2100 rpm for 5 minutes, mixing at a rotation speed of 2800 rpm for 10 minutes, and mixing at a rotation speed of 3500 rpm for 10 minutes. Preferably, in step (b), the operating temperature for mixing the nickel manganese compound material and the solid electrolyte by a mechanical method is 25°C to 45°C. Preferably, the chemical formula of the solid electrolyte is Li 1+z Al z Ti 2-z (PO4)3, where z≦2. Preferably, the mechanical method includes a mechanical fusion method. Preferably, in step (c), the step of mechanically mixing the lithium source and the composite material includes mixing at a rotation speed of 700 rpm for 5 minutes and mixing at a rotation speed of 1400 rpm for 30 minutes. Preferably, step (c) includes a second heat treatment process, the temperature range of the second heat treatment process is 300°C to 710°C, the treatment time of the second heat treatment process is 24 hours to 30 hours, and the temperature rise rate of the second heat treatment process is 2.5°C / min. Preferably, in step (c), the molar ratio of the nickel manganese compound material to the lithium source in the composite material is 1:1.02. Preferably, the weight percentage is between 0.2 wt.% and 0.3 wt.%. Preferably, the nickel manganese compound material has an average particle size of 10 μm to 20 μm, and the solid electrolyte material has an average particle size of 1 μm to 5 μm. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a conceptual structural diagram of a positive electrode material according to an embodiment of the present invention. [Figure 2A] 1 is a SEM image of the Ni0.25Mn0.75(OH)2 nickel manganese compound material of the present invention. [Figure 2B] 1 is a SEM image of a nickel manganese compound material of Ni0.25Mn0.75O of ​​the present invention. [Figure 2C] 1 is a SEM image of the lithium aluminum titanium phosphate (LATP) of the present invention. [Diagram 3] 1 is a flowchart of a method for producing a composite positive electrode material according to a first embodiment of the present invention. [Figure 4] In FIG. 4, 4A to 4D are SEM images of the positive electrode material of the first comparative example. [Diagram 5] In FIG. 5, 5A to 5D are SEM images of the positive electrode material of the first embodiment of the present invention. [Figure 6] In FIG. 6, 6A to 6D are SEM images of the positive electrode material of the second embodiment of the present invention. [Figure 7] In FIG. 7, 7A to 7D are SEM images of the positive electrode material of the third embodiment of the present invention. [Figure 8]FIG. 2 is a diagram showing potential-capacity charge / discharge curves of the first comparative example, the first embodiment, the second embodiment, and the third embodiment of the present invention. [Figure 9] FIG. 11 is a graph showing discharge curves of capacity retention rate versus number of cycles for the first comparative example, the first embodiment, the second embodiment, and the third embodiment of the present invention. [Figure 10] 4 is a flowchart of a method for producing a composite positive electrode material according to a second embodiment of the present invention. [Figure 11] In FIG. 11, 11A to 11D are SEM images of the positive electrode material of the fourth embodiment of the present invention. [Figure 12] In FIG. 12, 12A to 12D are SEM images of the positive electrode material of the fifth embodiment of the present invention. [Figure 13] In FIG. 13, 13A to 13D are SEM images of the positive electrode material of the sixth embodiment of the present invention. [Figure 14] FIG. 11 is a diagram showing potential-capacity charge / discharge curves of the first comparative example, the fourth example, the fifth example, and the sixth example of the present invention. [Figure 15] FIG. 11 is a graph showing discharge curves of capacity retention rate versus number of cycles for the first comparative example, the fourth embodiment, the fifth embodiment, and the sixth embodiment of the present invention. [Figure 16] FIG. 11 is a diagram showing potential-capacity charge / discharge curves of the second comparative example, the third comparative example, the first embodiment of the present invention, and the fourth embodiment. [Figure 17] FIG. 11 is a graph showing discharge curves of capacity retention rate versus number of cycles for the third comparative example, the first embodiment of the present invention, and the fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Some exemplary embodiments embodying the features and advantages of the present invention will be described in detail in the following. The present invention may be modified in various ways without departing from the scope of the present invention, and the following description and drawings are used to describe the present invention and are not intended to limit the present invention. In addition, in the detailed description of the present invention, the arrangement of a first feature on or above a second feature includes an embodiment in which the arranged first feature and the arranged second feature are directly connected to each other, and an embodiment in which the first feature and the second feature are not directly connected to each other via another structure between the first feature and the second feature. In addition, the terms "first", "second", "third", etc. are used to describe different configurations described in the claims, and these configurations are not limited to the terms, and in the content related to the embodiments, although the corresponding configurations are represented by different symbols, the first configuration can be represented as the second configuration and the second configuration can be represented as the first configuration, without departing from the embodiments of the present invention. In addition, the term "and / or" means one and / or a combination of the relevant elements or all of them. The term "approximately" refers to an average value within a standard error range generally accepted by a person skilled in the art. Unless expressly defined in the embodiments relating to operation / operation, all numerical ranges, amounts, values, percentages, etc. described herein (e.g., angles, durations, temperatures, operating conditions, ratios and corresponding percentages, etc.) should be understood in all embodiments by the terms "about" or "substantially". In addition, unless otherwise stated in the content, all numerical values ​​in the present invention and claims can be taken as approximations that can be varied as necessary. For example, each parameter may be interpreted in light of at least the number of significant digits described, applying ordinary rounding rules. In addition, numerical ranges herein can be expressed as ranges from one endpoint to the other endpoint or between two endpoints. It should be noted that all ranges described herein include the endpoints unless otherwise defined.

