Transfer mold, object to be transferred, and method for producing the same
A transfer mold with a wrinkle-like uneven structure, formed using a curable (meth)acrylate composition and vacuum ultraviolet curing, addresses the challenges of achieving uniform matte properties and scratch resistance in architectural and display materials, ensuring high transparency and durability.
Patent Information
- Application Number
- JP2024144329
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing methods for imparting matte properties to architectural materials and display members suffer from insufficient matting effects, uneven hardness and scratch resistance, and issues with durability and compatibility of materials, leading to quality problems and non-uniform performance.
A transfer mold with a wrinkle-like uneven structure, characterized by specific roughness parameters (RSm and Sa) and local inclination angles (θa), is created using a curable composition that includes (meth)acrylate, which is cured using vacuum ultraviolet rays to form a matte surface with excellent matte properties.
The solution provides a transfer mold and object with superior matte properties, enhanced scratch resistance, and uniform hardness, suitable for anti-glare films and displays, while maintaining high transparency and durability.
Smart Images

Figure 2024161113000001 
Figure 2024161113000002 
Figure 2024161113000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a transfer mold, a transfer target, and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art In order to impart a matte finish to building materials such as wallpaper, display members, decorative films and other members, fine irregularities are sometimes imparted to the surface of the base material. Patent Document 1 discloses a method for providing fine unevenness by hairline processing, sandblasting, matte processing, etc., on transfer foil film used in the molding of decorative sheets for building materials, various parts of home appliances such as refrigerators and washing machines, various parts of office automation products such as personal computers, packaging containers, etc. Patent Document 2 discloses a method for forming surface irregularities on a light diffusing film used in a backlight unit of a liquid crystal display, in which acrylic particles are dispersed in a resin binder. Patent Document 3 discloses a method for forming surface irregularities by phase separation to prevent anti-Newton rings. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-231727 A [Patent Document 2] Japanese Patent Application Publication No. 7-218705 [Patent Document 3] JP 2011-2820 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the method of forming the irregularities described in Patent Document 1 does not provide a sufficient matte effect. Moreover, in the case of sandblasting, sand remaining in the film can cause quality problems. In the method described in Patent Document 2, the acrylic particles fall off during use, which may impair visibility when used in displays and the like. In the method described in Patent Document 3, the uneven structure is formed by using compounds that are incompatible with each other, so the components are not uniform in the layer that forms the uneven structure. As a result, the hardness and scratch resistance are locally non-uniform, resulting in areas with poor performance, and the uneven strength has the disadvantage of being prone to partial chipping during the transfer process. In addition, the refractive index also has the disadvantage of changing within the plane depending on the material used. In addition, if a polymer that does not contribute to hardening is used, the hardness and scratch resistance of the entire uneven structure are reduced, making it unsuitable for transfer applications. Furthermore, in the case of the phase separation method, it is necessary to use a material having a highly polar functional group, such as a cellulose ester, in order to make the materials incompatible with each other. However, the use of such a material results in poor resistance to moist heat and dimensional stability, making it unsuitable for transfer applications. Furthermore, due to the nature of phase separation, a release agent cannot be added because it would cause leveling, and so there is also the disadvantage that a release layer must be provided for transfer (resulting in a two-layer structure).
[0005] An object of the present invention is to provide a transfer mold and a transfer object having excellent matte properties, and methods for producing the same. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A transfer type in which the transfer surface has a wrinkled uneven structure, and the average length of the roughness curve element (RSm) of the transfer surface according to JIS B0601:2013 is 1 to 1000 μm, and the arithmetic mean height (Sa) defined in ISO25178 is 0.1 to 1000 μm. [2] The transfer mold according to [1], wherein the average value (θa) of the local inclination angle of the transfer surface is 2° or more. [3] A transfer mold according to [1] or [2], wherein the 60° gloss of the transfer surface is 50 or less. [4] The transfer mold according to any one of [1] to [3] above, wherein the transfer surface is a cured film of a curable composition. [5] The transfer mold according to [4] above, wherein the curable composition contains a (meth)acrylate. [6] The transfer mold according to [4] or [5] above, having the cured film on a substrate. [7] The transfer mold according to [6] above, wherein the substrate is a film. [8] The method for producing a transfer mold according to [6] or [7] above, comprising laminating a curable composition on a substrate and curing the composition by irradiating it with vacuum ultraviolet light. [9] A transfer object having a transfer surface having a wrinkled uneven structure, the transfer surface having a roughness curve element average length (RSm) of 1 to 1000 μm according to JIS B0601:2013, and an arithmetic mean height (Sa) defined in ISO25178 of 0.1 to 1000 μm.
[10] The object according to [9], wherein the average local inclination angle (θa) of the transferred surface is 2° or more.
[11] The object according to [9] or
[10] , wherein the 60° gloss of the transferred surface is 50 or less.
[12] The object for transferring a signal according to any one of the above [9] to
[11] , wherein the surface for transferring a signal is a cured film of a curable composition.
[13] The object according to
[12] , wherein the curable composition contains a (meth)acrylate.
[14] The object to be transferred according to
[12] or
[13] above, having the cured film on a substrate.
[15] The object according to
[14] above, wherein the substrate is a film.
[16] A method for producing a transfer object according to any one of the above [9] to
[15] , comprising transferring a wrinkled uneven structure of a transfer surface of a transfer mold according to any one of the above [1] to [7] as a negative pattern. Effect of the Invention
[0007] The transfer mold and the object to be transferred of the present invention have excellent matt luster. According to the method for producing the transfer mold and the object to be transferred of the present invention, a transfer mold and an object to be transferred that have excellent matt luster can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, "(meth)acrylate" is a general term for acrylate or methacrylate, and "(meth)acrylic" is a general term for acrylic and methacrylic. The symbol "~" indicating a range of values means that the values before and after it are included as the lower and upper limits.
[0009] [Transfer type] The transfer mold of the present invention has a wrinkled uneven structure on the transfer surface, and the average length (RSm) of the roughness curve element according to JIS B0601:2013 of the transfer surface is 1 to 1000 μm, and the arithmetic mean height (Sa) defined by ISO25178 is 0.1 to 1000 μm. This gives the transfer mold a matte finish. The transfer mold of the present invention is suitable for producing an anti-glare film because of its excellent matte finish.
[0010] It is preferable that the uneven surface structure of the transfer mold be formed by a cured film, in consideration of durability and ease of manufacture.
[0011] (Thickness of transfer mold) The thickness of the layer forming the concave-convex structure of the transfer mold (thickness of the cured film (convex-convex layer)) is preferably in the range of 0.1 to 100 μm, more preferably 0.2 to 20 μm, further preferably 0.3 to 10 μm, and particularly preferably 0.3 to 7 μm. If the thickness of the cured product is within the above range, it is easy to achieve the desired matte finish. The thickness of the cured film indicates the maximum thickness of the uneven layer, and is determined by observing a cross section with an electron microscope.
[0012] (average length of roughness curve element) The average length of the roughness curve element in the uneven structure of the cured film is the average length of the roughness curve element (RSm, hereinafter also simply referred to as "RSm") according to JIS B0601:2013. The evaluation length for calculating RSm was 236.87 μm. The preferred range of RSm is 1 to 1000 μm, preferably 1.5 to 150 μm, more preferably 2 to 100 μm, even more preferably 3 to 60 μm, particularly preferably 4 to 50 μm, and most preferably 5 to 35 μm. When within the above range, the film has excellent matte properties, and when the transferred object is used in a display or the like, the film has excellent visibility and scratch resistance, resulting in a well-balanced performance.
[0013] (arithmetic mean height) The arithmetic mean height of the uneven structure of the cured film is the arithmetic mean height (Sa, hereinafter also simply referred to as "Sa") defined by ISO25178. The evaluation area for calculating Sa is 177.60 μm × 236.87 μm. Sa is 0.1 to 1000 μm, preferably 0.1 to 100 μm, more preferably 0.15 to 20 μm, even more preferably 0.2 to 10 μm, particularly preferably 0.3 to 5 μm, and most preferably 0.4 to 3 μm. Within the above range, the film has excellent matte properties, and when the transferred object is used in a display or the like, the film has excellent visibility and scratch resistance, resulting in a well-balanced performance.
[0014] (Average value of the inclination angle of the uneven structure) The average value of the local inclination angle (θa, hereinafter also simply referred to as "θa") in the concave-convex structure of the cured film can be measured by the method described in the Examples described later. The evaluation length for calculating θa was 236.87 μm. θa is preferably 2° or more, more preferably 4° or more, even more preferably 7° or more, particularly preferably 10° or more, and most preferably 12° or more, and the upper limit may be 90°. The higher θa, the better the matte property.
[0015] (Hayes) When the transfer mold has a cured film, the haze of the cured film measured by the method described in the Examples below is preferably 1% or more, more preferably 3% or more, even more preferably 5% or more, particularly preferably 10% or more, and most preferably 20% or more, with the upper limit being, for example, 99%. If the haze is equal to or more than the lower limit, the matte property is easily improved. In particular, when used for anti-glare applications in various displays, the range is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more, with the upper limit being, for example, 99%. Depending on the application, the higher the range, the more preferable it is. If the range is equal to or greater than the lower limit, the anti-glare properties are likely to be good.
[0016] (Gross) The 60° gloss (60° specular gloss) of the transfer surface measured by the method described in the Examples below is preferably 50 or less, more preferably 30 or less, even more preferably 20 or less, particularly preferably 15 or less, and most preferably 11 or less, with the lower the better. When it is equal to or less than the upper limit, the matte finish is excellent. Similarly, the 20° gloss is preferably 30 or less, more preferably 20 or less, even more preferably 10 or less, particularly preferably 5 or less, and most preferably 2 or less, with the lower the better. When the gloss is equal to or less than the upper limit, the matte properties are excellent.
[0017] (Total light transmittance) When searching for defects in the uneven structure of the transfer mold, it is preferable that the material has transparency. The total light transmittance measured by the method described in the examples below is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, particularly preferably 80% or more, and most preferably 90% or more, and the higher the better (the upper limit is 100%). When the total light transmittance is in the above range, the material has excellent transparency.
[0018] (Pencil hardness) The pencil hardness of the transfer surface measured by the method described in the Examples below is preferably F or more, more preferably H or more, and even more preferably 2H or more. Within the above range, a transferred product can be obtained that is excellent in abrasion resistance and resistance to scratches in steps before and after transfer, and has few defects due to scratches on the transfer mold.
[0019] [Method of manufacturing a transfer mold] An example of the transfer mold of the present invention is one made of a cured film, and may be one made of a cured product of a curable composition containing an active energy ray-curable compound. The transfer mold of the present invention can be produced, for example, by laminating a curable composition on a substrate and curing it by irradiating it with vacuum ultraviolet light. The curable composition preferably contains an active energy ray curable compound. By irradiating the curable composition with active energy rays, the surface side of the coating film of the curable composition is cured first to form a cured coating film. When the inside of the coating film is subsequently cured, the cured coating film on the surface side buckles, forming a cured film having wrinkled unevenness on the surface. The curable composition and the method for producing a cured film using the same will be described in detail later.
[0020] (Transfer-type curable composition) The curable composition may further contain an organic solvent and other components in addition to the active energy ray-curable compound.
[0021] (Active energy ray curable compound) As the active energy ray curable compound, (meth)acrylate is a suitable material. The (meth)acrylate is not particularly limited, and a mixture of one or more monofunctional (meth)acrylates, bifunctional (meth)acrylates, and polyfunctional (meth)acrylates, a commercially available curable resin material, or a material to which other components are further added as long as the object of the present embodiment is not impaired can be used. Among these, monofunctional or bifunctional (meth)acrylates are preferred from the viewpoint of easily forming a wrinkled uneven structure. Furthermore, for applications requiring scratch resistance, bifunctional (meth)acrylates are more preferred. Although the use of polyfunctional (meth)acrylates is a preferred form in that scratch resistance and hardness are improved, depending on the compound used, it may be difficult to form a wrinkled uneven structure, so attention should be paid to the type of compound used and the blending ratio.
[0022] The difunctional polyfunctional (meth)acrylate is not particularly limited, but examples thereof include alkanediol di(meth)acrylates such as 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecanedimethylol di(meth)acrylate, and the like, bisphenol-modified di(meth)acrylates such as bisphenol A ethylene oxide-modified di(meth)acrylate and bisphenol F ethylene oxide-modified di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, urethane di(meth)acrylate, and epoxy di(meth)acrylate. Among these, in consideration of the ease of forming a wrinkled uneven structure, a structure without branching is preferable, alkyldiol di(meth)acrylate is more preferable, and alkyldiol di(meth)acrylate having 4 to 18 carbon atoms is even more preferable.
[0023] The monofunctional (meth)acrylate is not particularly limited, but examples thereof include alkyl (meth)acrylates such as methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and methoxypropyl (meth)acrylate; acrylate, alkoxyalkyl (meth)acrylates such as ethoxypropyl (meth)acrylate, aromatic (meth)acrylates such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate, amino group-containing (meth)acrylates such as diaminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate, ethylene oxide-modified (meth)acrylates such as methoxyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate and phenylphenol ethylene oxide-modified (meth)acrylate, glycidyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate.
[0024] The trifunctional or higher polyfunctional (meth)acrylate is not particularly limited, and examples thereof include ethylene oxide-modified (meth)acrylates such as dipentaerythritol hexa(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and ethylene oxide-modified pentaerythritol tetra(meth)acrylate. Examples of the urethane acrylate include trifunctional (meth)acrylate, isocyanuric acid ethylene oxide modified tri(meth)acrylate, isocyanuric acid modified tri(meth)acrylate such as ε-caprolactone modified tris(acryloxyethyl)isocyanurate, pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, etc. Among these, ethylene oxide modified type and trifunctional (meth)acrylate are preferred in consideration of the ease of forming a wrinkled uneven structure.
[0025] In addition, active energy ray-curable compounds other than (meth)acrylates can also be used in the curable composition, such as vinyl compounds (e.g., (meth)acrylic acid, styrene, vinyl halides, vinyl acetate, etc.), and diene compounds (e.g., vinylidene halides, 1,3-butadiene, isoprene, chloroprene, etc.).
[0026] When an active energy ray curable compound is used in the formation of a transfer mold, the content of the compound derived from the active energy ray curable compound in the transfer mold is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 50% by mass or more, and most preferably 60% by mass or more. There is no particular upper limit and it may be 100% by mass, but it is preferably 99% by mass or less, more preferably 98% by mass or less. In the above range, a wrinkled uneven structure is easily formed, and a cured film excellent in hardness and scratch resistance can be formed, and a suitable transfer mold can be obtained.
