Region-selective thin-film formation method
The region-selective thin film forming method using Group 5 metal precursors with alkyl and halogen substitutions enables selective deposition on growth regions, simplifying processes and reducing costs by omitting etching steps and minimizing leakage.
Patent Information
- Application Number
- JP2024069838
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-15
AI Technical Summary
Existing thin film deposition methods lack the ability to selectively form high-quality films on specific areas of a substrate, leading to unnecessary process steps and increased costs.
A region-selective thin film forming method using Group 5 metal precursor compounds, such as niobium, tantalum, or vanadium, with specific alkyl and halogen substitutions, and optionally a selectivity-imparting agent, to adsorb and react on designated growth regions while suppressing deposition in non-growth regions.
The method achieves selective thin film deposition with enhanced selectivity, omitting subsequent etching steps, reducing manufacturing time and costs, and minimizing leakage current.
Smart Images

Figure 2024160957000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for selectively forming a thin film in an area, and more particularly to a Group 5 metal compound capable of forming a Group 5 metal-containing thin film having excellent thermal stability, a low growth per cycle (GPC) rate during a deposition process, and a high residue content, and a method for forming a Group 5 metal-containing thin film using the same. [Background technology]
[0002] As electronic technology develops, there is a rapid demand for miniaturization and weight reduction of electronic elements used in various electronic devices. In order to form miniaturized electronic elements, various physical and chemical deposition methods have been proposed, and various researches are underway to manufacture various electronic elements such as metal thin films, metal oxide thin films, and metal nitride thin films by such deposition methods.
[0003] In the manufacture of semiconductor devices, metal thin films are generally formed using a metal organic chemical vapor deposition (MOCVD) or atomic layer deposition (ALD) process.
[0004] Among these, the ALD deposition process is a technology that forms ultra-thin films by exposing metal precursor compounds and reactants, which are the raw materials for the thin film, to the substrate surface in a vacuum state, and has the advantage of being able to control the thickness finely and form high-quality thin films.In addition, the ALD deposition process has the advantage of being excellent in step coverage because of the self-limiting reaction, and being a relatively low-temperature process, it is possible to avoid deterioration of device characteristics due to thermal diffusion.
[0005] In the ALD deposition process, thin films are formed through surface chemical reactions, so the surface characteristics differ depending on the material of the substrate surface, which results in differences in the initial growth behavior of the thin film. By selectively depositing a thin film in a specific area using these characteristics, subsequent processes such as etching can be omitted, simplifying the process steps and thus reducing manufacturing time and production costs. Therefore, there has been active research into methods for selectively depositing a thin film in a specific area. Summary of the Invention [Problem to be solved by the invention]
[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to selectively form a high quality thin film on a substrate, thereby simplifying the process and reducing costs by eliminating subsequent processes.
[0007] The object of the present invention is not limited to the above-mentioned objects, and other objects not mentioned herein will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0008] The method for forming a region-selective thin film according to an embodiment of the present invention includes a substrate preparation step of supplying a substrate having a growth region and a non-growth region into a chamber and stabilizing the substrate, a precursor supply step of supplying a metal precursor compound into the chamber and adsorbing the metal precursor compound onto the substrate, a purging step of purging the chamber, and a thin film formation step of supplying a reactant into the chamber to react with the metal precursor compound to form a thin film, wherein the metal precursor compound is a Group 5 metal precursor compound represented by Chemical Formula 1 below.
[0009] [C1] [ka] (In the above Chemical formula 1, M is any one selected from the group 5 metal elements niobium (Nb), tantalum (Ta), and vanadium (V); R1, R2, and R3 are each independently selected from linear alkyl groups having 1 to 6 carbon atoms and branched alkyl groups having 3 to 6 carbon atoms; and X is each independently a halogen element.)
[0010] According to another embodiment of the present invention, the method further includes a selectivity imparting agent supplying step between the substrate preparing step and the precursor supplying step, for supplying a selectivity imparting agent to the chamber to cause the selectivity imparting agent to be adsorbed on the substrate.
[0011] Further details of the embodiments are included in the detailed description and the drawings. Effect of the Invention
[0012] A thin film formed by the area selective thin film formation method according to an embodiment of the present invention has an excellent selectivity between non-growth regions and growth regions, and subsequent processes such as an etching process can be omitted after deposition of the thin film, simplifying the process steps, thereby providing process advantages that can reduce manufacturing time and production costs.
[0013] In addition, the method for selectively depositing a thin film according to an embodiment of the present invention can minimize leakage current by preventing a thin film from being deposited on an unnecessary area.