[0010] 1 is a structural conceptual diagram of a composite positive electrode material according to an embodiment of the present invention. In this embodiment, the composite positive electrode material 1 includes a core layer 10 and a coating layer 20 that covers the core layer 10. The core layer 10 is made of a lithium nickel manganese oxide positive electrode material LMNO, and the composition of the lithium nickel manganese oxide positive electrode material LMNO is LiNi 0.5 Mn 1.5 O4. The coating layer 20 is made of lithium aluminum titanium phosphate (Li 1.3 Al 0.3 Ti 1.7 In this embodiment, the lithium nickel manganese oxide cathode material LMNO is a high-voltage cathode material that does not contain cobalt element and has a relatively high redox potential and energy density. The composite cathode material 1 can be used in a liquid electrolyte 30, and Li + The ions 11 can pass through the coating layer 20 formed of a solid electrolyte and undergo intercalation or deintercalation into the lithium nickel manganese oxide positive electrode material LMNO of the inner core layer 10. The composite positive electrode material 1 of the present invention is formed by mixing lithium aluminum titanium phosphate (LATP) into a pretreatment material of the lithium nickel manganese oxide positive electrode material LMNO by a mechanical method such as a mechanofusion method to form the lithium nickel manganese oxide positive electrode material LMNO. The pretreatment material can be, for example, Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 The nickel manganese compound material of O, and the lithium nickel manganese oxide positive electrode material LMNO are not directly used in the coating process. 0.25 Mn 0.75 FIG. 2B is a SEM image of the Ni(OH)2 nickel manganese compound material of the present invention. 0.25 Mn 0.75FIG. 2C is an SEM image of the lithium aluminum titanium phosphate (LATP) of the present invention. Of course, the types, composition ratios, and material properties of the core layer 10 and the coating layer 20 covering the core layer 10 used in the composite positive electrode material 1 of the present invention can be adjusted according to the requirements of actual applications, and are not limited thereto. Hereinafter, a method for manufacturing the composite positive electrode material 1 of the present invention, in which the precursor and the solid electrolyte are treated by a mixing method of a dry mechanical fusion method, will be described.