[0027] (resin) As the transfer mold, various resins can be further used for the purpose of improving adhesion to the substrate, etc. As the resin, various conventionally known resins can be used, for example, acrylic resin, polyester resin, polyurethane resin, polyvinyl resin, etc., and among these, acrylic resin is preferable in terms of excellent transparency and affinity with (meth)acrylate.
[0028] In addition, as the resin used for the transfer mold, particularly in the case of a transfer mold made of a cured film, it is preferable to have an active energy ray-curable functional group such as a carbon-carbon double bond in consideration of improving scratch resistance and hardness. Examples of the active energy ray-curable functional group include a (meth)acryloyl group and a vinyl ether compound. Among these, a (meth)acryloyl group, particularly an acryloyl group, is preferable in consideration of ease of introduction and reactivity.
[0029] In further investigation, we found that when a resin with active energy ray-curable functional groups was used, not only were the properties directly related to the active energy ray-curable functional groups, such as improved scratch resistance and hardness, improved, but also wrinkle-like irregularities were reduced. In other words, it was found that the Rsm and Sa of the transfer surface were reduced. In addition, there were cases where the haze increased and the gloss decreased. These properties have a synergistic effect on the matte finish, and are particularly important in applications where visibility is important, such as display applications.
[0030] As an acrylic resin having an active energy ray-curable functional group such as a carbon-carbon double bond, for example, a method of introducing the double bond can be mentioned, for example, a method of reacting an acrylic resin having an epoxy group with a compound having a double bond and a carboxyl group (Method 1), a method of reacting an acrylic resin having a carboxyl group with a compound having a double bond and an epoxy group (Method 2), a method of reacting an acrylic resin having a hydroxyl group with a compound having a double bond and a carboxyl group (Method 3), a method of reacting an acrylic resin having a carboxyl group with a compound having a double bond and a hydroxyl group (Method 4), a method of reacting an acrylic resin having an isocyanate group with a compound having a double bond and a hydroxyl group (Method 5), a method of reacting an acrylic resin having a hydroxyl group with a compound having a double bond and an isocyanate group (Method 6), etc. In addition, the above methods may be used in combination. In the following, a radically polymerizable monomer having a carbon-carbon double bond may be referred to as a vinyl monomer.
[0031] In the method 1, examples of vinyl monomers having an epoxy group used to obtain an acrylic resin having an epoxy group include glycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate. Among these, glycidyl (meth)acrylate is preferred, and glycidyl methacrylate is particularly preferred, in consideration of good reactivity and ease of use of the material. These may be used alone or in combination of two or more.
[0032] In addition, examples of the compound having a double bond and a carboxyl group in the method 1 include (meth)acrylic acid, carboxyethyl (meth)acrylate, an adduct of glycerin di(meth)acrylate and succinic anhydride, an adduct of pentaerythritol tri(meth)acrylate and succinic anhydride, and an adduct of pentaerythritol tri(meth)acrylate and phthalic anhydride. Among these, (meth)acrylic acid and an adduct of pentaerythritol tri(meth)acrylate and succinic anhydride are preferred, (meth)acrylic acid is more preferred, and acrylic acid is even more preferred. The compound having a double bond and a carboxyl group may be used alone or in combination of two or more.
[0033] In the method 2, examples of the vinyl monomer having a carboxyl group used to obtain the acrylic resin having a carboxyl group include (meth)acrylic acid, carboxyethyl (meth)acrylate, and polybasic acid-modified (meth)acrylate. Among these, (meth)acrylic acid is preferred, and acrylic acid is more preferred. These may be used alone or in combination of two or more.
[0034] In the method 2, examples of the compound having a double bond and an epoxy group include glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether. Among these, glycidyl (meth)acrylate is preferred. These may be used alone or in combination of two or more.
[0035] In the method 3, examples of the vinyl monomer having a hydroxyl group used to obtain the acrylic resin having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and hydroxypropyl (meth)acrylate. These may be used alone or in combination of two or more.
[0036] In the method 3, the compound having a double bond and a carboxyl group may be the same as the compound in the method 1.
[0037] In the method 4, the acrylic resin having a carboxyl group may be the same as that in the method 2.
[0038] In the method 4, examples of the compound having a double bond and a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and hydroxypropyl (meth)acrylate. These may be used alone or in combination of two or more.
[0039] In the method 5, examples of the vinyl monomer having an isocyanate group used to obtain an acrylic resin having an isocyanate group include isocyanate ethyl (meth)acrylate.
[0040] In the method 5, the compound having a double bond and a hydroxyl group may be, for example, the same compound as that exemplified in the method 4.
[0041] In the method 6, the acrylic resin having a hydroxyl group may be the same as the compound in the method 3.
[0042] In the method 6, an example of the compound having a double bond and an isocyanate group is isocyanate ethyl (meth)acrylate. These may be used alone or in combination of two or more.
[0043] Among the above methods, method 1 is preferred because the reaction is easy to control. In method 1, the double bond is introduced by a ring-opening addition reaction between the epoxy group of the acrylic resin having an epoxy group and the carboxyl group of the compound having a double bond and a carboxyl group.
[0044] In the above-mentioned method 1, the monomer having an epoxy group in the acrylic resin having an epoxy group is preferably 5% by weight or more, more preferably 10% by weight or more, and even more preferably 15% by weight or more of the total amount of monomers constituting the acrylic resin having an epoxy group. The upper limit is not particularly limited, but is preferably 99.9% by weight or less, more preferably 80% by weight or less, even more preferably 70% by weight or less, particularly preferably 50% by weight or less, and most preferably 40% by weight or less. By using it in this range, not only the adhesion of the cured film to the substrate, scratch resistance, and hardness are improved, but also wrinkle-like unevenness tends to be finer, and a decrease in RSm, a decrease in Sa, and in some cases an increase in haze and a decrease in gloss can be achieved.
[0045] In the method 1, the compound having a double bond and a carboxyl group is preferably 10 to 150 mol %, more preferably 30 to 130 mol %, and even more preferably 50 to 110 mol %, relative to the epoxy group in the acrylic resin having an epoxy group. By using the compound in the above range, the reaction can be carried out without excess or deficiency, and it is preferable from the viewpoint of reducing the residue of the raw material.
[0046] Furthermore, the acrylic resin, such as the above-mentioned acrylic resin having an epoxy group, may be a copolymer of (meth)acrylates other than those mentioned above or other vinyl monomers. The polymerization reaction of these raw materials is usually radical polymerization, and can be carried out under conventionally known conditions.
[0047] Examples of monomers that can be used in combination as raw materials include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, methoxy(poly)ethylene glycol (meth)acrylate, methoxy(poly)propylene glycol (meth)acrylate, methoxy(poly)ethylene glycol (poly)propylene glycol (meth)acrylate, octoxy(poly)ethylene glycol (meth)acrylate, octoxy(poly)propylene ... Examples of the monomer include (meth)acrylates such as octoxytetramethylene glycol (meth)acrylate, lauroxy(poly)ethylene glycol (meth)acrylate, and stearoxy(poly)ethylene glycol (meth)acrylate; acrylamides such as ethyl(meth)acrylamide, n-butyl(meth)acrylamide, i-butyl(meth)acrylamide, t-butyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N-hydroxypropyl(meth)acrylamide, and N,N-dihydroxyethyl(meth)acrylamide; and styrene monomers such as styrene, p-chlorostyrene, and p-bromostyrene. These monomers may be used alone or in combination of two or more.
[0048] The acrylic resin can be produced by a radical polymerization reaction using the above-mentioned raw material vinyl monomers. The radical polymerization reaction is preferably carried out in an organic solvent in the presence of a radical polymerization initiator.
[0049] Examples of organic solvents used in radical polymerization include ketone solvents such as acetone and methyl ethyl ketone (MEK), alcohol solvents such as ethanol, methanol, isopropyl alcohol (IPA), and isobutanol, ether solvents such as ethylene glycol dimethyl ether and propylene glycol monomethyl ether, ester solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and 2-ethoxyethyl acetate, and aromatic hydrocarbon solvents such as toluene. These organic solvents may be used alone or in combination of two or more.
[0050] Examples of radical polymerization initiators used in radical polymerization include organic peroxides such as benzoyl peroxide and di-t-butyl peroxide; and azo compounds such as 2,2'-azobisbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). These radical polymerization initiators may be used alone or in combination of two or more. The radical polymerization initiator is preferably used in the range of 0.01 to 5 parts by weight per 100 parts by weight of the total of the vinyl monomers as the raw material.
[0051] In addition, during radical polymerization, a chain transfer agent can be used for the purpose of controlling the weight average molecular weight of the acrylic resin. Examples of the chain transfer agent include butanethiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, octadecanethiol, cyclohexyl mercaptan, thiophenol, octyl thioglycolate, octyl 2-mercaptopropionate, octyl 3-mercaptopropionate, 2-ethylhexyl mercaptopropionate, 2-ethylhexyl thioglycolate, butyl-3-mercaptopropionate, mercaptopropyltrimethoxysilane, methyl-3-mercaptopropionate, 2,2-(ethylenediaminetetraacetate), ... Examples of thiol compounds include thiol compounds such as oxy)diethanethiol, ethanethiol, 4-methylbenzenethiol, octanoic acid 2-mercaptoethyl ester, 1,8-dimercapto-3,6-dioxaoctane, decane trithiol, dodecyl mercaptan, diphenyl sulfoxide, dibenzyl sulfide, 2,3-dimethylcapto-1-propanol, mercaptoethanol, thiosalicylic acid, thioglycerol, thioglycolic acid, 3-mercaptopropionic acid, thiomalic acid, mercaptoacetic acid, mercaptosuccinic acid, and 2-mercaptoethanesulfonic acid. These compounds may be used alone or in combination of two or more.
[0052] The amount of the chain transfer agent used is preferably 0.1 to 25 parts by weight, more preferably 0.5 to 20 parts by weight, and even more preferably 1.0 to 15 parts by weight, based on 100 parts by weight in total of the vinyl monomers as the raw material.
[0053] The reaction time of the radical polymerization is preferably 1 to 20 hours, more preferably 3 to 12 hours, and the reaction temperature is preferably 40 to 120°C, more preferably 50 to 100°C.
[0054] In order to react a compound having a double bond and a carboxyl group with an acrylic resin, the compound having a double bond and a carboxyl group is added to the acrylic resin obtained as described above, and the reaction is usually carried out for about 3 to 9 hours at a temperature of usually 90 to 140 ° C., preferably 100 to 120 ° C., in the presence of one or more catalysts such as triphenylphosphine, tetrabutylammonium bromide, tetramethylammonium chloride, and triethylamine. Here, the catalyst is preferably used in a ratio of about 0.5 to 3 parts by weight per 100 parts by weight of the total of the raw material (meth)acrylic acid ester polymer and the compound having a double bond and a carboxyl group. This reaction may be carried out continuously after the acrylic resin is produced by polymerization reaction, or may be carried out by adding the compound having a double bond and a carboxyl group after the acrylic resin is once separated from the reaction system.
[0055] The amount of double bonds in the acrylic resin is preferably in the range of 0.1 to 10 mmol / g, more preferably 0.2 to 7.0 mmol / g, further preferably 0.5 to 5.0 mmol / g, particularly preferably 0.8 to 4.0 mmol / g, and most preferably 1.0 to 3.0 mmol / g. By using within this range, not only is it possible to improve the adhesion of the cured film to the substrate, the scratch resistance, and the hardness, but it is also possible to make the wrinkled uneven shape finer, and it is possible to achieve a decrease in Rsm, a decrease in Sa, and in some cases an increase in haze and a decrease in gloss. The amount of double bonds means the concentration of (meth)acryloyl groups in the acrylic resin, that is, the amount of (meth)acryloyl groups introduced.
[0056] The weight average molecular weight (Mw) of the resin should be appropriately selected depending on the application of the curable composition, but is usually 5000 or more, preferably 7000 or more, more preferably 9000 or more, and usually 200000 or less, preferably 100000 or less, more preferably 70000 or less, and even more preferably 50000 or less. Within the above range, it is easy to form surface irregularities. The weight average molecular weight (Mw) of the resin can be determined as a converted value based on polystyrene standard using gel permeation chromatography (GPC). Specific measurement conditions are shown in the examples below.
[0057] When the transfer mold contains a resin, the content is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of the appearance and adhesion of the cured film. If the resin content is too high, there is a concern that the hardness of the cured film will decrease.
[0058] (particle) In order to further improve the matte property due to the wrinkled uneven structure of the transfer mold, it is also possible to use particles. The particles are not particularly limited, and conventionally known ones can be used. Specific examples include inorganic particles such as silica, hollow silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. The inorganic particles may be particles surface-modified with a silane coupling agent having a reactive group such as a (meth)acryloyl group. The organic particles are preferably of a crosslinked type in order to maintain the shape, and crosslinked acrylic resin particles and crosslinked styrene resin particles are more preferable. Two or more of these particles may be used in combination.
[0059] The average primary particle size of the particles is preferably in the range of 0.01 to 30 μm, more preferably 0.05 to 10 μm, further preferably 0.1 to 5 μm, and particularly preferably 0.5 to 3 μm. When within this range, the matte properties are excellently improved.
[0060] When the transfer mold contains particles, the content is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 8% by mass or less, based on the non-volatile content, from the viewpoint of improving the matte property. There is no particular lower limit, but the content is preferably 0.1% by mass or more, more preferably 1% by mass or more. If the amount of particles is too large, they are likely to fall off, so care must be taken.
[0061] (Antistatic agent) An antistatic agent can be used in the transfer mold. By including an antistatic agent, the transfer mold can be given antistatic properties, which can contribute to preventing adhesion of foreign matter such as dust due to peeling charge, etc., thereby reducing defects due to transfer and obtaining a transfer target as designed.
[0062] The antistatic agent is not particularly limited, and a conventionally known antistatic agent can be used. Examples of the antistatic agent include organic compounds such as polymeric and surfactant types, and inorganic compounds such as metal oxides. Among these, organic compounds are preferred because of the ease of forming a concave-convex structure. Furthermore, polymeric antistatic agents are more preferred because of their good heat resistance, moist heat resistance, and durability. Examples of polymeric antistatic agents include compounds having an ammonium group, polyether compounds, compounds having a sulfonic acid group, betaine compounds, and conductive polymers. Among these, compounds having an ammonium group are more preferred in consideration of the coating appearance.
[0063] The antistatic agent may also be a compound having an active energy ray-curable functional group. An example of the active energy ray-curable functional group is a (meth)acryloyl group. By containing the functional group, it can contribute to the formation of a concave-convex structure and also contribute to the improvement of properties such as scratch resistance.