[0014] The effects of the present invention are not limited to the above-mentioned examples, and various other effects are included within the scope of the present invention. [Brief description of the drawings]
[0015] [Figure 1] 1 is a process flow chart illustrating a method for forming a region-selective thin film in accordance with an embodiment of the present invention. [Diagram 2] 10 is a process flow chart illustrating a method for forming a region-selective thin film in accordance with another embodiment of the present invention. [Diagram 3]1 is a graph showing thickness changes by cycle for each of Example 1, Example 2, Comparative Example 1, and Comparative Example 2. [Figure 4a] 1 is a graph showing the results of XPS analysis of a SiN region of a niobium-containing thin film according to Comparative Example 2. [Figure 4b] 1 is a graph showing the results of XPS analysis of a TiN region of a niobium-containing thin film according to Comparative Example 2. [Figure 5a] 1 is a graph showing the results of XPS analysis of a SiN region of a niobium-containing thin film according to Example 2. [Figure 5b] 1 is a graph showing the results of XPS analysis of a TiN region of a niobium-containing thin film according to Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The advantages and features of the present invention, and the methods for achieving them, will become apparent from the following detailed description of the embodiments in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms. The embodiments are provided solely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the present invention of the scope of the invention. The present invention is only defined by the scope of the claims.
[0017] In describing the present invention, if it is determined that a specific description of related publicly known technology may unnecessarily obscure the gist of the present invention, the detailed description will be omitted. When "including," "having," "being made," and the like are used in the present invention, other parts may be added since "only" is not used. When a component is expressed in the singular, it includes the case where it includes the plural, unless otherwise expressly specified.
[0018] When interpreting elements, they are interpreted as including a margin of error even if there is no other explicit description.
[0019] FIG. 1 is a flow chart of steps for explaining a method for selectively forming a thin film according to an embodiment of the present invention.
[0020] Referring to FIG. 1, the region-selective thin film formation method includes a substrate preparation step (S110) of supplying a substrate including a growth region and a non-growth region into a chamber and stabilizing it, a precursor supply step (S120) of supplying a metal precursor compound into the chamber and adsorbing it onto the substrate, a first purge step (S130) of purging the inside of the chamber, a thin film formation step (S140) of supplying a reactant into the chamber to react with the metal precursor compound to form a thin film, and a second purge step (S150) of purging the inside of the chamber after the thin film formation step.
[0021] Each step will be described in detail below. For ease of explanation, the thin film is formed by an atomic layer deposition (ALD) method, but is not limited thereto. As another example, the thin film may be formed by a metal organic chemical vapor deposition (MOCVD) method.
[0022] First, in the substrate preparation step (S110), a substrate including a growth region and a non-growth region is supplied to a chamber and stabilized. The substrate including the growth region and the non-growth region is prepared so that a thin film can be selectively formed on the region. The growth region is a region where a thin film is grown, and the non-growth region is a region where the thin film growth is inhibited.
[0023] For example, the growth region may include one or more of TiN and NbN, such materials not inhibiting the reactivity of the precursors therein allowing a thin film to form.
[0024] For example, the non-growth region may include one or more of Si, SiN, SiO2, SiCO, SiOCN, and SiCN. Such materials may inhibit the reactivity of the precursors and inhibit the formation of the thin film.
[0025] In this manner, by using a substrate including growth and non-growth regions, a thin film can be deposited in the growth regions, while the growth of the thin film is inhibited in the non-growth regions, enabling area-selective thin film formation.
[0026] After the substrate is fed into the chamber, the process includes purging the chamber with an inert gas such as argon, nitrogen, or helium to remove impurities from the chamber, thereby suppressing the generation of by-products due to side reactions and forming a high-quality thin film.
[0027] After purging the chamber with the inert gas, a step may be included to allow the temperature of the substrate to stabilize to a desired level.
[0028] For example, the temperature of the substrate may be maintained at a temperature of 50° C. to 700° C. or 100° C. to 600° C. Within this range, the metal precursor compound exists in a gas phase, and the deposition process described below can proceed smoothly.
[0029] Next, the precursor supply step (S120) is a step of supplying a metal precursor compound into the chamber and allowing it to be adsorbed onto the substrate.
[0030] For example, the metal precursor compound may be supplied to the substrate by any one of a bubbling method, a vapor phase mass flow controller method, a direct gas injection (DGI) method, a direct liquid injection (DLI) method, a liquid transfer method in which the metal precursor compound is dissolved in an organic solvent and transferred, and the like.
[0031] The metal precursor compound thus supplied is adsorbed to the growth region of the substrate. At this time, the metal precursor compound may be partially adsorbed to the non-growth region of the substrate, but may be adsorbed at a high density to the growth region and only partially to the non-growth region.