[0011] FIG. 3 is a flow chart of a method for producing a composite positive electrode material in the first embodiment of the present invention. In this embodiment, a nickel manganese compound material is first provided, where the nickel manganese compound material is Ni 0.25 Mn 0.75 (OH)2 (Step S01). 0.25 Mn 0.75 The (OH)2 nickel manganese compound material has an average particle size of 10 μm to 20 μm, for example, 12.90 μm, and a surface area of ​​0.6 m 2 / g. Next, a lithium aluminum titanium phosphate (LATP) solid electrolyte material is provided, and the average particle size of the solid electrolyte material is 1 μm to 5 μm, for example, 1.79 μm. 0.25 Mn 0.75 The (OH)2 nickel manganese compound material and the LATP solid electrolyte material are mixed by a mechanical method to form a composite material (step S02). 0.25 Mn 0.75The weight percentage of the LATP solid electrolyte material to the (OH)2 nickel manganese compound material is 0.2 wt.% to 1.0 wt.%. In this embodiment, the mechanical method refers to a dry mechanical fusion method. In step S02, mixing the nickel manganese compound material and the solid electrolyte by a mechanical method includes mixing at a rotation speed of 700 rpm for 5 minutes, mixing at a rotation speed of 1400 rpm for 5 minutes, mixing at a rotation speed of 2100 rpm for 5 minutes, mixing at a rotation speed of 2800 rpm for 10 minutes, and mixing at a rotation speed of 3500 rpm for 10 minutes. The operating temperature of mixing the nickel manganese compound material and the solid electrolyte by a mechanical method is 25°C to 45°C. After the mixing by the mechanical method, a first heat treatment process is performed (step S03). The first heat treatment temperature is 300° C. to 850° C., the treatment time of the first heat treatment step is 5 hours to 7 hours, and the temperature rise rate of the first heat treatment step is 2.5° C. / min.

[0012] Next, as shown in step S04, a lithium source, such as lithium hydroxide, is provided, and the lithium source and the composite material are mixed and sintered to form a composite positive electrode material. 0.25 Mn 0.75 The (OH)2 nickel manganese compound material has a molar ratio of 1:1.02 with respect to the lithium source. The sintering in step S04 is a second heat treatment process, in which the temperature range of the second heat treatment process is 300°C to 710°C, the treatment time of the second heat treatment process is 24 hours to 30 hours, and the temperature rise rate of the second heat treatment process is 2.5°C / min. As shown in FIG. 1, the composite positive electrode material 1 includes a core layer 10 and a coating layer 20, and the core layer 10 is LiNi 0.5 Mn 1.5 O4, and a coating layer 20 covers the core layer 10, the coating layer 20 being made of a LATP solid electrolyte material.

[0013] In this embodiment, in order to obtain an optimal solid electrolyte coating effect, Ni 0.25 Mn 0.75The weight percentage range of the LATP solid electrolyte material to the (OH)2 nickel manganese compound material is controlled to be 0.2 wt.% to 1.0 wt.%.

[0014] 4A to 4D are SEM images of the first comparative example. In the first comparative example, a lithium nickel manganese oxide positive electrode material LMNO (LiNi 0.5 Mn 1.5 O4) is not coated with the LATP solid electrolyte.

[0015] 5A to 5D are SEM images of a composite positive electrode material according to a first embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the (OH)2 nickel manganese compound material is 0.2 wt.%, and a composite positive electrode material is prepared by the above steps S01 to S04.

[0016] 6A to 6D are SEM images of a composite positive electrode material according to a second embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the (OH)2 nickel manganese compound material is 0.5 wt.%, and a composite positive electrode material is prepared by the above steps S01 to S04.

[0017] 7A to 7D are SEM images of a composite positive electrode material according to a third embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the (OH)2 nickel manganese compound material is 1.0 wt.%, and a composite positive electrode material is prepared by the steps S01 to S04.

[0018] FIG. 8 is a potential-capacity charge-discharge curve diagram of the first comparative example, the first embodiment of the present invention, the second embodiment, and the third embodiment. This is a measurement of the button batteries manufactured in the first comparative example, the first embodiment of the present invention, the second embodiment, and the third embodiment at a 0.1C charge-discharge rate (C-rate). The positive electrode sheet of the button battery is composed of a positive electrode material, a conductive agent, and a binder in a ratio of 94:4:2, and the negative electrode sheet is lithium metal. The electrolyte of the button battery includes 1.15 M lithium hexafluorophosphate (LiPF6), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and 5 wt% fluoroethylene carbonate (FEC). The results of the 0.1C first cycle and second cycle charge-discharge capacity are shown in Table 1. Table 1 also shows the performance results after the samples of the first comparative example and the first, second and third examples of the present invention were charged at 0.2 and discharged at 1C / 2C / 3C / 5C. As shown in FIG. 8 and Table 1, the first, second and third examples of the present invention all have better capacitance and rate performance than the first comparative example. Thus, the present invention is a method for producing Ni by dry mechanical mixing. 0.25 Mn 0.75 After mixing the (OH)2 nickel manganese compound material with the LATP solid electrolyte material, a lithium source can be added, and then mixing and sintering processes can be carried out to obtain a composite positive electrode material having a core layer and a coating layer, which can be found to be helpful in improving the capacitance performance and rate performance of the lithium nickel manganese oxide positive electrode material LMNO. [Table 1]

