Oil-based ballpoint pen ink composition and oil-based ballpoint pen employing the same

The ink composition for oil-based ballpoint pens, featuring a compound with alkylene oxide structure, enhances lubricity and reduces wear, addressing high-pressure writing resistance and tip drying issues, thus improving writing quality and performance.

JP2024161136AActive Publication Date: 2024-11-15PILOT PEN CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024145762
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing oil-based ballpoint pens suffer from poor writing quality due to high writing resistance and wear of the ball seat under high pressure, leading to issues like line skipping and smearing, and the tip drying out, which affects writing performance.

Method used

An ink composition for oil-based ballpoint pens containing a compound represented by a specific formula, along with a solvent, surfactant, and colorant, which improves lubricity and reduces writing resistance, wear, and enhances ink followability.

Benefits of technology

The ink composition effectively reduces writing resistance and wear of the ball seat under high pressure, improving writing quality and performance, even when the tip is exposed to the atmosphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161136000001
    Figure 2024161136000001
  • Figure 2024161136000002
    Figure 2024161136000002
  • Figure 2024161136000003
    Figure 2024161136000003
Patent Text Reader

Abstract

To provide an oil-based ballpoint pen ink composition which inhibits wear of a ball seat under high writing pressure (writing loads of 300-500 gf), improves a writing feel, and is excellent in the capability of starting writing, ink temporal stability and ink followability; and an oil-based ballpoint pen employing the same.SOLUTION: An oil-based ballpoint pen ink composition contains a colorant, an organic solvent, and a compound represented by the general formula (Chemical Formula 1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink composition for an oil-based ballpoint pen and an oil-based ballpoint pen using the same. [Background technology]

[0002] When writing with a writing instrument, the writing feel of a ballpoint pen or marking pen can be easily affected by the writing resistance between the writing tip and the surface being written on. In particular, a ballpoint pen has a ballpoint pen tip attached to an ink reservoir, which comprises a metal tip made of stainless steel or the like at the tip and a transfer ball made of a metal such as super steel that is held in a ball receiving seat of the metal tip. When writing, the rotation of the ball causes wear to the ball seat, resulting in problems such as skipped lines and smudges in the handwriting and a poor writing feel, leaving room for improvement. Furthermore, if the tip end is left exposed to the atmosphere, the solvent in the ink evaporates, and when the colorant and resin dry and harden, the handwriting is likely to become smudged when the pen is first written.

[0003] In order to solve these problems, numerous ink compositions for oil-based ballpoint pens have been proposed that use various lubricants for the purpose of improving lubricity, etc., in order to reduce the writing resistance between the writing tip and the surface being written on during writing.

[0004] As oil-based ink compositions using such additives, JP-A-5-331403 "Oil-based Ballpoint Pen Ink" is an example of an ink composition using alkyl β-D-glucoside, JP-A-7-196971 "Ink Composition for Oil-based Ballpoint Pens" is an example of an ink composition using polyethylene glycol with an average molecular weight of 200 to 4,000,000, JP-A-2007-176995 "Oil-based Ballpoint Pen Ink" is an example of an ink composition using N-acylamino acid, N-acylmethyltauric acid, or N-acylmethylalanine, and JP-A-2007-176995 "Oil-based Ballpoint Pen Ink" is an example of an ink composition using deca-macadamia nut oil fatty acid decaglycerol. An example of an ink composition containing at least ceryl and a polyoxyethylene alkyl ether in which the alkyl group has 16 or more carbon atoms and which is solid at room temperature is disclosed in JP 2008-88264 A, entitled "Oil-based ink composition for ballpoint pens." An example of an ink composition containing an N-acylamino acid and an N-acylmethyltaurine is disclosed in JP 2003-192972 A, entitled "Ink for water-based ballpoint pens." An example of an ink composition containing an isoprene sulfonic acid-acrylic acid copolymer is disclosed in JP 2006-282870 A, entitled "Water-based ink composition for ballpoint pens." [Prior art documents] [Patent documents]