[0032] If necessary, the metal precursor compound may be supplied together with a carrier gas or a diluent gas. The carrier gas is unreactive with the metal precursor compound, is lighter than the metal precursor compound, and can easily transport the vaporized metal precursor compound to the reaction chamber. The diluent gas is unreactive with the metal precursor compound and does not induce side reactions, and can easily control the reaction, such as the growth rate of the thin film, by controlling the flow rate. For example, each of the carrier gas and the diluent gas may be one or more selected from argon (Ar), nitrogen (N2), helium (He), and hydrogen (H2).
[0033] For example, the metal precursor compound may be mixed with a carrier gas or diluent gas including one or more selected from argon (Ar), nitrogen (N2), helium (He) and hydrogen (H2) and transported onto the substrate by bubbling, direct gas injection, or direct liquid injection.
[0034] The metal precursor compound is a Group 5 metal precursor compound represented by Chemical Formula 1.
[0035] [C1] [ka]
[0036] In Chemical formula 1, M may be any one selected from the metal elements of Group 5. For example, M may be any one selected from niobium (Nb), tantalum (Ta), and vanadium (V).
[0037] In Chemical formula 1, R1, R2, and R3 may each be independently selected from a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms. When a cyclopentadiene ligand is substituted with the substituents R2 and R3, the bonding strength between the Group 5 metal and the ligand compound may be reduced compared to a Group 5 metal compound containing an unsubstituted cyclopentadiene ligand. This may reduce the amount of unwanted residues in the thin film formed during the deposition process.
[0038] Preferably, for example, in Chemical formula 1, R1 may be a branched alkyl group having 3 to 4 carbon atoms, and R2 and R3 may each be a linear alkyl group having 1 to 6 carbon atoms. In this case, the content of unnecessary residues in the thin film during the deposition process is further reduced, and a high-quality metal thin film can be provided.
[0039] In Chemical formula 1, R2 and R3 may be different from each other. When the substituents R2 and R3 bonded to the cyclopentadiene ligand are different from each other and have an asymmetric structure, the melting point of the precursor compound is low and the precursor compound can exist in a liquid state at room temperature, so that a metal thin film having high reproducibility and uniform physical properties can be formed.
[0040] In one embodiment of the present invention, in the case of a Group 5 metal compound in which R2 and R3 are substituted with different alkyl groups, an asymmetric Group 5 metal compound in which one of R2 and R3 is hydrogen has an advantage of having a high vapor pressure and being easy to deposit.
[0041] In addition, when the sum of the carbon numbers of R2 and R3 is the same, a Group 5 metal compound having an asymmetric structure in which R2 and R3 are different from each other has a higher vapor pressure than a Group 5 metal compound having a symmetric structure in which R2 and R3 are the same, and thus a high-quality metal thin film can be easily formed through a deposition process.
[0042] In Chemical formula 1, the sum of the carbon number of R2 and the carbon number of R3 may be 3 or less. In this case, there is an advantage that the compound has excellent thermal stability and high vapor pressure, and can exist in a liquid state at room temperature, and therefore the deposition process is easy. In Chemical formula 1, if the sum of the carbon number of R2 and the carbon number of R3 is more than 3, the Group 5 metal compound can exist in a liquid state at room temperature, but may exhibit high viscosity characteristics. Therefore, in terms of ease of processing and forming a high-quality Group 5 metal thin film, the sum of the carbon number of R2 and the carbon number of R3 in Chemical formula 1 may be 3 or less.
[0043] In Chemical formula 1, X may be each independently a halogen element. Specifically, for example, X may be each independently any one selected from fluorine (F), chlorine (Cl), bromine (Br) and iodine (I), and preferably, for example, X may be each chlorine (Cl).
[0044] Specifically, for example, the metal precursor compound may be selected from compounds represented by the following formulas 1a, 1b, and 1c, but is not limited thereto.
[0045] [Case 1a] [ka] [C1b] [ka] [C1c] [ka]
[0046] In formulas 1a, 1b and 1c, M may be each independently any one selected from the group consisting of niobium (Nb), tantalum (Ta) and vanadium (V).
[0047] Next, the first purge step (S130) is a step of purging the inside of the chamber with an inert gas. For example, the inert gas may be one or more selected from argon, nitrogen, helium, etc. Purging the inside of the chamber with an inert gas such as argon can remove unadsorbed precursors and by-products, and a high-quality thin film can be formed.
[0048] Next, the thin film forming step (S140) is a step of supplying reactants into the chamber to react with the metal precursor compound to form a thin film.
[0049] Reactants are provided inside the chamber and the substrate is exposed to the reactants, where they react with the metal precursor compounds adsorbed on the growth region to form a thin film.
[0050] For example, the reactant may be one or more reactive gases selected from water vapor (H2O), oxygen (O2), and ozone (O3), which can easily react with the precursor compound to form a good quality thin film.
[0051] For example, the above steps can be performed at a temperature range of 50° C. to 700° C. and a pressure of 10 Torr or less. In this case, a high-quality thin film can be easily formed.