[0019] FIG. 9 is a capacity retention vs. cycle number discharge curve diagram of the first comparative example, the first embodiment, the second embodiment, and the third embodiment of the present invention. This is a measurement of the button batteries manufactured in the first comparative example, the first embodiment, the second embodiment, and the third embodiment of the present invention at a 1C charge / discharge rate (C-rate). As shown in FIG. 9, the capacity retention of the first to third embodiments of the present invention is all superior to that of the first comparative example. Thus, by using the composite positive electrode material formed by the manufacturing method of the present invention, the cycle performance of the lithium nickel manganese oxide positive electrode material LMNO can be improved and the cycle life can be extended.

[0020] FIG. 10 is a flow chart of a method for producing a composite positive electrode material in a second embodiment of the present invention. In this embodiment, a nickel manganese compound material is first provided, and the nickel manganese compound material is Ni 0.25 Mn 0.75 In this embodiment, Ni 0.25 Mn 0.75 O is Ni 0.25 Mn 0.75 (OH)2 is pre-oxidized. As shown in step S00', Ni 0.25 Mn 0.75 (OH)2 is obtained, a preliminary oxidation process is carried out, and Ni 0.25 Mn 0.75 O. Ni 0.25 Mn 0.75 O nickel manganese compound material can be obtained. 0.25 Mn 0.75 O. Ni 0.25 Mn 0.75 The nickel manganese compound material has an average particle size of 10 μm to 20 μm, for example, 13.96 μm, and a surface area of ​​20.49 m. 2 The temperature range of the preliminary oxidation process is 300° C. to 850° C., the treatment time of the preliminary oxidation process is 5 hours to 7 hours, and the temperature rise rate of the preliminary oxidation process is 2.5° C. / min. In another embodiment, Ni 0.25 Mn 0.75O may be obtained by other processing processes, and the present invention is not limited thereto. Next, as shown in step S02', a lithium aluminum titanium phosphate LATP solid electrolyte material is provided, and Ni 0.25 Mn 0.75 The NiO nickel manganese compound material and the LATP solid electrolyte material are mixed by the dry mechanofusion method to form a composite material. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the O nickel manganese compound material is 0.2 wt.% to 1.0 wt.%. In step S02', mixing the nickel manganese compound material and the solid electrolyte by a mechanical method includes mixing at a rotation speed of 700 rpm for 5 minutes, mixing at a rotation speed of 1400 rpm for 5 minutes, mixing at a rotation speed of 2100 rpm for 5 minutes, mixing at a rotation speed of 2800 rpm for 10 minutes, and mixing at a rotation speed of 3500 rpm for 10 minutes. The operating temperature of mixing the nickel manganese compound material and the solid electrolyte by a mechanical method is 25°C to 45°C. After the mixing by the mechanical method, a first heat treatment process is performed (step S03'). The temperature range of the first heat treatment process is 300°C to 750°C, the treatment time of the first heat treatment process is 5 hours to 7 hours, and the temperature rise rate of the first heat treatment process is 2.5°C / min.

[0021] Next, as shown in step S04', a lithium source, such as lithium hydroxide, is provided, and the lithium source is mixed with the composite material and sintered to form a composite cathode material. 0.25 Mn 0.75 The molar ratio of the LiNiO nickel manganese compound material to the lithium source is 1:1.02. The sintering in step S04' is a second heat treatment process, in which the temperature range is 300°C to 710°C, the treatment time is 24 hours to 30 hours, and the temperature rise rate is 2.5°C / min. As shown in FIG. 1, the composite positive electrode material 1 includes a core layer 10 and a coating layer 20, and the core layer 10 is made of LiNi 0.5 Mn 1.5O4, and a coating layer 20 covers the core layer 10, the coating layer 20 being made of an LATP solid electrolyte material.

[0022] In this embodiment, in order to obtain an optimal solid electrolyte coating effect, Ni 0.25 Mn 0.75 The weight percentage range of the LATP solid electrolyte material relative to the O nickel manganese compound material is controlled to be 0.2 wt.% to 1.0 wt.%.