[0005] [Patent Document 1] "Unexamined Japanese Patent Publication No. 5-331403" [Patent Document 2] "Unexamined Japanese Patent Publication No. 7-196971" [Patent Document 3] "JP Patent Publication No. 2007-176995" [Patent Document 4] "JP Patent Publication No. 2008-88264" [Patent Document 5] "JP Patent Publication No. 2003-192972" [Patent Document 6] "JP Patent Publication No. 2006-282870" Summary of the Invention [Problem to be solved by the invention]

[0006] However, when various additives such as those described in Patent Documents 1 to 6 are used, although some of the additives can reduce the writing resistance between the writing tip and the surface being written on to some extent, they are not satisfactory and there is room for improvement. Furthermore, in recent years, ballpoint pen ink has become less viscous to improve the writing feel, and when writing with high writing pressure (high writing pressure resistance, writing load 300-500gf), the lubricity is easily affected, and the ball seat wears out, which easily affects the writing performance. Therefore, in order to further reduce the writing resistance between the writing tip and the writing surface, there is a demand for improving the lubricity and improving the resistance to high writing pressure. In addition, in the case of a retractable ballpoint pen such as a knock type ballpoint pen or a twist type ballpoint pen, this is important because the writing performance is easily affected if the tip end is left exposed to the atmosphere. For this reason, it is necessary to satisfy both the lubricity under high writing pressure (writing load of 300 to 500 gf) and writing performance.

[0007] The object of the present invention is to provide an ink composition for an oil-based ballpoint pen which suppresses wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), improves the writing feel, and has good writing start performance and ink following properties, and to provide an oil-based ballpoint pen using the same. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention "1. An ink composition for a writing instrument, comprising a colorant, a solvent, and a compound represented by the general formula (Chemical Formula 1). [ka] 2. The ink composition for a writing instrument according to item 1, wherein the content of the compound represented by the general formula (Chemical Formula 1) is 0.1 to 40% by mass based on the total amount of the ink composition. 3. The ink composition for a writing instrument according to item 1 or 2, wherein the hydroxyl value (mgKOH / g) of the general formula (Chemical Formula 1) is 100 to 1000 (mgKOH / g). 4. The ink composition for a writing instrument according to any one of items 1 to 3, wherein the solvent is an aromatic alcohol. 5. The ink composition for a writing instrument according to any one of items 1 to 4, characterized in that the ink composition for a writing instrument contains a surfactant. 6. The ink composition for a writing instrument according to item 5, wherein the surfactant is a nonionic surfactant. 7. The ink composition for a writing instrument according to item 5 or 6, wherein the surfactant is a phosphate ester surfactant or a fatty acid. 8.20℃, shear rate 5sec -1 8. The ink composition for a writing instrument according to any one of items 1 to 7, characterized in that the ink viscosity at 200° C. is 30,000 mPa·s or less. 9. A writing instrument containing the ink composition for a writing instrument according to any one of items 1 to 8. 10. A ballpoint pen, characterized in that it has a ballpoint pen tip that rotatably holds a ball at the tip of an ink reservoir, and the ink composition for a writing instrument according to any one of items 1 to 8 is contained in the ink reservoir. Effect of the Invention

[0009] The present invention has made it possible to obtain an ink composition for oil-based ballpoint pens that improves lubricity, thereby maintaining lubricity between the writing tip and the surface being written on (including lubricity between the ball and the tip body), suppressing the writing resistance of the writing tip, suppressing wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), improving the writing feel, and providing good writing start performance and ink following properties, as well as an oil-based ballpoint pen using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail. In this specification, unless otherwise specified, "parts", "%", "ratio" and the like indicating the composition are based on mass, and the content is the mass% of the constituent components based on the mass of the ink composition.