[0052] Next, the second purge step (S150) is a step of purging the inside of the chamber after the thin film formation step. In the second purge step, when a thin film of a desired thickness is formed, the inside of the chamber is purged with one or more inert gases selected from argon, nitrogen, helium, etc., to remove unreacted materials and by-products, etc.
[0053] According to an embodiment of the present invention, the precursor compound represented by Chemical formula 1 enables selective deposition by suppressing nucleation growth on non-growth regions including Si. Therefore, after deposition of the thin film, subsequent processes such as an etching process can be omitted, simplifying the process steps, thereby providing a process advantage of reducing manufacturing time and production costs. In addition, leakage current can be minimized by preventing deposition of the thin film on unnecessary regions.
[0054] FIG. 2 is a flow chart of steps for explaining a method for selectively forming a thin film according to another embodiment of the present invention.
[0055] Referring to FIG. 2, the region-selective thin film formation method includes a substrate preparation step (S210) of supplying a substrate having a growth region and a non-growth region into a chamber and stabilizing it, a selectivity imparting agent supply step (S220) of supplying a selectivity imparting agent into the chamber to be adsorbed onto the substrate, a first purge step (S230) of purging the inside of the chamber, a precursor supply step (S240) of supplying a metal precursor compound into the chamber to be adsorbed onto the substrate, a second purge step (S250) of purging the inside of the chamber, a thin film formation step (S260) of supplying a reactant into the chamber to react with the metal precursor compound to form a thin film, and a third purge step (S270) of purging the inside of the chamber after the thin film formation step.
[0056] The region-selective thin film formation method according to another embodiment shown in Fig. 2 is substantially the same as the thin film formation method according to the embodiment shown in Fig. 1, except that it further includes a selectivity imparting agent supply step and a purge step between the substrate preparation step and the precursor supply step, and therefore, a duplicated description of the same process steps will be omitted.
[0057] A method for forming a region-selective thin film according to another embodiment of the present invention includes a step of providing a selectivity imparting agent (S220) following a step of preparing a substrate (S210).
[0058] The selectivity imparting agent supply step (S220) is a step in which a selectivity imparting agent is supplied to the chamber and adsorbed onto the substrate. The selectivity imparting agent thus supplied is adsorbed onto the non-growth region of the substrate. At this time, the selectivity imparting agent is adsorbed onto the non-growth region of the substrate at a high density, and although a portion of the selectivity imparting agent may also be adsorbed onto the growth region, an extremely small portion of the selectivity imparting agent is adsorbed onto the non-growth region of the substrate.
[0059] The selectivity imparting agent may be a compound represented by formula II.
[0060] [C2] [ka]
[0061] In Chemical Formula 2, a, b, c, and d are each independently an integer of 0 to 8; 11 ~R 13 are each independently an alkyl group having 1 to 8 carbon atoms; R 14 may be selected from hydrogen, an alkyl group having 1 to 8 carbon atoms, and an alkoxy group having 1 to 8 carbon atoms.
[0062] For example, in Chemical Formula 2, a, b, c, and d are each independently an integer of 0 to 1; R 11 ~R 13 are each independently a linear alkyl group having 1 to 3 carbon atoms, and R 14 may be hydrogen or a linear alkyl group having 1 to 3 carbon atoms.
[0063] The selectivity imparting agent as described above has excellent interaction with the non-growth region material, such as a material containing one or more of Si, SiN, SiO2, SiCO, SiOCN, and SiCN, and can be adsorbed at a high density in the non-growth region.
[0064] The selectivity imparting agent has low reactivity with the metal precursor compound, and therefore can effectively suppress the growth of the thin film in the non-growth region, thereby further increasing the selectivity ratio between the non-growth region and the growth region when the step of supplying the selectivity imparting agent is included, further facilitating the region-selective formation of the thin film.
[0065] Preferably, for example, the selectivity imparting agent may be a compound represented by the following formula 2a: In this case, there is an even greater advantage in selectivity.
[0066] [chemical 2a] [ka]
[0067] The selectivity imparting agent may be supplied in the same manner as the above-mentioned precursor compound. For example, the selectivity imparting agent may be supplied to the substrate by any one of a bubbling method, a vapor phase mass flow controller method, a direct gas injection (DGI) method, a direct liquid injection (DLI) method, a liquid transfer method in which the selectivity imparting agent is dissolved in an organic solvent and transferred, and the like.
[0068] If necessary, the selectivity imparting agent may be supplied with a carrier gas or a diluent gas, for example, the carrier gas and the diluent gas may each be one or more selected from argon (Ar), nitrogen (N2), helium (He) and hydrogen (H2).