[0023] 11A to 11D are SEM images of a composite positive electrode material according to a fourth embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the O nickel manganese compound material is 0.2 wt.%, and a composite positive electrode material is prepared by the steps S01' to S04'.

[0024] 12A to 12D are SEM images of a composite positive electrode material according to a fifth embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the O nickel manganese compound material is 0.3 wt.%, and a composite positive electrode material is prepared by the steps S01' to S04'.

[0025] 13A to 13D are SEM images of a composite positive electrode material according to a sixth embodiment of the present invention. 0.25 Mn 0.75 The weight percentage of the LATP solid electrolyte material to the O nickel manganese compound material is 0.5 wt.%, and a composite positive electrode material is prepared by the steps S01' to S04'.

[0026] FIG. 14 is a potential-capacity charge-discharge curve diagram of the first comparative example, the fourth embodiment, the fifth embodiment, and the sixth embodiment of the present invention. This is a measurement of the button batteries manufactured in the first comparative example, the fourth embodiment, the fifth embodiment, and the sixth embodiment of the present invention at a 0.1C charge-discharge rate (C-rate). The positive electrode sheet of the button battery is composed of a positive electrode material, a conductive agent, and a binder in a ratio of 94:4:2, and the negative electrode sheet is lithium metal. The electrolyte of the button battery includes 1.15 M lithium hexafluorophosphate (LiPF6), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and 5 wt% fluoroethylene carbonate (FEC). The results of the 0.1C first cycle and second cycle charge-discharge capacity are shown in Table 2. Table 2 also shows the rate performance results after the samples of the first comparative example and the fourth, fifth and sixth examples of the present invention were charged for 0.2 and discharged at 1C / 2C / 3C / 5C. As shown in FIG. 14 and Table 2, the capacitance and rate performances of the fourth, fifth and sixth examples of the present invention are all superior to those of the first comparative example. Thus, it is possible to obtain Ni by using a dry mechanical mixing method as in the present invention. 0.25 Mn 0.75 After mixing the O nickel manganese compound material and the LATP solid electrolyte material, a lithium source is added and mixed, and then sintering is performed to form a composite positive electrode material having a core layer and a coating layer, thereby improving the capacity performance and rate performance of the lithium nickel manganese oxide positive electrode material LMNO. [Table 2]

[0027] FIG. 15 is a room temperature 1C cycle life curve diagram of the first comparative example, the fourth embodiment, the fifth embodiment, and the sixth embodiment of the present invention. This is a result of measuring the button batteries manufactured in the first comparative example, the fourth embodiment, the fifth embodiment, and the sixth embodiment of the present invention at a 1C charge / discharge rate (C-rate). As shown in FIG. 15, the capacity retention rates of the fourth to sixth embodiments of the present invention are all superior to the capacity retention rate of the first comparative example. Thus, by using the composite positive electrode material formed by the manufacturing method of the present invention, the cycle performance of the lithium nickel manganese oxide positive electrode material LMNO can be improved and the cycle life can be extended.

[0028] As described above, the present invention provides a method for manufacturing a solid electrolyte material comprising: 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 By controlling the weight percentage range of nickel manganese compound materials such as O to 0.2 wt.% to 1.0 wt.%, a composite positive electrode material with excellent coating effect can be obtained. 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 It is more preferable that the weight percentage of the LATP solid electrolyte material with respect to the nickel manganese compound material such as O is 0.2 wt.% to 0.3 wt.%. In other words, the present invention can form a coating layer with improved rate performance of the lithium nickel manganese oxide positive electrode material LMNO by simply adding a small amount of lithium aluminum titanium phosphate LATP solid electrolyte, further reducing the manufacturing cost and obtaining an optimal solid electrolyte coating effect. On the other hand, the composite positive electrode material of the present invention forms the lithium nickel manganese oxide positive electrode material LMNO by mixing lithium aluminum titanium phosphate (LATP) into the pretreatment material of the lithium nickel manganese oxide positive electrode material LMNO. The pretreatment material can be, for example, Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75O nickel manganese compound material, and the lithium nickel manganese oxide positive electrode material LMNO is not directly used in the coating process.