[0064] The compound having an ammonium group is a compound having an ammonium group in the molecule, and examples thereof include ammonium compounds of aliphatic amines, alicyclic amines, and aromatic amines. The compound having an ammonium group is preferably a compound having a polymer type ammonium group, and the ammonium group is preferably a structure in which it is incorporated in the main chain or side chain of the polymer, not as a counter ion. In addition, among the polymers, those capable of increasing the concentration of ammonium groups are preferable in order to effectively impart antistatic properties, and for this purpose, (meth)acrylic polymers are preferable. For example, a polymer having an ammonium group can be made from a polymer obtained by polymerizing a monomer containing an addition polymerizable ammonium group or a precursor of an ammonium group such as an amine, and is preferably used. The polymer may be a polymer obtained by polymerizing a monomer containing an addition polymerizable ammonium group or a precursor of an ammonium group such as an amine alone, or may be a copolymer of a monomer containing these and another monomer.
[0065] Examples of the ammonium group or the precursor monomer of the ammonium group such as amine include (meth)acrylic acid esters of amino alcohols, specifically, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, N,N-diethylaminopropyl (meth)acrylate, N,N-dimethylaminobutyl (meth)acrylate, N,N-diethylaminobutyl (meth)acrylate, and N,N-dihydroxyethylaminoethyl (meth)acrylate, and N,N-dimethylaminoethyl (meth)acrylate is particularly preferably used. The two alkyl groups of the N,N-dialkylamino group may be different.
[0066] Examples of the ammonium group of the N,N-dialkylamino group-containing monomer include commercially available N,N-dimethylaminoethyl methacrylate quaternized with methyl chloride [e.g., trade name "Light Ester (registered trademark) DQ-100", manufactured by Kyoeisha Chemical Co., Ltd.]. The ammonium group of the N,N-dialkylamino group-containing monomer can also be produced, for example, by a quaternization reaction of a (meth)acrylic acid ester of an amino alcohol.
[0067] In the case of a (meth)acrylic polymer, it may contain a polymerizable monomer unit other than an ammonium group or a precursor monomer of an ammonium group such as an amine. Examples of such a polymerizable monomer include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, and tridecyl (meth)acrylate; (meth)acrylic acid esters of the above amino alcohols; 2-hydroxyethyl (meth)acrylate, 2-methylethyl (meth)acrylate, and 2-methylethyl (meth)acrylate; and the like. Examples of the hydroxyalkyl (meth)acrylates include hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate; various (meth)acrylates such as benzyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, butoxyethyl (meth)acrylate, cyanoethyl (meth)acrylate, and glycidyl (meth)acrylate; styrene, methylstyrene, and the like. These may be used alone or in combination of two or more. Among these, when a polymerizable monomer having a highly hydrophobic long-chain alkyl group is contained, it is preferable because it can be segregated at the air interface of the cured film to enhance the antistatic property of the cured film. The polymerizable monomer having such a long-chain alkyl group is preferably an alkyl(meth)acrylate having 8 to 30 carbon atoms, more preferably an alkyl(meth)acrylate having 12 to 22 carbon atoms, such as lauryl(meth)acrylate, tridecyl(meth)acrylate, and stearyl(meth)acrylate.
[0068] When the compound having an ammonium group is realized as a (meth)acrylic polymer, the ratio of the ammonium group-containing monomer unit in the polymer is preferably 5 to 95% by mass, more preferably 10 to 90% by mass, further preferably 20 to 80% by mass, and particularly preferably 30 to 70% by mass. The higher this ratio, the higher the antistatic property becomes, and the lower this ratio, the better the appearance of the cured layer after coating tends to be, so using it in the above range will achieve a good balance. In the case where a long-chain alkyl group is used in combination, the proportion of the long-chain alkyl group-containing monomer unit in the polymer is preferably 80% by mass or less, more preferably 50% by mass or less, and further preferably 40% by mass or less. By using the long-chain alkyl group in the above range, antistatic properties are easily exhibited.
[0069] When the compound having an ammonium group is realized as a (meth)acrylic polymer, the weight average molecular weight of the polymer is preferably from 800 to 120,000, and more preferably from 2,000 to 60,000.
[0070] When the compound having an ammonium group is realized as a (meth)acrylic polymer, the polymer can be produced by a radical polymerization reaction using the above-mentioned raw material monomers. The radical polymerization reaction is preferably carried out in an organic solvent in the presence of a radical polymerization initiator.
[0071] Examples of organic solvents used in radical polymerization reactions include ketone solvents such as acetone and methyl ethyl ketone (MEK), alcohol solvents such as ethanol, methanol, isopropyl alcohol (IPA), and isobutanol, ether solvents such as ethylene glycol dimethyl ether and propylene glycol monomethyl ether, ester solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and 2-ethoxyethyl acetate, and aromatic hydrocarbon solvents such as toluene. These organic solvents may be used alone or in combination of two or more.
[0072] Examples of radical polymerization initiators used in the radical polymerization reaction include organic peroxides such as benzoyl peroxide and di-t-butyl peroxide; and azo compounds such as 2,2'-azobisbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). These radical polymerization initiators may be used alone or in combination of two or more. The radical polymerization initiator is preferably used in an amount of 0.01 to 5 parts by mass relative to 100 parts by mass of the total of the raw material monomers.
[0073] In addition, in the case of radical polymerization reaction, a chain transfer agent can be used for the purpose of controlling the weight average molecular weight of the polymer. Examples of the chain transfer agent include butanethiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, octadecanethiol, cyclohexyl mercaptan, thiophenol, octyl thioglycolate, octyl 2-mercaptopropionate, octyl 3-mercaptopropionate, 2-ethylhexyl mercaptopropionate, 2-ethylhexyl thioglycolate, butyl-3-mercaptopropionate, mercaptopropyltrimethoxysilane, methyl-3-mercaptopropionate, 2,2-(ethylenediaminetetraacetate), ... Examples of the thiol-based compounds include thiol compounds such as oxy)diethanethiol, ethanethiol, 4-methylbenzenethiol, octanoic acid 2-mercaptoethyl ester, 1,8-dimercapto-3,6-dioxaoctane, decane trithiol, dodecyl mercaptan, diphenyl sulfoxide, dibenzyl sulfide, 2,3-dimethylcapto-1-propanol, mercaptoethanol, thiosalicylic acid, thioglycerol, thioglycolic acid, 3-mercaptopropionic acid, thiomalic acid, mercaptoacetic acid, mercaptosuccinic acid, and 2-mercaptoethanesulfonic acid. These may be used alone or in combination of two or more.
[0074] The amount of the chain transfer agent used is preferably 0.1 to 25 parts by weight, more preferably 0.5 to 20 parts by weight, and even more preferably 1.0 to 15 parts by weight, based on 100 parts by weight of the total of the raw material monomers.
[0075] The reaction time of the radical polymerization reaction is preferably 1 to 20 hours, more preferably 3 to 12 hours, and the reaction temperature is preferably 40 to 120°C, more preferably 50 to 100°C.
[0076] Examples of polyether compounds as antistatic agents include polyethylene oxide, polyether ester amide, and acrylic resins having polyethylene glycol in the side chain.
[0077] The compound having a sulfonic acid group as an antistatic agent is a compound that contains sulfonic acid or a sulfonate salt in the molecule, and for example, a compound that contains a large amount of sulfonic acid or a sulfonate salt, such as polystyrene sulfonic acid, is preferably used.
[0078] Examples of conductive polymers as antistatic agents include polythiophenes, polyanilines, polypyrroles, polyacetylenes, etc., and among them, polythiophenes, such as poly(3,4-ethylenedioxythiophene) in combination with polystyrene sulfonic acid, are preferably used. Conductive polymers are more suitable than the other antistatic agents mentioned above in that they have a low resistance. However, in applications where coloring or cost is a concern, it becomes necessary to take measures such as reducing the amount of use.
[0079] Examples of surfactants as antistatic agents include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Among these, from the viewpoint of improving antistatic properties and compatibility with various resins, anionic surfactants and nonionic surfactants are preferred, and anionic surfactants are particularly preferred.
[0080] Examples of anionic surfactants include sulfonic acid types such as alkyl sulfonates, alkylaryl sulfonates, and ester sulfonates, phosphoric acid types such as alkyl phosphates or salts thereof, polyoxyalkylene alkyl ether phosphates or salts thereof, sulfate types such as alkyl sulfates and alkyl ether sulfates, and carboxylate types such as alkyl fatty acid salts. Among these, sulfonic acid types are preferred from the viewpoint of excellent antistatic properties.
[0081] Examples of sulfonic acid type anionic surfactants include alkyl sulfonates such as decyl sulfonate, dodecyl sulfonate, tetradecyl sulfonate, hexadecylsulfonate, and octadecyl sulfonate, alkyl aryl sulfonates such as butyl benzene sulfonate, hexyl benzene sulfonate, octyl benzene sulfonate, decyl benzene sulfonate, dodecyl benzene sulfonate, tetradecyl benzene sulfonate, hexadecyl benzene sulfonate, octadecyl benzene sulfonate, dibutyl naphthalene sulfonate, and triisopropyl naphthalene sulfonate, and ester sulfonates such as dibutyl sulfosuccinate, dioctyl sulfosuccinate, dodecyl sulfoacetate, and nonylphenoxy polyethylene glycol sulfoacetate. Among these, from the viewpoint of excellent antistatic properties, the number of carbon atoms in the alkyl group is 8 or more, preferably 10 to 22, and more preferably 12 to 18. The salt is preferably a metal salt, more preferably an alkali metal salt such as lithium, sodium or potassium, and even more preferably a sodium salt. As for the type, alkylsulfonate is preferred from the viewpoint of antistatic properties.
[0082] Examples of the phosphoric acid type anionic surfactants include alkyl phosphoric acid esters or salts thereof such as butyl phosphoric acid ester, butyl phosphoric acid ester salts, hexyl phosphoric acid ester, hexyl phosphoric acid ester salts, octyl phosphoric acid ester, octyl phosphoric acid ester salts, decyl phosphoric acid ester, decyl phosphoric acid ester salts, lauryl phosphoric acid ester, lauryl phosphoric acid ester salts, tetradecyl phosphoric acid ester, tetradecyl phosphoric acid ester salts, hexadecyl phosphoric acid ester, hexadecyl phosphoric acid ester salts, stearyl phosphoric acid ester, and stearyl phosphoric acid ester salts; polyoxyethylene butyl ether phosphate, polyoxyethylene butyl ether phosphate salts, polyoxyethylene hexyl ether phosphate, polyoxyethylene hexyl ether phosphate salts, polyoxyethylene octyl ether phosphate, polyoxyethylene octyl ether phosphate salts, polyoxyethylene decyl ether phosphate, and polyoxyethylene Examples of the polyoxyalkylene alkyl ether phosphate ester include polyoxyalkylene alkyl ether phosphate esters or salts thereof, such as polyoxyethylene decyl ether phosphate salts, polyoxyethylene lauryl ether phosphate ester, polyoxyethylene lauryl ether phosphate salts, polyoxyethylene tetradecyl ether phosphate ester, polyoxyethylene tetradecyl ether phosphate salts, polyoxyethylene hexadecyl ether phosphate ester, polyoxyethylene hexadecyl ether phosphate salts, polyoxyethylene stearyl ether phosphate ester, polyoxyethylene stearyl ether phosphate salts, polyoxypropylene octyl ether phosphate ester, polyoxypropylene octyl ether phosphate ester salts, polyoxypropylene decyl ether phosphate ester, polyoxypropylene decyl ether phosphate ester salts, polyoxypropylene lauryl ether phosphate ester and polyoxypropylene lauryl ether phosphate salts.
[0083] Among these, from the viewpoints of surfactant performance and antistatic performance, alkyl phosphate salts and polyoxyalkylene alkyl ether phosphate esters or salts thereof are preferred.
[0084] As for the alkyl phosphate salts, the number of carbon atoms in the alkyl group is 4 or more, preferably 4 to 22, and more preferably in the range of 6 to 12, and as for the polyoxyalkylene alkyl ether phosphate ester or a salt thereof, the number of carbon atoms in the alkyl group is 4 or more, preferably 6 to 22, and more preferably in the range of 8 to 18. As the salts, metal salts and amine salts are preferred, and in particular, alkali metal salts such as lithium, sodium, and potassium, alkylamine salts, and alcoholamine salts are more preferred, and sodium salts and monoethanolamine salts are even more preferred.
[0085] When an antistatic agent is used to impart antistatic properties to the transfer mold, the content of the antistatic agent in the transfer mold is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 1.0% by mass or more, and most preferably 2.0% by mass or more. There is no particular limit to the upper limit, and it may be 100% by mass, but in consideration of the hardness of the cured film, it is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, particularly preferably 10% by mass or less, and most preferably 8% by mass or less. When it is equal to or more than the lower limit, the antistatic properties are excellent.
[0086] (Release agent) The transfer mold may contain a release agent, for example, a compound having a fluorine atom or a silicone compound, in order to improve the antifouling property and transferability. By containing the compound in the transfer mold, transfer abnormalities due to contamination can be reduced. In addition, this leads to the transfer material being easily peeled off from the transfer mold during transfer, and for example, it is not necessary to provide a release layer (two-layer structure) on the transfer mold, which improves productivity, and contributes to the production of a transfer target with fewer foreign matter defects caused by the transfer material remaining on the transfer mold, which is a preferred embodiment.
[0087] The compound having a fluorine atom is a compound that contains a fluorine atom in the compound.As the compound having a fluorine atom, an organic fluorine compound is preferably used, for example, a compound containing a perfluoroalkyl group, a perfluoropolyether compound, a polymer of an olefin compound containing a fluorine atom, an aromatic fluorine compound such as fluorobenzene, etc. From the viewpoint of antifouling, a compound having a perfluoroalkyl group or a perfluoropolyether compound is preferable.Furthermore, the fluorine compound can also be a silicone compound or a compound containing a long-chain alkyl compound.
[0088] Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof; and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and staining resistance, it is preferable to use a polymer. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of stain resistance, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. It may also be a polymer with a compound containing a silicone compound or a long-chain alkyl compound.
[0089] Silicone compounds are compounds having a silicone structure in the molecule, and examples thereof include alkyl silicones such as dimethyl silicone and diethyl silicone, and phenyl silicone and methylphenyl silicone having a phenyl group. Silicones having various functional groups can also be used, and examples thereof include ether groups, hydroxyl groups, amino groups, epoxy groups, carboxylic acid groups, halogen groups such as fluorine, perfluoroalkyl groups, various alkyl groups, and various aromatic groups, and other hydrocarbon groups. As other functional groups, silicones having vinyl groups and hydrogen silicones in which hydrogen atoms are directly bonded to silicon atoms are also common, and it is also possible to use both in combination as addition type silicones (types obtained by the addition reaction of vinyl groups and hydrogen silane). In addition, a method of introducing a double bond such as an acryloyl group and reacting at the double bond is also preferred.