[0069] For example, the selectivity imparting agent may be mixed with a carrier gas or diluent gas including one or more selected from argon (Ar), nitrogen (N2), helium (He) and hydrogen (H2) and transported onto the substrate by a bubbling method, a direct gas injection method, or a direct liquid injection method.
[0070] The method includes a first purge step (S230) following the selectivity imparting agent supply step (S220). The first purge step (S230) is a step of purging the inside of the chamber with an inert gas. Purging the chamber with an inert gas removes unadsorbed selectivity imparting agent and impurities, allowing a high-quality thin film to be formed.
[0071] The precursor supply step (S240), the second purge step (S250), the thin film formation step (S260), and the third purge step (S270) that are performed next are the same as the corresponding steps of the thin film formation method according to one embodiment shown in Fig. 1. Therefore, a duplicated description will be omitted.
[0072] According to another embodiment of the present invention, the method for forming a region-selective thin film includes a step of supplying a selectivity imparting agent, which can further suppress the growth of a precursor compound in a non-growth region. This can provide a process advantage of further increasing the selectivity between the non-growth region and the growth region, and simplifying the process steps by eliminating subsequent processes such as an etching process after the deposition of the thin film, thereby reducing manufacturing time and production costs. In addition, leakage current can be minimized by preventing the deposition of a thin film in an unnecessary region.
[0073] The method for forming a region-selective thin film according to the present invention will be described in more detail below with reference to the following examples, which are presented only to aid in the understanding of the present invention and are not intended to limit the present invention.
[0074] [Example 1] A niobium-containing thin film was formed on a substrate including an area formed of a titanium nitride film (TiN) and an area formed of a silicon nitride film (SiN) using a niobium-containing precursor, tBuN=Nb(EtMeCp)Cl2, represented by the following formula 1a. The specific thin film formation method is as follows.
[0075] [Case 1a] [ka]
[0076] A wafer piece including an area of 2cm x 2cm formed with a titanium nitride film and an area of a silicon nitride film was placed in a load lock using a fixture wafer and then transferred to an atomic layer deposition chamber. Thereafter, argon was supplied to stabilize the temperature of the substrate so that it reached the target level. The precursor tBuN=Nb(EtMeCp)Cl2 was supplied by vaporizing the liquid precursor through a liquid delivery system (LDS) in a vaporizer. The precursor flow rate was 0.02g per minute, and the carrier gas was 600sccm. Ozone was used as the reactive gas, with a flow rate of 600sccm and an ozone concentration of 170g / cm. 3 was supplied.
[0077] The selective deposition method of a niobium-containing thin film through an ALD process is as follows, and the following process was carried out as one cycle.
[0078] 1) A step of supplying the precursor tBuN=Nb(EtMeCp)Cl2 to a reaction chamber through a liquid delivery system (LDS) to adsorb the precursor.
[0079] 2) Supplying argon, an inert gas, into the reaction chamber to remove unadsorbed precursors and by-products.
[0080] 3) A step of supplying ozone, which is a reactive gas, into the reaction chamber to react with the adsorbed precursor and form a niobium oxide film.
[0081] 4) supplying an inert gas into the reaction chamber to remove any unreacted materials or by-products that have been decomposed;
[0082] [Example 2] The procedure was the same as in Example 1, except for the supply of a selectivity imparting agent. Trimethyl orthoformate (TMOF) was used as the selectivity imparting agent. The selectivity imparting agent TMOF was supplied by vaporizing liquid TMOF in a vaporizer through a liquid delivery system (LDS) in the same manner as the tBuN=Nb(EtMeCp)Cl2 precursor. The flow rate of the selectivity imparting agent TMOF was 0.02 g per minute, and the carrier gas was supplied at 200 sccm.
[0083] The selective deposition method of a niobium-containing thin film through an ALD process is as follows, and the following process was carried out as one cycle.
[0084] 1) The selectivity imparting agent TMOF is supplied to the reaction chamber through the LDS (Liquid Delivery System) method and adsorbed.
[0085] 2) Supplying argon, an inert gas, into the reaction chamber to remove unadsorbed TMOF and by-products.
[0086] 3) Supplying the precursor tBuN=Nb(EtMeCp)Cl2 to the reaction chamber through a liquid delivery system (LDS) to adsorb the precursor.
[0087] 4) Supplying argon, an inert gas, into the reaction chamber to remove unadsorbed precursors and by-products.
[0088] 5) A step of supplying ozone, which is a reactive gas, into the reaction chamber to react with the adsorbed precursor and form a niobium oxide film.
[0089] 6) supplying an inert gas into the reaction chamber to remove any unreacted decomposed materials or by-products;
[0090] [Comparative Example 1] A niobium-containing thin film was formed in the same manner as in Example 1, except that TBTDEN (Tert-butylimido tris(diethylamido) niobium) was used as the precursor.