[0029] In the second comparative example, a lithium nickel manganese oxide positive electrode material LMNO was obtained, and 0.2 wt.% LATP solid electrolyte material was added. The average particle size of the lithium nickel manganese oxide positive electrode material LMNO was about 15.13 μm and the surface area was 0.31 m. 2 / g. A second comparative example can be obtained by coating the LATP solid electrolyte material on the surface of the lithium nickel manganese oxide positive electrode material LMNO using the same mixing method.

[0030] In the third comparative example, a lithium nickel manganese oxide positive electrode material LMNO was obtained, and 0.2 wt.% LATP solid electrolyte material was added. The average particle size of the lithium nickel manganese oxide positive electrode material LMNO was about 15.13 μm, and the surface area was 0.31 m. 2 The third comparative example can be obtained by coating the LATP solid electrolyte material on the surface of the lithium nickel manganese oxide positive electrode material LMNO using the same mixing method, and then performing a sintering process.

[0031] FIG. 16 is a diagram showing the potential-capacity charge-discharge curves of Comparative Example 2, Comparative Example 3, Example 1 of the present invention, and Example 4. This is a measurement of the button batteries manufactured in Comparative Example 2, Comparative Example 3, Example 1 of the present invention, and Example 4 at a 0.1C charge-discharge rate (C-rate). The results of the 0.1C first cycle and second cycle charge-discharge capacity are shown in Table 3. Table 3 also shows the rate performance results after the samples of Comparative Example 2, Comparative Example 3, Example 1 of the present invention, and Example 4 are charged at 0.2 and discharged at 1C / 2C / 3C / 5C. As shown in FIG. 16 and Table 3, the capacity performance and rate performance of the first and fourth examples of the present invention are both better than those of Comparative Example 2 and Comparative Example 3. As a result, when a composite positive electrode material is manufactured by mixing a nickel manganese compound material and an LATP solid electrolyte material using a dry mechanical mixing method as in the present invention, adding a lithium source, mixing, and sintering the material, the capacity performance and rate performance are superior to those obtained by directly coating the LATP solid electrolyte material on the lithium nickel manganese oxide positive electrode material LMNO. [Table 3]

[0032] FIG. 17 is a room temperature 1C cycle life curve diagram of the third comparative example, the first embodiment of the present invention, and the fourth embodiment. This is a measurement of the button batteries manufactured in the third comparative example, the first embodiment of the present invention, and the fourth embodiment at a 1C charge / discharge rate (C-rate). As shown in FIG. 17, the capacity retention rates of the first and fourth embodiments of the present invention are all superior to that of the third comparative example. In addition, the cycle life after 200 cycles of the first and fourth embodiments of the present invention is increased by 10% compared to the third comparative example. Thus, in the method of forming the lithium nickel manganese oxide positive electrode material LMNO by mixing lithium aluminum titanium phosphate (LATP) into the pretreatment material of the lithium nickel manganese oxide positive electrode material LMNO by a mechanical method such as the mechanofusion method, Mn 3+Reduces the formation of Mn 3+ This can prevent the metal from dissolving from the positive electrode material and being reduced and deposited on the negative electrode, causing electrical deterioration during cycling.

[0033] In addition, the present invention uses a mixing method of a dry mechanical fusion method to mix the nickel manganese compound material with a solid electrolyte, and completes the surface coating of the solid electrolyte at the same time as the heat treatment of the lithium manganese oxide positive electrode material LMNO. This makes the manufacturing process simple and fast, and the resulting composite positive electrode material can reliably improve the performance of the positive electrode material, which is superior to directly coating the lithium manganese oxide positive electrode material LMNO with a solid electrolyte. In addition, in order to obtain an optimal solid electrolyte coating effect, the present invention can form a coating layer that improves the rate performance of the lithium nickel manganese oxide positive electrode material LMNO by simply adding a small amount of lithium aluminum titanium phosphate LATP solid electrolyte, which can further reduce the manufacturing cost. By controlling the mixing method, operating temperature, rotation speed and time of the lithium aluminum titanium phosphate (LATP) and the pretreatment material, the structural defects of the solid electrolyte coating layer caused by high temperature or excessive friction between particles can be prevented, and at the same time, the lithium nickel manganese oxide positive electrode material LMNO can exhibit low impedance and good charge and discharge performance due to the coating layer of the LATP solid electrolyte. Of course, Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 O nickel manganese compound material, lithium aluminum titanium phosphate (Li 1.3 Al 0.3 Ti 1.7 (PO4)3, LATP) solid electrolyte, and lithium nickel manganese oxide positive electrode material (LiNi 0.5 Mn 1.5 The composition of O4, LMNO) can be adjusted according to actual demand. For example, Ni x Mn y (OH)2 or Ni x Mn y LiO nickel manganese compound material 1+z Al z Ti2-z Lithium aluminum titanium phosphate (Li) can also be obtained by mixing the lithium source with a (PO4)3 solid electrolyte (where x+y=1, z≦2) and then adding and mixing the lithium source and sintering the mixture. 1+z Al z Ti 2-z (PO4)3) is used as the lithium nickel manganese oxide positive electrode material LiNi 2x Mn 2y A composite cathode material coated on the surface of O4 can be obtained, the details of which are omitted here.