[0090] In addition, as the silicone compound, modified silicones such as acrylic grafted silicone, silicone grafted acrylic, amino modified silicone, perfluoroalkyl modified silicone, etc. are also usable. In consideration of heat resistance and contamination, it is preferable to use a curable silicone resin, and as the type of curable type, any curing reaction type such as condensation type, addition type, active energy ray curable type, etc. can be used.
[0091] In addition, the above-mentioned compound having a fluorine atom or silicone compound is also preferably a compound having an active energy ray curable functional group. Examples of the active energy ray curable functional group include a (meth)acryloyl group and a vinyl ether compound. Among these, in consideration of ease of introduction and reactivity, a (meth)acryloyl group, particularly an acryloyl group, is preferred. By containing the functional group, it can contribute to the formation of a concave-convex structure and also contribute to the improvement of properties such as scratch resistance.
[0092] The content of the compound having a fluorine atom or the silicone compound in the transfer mold is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.3% by mass or more, particularly preferably 0.5% by mass or more, and most preferably 0.7% by mass or more. There is no particular limit to the upper limit, and it may be 100% by mass, but considering the hardness of the cured film, it is preferably 50% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, particularly preferably 5% by mass or less, and most preferably 3% by mass or less. If it is more than the above lower limit, it has excellent transferability and antifouling properties.
[0093] (Photopolymerization initiator) When the transfer mold is formed from a cured film (active energy ray curable compound), a photopolymerization initiator may be used to promote the curing of the cured film. The molecular weight of the photopolymerization initiator is preferably 1000 or less. Specific examples include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin phenyl ether, benzyl diphenyl disulfide, dibenzyl, diacetyl, anthraquinone, naphthoquinone, 3,3'-dimethyl-4-methoxybenzophenone, benzophenone, p,p'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, pivaloin ethyl ether, benzyl dimethyl ketal, 1,1-dichloroacetophenone, pt-butyl dichloroacetophenone, and the like. Examples of the photopolymerization initiator include phenone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-diethylthioxanthone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-dichloro-4-phenoxyacetophenone, phenyl glyoxylate, α-hydroxyisobutylphenone, dibenzosparone, 1-(4-isopropylphenyl)-2-hydroxy-2-methyl-1-propanone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, tribromophenyl sulfone, tribromomethylphenyl sulfone, etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0094] When a photopolymerization initiator is used in the transfer mold, the content of compounds derived therefrom is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 8% by mass or less, and particularly preferably 6% by mass or less, from the viewpoints of promoting curing and the hardness of the cured film.
[0095] (Leveling agent) To improve the appearance of the transfer mold, a leveling agent can be used. Examples of the leveling agent include acrylic leveling agents, silicone leveling agents, fluorine-based leveling agents, etc. These leveling agents may be used alone or in combination of two or more kinds.
[0096] When the transfer film contains a leveling agent, the content thereof is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the non-volatile content, from the viewpoint of improving the appearance of the cured film.
[0097] (Various additives) The transfer mold may contain a polymerization accelerator such as a compound containing a thiol group, a plasticizer, a surfactant, an antioxidant, an ultraviolet absorber, etc., within the scope of not impairing the effects of the present invention.
[0098] (Organic solvent) When the transfer mold is formed from a cured film, an organic solvent may be used as necessary in the curable composition for the purpose of improving workability when applying the composition to a substrate. Examples of organic solvents include aromatic solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone, acetone, methyl isobutyl ketone, and cyclohexanone; ether solvents such as diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, anisole, and phenetole; ester solvents such as ethyl acetate, butyl acetate, isopropyl acetate, and ethylene glycol diacetate; amide solvents such as dimethylformamide, diethylformamide, and N-methylpyrrolidone; cellosolve solvents such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; and halogen-based solvents such as dichloromethane and chloroform. These organic solvents may be used alone or in combination of two or more. Among these organic solvents, ester-based solvents, ether-based solvents, alcohol-based solvents and ketone-based solvents are preferred in that they can easily improve workability during coating.
[0099] The ratio of the organic solvent to 100 parts by mass of the nonvolatile content of the curable composition is preferably from 10 to 1,900 parts by mass, more preferably from 40 to 400 parts by mass, from the viewpoint of improving operability in coating operation. The non-volatile content of the curable composition is the total mass of components other than the solvent such as the organic solvent. The non-volatile content of the curable composition can be measured by a conventionally known method, for example, by measuring the change in weight when 1 g of the composition is spread and heated at 100° C. for 1 hour to volatilize the organic solvent.
[0100] (Formation of coating film) As a method for forming a transfer mold using a cured film, the transfer mold can be formed by applying the curable composition onto the surface of a substrate or an article to form a coating film, drying the coating film as necessary, and then irradiating the coating film with active energy rays. The method for applying the curable composition is not particularly limited, and the composition can be applied by a known method such as dip coating, air knife coating, curtain coating, spin coating, roller coating, bar coating, wire bar coating, gravure coating, or spray coating.
[0101] When the curable composition contains an organic solvent, it is preferable to previously heat-dry the composition before irradiation with active energy rays. By previously heat-drying the composition, the solvent in the coating film can be effectively removed. The drying temperature for the heat drying is preferably from 30° C. to 200° C., more preferably from 40° C. to 150° C. The drying time is preferably from 0.01 to 30 minutes, more preferably from 0.1 to 10 minutes.
[0102] (Irradiation with active energy rays) As the active energy rays, it is important that they have high energy in order to effectively harden the surface of the film, so vacuum ultraviolet rays (ultraviolet rays with a wavelength of 200 nm or less) are preferred. Among them, excimer light with a half-width of 50 nm or less is optimal, and examples of such light include argon (126 nm), krypton (146 nm), xenon (172 nm), and argon-fluorine (193 nm). Among these, xenon excimer light is preferred in consideration of ease of use, effective formation of unevenness, and hardening properties of the cured film.
[0103] When vacuum ultraviolet rays are used, the cumulative amount of irradiation is preferably 1 to 3000 mJ / cm. 2 , more preferably 3 to 1000 mJ / cm 2 , and more preferably 5 to 500 mJ / cm 2 , particularly preferably 10 to 100 mJ / cm 2 The illuminance is preferably in the range of 1 to 500 mW / cm 2 , more preferably 2 to 300 mW / cm 2 , and more preferably 3 to 100 mW / cm 2 The range is.
[0104] In addition, the vacuum ultraviolet irradiation is preferably performed in an environment with low oxygen content, such as a nitrogen atmosphere, etc. The oxygen concentration is preferably 10% or less, more preferably 5% or less, further preferably 3% or less, and particularly preferably 1% or less.
[0105] After the above-mentioned vacuum ultraviolet irradiation, it is preferable to irradiate the cured film with an active energy ray other than vacuum ultraviolet rays in order to cure the film to a deep portion. Examples of the active energy ray other than vacuum ultraviolet rays include ultraviolet rays and electron beams, and among these, ultraviolet rays are more preferable in consideration of the curability of the cured film. The cumulative amount of ultraviolet light to be irradiated is preferably 1 to 5000 mJ / cm 2 , more preferably 50 to 3000 mJ / cm 2 , and more preferably 100 to 1000 mJ / cm 2 , particularly preferably 200 to 700 mJ / cm 2 The illuminance is preferably in the range of 1 to 1000 mW / cm 2 , more preferably 50 to 500 mW / cm 2 , and more preferably 80 to 300 mW / cm 2 The range is.
[0106] [Transfer target] The transfer object of the present invention is an object manufactured by transferring the shape of the transfer mold using the above-mentioned transfer mold as a negative pattern. The transfer object has a wrinkled uneven structure on the transfer surface, and the transfer surface has a mean length of roughness curve elements (RSm) according to JIS B0601:2013 of 1 to 1000 μm and an arithmetic mean height (Sa) defined by ISO25178 of 0.1 to 1000 μm. This gives the transfer object a matte finish and makes it suitable for use in optical applications such as display members.
[0107] (Thickness of the transfer material) The thickness of the transfer target (the layer forming the uneven structure of the transfer target) is preferably in the range of 0.1 to 1000 μm, more preferably 0.2 to 200 μm, further preferably 0.3 to 100 μm, and particularly preferably 0.5 to 30 μm. If the thickness of the transfer target is within the above range, it is easy to achieve the desired matte finish and easy to adjust the hardness. The thickness of the transferred material indicates the maximum thickness of the concave-convex layer, and is determined by observing the cross section with an electron microscope.
[0108] (RSm, Sa, θa of the transcription target) The RSm, Sa, and θa of the transfer surface of the transfer object are preferably in the same range as the transfer mold described above. Another feature of the transfer object of the present invention is that it has a similar structure to the transfer mold. That is, the structure of the transfer mold has a similar shape above and below with the zero plane as the center in the height direction, and the transfer object made by the transfer mold also has a similar shape to the transfer mold. As a result, once the shape of the transfer mold is determined, the shape is the shape of the transfer object that is expected, making it easy to design the transfer object. In addition, normally, in order to create the same shape as the transfer mold, transfer must be repeated twice (that is, a transfer object to which the transfer mold is transferred is created, and this transfer object is then used as a transfer mold to create a further transfer object, otherwise the shape will not be the same as the initial transfer mold), but according to the transfer mold of the present invention, a shape similar to the transfer mold can be manufactured by a single transfer, which is advantageous in terms of cost and probability of defect occurrence.
[0109] The above RSm, Sa, and θa of the transfer object of the present invention are preferably in the range of −50 to 50% of the corresponding characteristic values of the transfer mold, more preferably in the range of −30 to 30%, further preferably in the range of −20 to 20%, and particularly preferably in the range of −10 to 10%. If they are within the range, the transfer object described above can be easily designed, and a desired shape can be obtained without performing two transfers.
[0110] Furthermore, in terms of the difference between the transfer target and the transfer mold for each characteristic, the absolute value of the difference is preferably 25 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, particularly preferably 10 μm or less, and most preferably 5 μm or less, for RSm, preferably 5 μm or less, more preferably 3 μm or less, even more preferably 2 μm or less, particularly preferably 1 μm or less, and most preferably 0.5 μm or less, and for θa, preferably 5° or less, more preferably 3° or less, even more preferably 2° or less, and particularly preferably 1° or less. If it is within this range, the transfer target can be easily designed, and the desired shape can be obtained without transferring twice.
[0111] (Haze of the transferred object, 60° gloss, 20° gloss) The haze of the transferred object (for example, when it is formed of a cured film, the haze of the cured film), 60° gloss, and 20° gloss are also preferably in the same ranges as those of the transfer mold. At 60° gloss, it is preferably in the range of -50 to 50% of the same characteristic of the transfer mold, more preferably in the range of -30 to 30%, even more preferably in the range of -20 to 20%, particularly preferably in the range of -10% to 10%, and most preferably in the range of -5% to 5%. If it is within this range, it becomes easy to design the transfer target as described above.
[0112] Furthermore, in terms of the difference between the transfer target and the transfer mold in each characteristic, the absolute value of the difference is preferably 20 or less, more preferably 10 or less, even more preferably 5 or less, particularly preferably 4 or less, and most preferably 1 or less, for 60° gloss, and is preferably 10 or less, more preferably 5 or less, even more preferably 3 or less, and particularly preferably 1 or less, for 20° gloss. If it is within this range, it becomes easy to design the transfer target as described above.
[0113] (Total light transmittance of the transfer target) The total light transmittance of the transfer target is not particularly limited, but is preferably high when used in an optical film for a display, such as an anti-glare film, etc. The total light transmittance including the substrate is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, particularly preferably 80% or more, and most preferably 90% or more, and the higher the better (the upper limit is 100%).
[0114] (Pencil hardness of the transfer target) The hardness of the transfer target is not particularly limited. For example, in the case of an adhesive, it is preferable that the performance of the adhesive is not reduced. On the other hand, when used for optical purposes such as displays, such as anti-glare and blocking prevention, a higher hardness may be preferable. When used for applications where a higher hardness is preferable, the pencil hardness is F or more, more preferably H or more, even more preferably 2H or more, and particularly preferably 3H or more. When the hardness is within the above range, it is excellent in abrasion resistance, excellent in preventing scratches on the transfer target, and can be made with few defects.
[0115] In particular, the transfer object is created by transferring the shape from the transfer mold, so there are fewer restrictions on the transfer material. Therefore, it is possible to design it to have a higher hardness than the transfer mold, and the transfer object made by the method of the present invention is suitable when a higher hardness is required, such as for optical applications.
[0116] (Curable composition for transfer object) An example of the transfer target of the present invention is a cured film, and may be a cured product of a curable composition containing an active energy ray-curable compound.
[0117] The transfer material of the present invention has excellent matte properties and is therefore suitable for use as an anti-glare film.
[0118] As long as the transfer target has the above structure, there is no particular restriction on the material of the transfer target. Examples of the transfer target include a method in which a cured material is brought into contact with a transfer mold in an uncured state (fluid state) and then cured to create a transfer target, and a method in which a transfer mold is pressed against a transfer target material (e.g., an adhesive) to create a transfer target. Among these methods, in consideration of the durability and stability of the transfer target, as well as ease of manufacture, it is preferable that the transfer target be formed from a curable compound (i.e., a cured film). Specifically, a method in which a coating film of a curable composition is formed and the coating film is cured can be exemplified.
[0119] As the curable compound, a conventionally known compound such as active energy ray curable or heat curable can be used. Among these, in consideration of ease of production, repeated use of the transfer mold, durability of the transferred object, etc., active energy ray curable compounds are preferred, and ultraviolet ray curable compounds are more preferred.
[0120] As the active energy ray curable compound, (meth)acrylates that can be used in a transfer mold are also suitable materials for the transfer target. For applications requiring high hardness, it is preferable to use trifunctional or higher polyfunctional (meth)acrylates among (meth)acrylates, and more preferably hexafunctional or higher (meth)acrylates. For example, dipentaerythritol hexa(meth)acrylate, pentaerythritol tetra(meth)acrylate, and trifunctional or higher urethane (meth)acrylates are preferred, and dipentaerythritol hexa(meth)acrylate and hexafunctional or higher urethane (meth)acrylates are particularly preferred.
[0121] In addition, it is also possible to use active energy ray-curable compounds other than (meth)acrylates in the curable composition, such as vinyl compounds, such as styrene, vinyl halides, and vinyl acetate, and diene compounds, such as vinylidene halides, 1,3-butadiene, isoprene, and chloroprene.