[0011] The feature of the present invention is to provide an ink composition for oil-based ballpoint pens, which is characterized by containing a colorant, an organic solvent, and a compound represented by the general formula (Chemical formula 1). This is because the lubricating layer formed by containing the compound represented by the general formula (Chemical formula 1), which is an alkylene oxide-containing substance, maintains the lubricity between the writing tip and the surface to be written (including the lubricity between the ball and the tip body), suppresses the writing resistance of the writing tip, suppresses the wear of the ball seat under high writing pressure (writing load 300 to 500 gf), improves the writing feel, and even if the writing tip is left in the air, it is possible to improve the writing performance by suppressing the evaporation of the solvent in the ink. Therefore, it is possible to suppress the wear of the ball seat under high writing pressure (writing load 300 to 500 gf), and improve both the writing feel and the writing performance, and when used in ballpoint pen ink, it is effective and preferable. In particular, since oil-based ballpoint pens are expected to be used for writing on copy paper and therefore require a higher writing pressure than normal (high-pressure writing), it is desirable for the ink to have good resistance to high writing pressure (writing load of 300 to 500 gf). Therefore, it is most effective and preferable to use the ink in oil-based ballpoint pen ink. [ka]

[0012] (Compound represented by general formula (Chemical Formula 1)) The compound represented by the general formula (Chemical Formula 1) used in the present invention is a compound having an alkylene oxide in its structure, and examples thereof include pentaerythritol polyoxyalkylene ether, trimethylolpropane tripolyoxyalkylene ether, etc., and specifically includes pentaerythritol polyoxypropylene ether, pentaerythritol polyoxyethylene ether, etc., pentaerythritol polyoxypropylene ether, trimethylolpropane tripolyoxyalkylene ether, etc., and examples thereof include PNT-40 (average number of moles of ethylene oxide added: 4), PNT-F40 (average number of moles of propylene oxide added: 4), TMP-F32 (propylene oxide added), TMP-30 (average number of moles of ethylene oxide added: 3), TMP-60 (average number of moles of ethylene oxide added: 6), TMP-60 (average number of moles of ethylene oxide added: 6) (Nippon Nyukazai Co., Ltd.), etc. These compounds represented by the general formula (Chemical Formula 1) have alkylene oxide in their structure and are hydrophilic and lipophilic. The presence of a highly polar hydrophilic group in the structure makes them more easily adsorbed to the metal material of the ballpoint pen tip, further improving lubricity. This makes it possible to suppress wear of the ball seat and improve the writing feel even under high writing pressure (writing load of 300 to 500 gf). Furthermore, since the compound represented by the general formula (Chemical Formula 1) is difficult to evaporate, even if the writing tip is left in the air, it is preferable because it can improve the writing performance and suppress the ink thickening of the ink composition for writing instruments as much as possible, thereby improving the ink tracking property. Furthermore, when a pigment is used as a colorant, the ink viscosity generally increases over time due to the pigment agglomeration, and the ink tracking property decreases, but since the polar group in the structure of the compound represented by the general formula (Chemical Formula 1) is adsorbed to the pigment surface and the pigment is stably dispersed in the ink, the increase in the ink viscosity due to the pigment agglomeration is suppressed, and the ink tracking property can be improved.

[0013] In addition, the compound represented by the general formula (chemical formula 1) has many branched chains and forms a bulky structure, which makes it easy to form a thicker lubricating film, and by improving the lubricity, it is easy to suppress the wear of the ball seat and improve the writing feel even under high writing pressure (writing load 300 to 500 gf), so it is preferable to contain pentaerythritol polyoxyalkylene ether represented by the general formula (chemical formula 2). Furthermore, when used in oil-based ink, it is preferable that R1 in the general formula (chemical formula 1) and the general formula (chemical formula 2) is a methyl group, because the compound has excellent lipophilicity by having a propylene oxide group, which makes it easy to stabilize in the ink and to easily obtain the effects of the present invention, and from a further consideration, it is preferable to contain pentaerythritol polyoxypropylene ether in which R1 in the general formula (chemical formula 2) is a methyl group. [ka]

[0014] In the compounds represented by the general formulas (Chemical Formula 1) and (Chemical Formula 2), the average number of moles of alkylene oxide added (k+l+m+n) is preferably 1 to 20 in consideration of suppressing wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), improving the writing feel, and further improving the writing performance. In consideration of making the compound more stable in the ink and making it easier to obtain the effects of the present invention, the average number of moles of alkylene oxide added is preferably 1 to 15. Furthermore, in consideration of suppressing wear of the ball seat under high writing pressure, improving the writing feel, and improving the writing performance, the average number of moles of alkylene added is preferably 1 to 10, and more preferably 1 to 6. In particular, when considering the suppression of wear of the ball seat under high writing pressure, it is preferable that R1 is a methyl group, and in that case, the average number of moles of propylene oxide added (k+l+m+n) is preferably 1 to 20, and from further consideration, the average number of moles of propylene oxide added is preferably 1 to 15, more preferably 1 to 10, and further preferably 1 to 6.