[0034] As described above, the present invention provides a method for manufacturing a composite positive electrode material, which uses a dry mechanical fusion method to process a precursor and a solid electrolyte to form a positive electrode material, and simultaneously completes the surface coating of the solid electrolyte. This makes the manufacturing process simple and quick, and effectively improves the performance of the positive electrode material. 1.3 Al 0.3 Ti 1.7 The present invention uses a dry mechanical mixing method to coat the (PO4)3,LATP) solid electrolyte, and Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 A composite positive electrode material having a core layer and a coating layer can be formed by first mixing the nickel manganese compound material of O with the solid electrolyte material, then adding a lithium source, mixing, and sintering. The inner core layer is LiNi 0.5 Mn 1.5O4, and the outer coating layer is made of a solid electrolyte material. The lithium aluminum titanium phosphate (LATP) solid electrolyte has excellent inherent ion conduction properties, so when the lithium aluminum titanium phosphate (LATP) coats the surface of the lithium nickel manganese oxide positive electrode material LMNO to form a composite positive electrode material, it helps to improve the rate performance and cycle performance of the lithium nickel manganese oxide positive electrode material LMNO, and the lithium aluminum titanium phosphate (LATP) coating layer can also provide a protective function to delay the damage caused by the electrolyte to the material surface. In addition, to achieve the optimal solid electrolyte coating effect, the solid electrolyte material is made of Ni 0.25 Mn 0.75 (OH)2 or Ni 0.25 Mn 0.75 The weight percentage range of the nickel manganese compound material such as O is controlled to 0.2 wt.% to 1.0 wt.%, and more preferably to 0.2 wt.% to 0.3 wt.%. That is, in the present invention, by simply adding a small amount of lithium aluminum titanium phosphate (LATP) solid electrolyte, a coating layer that improves the rate performance of the lithium nickel manganese oxide positive electrode material LMNO can be formed, and the manufacturing cost can be further reduced. Rather than directly coating the lithium nickel manganese oxide positive electrode material LMNO with lithium aluminum titanium phosphate (LATP), the present invention forms the lithium nickel manganese oxide positive electrode material LMNO by mixing the lithium aluminum titanium phosphate (LATP) into the pretreatment material of the lithium nickel manganese oxide positive electrode material LMNO by a mechanical method such as a mechanofusion method, for example, so that the lithium nickel manganese oxide positive electrode material LMNO can be formed without any problem. 3+ The production of Mn 3+It can prevent the lithium manganese oxide (LMNO) from dissolving from the positive electrode material and reducing and depositing on the negative electrode, which causes electrical deterioration during cycling. The operating temperature of the mixing process is, for example, 25°C to 45°C, and the rotation speed is 700 rpm to 3500 rpm, and the mixing time is 5 minutes to 30 minutes in stages. By controlling the mixing method, operating temperature, rotation speed and time of the lithium aluminum titanium phosphate (LATP) and the pretreatment material, the structural defects of the solid electrolyte coating layer caused by high temperature or excessive friction between particles can be prevented, and at the same time, the lithium nickel manganese oxide positive electrode material LMNO can exhibit low impedance and good charge and discharge performance due to the coating layer of the LATP solid electrolyte.