[0091] [Comparative Example 2] A niobium-containing thin film was formed in the same manner as in Example 2, except that TBTDEN (Tert-butylimido tris(diethylamido) niobium) was used as the precursor.
[0092] [Experimental Example 1] The thickness change due to the cycles was investigated for the niobium-containing thin films deposited on the Si substrates in Example 1, Example 2, Comparative Example 1, and Comparative Example 2. Figure 3 is a graph showing the thickness change due to the cycles for each of Example 1, Example 2, Comparative Example 1, and Comparative Example 2.
[0093] 3, when comparing the incubation periods of the niobium-containing thin films on the Si substrate, it can be seen that the incubation period of the niobium thin film formed from the tBuN=Nb(EtMeCp)Cl2 precursor in Example 1 is much longer than that of the niobium thin film formed from the TBTDEN precursor in Comparative Example 1. This means that the strength of the Nb-Cl bond of tBuN=Nb(EtMeCp)Cl2 is stronger and the reactivity is relatively weaker compared to the Nb-N bond of TBTDEN, and the nucleation growth of tBuN=Nb(EtMeCp)Cl2 on the Si substrate is slower than that of TBTDEN.
[0094] In addition, it can be seen that when the selectivity imparting agent TMOF is used, the nucleus growth is suppressed and the incubation period is further extended. In this case, it can be seen that when the selectivity imparting agent TMOF is used for tBuN=Nb(EtMeCp)Cl2 in Example 2, the incubation period is much longer than when the selectivity imparting agent TMOF is used for TBTDEN in Comparative Example 2. This can be analyzed as the adsorbed selectivity imparting agent may have the effect of interacting with TBTDEN, which has a relatively high reactivity, and desorbing, but since the reactivity with tBuN=Nb(EtMeCp)Cl2 is relatively low, the interaction occurs less, and the nucleus growth suppression effect by the selectivity imparting agent is more strongly exhibited.
[0095] From this, it can be seen that when forming a niobium thin film on a Si substrate, if tBuN=Nb(EtMeCp)Cl2 is used as a precursor, nucleus growth is suppressed more than when TBTDEN is used, enabling selective deposition, and if a selectivity imparting agent is used, nucleus growth is further suppressed and the selectivity can be further improved.
[0096] [Experimental Example 2] In order to investigate the region selectivity characteristics of the niobium-containing thin film according to Comparative Example 2, XPS (X-ray photoelectron spectroscopy) analysis was performed, and deposition was carried out while changing the cycle from 3 to 30 cycles. The content of niobium present in the region containing SiN and the region containing TiN was analyzed through XPS. FIG. 4a is an XPS Nb 3d peak graph for the SiN region of the niobium-containing thin film according to Comparative Example 2, and FIG. 4b is an XPS Nb 3d peak graph for the TiN region of the niobium-containing thin film according to Comparative Example 2.
[0097] 4a and 4b, it can be seen that in the SiN region, the Nb 3d peak changes little as the number of cycles increases, whereas in the TiN region, the Nb 3d peak increases rapidly as the number of cycles increases. In addition, when comparing the atomic concentration of niobium, it can be seen that there is almost no change in the concentration in the SiN region, whereas the concentration increases rapidly in the TiN region.
[0098] This can be interpreted as the reason why the selectivity imparting agent TMOF is adsorbed relatively more in the non-growth region where SiN is formed, delaying the nucleation growth of the TBTDEN precursor in the subsequent step. However, in the case of niobium thin film using TBTDEN precursor and selectivity imparting agent TMOF, it can be confirmed that the growth in the non-growth region of SiN is not completely suppressed, and the Nb 3d peak increases as the cycle increases.
[0099] Table 1 below shows the niobium concentration and selectivity of the niobium-containing thin film after cycling using the selectivity imparting agent TMOF and the precursor TBTDEN.
[0100] [Table 1]
[0101] Referring to Table 1, it can be seen that when a selectivity imparting agent is applied to TBTDEN, the selectivity between the SiN region and the TiN region is at a level of about 1:3 to 1:4.
[0102] [Experimental Example 3] In order to investigate the region selectivity of the niobium-containing thin film according to Example 2, XPS (X-ray photoelectron spectroscopy) analysis was performed, and deposition was carried out while changing the cycle from 5 to 30 cycles. The content of niobium present in the region containing SiN and the region containing TiN was analyzed through XPS. Figure 5a is an XPS Nb 3d peak graph for the SiN region of the niobium-containing thin film according to Example 2, and Figure 5b is an XPS Nb 3d peak graph for the TiN region of the niobium-containing thin film according to Example 2.