[0122] When an active energy ray curable compound is used in forming the transfer target, the content of the compound derived from the active energy ray curable compound in the layer forming the uneven structure of the transfer target is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, particularly preferably 50% by mass or more, and most preferably 60% by mass or more. There is no particular upper limit and it may be 100% by mass, but it is preferably 99% by mass or less, more preferably 98% by mass or less. In the above range, a transfer target (cured film) with excellent hardness can be formed. In particular, in applications requiring improved hardness and scratch resistance of the transferred object, it is preferable for the content of trifunctional or higher polyfunctional (meth)acrylate to be high, and the content of compounds derived from trifunctional or higher polyfunctional (meth)acrylate is preferably 5 mass% or more, more preferably 20 mass% or more, even more preferably 30 mass% or more, and particularly preferably 40 mass% or more, with the upper limit being in the range of 100 mass%. In applications where hardness is more important, it is preferable to use a hexa- or higher functional (meth)acrylate. In that case, the content of the compound derived from the hexa- or higher functional (meth)acrylate is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more, with the upper limit being in the range of 100% by mass.
[0123] In forming the transfer object, it is also possible to use various resins, particles, antistatic agents, antifouling agents, photopolymerization initiators, leveling agents, organic solvents, etc., in the same manner as in forming the transfer mold.
[0124] (Method of manufacturing the transferred object) Regarding the method for forming the transfer target, in the case of forming the transfer target by a cured film, the transfer target can be formed by applying the curable composition onto the surface of a substrate or an article to form a coating film, drying it as necessary, and then curing the coating film. The coating method is not particularly limited, and the coating can be applied by a known method such as dip coating, air knife coating, curtain coating, spin coating, roller coating, bar coating, wire bar coating, gravure coating, spray coating, etc.
[0125] When the curable composition contains an organic solvent, it is preferable to previously heat-dry the composition, which makes it possible to effectively remove the solvent in the coating film. The drying temperature for the heat drying is preferably from 30° C. to 200° C., more preferably from 40° C. to 150° C. The drying time is preferably from 0.01 to 30 minutes, more preferably from 0.1 to 10 minutes.
[0126] In forming a transfer target using an active energy ray-curable compound, the transfer target is formed as a cured film by irradiating with active energy rays to cure the compound. As the active energy rays, active energy rays other than vacuum ultraviolet rays are preferable in order to cure the compound to a deep portion, and examples of the active energy rays include ultraviolet rays and electron beams. Among these, ultraviolet rays are more preferable in consideration of the curability of the cured film.
[0127] The cumulative amount of ultraviolet light to be irradiated is preferably 1 to 5000 mJ / cm 2 , more preferably 50 to 3000 mJ / cm 2 , and more preferably 100 to 1000 mJ / cm 2 , particularly preferably 200 to 700 mJ / cm 2 The illuminance is preferably in the range of 1 to 1000 mW / cm 2 , more preferably 50 to 500 mW / cm 2 , and more preferably 80 to 300 mW / cm 2 The range is.
[0128] [Layers other than the concave-convex layer of the transfer mold] The transfer mold of the present invention may have a substrate layer in addition to a layer (concave-convex layer) having a concave-convex structure that forms a transfer surface. The transfer mold may also have one or more layers selected from the group consisting of a primer layer provided between the concave-convex layer and the substrate layer, and a back functional layer provided on the surface of the substrate layer opposite to the concave-convex layer side. In addition, the transfer mold may have a surface functional layer provided on the surface of the concave-convex layer opposite to the substrate layer side, as long as it does not impair the effects of the present invention.
[0129] (Transfer mold base layer) The substrate layer may be a known one, for example a resin substrate, a metal substrate, or a paper substrate. Among these, the resin substrate is preferred from the viewpoint of processability. The resin substrate may be a single layer or a multi-layer structure of two or more layers, and is not particularly limited. It is preferable that the resin substrate is a multi-layer structure of two or more layers, each layer having its own characteristics, and multi-functionality is achieved.
[0130] As the resin substrate, various resin films (sheets) can be used, such as polyester film, poly(meth)acrylate film, polyolefin film, polycarbonate film, polyimide film, triacetyl cellulose film, polystyrene film, polyvinyl chloride film, polyvinyl alcohol film, nylon film, etc. When the laminate is used for display applications, polyester films, poly(meth)acrylate films, polyolefin films, polycarbonate films, polyimide films, and triacetyl cellulose films are preferred. Among these, polyester films, poly(meth)acrylate films, and polyolefin films are preferred for anti-glare applications, and polyester films are more preferred in terms of transparency, moldability, and versatility. The polyester film may be a non-stretched film or a stretched film, and a stretched film is preferable. Among them, a uniaxially stretched film stretched in one direction or a biaxially stretched film stretched in two directions is preferable, and a biaxially stretched film is more preferable from the viewpoint of excellent balance of mechanical properties and flatness.
[0131] The polyester constituting the polyester film that can be used as the base layer may be either a homopolyester or a copolymer polyester. The homopolyester is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. The aromatic dicarboxylic acid and the aliphatic glycol may each be used alone or in combination of two or more. Examples of the dicarboxylic acid component of the copolymer polyester include isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, and oxycarboxylic acid. Examples of the glycol component include ethylene glycol, diethylene glycol, propylene glycol, butanediol, 4-cyclohexanedimethanol, and neopentyl glycol. The dicarboxylic acid component and the glycol component may each be used alone or in combination of two or more. Representative examples of polyester include polyethylene terephthalate and polyethylene naphthalate.
[0132] As the polyester film, from among the above, films formed from polyethylene terephthalate and polyethylene naphthalate are more preferable in consideration of mechanical strength and heat resistance, and from the viewpoint of ease of production and handleability for applications such as a surface protection film, a film formed from polyethylene terephthalate is more preferable.
[0133] The poly(meth)acrylate constituting the poly(meth)acrylate film that can be used as the base layer may be any one having a unit based on (meth)acrylate, and various acrylic resins can be used. Examples of the (meth)acrylate include alkyl (meth)acrylates having an alkyl group with 1 to 4 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and alkyl (meth)acrylates having an alkyl group with a larger number of carbon atoms. In consideration of transparency, processability, and chemical resistance, the poly(meth)acrylate preferably contains as a main component a unit based on an alkyl(meth)acrylate having 1 to 4 carbon atoms, more preferably contains as a main component at least one selected from the group consisting of units based on methyl(meth)acrylate and units based on ethyl(meth)acrylate, and particularly preferably contains as a main component a unit based on methyl(meth)acrylate. It is also possible to impart properties such as flexibility to the poly(meth)acrylate by incorporating units based on (meth)acrylates other than alkyl (meth)acrylates or units based on other monomers. The proportion of units based on alkyl (meth)acrylate having 1 to 4 carbon atoms relative to the total mass of the poly(meth)acrylate is preferably 50% by mass or more, and more preferably 80% by mass or more.
[0134] The base layer may contain particles for the purposes of imparting easy slippage, preventing scratches during each process, and improving blocking resistance. The type of particles can be appropriately selected according to the purpose, and is not particularly limited. Specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. Furthermore, when the base layer includes a polyester film, precipitated particles obtained by precipitating a part of a metal compound such as a catalyst during the polyester manufacturing process can also be used. Among these, silica particles and calcium carbonate particles are preferred because they are particularly effective in small amounts. The shape of the particles is not particularly limited, and any of spherical, block, rod-like, flat, etc. is acceptable. There are also no particular limitations on the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination, if necessary.
[0135] The average particle size of the particles is preferably 10 μm or less, more preferably 0.01 to 5 μm, and further preferably 0.01 to 3 μm. If the average particle size is 10 μm or less, problems due to a decrease in the transparency of the base layer are unlikely to occur. The average particle size of the particles is the cumulative 50% (mass basis) value in the equivalent sphericity distribution measured by a centrifugal sedimentation type particle size distribution measuring device.
[0136] When the base layer contains particles, the content of the particles in the base layer cannot be generally determined because it depends on the average particle size of the particles, but is preferably 5% by mass or less, more preferably in the range of 0.0003 to 3% by mass, and even more preferably in the range of 0.0005 to 1% by mass, based on the total mass of the layer containing the particles in the base layer. If the content of the particles is 5% by mass or less, defects such as particle dropout and reduced transparency of the base layer are unlikely to occur.
[0137] The base layer may contain additives other than the above-mentioned particles as necessary, such as known additives such as ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, and pigments.
[0138] The thickness of the substrate layer is not particularly limited as long as it is within a range that allows film formation, but is preferably in the range of 2 to 350 μm, more preferably 5 to 250 μm, and further preferably 10 to 100 μm.
[0139] (Transfer-type primer layer) The primer layer is provided between the base layer and the irregularity layer in order to impart various functions. Examples of the primer layer include an adhesion improving layer and an antistatic layer. The primer layer may have multiple functions.
[0140] In a preferred embodiment, the primer layer is an adhesion improving layer. If the adhesion between the base layer and the uneven layer is insufficient, the laminate may not be usable depending on the application. By having the adhesion improving layer, the adhesion between the base layer and the uneven layer is improved, and the uneven layer is less likely to peel off from the base layer during the transfer process. When the primer layer is an adhesion improving layer, the primer layer preferably contains either one or both of a resin and a compound derived from a crosslinking agent from the viewpoint of improving adhesion between the base layer and the uneven layer.
[0141] In another preferred embodiment, the primer layer is an antistatic layer. If the primer layer is an antistatic layer, adhesion of dust and the like due to peeling electrification or frictional electrification to the outermost surface of the laminate, particularly the outermost surface on the side where the uneven layer is present relative to the base layer, can be reduced. This can reduce defects due to foreign matter contamination during the transfer process. In order to make the primer layer an antistatic layer, for example, an antistatic agent may be contained in the primer layer.
[0142] As the resin, a conventionally known resin can be used. Specific examples of the resin include polyester resin, acrylic resin, urethane resin, polyvinyl resin (polyvinyl alcohol, vinyl chloride-vinyl acetate copolymer, etc.), etc. Among them, polyester resin, acrylic resin, and urethane resin are preferred in consideration of adhesion performance and coating property. When the substrate layer is a resin film, the resin of the substrate layer is preferably the same type of resin as the resin of the resin film from the viewpoint of the affinity between the primer layer and the substrate layer.For example, when the substrate layer is a polyester film, the primer layer preferably contains a polyester resin.When the substrate layer is a poly(meth)acrylate film, the primer layer preferably contains an acrylic resin.
[0143] The polyester resin may be one whose main components are a polyvalent carboxylic acid and a polyvalent hydroxy compound. Examples of polyvalent carboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, trimellitic acid monopotassium salt, and ester-forming derivatives thereof. Examples of polyhydric hydroxy compounds include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of these compounds may be appropriately selected and subjected to a conventional polycondensation reaction to synthesize a polyester resin.
[0144] The acrylic resin is a polymer of polymerizable monomers including a (meth)acrylic monomer. Examples of the acrylic resin include homopolymers and copolymers of (meth)acrylic monomers, and copolymers of (meth)acrylic monomers and polymerizable monomers other than (meth)acrylic monomers. The acrylic resin may be a copolymer of such a polymer with another polymer (e.g., polyester, polyurethane, etc.). Such a copolymer is, for example, a block copolymer or a graft copolymer. Alternatively, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of a polyester. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of a polyurethane. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a solution or dispersion of another polymer.
[0145] The polymerizable monomer is not particularly limited, but particularly representative compounds include, for example, carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethyl Examples of suitable monomers include alkyl (meth)acrylates such as dihexyl (meth)acrylate and lauryl (meth)acrylate; nitrogen-containing monomers such as (meth)acrylamide, diacetone acrylamide, N-methylol acrylamide and (meth)acrylonitrile; styrene-based compounds such as styrene, α-methylstyrene, divinylbenzene and vinyl toluene, vinyl esters such as vinyl propionate and vinyl acetate; silicon-containing monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; vinyl halides such as vinyl chloride and vinylidene chloride; and conjugated dienes such as butadiene.
[0146] The urethane resin is a polymeric compound having a urethane bond in the molecule, and is typically synthesized by reacting a polyol with a polyisocyanate compound. A chain extender may be used when synthesizing the urethane resin. Examples of polyols used to obtain the urethane resin include polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, etc. These compounds may be used alone or in combination of two or more.
[0147] Polycarbonate polyol is obtained by the reaction (dealcoholization reaction) of polyhydric alcohol with carbonate compound. Examples of polyhydric alcohol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, etc. Examples of carbonate compounds include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, etc. Specific examples of polycarbonate polyols include poly(1,6-hexylene) carbonate, poly(3-methyl-1,5-pentylene) carbonate, and the like.
[0148] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene ether glycol, and polyhexamethylene ether glycol.
[0149] Examples of polyester polyols include those obtained by reacting a polyvalent carboxylic acid or an acid anhydride thereof with a polyhydric alcohol, and those having a derivative unit of a lactone compound such as polycaprolactone. Examples of the polyvalent carboxylic acid include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, fumaric acid, maleic acid, terephthalic acid, and isophthalic acid. Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2-methyl-2-propyl-1,3-propanediol, 1 ,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-2-hexyl-1,3-propanediol, cyclohexanediol, bishydroxymethylcyclohexane, dimethanolbenzene, bishydroxyethoxybenzene, alkyldialkanolamines, lactonediols, and the like.
[0150] As the polyol, in consideration of adhesion performance, polyester polyol and polycarbonate polyol are preferred, and polyester polyol is particularly preferred.
[0151] Examples of polyisocyanate compounds used to obtain urethane resins include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate; aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate; aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate. These may be used alone or in combination of two or more.
[0152] There are no particular limitations on the chain extender as long as it has two or more active groups that react with an isocyanate group, and generally, a chain extender having two hydroxyl groups or two amino groups can be mainly used. Examples of chain extenders having two hydroxyl groups include glycol compounds such as aliphatic glycols such as ethylene glycol, propylene glycol, and butanediol; aromatic glycols such as xylylene glycol and bishydroxyethoxybenzene; and ester glycols such as neopentyl glycol hydroxypivalate. Examples of chain extenders having two amino groups include aromatic diamines such as tolylenediamine, xylylenediamine, and diphenylmethanediamine; aliphatic diamines such as ethylenediamine, propylenediamine, hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, trimethylhexanediamine, 2-butyl-2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, dicyclohexylmethanediamine, isopropylidincyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, and 1,3-bisaminomethylcyclohexane.
[0153] The urethane resin is typically used in the form of a dispersion or solution. The medium for the dispersion or solution may be a solvent, but is preferably water. The aqueous dispersion or solution of the urethane resin may be a forced emulsification type using an emulsifier, a self-emulsification type in which a hydrophilic group is introduced into the structure of the urethane resin, or a water-soluble type, etc. In particular, a self-emulsification type in which an ionic group is introduced into the structure of the urethane resin to form an ionomer is preferred, since it has excellent storage stability of the liquid and excellent water resistance and transparency of the resulting primer layer.