[0035] The present invention can be modified or changed in various ways by those skilled in the art, but all such modifications and changes are included in the scope of the claims of the present invention without departing from the technical spirit of the present invention. [Explanation of symbols]

[0036] 1: Composite cathode material 10: Core layer 11: Li+ ion 20: Covering layer 30: Electrolyte S01~S04, S00'~S04': Step

Claims

1. 1. A method for producing a composite positive electrode material, comprising: A nickel manganese compound material is provided, the nickel manganese compound material comprising Ni x Mn y (OH) 2 Or Ni x Mn y O and x+y=1; and (b) providing a solid electrolyte material, and mixing the nickel manganese compound material and the solid electrolyte material by mechanical mixing to form a composite material, the weight percentage of the solid electrolyte material to the nickel manganese compound material being 0.2 wt. % to 1.0 wt. %; Providing a lithium source, mixing the lithium source with the composite material and sintering to form the composite positive electrode material, the composite positive electrode material comprising a core layer and a coating layer, the core layer being LiNi 2x Mn 2y O 4 and step (c), wherein the coating layer covers the core layer, the coating layer being composed of the solid electrolyte material.

2. The nickel manganese compound material is Ni 0.25 Mn 0.75 (OH) 2 and in step (b), a first heat treatment process is performed after the mechanical mixing, the temperature range of the first heat treatment process is 300° C. to 850° C., the treatment time of the first heat treatment process is 5 hours to 7 hours, and the heating rate of the first heat treatment process is 2.5° C. / min.

3. The nickel manganese compound material is Ni 0.25 Mn 0.75 2. The method for producing a composite positive electrode material according to claim 1, wherein the temperature range of the pre-oxidation process is 300° C. to 850° C., the treatment time of the pre-oxidation process is 5 hours to 7 hours, and the heating rate of the pre-oxidation process is 2.5° C. / min.

4. 4. The method of claim 3, wherein in step (b), after the mechanical mixing, a first heat treatment process is performed, the temperature range of the first heat treatment process is 300° C. to 750° C., the treatment time of the first heat treatment process is 5 hours to 7 hours, and the heating rate of the first heat treatment process is 2.5° C. / min.

5. 2. The method of claim 1, wherein in step (b), the process of mechanically mixing the nickel manganese compound material and the solid electrolyte includes mixing at a rotation speed of 700 rpm for 5 minutes, mixing at a rotation speed of 1400 rpm for 5 minutes, mixing at a rotation speed of 2100 rpm for 5 minutes, mixing at a rotation speed of 2800 rpm for 10 minutes, and mixing at a rotation speed of 3500 rpm for 10 minutes.

6. 2. The method for producing a composite positive electrode material according to claim 1, wherein in step (b), the operating temperature of mixing the nickel manganese compound material and the solid electrolyte by the mechanical method is 25° C. to 45° C.

7. The chemical formula of the solid electrolyte is Li 1+z A z Ti 2-z (P.O. 4 ) 3 2. The method of claim 1, wherein z is less than or equal to 2.

8. The method of claim 1 , wherein the mechanical method comprises a mechanical fusion method.

9. 2. The method of claim 1, wherein in step (c), the process of mechanically mixing the lithium source and the composite material includes mixing at a rotation speed of 700 rpm for 5 minutes and mixing at a rotation speed of 1400 rpm for 30 minutes.

10. 2. The method for producing a composite positive electrode material according to claim 1, wherein the step (c) includes a second heat treatment process, the temperature range of the second heat treatment process is 300° C. to 710° C., the treatment time of the second heat treatment process is 24 hours to 30 hours, and the temperature rise rate of the second heat treatment process is 2.5° C. / min.

11. 2. The method of claim 1, wherein in step (c), the molar ratio of the nickel manganese compound material to the lithium source in the composite material is 1:1.

02.

12. 2. The method of claim 1, wherein the weight percentage is between 0.2 wt. % and 0.3 wt. %.

13. 2. The method for producing a composite positive electrode material according to claim 1, wherein the nickel manganese compound material has an average particle size of 10 μm to 20 μm, and the solid electrolyte material has an average particle size of 1 μm to 5 μm.

Citation Information

Patent Citations

  • Surface coverage method for high-voltage nickel manganese acid lithium anode material

    CN102683709A

  • Modified high-specific-capacity high-nickel ternary positive electrode material and preparation method thereof

    CN111600014A

  • Nickel-manganese spinel type positive electrode material as well as preparation method and application thereof

    CN114388812A

  • Nonaqueous electrolyte secondary battery

    JP2014103098A

  • Positive electrode active material composite for lithium ion secondary battery and manufacturing method thereof