[0103] 5a and 5b, when using the selectivity imparting agent TMOF and the precursor tBuN=Nb(EtMeCp)Cl2, the Nb 3d peak on the SiN region is very low, and even with an increase in cycles, the Nb 3d peak does not change, so it can be seen that the growth of tBuN=Nb(EtMeCp)Cl2 is almost suppressed. In contrast, it can be seen that the Nb 3d peak increases further as the cycles increase on the TiN region, so it can be seen that the growth on the TiN region proceeded normally. This can be analyzed as the selectivity imparting agent TMOF is strongly adsorbed on the SiN region, and the interaction between tBuN=Nb(EtMeCp)Cl2 and TMOF is relatively weak, so the growth on the SiN region is completely suppressed.
[0104] Table 2 below shows the niobium concentration and selectivity by cycling a niobium-containing thin film using the selectivity imparting agent TMOF and the precursor tBuN=Nb(EtMeCp)Cl2.
[0105] [Table 2]
[0106] Referring to Table 2, when a selectivity imparting agent is applied to tBuN=Nb(EtMeCp)Cl2, the selectivity between the SiN region and the TiN region is about 1:11 to 1:14, which is a much higher selectivity than when TBTDEN is used.
[0107] To summarize the above experimental examples, when tBuN=Nb(EtMeCp)Cl2 is used as a precursor in forming a niobium thin film, it shows region selectivity without using a selectivity imparting agent, and when a selectivity imparting agent is further included, the selectivity ratio is further increased, and subsequent processes such as an etching process can be omitted after deposition of the thin film, simplifying the process steps, thereby providing a process advantage that can reduce manufacturing time and production costs. In addition, it is possible to minimize leakage current by preventing deposition of the thin film in unnecessary areas.
[0108] A method for forming a region-selective thin film according to various embodiments of the present invention can be described as follows.
[0109] The method for forming a region-selective thin film according to an embodiment of the present invention includes a substrate preparation step of supplying a substrate having a growth region and a non-growth region into a chamber and stabilizing the substrate, a precursor supply step of supplying a metal precursor compound into the chamber and adsorbing the metal precursor compound onto the substrate, a purging step of purging the chamber, and a thin film formation step of supplying a reactant into the chamber to react with the metal precursor compound to form a thin film, wherein the metal precursor compound is a Group 5 metal precursor compound represented by Chemical Formula 1 below.
[0110] [C1] [ka] (In the above Chemical formula 1, M is any one selected from the group 5 metal elements niobium (Nb), tantalum (Ta), and vanadium (V); R1, R2, and R3 are each independently selected from linear alkyl groups having 1 to 6 carbon atoms and branched alkyl groups having 3 to 6 carbon atoms; and X is each independently a halogen element.)
[0111] According to another aspect of the present invention, the method may further include a purging step of purging the inside of the chamber after the thin film forming step.
[0112] According to another feature of the present invention, in Chemical formula 1, R1 may be a branched alkyl group having 3 to 4 carbon atoms, and R2 and R3 may each be a linear alkyl group having 1 to 6 carbon atoms.
[0113] According to another feature of the present invention, in Chemical formula 1, R2 and R3 are different from each other, and the sum of the number of carbon atoms in R2 and the number of carbon atoms in R3 may be 3 or less.
[0114] According to yet another feature of the invention, the growth region may include one or more of TiN and NbN.
[0115] According to yet another aspect of the invention, the non-growth region may include one or more of Si, SiN, SiO2, SiCO, SiOCN, and SiCN.
[0116] According to another aspect of the present invention, in the thin film forming step, the reactant may be one or more reactant gases selected from water vapor (H2O), oxygen (O2), and ozone (O3).
[0117] According to another aspect of the present invention, the steps may be performed at a substrate temperature in the range of 50 to 700°C.
[0118] According to another aspect of the present invention, a selectivity imparting agent supply step may be further included between the substrate preparation step and the precursor supply step, for supplying a selectivity imparting agent to the chamber to cause the selectivity imparting agent to be adsorbed on the substrate.
[0119] According to yet another feature of the present invention, the selectivity imparting agent may be a compound represented by the following formula 2:
[0120] [C2] [ka]
[0121] According to another aspect of the present invention, in the formula (2), a, b, c, and d are each independently an integer from 0 to 8; 11 ~R 13 are each independently an alkyl group having 1 to 8 carbon atoms; R 14 may be selected from hydrogen, an alkyl group having 1 to 8 carbon atoms, and an alkoxy group having 1 to 8 carbon atoms.
[0122] According to another aspect of the present invention, the thin film may be formed by a metal organic chemical vapor deposition (MOCVD) method or an atomic layer deposition (ALD) method.
[0123] According to another aspect of the present invention, the precursor supplying step may include a step of transporting the metal precursor compound to the substrate through one method selected from a bubbling method, a vapor phase mass flow controller (MFC) method, a direct gas injection (DGI) method, a direct liquid injection (DLI) method, and an organic solution supplying method in which the metal precursor compound is dissolved in an organic solvent and transported.