[0154] Examples of the ionic group to be introduced into the structure of the urethane resin include a carboxyl group, a sulfonic acid group, a phosphoric acid group, a phosphonic acid group, a quaternary ammonium salt group, and the like, with the carboxyl group being preferred. The carboxyl group is preferably in the form of a salt neutralized with a neutralizing agent such as ammonia, amine, alkali metals, inorganic alkalis, etc. Particularly preferred neutralizing agents are ammonia, trimethylamine, and triethylamine. In the urethane resin having a carboxyl group neutralized with a neutralizing agent, the carboxyl group from which the neutralizing agent is removed in the drying process after application can be used as a crosslinking reaction point with a crosslinking agent. This not only provides excellent stability in the liquid state before coating, but also makes it possible to further improve the durability, solvent resistance, water resistance, blocking resistance, etc. of the obtained primer layer.
[0155] Various methods can be used to introduce carboxyl groups into urethane resins at each stage of polymerization reaction. For example, there is a method of using a resin having a carboxyl group as a copolymerization component during prepolymer synthesis, or a method of using a component having a carboxyl group as one component of polyol, polyisocyanate compound, chain extender, etc. In particular, a method of using a carboxyl group-containing diol and introducing a desired amount of carboxyl groups by the amount of this component is preferred. For example, a carboxyl group-containing diol can be copolymerized with the diol used in synthesizing the urethane resin. Examples of the carboxyl group-containing diol include dimethylolpropionic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, bis-(2-hydroxyethyl)butanoic acid, and salts of these acids in which the carboxyl group has been neutralized with a neutralizing agent.
[0156] The primer layer preferably contains a compound derived from a crosslinking agent in order to make the primer layer stronger and improve performance such as adhesion. As the crosslinking agent, a known material can be used, for example, a melamine compound, an oxazoline compound, an isocyanate compound, an epoxy compound, a carbodiimide compound, a silane coupling compound, a hydrazide compound, an aziridine compound, etc. are listed. Among them, a melamine compound, an isocyanate compound, an epoxy compound, an oxazoline compound, a carbodiimide compound, and a silane coupling compound are preferred, and from the viewpoint of further improving adhesion and durability, a melamine compound, an oxazoline compound, an isocyanate compound, and an epoxy compound are more preferred, and a melamine compound, an oxazoline compound, and an isocyanate compound are particularly preferred. These crosslinking agents may be used alone or in combination of two or more. By using two or more types in combination, adhesion and durability may be further improved and become good.
[0157] The melamine compound is a compound having a melamine skeleton in the compound, and examples thereof include alkylolated melamine derivatives, compounds obtained by reacting an alkylolated melamine derivative with an alcohol to partially or completely etherify the same, and mixtures thereof. Examples of alcohols used for etherification include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, isobutanol, and the like. The melamine compound may be either a monomer or a dimer or higher polymer, or a mixture thereof. Furthermore, a product obtained by co-condensing a part of melamine with urea or the like may be used, and a catalyst may be used to increase the reactivity of the melamine compound. As the melamine compound, those having a hydroxyl group are preferred in consideration of reactivity with various compounds.
[0158] The isocyanate compound refers to a compound having an isocyanate derivative structure, such as an isocyanate compound or a blocked isocyanate compound. Examples of the isocyanate compound include aromatic isocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate; aliphatic isocyanate compounds having an aromatic ring such as α,α,α',α'-tetramethylxylylene diisocyanate; aliphatic isocyanate compounds such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic isocyanate compounds such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isopropylidenedicyclohexyl diisocyanate. In addition, polymers and derivatives such as biuretized products, isocyanurate products, uretdione products, and carbodiimide modified products of these isocyanate compounds are also included. These may be used alone or in combination of two or more. Among the above isocyanate compounds, from the viewpoint of avoiding yellowing due to ultraviolet rays, aliphatic isocyanate compounds or alicyclic isocyanate compounds are more preferable than aromatic isocyanate compounds.
[0159] Examples of the blocked isocyanate compound include compounds in which the isocyanate group of the isocyanate compound is blocked with a blocking agent. Examples of the blocking agent include bisulfites, phenolic compounds such as phenol, cresol, and ethylphenol, alcoholic compounds such as propylene glycol monomethyl ether, ethylene glycol, benzyl alcohol, methanol, and ethanol, active methylene compounds such as dimethyl malonate, diethyl malonate, methyl isobutanoyl acetate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone, mercaptan compounds such as butyl mercaptan and dodecyl mercaptan, lactam compounds such as ε-caprolactam and δ-valerolactam, amine compounds such as diphenylaniline, aniline, and ethyleneimine, acid amide compounds such as acetanilide and acetic acid amide, and oxime compounds such as formaldehyde, acetaldoxime, acetoneoxime, methyl ethyl ketoneoxime, and cyclohexanoneoxime. These may be used alone or in combination of two or more. As the blocked isocyanate compound, an isocyanate compound blocked with an active methylene compound is preferred from the viewpoint that the primer layer is less likely to be destroyed.
[0160] The isocyanate compound may be used alone or as a mixture or bond with various polymers. In terms of improving the dispersibility and crosslinking property of the isocyanate compound, it is preferable to use a mixture or bond with a polyester resin or a urethane resin.
[0161] The oxazoline compound is a compound having an oxazoline group in the molecule. The oxazoline compound is preferably a polymer containing an oxazoline group. The polymer containing an oxazoline group can be obtained by polymerization of an addition-polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition-polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. These may be used alone or in combination of two or more. Among these, 2-isopropenyl-2-oxazoline is suitable because it is easily available industrially. The other monomer is not particularly limited as long as it is a monomer that can be copolymerized with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylates such as alkyl (meth)acrylates (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, tertiary amine salts, and the like); unsaturated nitriles such as acrylonitrile and methacrylonitrile; (meth)acrylonitrile; Examples of such unsaturated amides include unsaturated amides such as N-alkyl(meth)acrylamides, N,N-dialkyl(meth)acrylamides (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. These may be used alone or in combination of two or more.
[0162] The amount of oxazoline groups per 1 g of the oxazoline compound is preferably in the range of 0.5 to 10 mmol / g, more preferably 1 to 9 mmol / g, further preferably 3 to 8 mmol / g, and particularly preferably 4 to 6 mmol / g. If the amount of oxazoline groups is within the above range, the durability of the coating film is improved and the adhesion can be easily adjusted.
[0163] An epoxy compound is a compound having an epoxy group in the molecule. Examples of epoxy compounds include condensates of epichlorohydrin and compounds having a hydroxyl group or an amino group (ethylene glycol, polyethylene glycol, glycerin, polyglycerin, bisphenol A, etc.), and include polyepoxy compounds, diepoxy compounds, monoepoxy compounds, and glycidylamine compounds. Examples of polyepoxy compounds include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether. Examples of diepoxy compounds include neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polytetramethylene glycol diglycidyl ether. Examples of the monoepoxy compound include allyl glycidyl ether, 2-ethylhexyl glycidyl ether, and phenyl glycidyl ether. Examples of the glycidylamine compound include N,N,N',N'-tetraglycidyl-m-xylylenediamine and 1,3-bis(N,N-diglycidylamino)cyclohexane.
[0164] A carbodiimide compound is a compound having one or more carbodiimide structures or carbodiimide derivative structures in the molecule. As the carbodiimide-based compound, in order to obtain better strength of the primer layer, etc., a polycarbodiimide-based compound having two or more carbodiimide structures or carbodiimide derivative structures in the molecule is more preferable.
[0165] Carbodiimide compounds can be synthesized by known techniques, and generally, condensation reaction of diisocyanate compounds is used. The diisocyanate compounds are not particularly limited, and both aromatic and aliphatic compounds can be used, and specific examples include tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexyl diisocyanate, dicyclohexylmethane diisocyanate, etc.
[0166] In order to improve the water solubility or water dispersibility of the polycarbodiimide compound, a surfactant may be added, or a hydrophilic monomer such as a polyalkylene oxide, a quaternary ammonium salt of a dialkylamino alcohol, or a hydroxyalkylsulfonate may be added, within a range that does not impair the effects of the present invention.
[0167] A silane coupling compound is an organosilicon compound that has an organic functional group and a hydrolyzable group such as an alkoxy group in one molecule. Examples of the silane coupling compound include epoxy group-containing compounds such as 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; vinyl group-containing compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; styryl group-containing compounds such as p-styryltrimethoxysilane and p-styryltriethoxysilane; (meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; (meth)acryloyl group-containing compounds such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2- Examples of such compounds include amino group-containing compounds such as (aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltriethoxysilane; isocyanurate group-containing compounds such as tris(trimethoxysilylpropyl)isocyanurate and tris(triethoxysilylpropyl)isocyanurate; and mercapto group-containing compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropylmethyldiethoxysilane.
[0168] As the silane coupling compound, among the above compounds, from the viewpoint of the strength of the primer layer, epoxy group-containing silane coupling compounds, double bond-containing silane coupling compounds such as vinyl groups and (meth)acrylic groups, and amino group-containing silane coupling compounds are more preferred.
[0169] These crosslinking agents react during the drying process and film-forming process to improve the performance of the primer layer. It is assumed that the crosslinking agent-derived compounds present in the formed primer layer include unreacted crosslinking agents, reacted compounds, or mixtures thereof.
[0170] The antistatic agent contained in the primer layer is not particularly limited, and any known antistatic agent can be used. Examples of the antistatic agent include compounds having an ammonium group, polyether compounds, compounds having a sulfonic acid group, betaine compounds, and conductive organic polymers.
[0171] The primer layer may contain particles to improve blocking and slip properties. The primer layer may contain additives such as antifoaming agents, coatability improvers, thickeners, organic lubricants, ultraviolet absorbers, antioxidants, foaming agents, dyes, and pigments, as necessary, within the scope of the present invention.
[0172] The proportion of the resin in 100% by mass of the primer layer is, for example, 5% by mass or more, preferably 10 to 99% by mass, more preferably 20 to 95% by mass, and even more preferably 30 to 90% by mass. If the proportion of the resin is within the above range, the adhesion performance and the appearance of the primer layer are more excellent.
[0173] The proportion of the compound derived from the crosslinking agent in 100% by mass of the primer layer is, for example, 80% by mass or less, preferably 0.5 to 65% by mass, more preferably 3 to 50% by mass, and further preferably 5 to 40% by mass. If the proportion of the compound derived from the crosslinking agent is within the above range, the adhesion performance and strength of the primer layer are more excellent.
[0174] The thickness of the primer layer depends on the material used in the primer layer and the performance to be achieved, so cannot be generalized, but is preferably in the range of 0.001 to 10 μm, more preferably 0.01 to 4 μm, and even more preferably 0.02 to 1 μm. The primer layer can be formed by a known method.
[0175] (Transfer-type surface functional layer) The surface functional layer of the transfer mold can be provided in order to impart various functions to the surface of the transfer mold (on the surface opposite to the base layer side of the uneven layer). Examples of the surface functional layer of the transfer mold include a release layer and an antistatic layer.
[0176] The release layer is provided to improve transferability. As the material used for the release layer, conventionally known materials such as silicone compounds, fluorine compounds, and compounds containing long-chain alkyl groups can be used. Among these, silicone compounds and fluorine compounds are preferred for exhibiting stronger release performance, and fluorine compounds and compounds containing long-chain alkyl groups are preferred from the viewpoint of not contaminating the transferred object.
[0177] Silicone compounds are compounds having a silicone structure in the molecule, and examples thereof include alkyl silicones such as dimethyl silicone and diethyl silicone, and phenyl silicone and methylphenyl silicone having a phenyl group. Silicones having various functional groups can also be used, and examples thereof include ether groups, hydroxyl groups, amino groups, epoxy groups, carboxylic acid groups, halogen groups such as fluorine, perfluoroalkyl groups, various alkyl groups, and various aromatic groups, and other hydrocarbon groups. As other functional groups, silicones having vinyl groups and hydrogen silicones in which hydrogen atoms are directly bonded to silicon atoms are also common, and it is also possible to use both in combination as addition type silicones (types obtained by the addition reaction of vinyl groups and hydrogen silane). In addition, a method of introducing a double bond such as an acryloyl group and reacting at the double bond is also preferred.
[0178] In addition, as the silicone compound, modified silicones such as acrylic grafted silicone, silicone grafted acrylic, amino modified silicone, perfluoroalkyl modified silicone, etc. are also usable. In consideration of heat resistance and contamination, it is preferable to use a curable silicone resin, and as the type of curable type, any curing reaction type such as condensation type, addition type, active energy ray curable type, etc. can be used.
[0179] The fluorine compound is a compound containing fluorine atoms in the compound.As the fluorine compound, an organic fluorine compound is preferably used, for example, a perfluoroalkyl group-containing compound, a polymer of an olefin compound containing a fluorine atom, an aromatic fluorine compound such as fluorobenzene, etc. are listed.From the viewpoint of mold releasability, it is preferable to use a compound having a perfluoroalkyl group.Furthermore, the fluorine compound can also be a compound containing a long chain alkyl compound as described later.
[0180] Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof, and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and staining resistance, it is preferable to use a polymer. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of stain resistance, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. It may also be a polymer with a compound containing a long-chain alkyl compound as described below.
[0181] The long-chain alkyl group-containing compound is a compound having a straight-chain or branched alkyl group having a carbon number of usually 6 or more, preferably 8 or more, and more preferably 12 or more. Examples of the alkyl group include a hexyl group, an octyl group, a decyl group, a lauryl group, an octadecyl group, and a behenyl group. Examples of the compound having an alkyl group include various long-chain alkyl group-containing polymer compounds, long-chain alkyl group-containing amine compounds, long-chain alkyl group-containing ether compounds, and long-chain alkyl group-containing quaternary ammonium salts. Considering heat resistance and stain resistance, a polymer compound is preferable. In addition, from the viewpoint of effectively obtaining antifouling properties, a polymer compound having a long-chain alkyl group in the side chain is more preferable.
[0182] The polymer compound having a long-chain alkyl group in the side chain can be obtained by reacting a polymer having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxyl group, acid anhydride, etc. Examples of the compound having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, reactive group-containing poly(meth)acrylic resin, etc. Among these, polyvinyl alcohol is preferable in consideration of antifouling properties and ease of handling.
[0183] Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, behenyl isocyanate, etc., long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, behenyl chloride, etc., long-chain alkyl group-containing amines, long-chain alkyl group-containing alcohols, etc. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.
[0184] Furthermore, polymeric compounds having a long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of long-chain alkyl (meth)acrylate include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.
[0185] The content of the release agent in the surface functional layer to achieve the above-mentioned release performance depends on the material used and cannot be generally stated, but in the case of silicone compounds and fluorine compounds, it is usually 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more, and the upper limit may be 100% by mass. In addition, in the case of using a compound containing a long chain alkyl group, it is usually 0.1% by mass or more, preferably 1% by mass or more, and even more preferably 3% by mass or more, and the upper limit may be 100% by mass. By using it in the above range, effective release performance can be obtained.
[0186] As the antistatic agent used when forming an antistatic layer as a surface functional layer for preventing dust adhesion, various conventionally known antistatic agents can be used.
[0187] The thickness of the surface functional layer of the transfer mold is preferably 5 times or less the height from the recesses to the protrusions formed by the uneven layer. This is because if the thickness is 5 times or more the height of the unevenness, the matte performance due to the unevenness is reduced. The thickness of the surface functional layer depends on the height of the unevenness and cannot be generally stated, but is usually in the range of 0.001 to 3 μm, preferably 0.005 to 2 μm, more preferably 0.01 to 1 μm, even more preferably 0.02 to 0.5 μm, and particularly preferably 0.03 to 0.2 μm. By using within the above range, it is possible to achieve both the expression of the function of the surface functional layer and the matte performance due to the unevenness of the uneven layer. The surface functional layer can be formed by a known method.
[0188] (Transfer-type back functional layer) The back functional layer of the transfer mold can be provided in order to impart various functions to the surface of the transfer mold opposite to the transfer side (the surface opposite to the concave-convex layer side of the base layer). Examples of the back surface functional layer include an adhesive layer, an antistatic layer, and an antiblocking layer.
[0189] The thickness of the transferable back functional layer depends on the material used for the back functional layer and the performance to be exhibited, so it cannot be generally stated, but is, for example, 0.001 to 30 μm. When the back functional layer is an adhesive layer, it is preferably 0.01 to 30 μm, more preferably 0.1 to 20 μm. When the back functional layer is an antistatic layer, it is preferably 0.001 to 10 μm, more preferably 0.01 to 5 μm. The back surface functional layer can be formed by a known method.
[0190] [Layers other than the uneven layer of the transfer target] The transfer target of the present invention may have a substrate layer in addition to the layer (concave-convex layer) having a concave-convex structure of the transfer target. The transfer target may have one or more layers selected from the group consisting of a primer layer provided between the concave-convex layer and the substrate layer, and a back functional layer provided on the surface of the substrate layer opposite to the concave-convex layer side. The transfer target may also have a surface functional layer provided on the surface of the concave-convex layer opposite to the substrate layer side, as long as it does not impair the effects of the present invention.
[0191] (Base layer of the transfer target) The substrate layer of the transfer object may be the same as the substrate layer of the transfer mold.
[0192] (Primer layer of transfer material) The primer layer of the transfer object can be the same as that of the transfer type. For example, an adhesion improving layer can provide sufficient adhesion between the base layer and the transfer object to prevent the transfer object from peeling off when used, and an antistatic layer can reduce dust adhering to the surface of the transfer object.
[0193] (Surface functional layer of the transfer target) The surface functional layer of the transfer target can be provided in order to impart various functions to the surface of the transfer target (on the side opposite to the base layer side of the uneven layer). Examples of the surface functional layer of the transfer target include an antifouling layer, an antistatic layer, a refractive index adjusting layer (antireflection layer, low reflection layer, etc.), an infrared absorbing layer, an ultraviolet absorbing layer, and a color correcting layer.
[0194] The antifouling layer is provided to improve the antifouling performance by imparting water repellency and oil repellency to the concave-convex layer. As the material used for the antifouling layer, conventionally known materials such as silicone compounds, fluorine compounds, and long-chain alkyl group-containing compounds can be used. Among these, silicone compounds and fluorine compounds are preferred for exhibiting stronger antifouling performance, and fluorine compounds and long-chain alkyl group-containing compounds are preferred from the viewpoint of not contaminating the other party with which the antifouling layer comes into contact. As for specific compounds, the same materials as those used for the release layer as the surface functional layer of the transfer mold can be mentioned.
[0195] As the antistatic agent used when forming an antistatic layer as a surface functional layer of the transfer target, various conventionally known antistatic agents can be used.
[0196] Examples of the refractive index adjusting layer include a high refractive index layer, a low refractive index layer, and a laminate thereof. When the purpose is to increase the refractive index, materials to be used when forming a refractive index adjusting layer as a surface functional layer of a transfer target may include, for example, aromatic-containing compounds such as benzene structure, bisphenol A structure, melamine structure, and fluorene structure, as well as condensed polycyclic aromatic compounds such as naphthalene, anthracene, phenanthrene, naphthacene, benzo[a]anthracene, benzo[a]phenanthrene, pyrene, benzo[c]phenanthrene, and perylene structures, which are considered to have high refractive indexes among aromatic compounds, metal oxides such as zirconium oxide, titanium oxide, zinc oxide, tin oxide, antimony oxide, yttrium oxide, indium oxide, cerium oxide, ATO (antimony tin oxide), and ITO (indium tin oxide), metal-containing compounds such as metal chelate compounds such as titanium chelate and zirconium chelate, compounds containing a sulfur element, and compounds containing a halogen element.
[0197] Metal oxides are preferably used in the form of particles since there is a concern that their adhesion may decrease depending on the form of use, and the average particle size thereof is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 25 nm or less, from the viewpoint of the appearance of the coating.
[0198] When forming a refractive index adjustment layer as a surface functional layer of a transfer target, a conventionally known material can be used if the objective is to reduce the refractive index, for example, acrylic resin or urethane resin is generally possible because of its low refractive index. In addition, compounds in which fluorine atoms are incorporated in the resin, such as fluororesins, compounds containing fluororesins in the main skeleton, and compounds containing perfluoroalkyl groups in the side chains, can be mentioned. In addition, examples of inorganic materials include hollow silica particles, fluorine atom-containing inorganic compounds such as magnesium fluoride and calcium fluoride, and hollow particles and nanoporous particles thereof.
[0199] The thickness of the surface functional layer of the transfer target is preferably 5 times or less the height from the concaves to the convexities formed by the uneven layer. This is because if the thickness is 5 times or more the height of the unevenness, the matte performance due to the unevenness is reduced. The thickness of the surface functional layer depends on the height of the unevenness and cannot be generalized, but is usually in the range of 0.001 to 3 μm, preferably 0.005 to 2 μm, more preferably 0.01 to 1 μm, even more preferably 0.02 to 0.5 μm, and particularly preferably 0.03 to 0.2 μm. By using within the above range, it is possible to achieve both the expression of the function of the surface functional layer and the matte performance due to the unevenness of the uneven layer. The surface functional layer can be formed by a known method.
[0200] (Back functional layer of the transfer target) The back functional layer of the transfer target can be provided on the surface of the base layer opposite to the concave-convex layer side (transfer target side) in order to impart various functions. Examples of the rear functional layer of the transfer target include an adhesive layer, an antistatic layer, a refractive index adjusting layer, and an antiblocking layer. The adhesive layer is provided to bond the laminate to various adherends. The antistatic layer is provided to prevent adhesion of surrounding dirt and the like due to peeling electrification or frictional electrification to the outermost surface of the laminate, particularly the outermost surface of the base layer opposite to the uneven layer side, and to prevent defects and the like caused thereby. The refractive index adjustment layer is provided, for example, to improve the total light transmittance of the laminate. The antiblocking layer is provided to reduce blocking of the laminate.
[0201] The adhesive layer may be formed using known adhesives, such as acrylic, polyester, urethane, rubber, etc. Of these, acrylic is preferred in view of versatility. The antistatic layer and the refractive index adjusting layer are similar to the antistatic layer and the refractive index adjusting layer as the surface functional layer, respectively.
[0202] The thickness of the back functional layer of the transfer target depends on the material used for the back functional layer and the performance to be achieved, so it cannot be generally stated, but is, for example, 0.001 to 30 μm. When the back functional layer is an adhesive layer, it is preferably 0.01 to 30 μm, more preferably 0.1 to 20 μm. When the back functional layer is an antistatic layer, it is preferably 0.001 to 10 μm, more preferably 0.01 to 5 μm. The back surface functional layer can be formed by a known method.
[0203] (Formation of surface functional layer and back functional layer) In both the transfer mold and the transferred object, with regard to the formation of the front surface functional layer and the back surface functional layer, it is preferable to produce a laminate in such a manner that the above-mentioned series of compounds are made into a solution or a dispersion in a solvent, and the liquid adjusted to a solid content concentration of approximately 0.1 to 80 mass % is coated onto a substrate.
[0204] Methods for forming the front surface functional layer and the back surface functional layer on both the transfer mold and the transferred object can be any conventional coating method, such as gravure coating, reverse roll coating, die coating, air doctor coating, blade coating, rod coating, bar coating, curtain coating, knife coating, transfer roll coating, squeeze coating, impregnation coating, kiss coating, spray coating, calendar coating, and extrusion coating.
[0205] In both the transfer mold and the transferee, the drying and curing conditions when forming the surface functional layer and the back functional layer on the substrate film are not particularly limited. In the case of the coating method, the drying temperature of the solvent such as water used in the coating liquid is usually 50 to 150°C, preferably 80 to 130°C, and more preferably 90 to 120°C. The drying time is generally 3 to 200 seconds, preferably 5 to 120 seconds. In addition, in order to improve the strength of the surface functional layer and the back functional layer, when the film is produced in the film production process, a heat treatment step is usually performed at a temperature of 150 to 270°C, preferably 170 to 230°C, and more preferably 180 to 210°C. The heat treatment time is generally 3 to 200 seconds, and preferably 5 to 120 seconds. EXAMPLES
[0206] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. The measurement and evaluation methods used in the present invention are as follows.
[0207] (1) Intrinsic viscosity of polyester 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (weight ratio), and measured at 30°C.
[0208] (2) Average primary particle diameter (d50:μm) The cumulative 50% value (by weight) in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device SA-CP3 manufactured by Shimadzu Corporation was taken as the average primary particle size.
[0209] (3) Weight average molecular weight of resin (Mw) The weight average molecular weight (Mw) of the resin was measured using a gel permeation chromatography (GPC) "HLC-8120" (manufactured by Tosoh Corporation). As the column, TSKgel G5000HXL*GMHXL-L (manufactured by Tosoh Corporation) was used. In addition, a calibration curve was created using F288 / F80 / F40 / F10 / F4 / F1 / A5000 / A1000 / A500 (manufactured by Tosoh Corporation) and styrene as standard polystyrene. The measurement was performed at a column oven temperature of 40°C using 100 μl of a solution in which the polymer was dissolved in tetrahydrofuran to a concentration of 0.4%. The weight average molecular weight (Mw) was calculated in terms of standard polystyrene.
[0210] (4) RSm, Sa and θa Using a surface profile measurement system (Hitachi High-Tech Science Corporation's scanning white light interference microscope "VS1330"), the surface profile of the cured film was measured by optical interference over an area of 236.9 μm x 177.6 μm, and the data was read after interpolation and baseline correction. The objective lens magnification during measurement was set to 20 times. The presence or absence of a wrinkled uneven structure was also confirmed in this evaluation. In addition, for the comparison of each physical property of the transfer mold and the transferred object, the percentage comparison was calculated by subtracting the physical property value of the transfer mold from the physical property value of the transferred object and dividing the result by the physical property value of the transfer mold. For the difference in each physical property, the absolute value of the value obtained by subtracting the physical property value of the transfer mold from the physical property value of the transferred object was calculated.
[0211] (5) Total light transmittance / haze The laminate in which the cured film was formed on the substrate was used as the measurement subject. The total light transmittance and haze were measured using a Nippon Denshoku Industries haze meter "SH7000" in accordance with JIS Z8722:2009 (geometric conditions of irradiation and reception of a transmitting object), JIS K7361-1:1997 (test method for total light transmittance of plastic transparent materials), and JIS K7136:2000 (method of determining haze of plastic transparent materials). Regarding haze, the haze of only the substrate was measured and subtracted from the measured haze of the laminate to evaluate the haze of only the concave-convex structure layer (cured film) due to the transfer mold or the transferred object.
[0212] (6) 20° and 60° gloss and matte The laminate having a cured film formed on a substrate was used as the measurement subject. The 20° and 60° gloss (20° and 60° specular gloss) was measured using a gloss meter "VG2000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS Z 8741-1997. The lower the gloss value, the better the matte property.
[0213] (7) Pencil hardness The pencil hardness of the cured film was measured according to JIS K5600-5-4:1999 General testing methods for paints - Part 5: Mechanical properties of coatings - Section 4: Scratch hardness (pencil method).
[0214] (8) Method for measuring surface resistance Using a high resistivity meter, Hiresta MCP-HP450, manufactured by Mitsubishi Chemical Analytech Co., Ltd., the surface resistivity was measured after the sample was conditioned for 30 minutes at an applied voltage of 100V, 23°C, and 50% RH. If the surface resistance value shows OVER, it means that the surface resistance value is too high to measure.
[0215] (9) Matte finish The laminate was placed in a room illuminated by a linear white fluorescent lamp, and the distance between the fluorescent lamp and the laminate was set at 2.5 m. The matte finish on the uneven layer side (reflection of the fluorescent lamp) was evaluated by visual inspection according to the following evaluation criteria A to D. Evaluations A to C are judgments that confirm the matte finish. A: The reflected image of the fluorescent light is very blurry and the outline of the fluorescent light cannot be seen. B: The reflected image of the fluorescent light is blurred, but you can faintly see its outline. C: The reflected image of the fluorescent light is slightly blurred, and although the outline can be seen, it appears wavy and appears dark white. D: The reflected image of the fluorescent light is clear, the contours can be clearly seen, and it appears linear and white.
[0216] (10) Magic stain-resistant (oil repellency and stain resistance) The uneven layer was written on with a Zebra Corp. oil-based black marker "Mackie Fine" and then visually observed and evaluated. The result was that the ink was repelled, indicating excellent oil repellency (stain resistance), and the ratings of A and B were judged to confirm stain resistance. A: The ink is being repelled. B: The ink is slightly repelled only at the edge of the writing. C: The ink is not repelled.
[0217] The materials used in the examples and comparative examples are as follows. (base material) Polyester (S1): Polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.63 dl / g obtained using magnesium acetate tetrahydrate and tetrabutyl titanate as polymerization catalysts. Polyester (S2): Polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.64 dl / g obtained using magnesium acetate tetrahydrate, orthophosphoric acid and germanium dioxide as polymerization catalysts. · Polyester (S3): Polyethylene terephthalate homopolymer containing 0.3 mass% silica particles with an average primary particle diameter of 2 μm.