[0124] According to another aspect of the present invention, in the precursor supply step, the metal precursor compound is transferred onto the substrate by a bubbling method, a direct gas injection method, or a direct liquid injection method together with a carrier gas, and the carrier gas may include one or more selected from the group consisting of argon (Ar), nitrogen (N2), helium (He), and hydrogen (H2).
[0125] Although the present invention has been described in detail through the embodiments, the present invention is not necessarily limited to these embodiments, and various modifications can be made within the scope of the technical idea of the present invention. Therefore, the embodiments disclosed in the present invention are for illustration purposes, not for limiting the technical idea of the present invention, and the scope of the technical idea of the present invention is not limited by these embodiments. Therefore, it should be understood that the embodiments described above are illustrative and not restrictive in all respects. The scope of protection of the present invention should be interpreted according to the following claims, and all technical ideas within the scope equivalent thereto should be interpreted as being included in the scope of the present invention.
Claims
1. a substrate preparation step of providing a substrate including growth and non-growth regions to the chamber and stabilizing the substrate; a precursor supply step of supplying a metal precursor compound to the interior of the chamber and allowing it to adsorb onto the substrate; A purging step for purging the interior of the chamber; and providing a reactant into the chamber to react with the metal precursor compound to form a thin film; The method for forming a region-selective thin film, wherein the metal precursor compound is a Group 5 metal precursor compound represented by the following Chemical Formula 1. [Chemical formula 1] 【Chemistry 11】 (In the above formula 1, M is any one selected from the group consisting of niobium (Nb), tantalum (Ta), and vanadium (V), which are group 5 metal elements; R 1 , R 2 and R 3 are each independently selected from a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and each X is independently a halogen element.
2. 2. The method of claim 1, further comprising a step of purging the inside of the chamber after the step of forming the thin film.
3. In the above formula 1, R 1 is a branched alkyl group having 3 to 4 carbon atoms, R 2 and R 3 and each of are a linear alkyl group having 1 to 6 carbon atoms.
4. In the above formula 1, R 2 and R 3 are different from each other, The R 2 and the number of carbon atoms in R 3 2. The method for forming a region-selective thin film according to claim 1, wherein the sum of the numbers of carbon atoms in the above is 3 or less.
5. 2. The method of claim 1, wherein the growth region includes at least one of TiN and NbN.
6. The non-growth region is made of Si, SiN, SiO 2 2. The method for selectively forming a thin film according to claim 1, wherein the thin film comprises at least one of SiCO, SiOCN and SiCN.
7. In the thin film forming step, the reactant is water vapor (H 2 O) and oxygen (O 2 ), ozone (O 3 2. The method for forming a thin film selectively according to claim 1, wherein the reactant gas is one or more selected from the group consisting of a nitrogen gas, a nitrogen gas, a nitrogen oxide, a nitrogen gas ...
8. 2. The method of claim 1, wherein the substrate preparation step is performed at a temperature of the substrate within a range of 50 to 700.degree.
9. 2. The method for forming a region-selective thin film according to claim 1, further comprising a selectivity-imparting agent supplying step between the substrate preparation step and the precursor supplying step, for supplying a selectivity-imparting agent to the chamber and causing the selectivity-imparting agent to be adsorbed on the substrate.
10. 10. The method for forming a region-selective thin film according to claim 9, wherein the selectivity imparting agent is a compound represented by the following Chemical Formula 2: [Chemical 2] 【Chemistry 12】 (In the above formula 2, a, b, c, and d are each independently an integer of 0 to 8; R 11 ~R 13 are each independently an alkyl group having 1 to 8 carbon atoms; R 14 is selected from hydrogen, an alkyl group having 1 to 8 carbon atoms, and an alkoxy group having 1 to 8 carbon atoms.
11. 2. The method of claim 1, wherein the thin film is formed by a metal organic chemical vapor deposition (MOCVD) method or an atomic layer deposition (ALD) method.
12. 2. The method of claim 1, wherein the precursor supplying step comprises transferring the metal precursor compound to the substrate through one method selected from the group consisting of a bubbling method, a vapor phase mass flow controller (MFC) method, a direct gas injection (DGI) method, a direct liquid injection (DLI) method, and an organic solution supplying method in which the metal precursor compound is dissolved in an organic solvent and transferred.
13. In the precursor supply step, the metal precursor compound is moved onto the substrate together with a carrier gas by the bubbling method, the direct gas injection method, or the direct liquid injection method; The carrier gas is argon (Ar), nitrogen (N 2 ), helium (He) and hydrogen (H 2 13. The method of claim 12, further comprising the steps of:
Citation Information
Cited By
Thin film formation method and manufacturing method of memory device including the same