[0218] (Production of acrylic resin (b1) having active energy ray-curable functional group) An acrylic resin (b1) having an active energy ray-curable functional group was prepared by the following method. In a flask equipped with a thermometer, a stirrer, and a reflux condenser, propylene glycol monomethyl ether (178 parts by mass), glycidyl methacrylate (20 parts by mass), methyl methacrylate (79 parts by mass), ethyl acrylate (1.0 part by mass), and 2,2'-azobis(2,4-dimethylvaleronitrile) (0.6 parts by mass) were added and reacted for 3 hours at 65°C. Then, 2,2'-azobis(2,4-dimethylvaleronitrile) (0.3 parts by mass) was further added and reacted for 3 hours, after which propylene glycol monomethyl ether (48 parts by mass) and p-methoxyphenol (0.5 parts by mass) were added and heated to 100°C. Next, acrylic acid (10 parts by mass) and triphenylphosphine (1.6 parts by mass) were added and reacted at 110°C for 6 hours to obtain an acrylic resin (b1) having a double bond capable of radical polymerization in the side chain with a double bond amount (acryloyl group concentration (amount of acryloyl group introduced)) of 1.2 mmol / g. The weight average molecular weight (Mw) was 48,800.
[0219] (Production of acrylic resin (b2) having active energy ray-curable functional group) An acrylic resin (b2) having an active energy ray-curable functional group was prepared by the following method. In a flask equipped with a thermometer, a stirrer, and a reflux condenser, propylene glycol monomethyl ether (157 parts by mass), glycidyl methacrylate (98 parts by mass), methyl methacrylate (1.0 part by mass), ethyl acrylate (1.0 part by mass), mercaptopropyl trimethoxysilane (1.9 parts by mass), 2,2'-azobis(2,4-dimethylvaleronitrile) (1.0 part by mass), and 1.9 parts by mass of γ-trimethoxysilylpropanethiol (KBM-803 manufactured by Shin-Etsu Chemical Co., Ltd.) were added and reacted at 65°C for 3 hours. Then, 2,2'-azobis(2,4-dimethylvaleronitrile) (0.5 parts by mass) was added and reacted for 3 hours, and then propylene glycol monomethyl ether (138 parts by mass) and p-methoxyphenol (0.45 parts by mass) were added and heated to 100°C. Next, acrylic acid (51 parts by mass) and triphenylphosphine (3.1 parts by mass) were added and reacted at 110°C for 6 hours to obtain an acrylic resin (b2) having a double bond capable of radical polymerization in the side chain with a double bond amount (acryloyl equivalent (amount of acryloyl group introduced)) of 4.6 mmol / g. The weight average molecular weight (Mw) was 17,700.
[0220] (Production of transferable curable composition) The materials shown below were mixed in the amounts (parts by mass, calculated as non-volatile content) shown in Table 1. Then, a mixed solvent of propylene glycol monomethyl ether (hereinafter, PGM) and methyl ethyl ketone (hereinafter, MEK) (PGM:MEK (mass ratio) 7:3) was added so that the solid concentration became 30 mass%, and the mixture was stirred until it became uniform, to obtain a coating liquid (transfer-type curable composition). (Meth)acrylate (a1): Urethane acrylate (Mitsubishi Chemical Corporation, Shiko UV-1700B) (three or more functional groups) (Meth)acrylate (a2): Modified epoxy acrylate (EBECRYL 3708, manufactured by Daicel-Allnex) (bifunctional) (Meth)acrylate (a3): 1,6-hexanediol diacrylate (bifunctional) (Meth)acrylate (a4): Dimethyloltricyclodecane diacrylate (Kyoeisha Chemical Co., Ltd. Light Acrylate DCP-A) (bifunctional) (Meth)acrylate (a5): Dipentaerythritol hexaacrylate (6 functional) (Meth)acrylate (a6): A mixture of pentaerythritol triacrylate (trifunctional) and pentaerythritol tetraacrylate (tetrafunctional) (Viscoat #300, manufactured by Osaka Organic Chemical Industry Co., Ltd.) (Meth)acrylate (a7): Polyester-based urethane (meth)acrylate (Mitsubishi Chemical Corporation, Shiko UT-6042 (bifunctional) (Meth)acrylate (a8): Methoxyethyl acrylate (2-MTA, manufactured by Osaka Organic Chemical Industry Co., Ltd.) (monofunctional) Acrylic resin (b1): Acrylic resin (b1) having an active energy ray-curable functional group produced by the above method. Acrylic resin (b2): Acrylic resin (b2) having an active energy ray-curable functional group produced by the above method. Acrylic resin (b3): BR-80 (acrylic copolymer) manufactured by Mitsubishi Chemical Corporation Release agent (compound containing fluorine atoms) (c1): Perfluoropolyether compound containing active energy ray-curable functional groups (KY-1203 manufactured by Shin-Etsu Chemical Co., Ltd.) Release agent (silicone compound) (c2): Silicone-containing polymer (GL-04R manufactured by Kyoeisha Chemical Co., Ltd.) Release agent (silicone compound) (c3): Silicone hexaacrylate (EBECRYL 1360 manufactured by Daicel-Allnex) Particles (d): Cross-linked acrylic particles with an average particle size of 1.8 μm (MX-180TA manufactured by Soken Chemical Industries, Ltd.) Photoinitiator (e): Omnirad 184 manufactured by IGM Resins BV Antistatic agent (f): (meth)acrylic polymer containing quaternary ammonium base (Nikka Taibo, manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 28,000)
[0221] [Table 1]
[0222] [Table 2]
[0223] (Composition for forming primer layer) The polyester resin (P1), urethane resin (P2), melamine compound (P3), and particles (P4) shown below were mixed in a ratio of polyester resin (P1) / urethane resin (P2) / melamine compound (P3) / particles (P4) (solid content mass ratio) = 60 / 25 / 10 / 5 to obtain a composition for forming a primer layer. Polyester resin (P1): Water dispersion of polyester resin having the following composition Monomer composition: (acid component) terephthalic acid / isophthalic acid / 5-sodium sulfoisophthalic acid / / (diol component) ethylene glycol / 1,4-butanediol / diethylene glycol = 56 / 40 / 4 / / 70 / 20 / 10 (mol%) · Urethane resin (P2): Water dispersion of polyester-based urethane resin with the following composition Isophorone diisocyanate: terephthalic acid: isophthalic acid: ethylene glycol: diethylene glycol: dimethylolpropanoic acid = 12: 19: 18: 21: 25: 5 (mol%) Melamine compound (P3): Hexamethoxymethylolmelamine Particles: (P4): Silica particles with an average primary particle size of 0.07 μm
[0224] (Polyester film base) The raw material for the outermost layer (surface layer) was a mixture of polyesters (S1), (S2), and (S3) in proportions of 91%, 3%, and 6% by mass, respectively, and the raw material for the intermediate layer was a mixture of polyesters (S1) and (S2) in proportions of 97% and 3% by mass, respectively. Each of these raw materials was supplied to two extruders and melted at 285°C. After that, they were co-extruded onto a cooling roll set at 40°C in a layer structure of two types and three layers (surface layer / intermediate layer / surface layer = extrusion amount 1:8:1), and then cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.1 times in the longitudinal direction at a film temperature of 85°C using the difference in roll peripheral speed, and then a composition for forming a primer layer was applied to one side of this longitudinally stretched film, which was then introduced into a tenter and dried at 95°C for 10 seconds.Then, the film was stretched 4.2 times in the transverse direction at 120°C, heat-treated at 230°C for 10 seconds, and then relaxed by 2% in the transverse direction to obtain a polyester film substrate 50 μm thick (after drying) and having a 0.1 μm thick primer layer on one side.
[0225] [Examples 1 to 6] A coating solution (transfer-type curable composition) shown in Table 1 was applied onto the primer layer of the polyester film, dried at 70°C for 1 minute, and irradiated with excimer light (half-value width 14 nm) from xenon (wavelength 172 nm) at a dose of 15 mJ / cm 2 , illuminance 5mW / cm 2 The coating film made of the coating solution in Table 1 was irradiated with a 172 nm xenon excimer light irradiator (Ushio Inc., lamp unit type: SUS05 (lamp house type: H0011, lighting power supply type: B0005), nitrogen flow (oxygen concentration 1% or less)) and then irradiated with a high-pressure mercury lamp in an air atmosphere with an accumulated light dose of 400 mJ / cm. 2 , illuminance 200mW / cm 2 The film was irradiated with ultraviolet light using a UV conveyor (a high-output UV device (model: US5-X1802-X1202) manufactured by Eye Graphics Co., Ltd.) to obtain a cured film (transfer mold) having a wrinkled uneven structure with a thickness (after drying) of 5 μm shown in Table 3. The obtained transfer mold had a wrinkled uneven structure and good matte properties. The properties of this transfer mold are shown in Table 3.
[0226] [Comparative Example 1] A cured film (transfer type (T-7)) was obtained by manufacturing in the same manner as in Example 1, except that excimer light was not used and curing was performed only by irradiation with ultraviolet light from a high-pressure mercury lamp. The obtained cured film was evaluated, and as shown in Table 3, no wrinkled uneven structure was formed, the surface was smooth, and no matte property was observed.
[0227] [Comparative Example 2] A cured film (transfer mold (T-8)) was obtained in the same manner as in Example 1, except that the composition of the transfer type curable composition in Example 1 was changed to the composition shown in Table 1. The obtained cured film was evaluated, and as shown in Table 3, no wrinkled uneven structure was formed, and the film had a convex surface shape.
[0228] [Table 3]
[0229] [Example 7] In order to impart releasability to the transfer target object, the B-1 liquid in Table 1 was applied onto the transfer mold (T-1) obtained in Example 1, dried at 70°C for 1 minute, and then exposed to a high-pressure mercury lamp with an integrated light intensity of 400 mJ / cm in an air atmosphere. 2 , illuminance 200mW / cm 2 The substrate was irradiated with ultraviolet light using a UV conveyor of a high-output UV device (model: US5-X1802-X1202) manufactured by Eye Graphics Co., Ltd., to form a release layer having a thickness (after drying) of 0.1 μm. A solvent-free coating liquid (curable composition C-1 for transfer object) shown in Table 2 was applied onto the release layer, and the polyester film before the transfer mold formation obtained in Example 1 was placed so that the primer layer of the polyester film and the curable composition for transfer object were in contact with each other. The polyester film was then exposed to an accumulated light amount of 400 mJ / cm 2 from a high-pressure mercury lamp in an air atmosphere. 2 , illuminance 200mW / cm 2 The laminate was exposed to ultraviolet light using a UV conveyor (a high-output UV device (model: US5-X1802-X1202) manufactured by Eye Graphics Co., Ltd.) to form a cured film having a thickness (after drying) of 9 μm. The obtained cured film was peeled off from the transfer mold (T-1) to obtain a laminate in which the transferred object was formed on the primer layer of the polyester film. The obtained object had a wrinkled uneven structure and had a good matte finish. The properties of this object are shown in Tables 4 to 6.
[0230] [Examples 8 to 13] A transfer target in the form of a cured film was obtained in the same manner as in Example 7, except that the composition of the curable composition for the transfer target was changed to the composition shown in Table 2. The properties of the obtained transfer target are shown in Tables 4 to 6.
[0231] [Example 14] A transfer target in the form of a cured film was obtained by the same production as in Example 7, except that a release layer was not provided and the transfer target curable composition shown in Table 2 was directly applied onto the transfer mold. The properties of the obtained transfer target are shown in Tables 4 to 6.
[0232] [Examples 15 to 19] A transfer target in the form of a cured film was obtained in the same manner as in Example 14, except that the composition of the curable composition for the transfer target was changed to the composition shown in Table 2. The properties of the obtained transfer target are shown in Tables 4 to 6.
[0233] [Comparative Example 3] In Example 7, the transfer target was produced in the same manner as in Example 7, except that the composition of the curable composition for the transfer target was changed to the composition shown in Table 2, and a transfer target was obtained in the form of a cured film. The transfer target obtained was a concave shape, and had a different shape from the transfer mold. Other properties are shown in Tables 4 to 6.
[0234] [Table 4]
[0235] [Table 5]
[0236] [Table 6]
Claims
1. A transfer mold having a cured film of a curable composition, the surface of the cured film constituting a transfer surface, the curable composition contains a difunctional (meth)acrylate and a trifunctional or higher multifunctional (meth)acrylate, a surface side of the coating film of the curable composition is cured by irradiation with vacuum ultraviolet light to form a cured coating, and then the inside of the coating film is cured by irradiation with active energy rays other than vacuum ultraviolet light, whereby the cured coating on the surface side is buckled to form a wrinkled uneven structure on the transfer surface; A transfer mold in which the average length (RSm) of the roughness curve elements of the transfer surface according to JIS B0601:2013 is 1 to 1000 μm, and the arithmetic mean height (Sa) defined in ISO 25178 is 0.1 to 1000 μm.
2. 2. The transfer mold according to claim 1, wherein an average value (θa) of the local inclination angle of the transfer surface is 2° or more.
3. 3. The transfer mold according to claim 1, wherein the 60° gloss of the transfer surface is 50 or less.
4. The transfer mold according to any one of claims 1 to 3, wherein the curable composition contains a (meth)acrylate.
5. The transfer mold according to any one of claims 1 to 4, comprising the cured film on a substrate.
6. The transfer mold according to claim 5 , wherein the substrate is a film.
7. A transfer object has a wrinkled uneven structure on a transfer surface of a transfer mold, the wrinkled uneven structure being transferred to the transfer surface of the transfer mold, the wrinkled uneven structure of the transfer surface is an uneven structure formed by buckling the cured coating on the surface side as a result of curing the surface side of the coating film of the curable composition by irradiation with vacuum ultraviolet light to form a cured coating, and then curing the inside of the coating film by irradiation with active energy rays other than vacuum ultraviolet light; the curable composition contains a difunctional (meth)acrylate and a trifunctional or higher multifunctional (meth)acrylate, The surface to be transferred has a roughness curve element average length (RSm) according to JIS B0601:2013 of 1 to 1000 μm, and an arithmetic mean height (Sa) defined in ISO 25178 of 0.1 to 1000 μm.
8. 8. The transferred object according to claim 7, wherein an average value (θa) of a local inclination angle of the transferred surface is 2° or more.
9. 9. The object according to claim 7, wherein the 60° gloss of the surface to be transferred is 50 or less.
10. The object according to any one of claims 7 to 9, wherein the object is a cured film of a curable composition.
11. The transfer-receiving material according to claim 10, wherein the curable composition constituting the transfer-receiving material contains a (meth)acrylate.
12. The object to which a transfer is to be performed according to claim 10 or 11, comprising the cured film on a substrate.
13. The object according to claim 12 , wherein the substrate is a film.
Citation Information
Patent Citations
Method for producing a film with a matt surface
EP2527408A1
Unmanned underwater monitoring / searching system, unmanned underwater searching machine, searching base system, monitoring center apparatus, and program
JP2005181199A
Resin molding and method for producing the same, and molding device
JP2017217773A
Antidazzle film, production method of the same, and use of the same