[0015] The hydroxyl value (mgKOH / g) of the compound represented by the general formula (Chemical Formula 1) is preferably 100 to 1000 (mgKOH / g), because within the above range, the stability with the colorant and other components is less affected and the effects of the present invention are more easily obtained. From further consideration, the hydroxyl value is preferably 300 to 800 (mgKOH / g), and from further consideration, the hydroxyl value is preferably 500 to 750 (mgKOH / g). In addition, the average weight molecular weight of the compound represented by the general formula (Chemical Formula 1) is preferably 2000 or less. This is because if the average weight molecular weight is too large, it is likely to affect the stability over time in the oil-based ink, making it difficult to obtain the effects of the present invention. From this perspective, the average weight molecular weight is preferably 1000 or less. The weight average molecular weight is a value obtained by GPC (gel permeation chromatography) in terms of polystyrene.

[0016] Furthermore, if the content of the compound represented by the general formula (Chemical Formula 1) is less than 0.1% by mass relative to the total amount of the ink composition, there is a risk that the effects of suppressing wear of the ball seat under high writing pressure, writing feel, writing performance, and ink followability as described above may not be obtained, and if it exceeds 40% by mass, there is a risk that the ink stability over time may be affected. Therefore, the content is preferably 0.1 to 40% by mass relative to the total amount of the ink composition, and more preferably 1 to 30% by mass in consideration of the above effects, and furthermore, if the balance between suppressing wear of the ball seat and writing feel, writing performance, and ink followability is taken into consideration, the content is preferably 3 to 25% by mass, and most preferably 8 to 25% by mass.

[0017] (solvent) The solvent used in the ink composition for writing instruments used in the present invention may be water, an organic solvent, or a mixed solvent of water and an organic solvent. In addition, the water may be any conventional water such as ion-exchanged water, distilled water, or tap water.

[0018] Examples of the organic solvent include water-insoluble organic solvents and water-soluble organic solvents. Specific examples of the organic solvent include glycol ether solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol dimethyl ether, ethylene glycol monophenyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol dimethyl ether, 3-methoxybutanol, and 3-methoxy-3-methylbutanol; glycol solvents such as diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, ethylene glycol, diethylene glycol, and glycerin; and alcohol solvents such as benzyl alcohol, methanol, ethanol, 1-propanol, 2-propanol, isopropanol, isobutanol, t-butanol, propargyl alcohol, allyl alcohol, 3-methyl-1-butyn-3-ol, ethylene glycol monomethyl ether acetate, and other higher alcohols. These organic solvents are generally used in ink compositions for oil-based ballpoint pens and ink compositions for aqueous ballpoint pens.

[0019] Among these organic solvents, aromatic alcohols have an aromatic ring, which improves lubricity, and are easily dissolved and stable with the compound represented by the general formula (Chemical Formula 1), so it is preferable to use aromatic alcohol solvents. In addition, when a glycol ether solvent is used, it is prone to moisture absorption, which softens the strength of the coating that is formed when the tip end dries, and tends to improve writing performance. Therefore, when a compound represented by the general formula (Chemical Formula 1) is used as in the present invention, it is more effective, and in consideration of lubricity and writing performance, it is preferable to use an aromatic glycol ether solvent.

[0020] Furthermore, in consideration of improving solubility, lubricity, and writing drying properties, the content of the solvent is preferably 10 to 90 mass% of the total amount of the ink composition, and more preferably 20 to 90 mass%, and more preferably 40 to 70 mass%.

[0021] (Coloring agent) The colorant used in the water-based ink composition and the oil-based ink composition of the present invention is not particularly limited and may be a dye, a pigment, or the like, and may be appropriately selected for use. Dyes and pigments may be used in combination.

[0022] In addition, as the colorant, it is preferable to use a pigment in consideration of lubricity, because the pigment particles can easily enter the gap between the ball and the tip body, acting like a bearing, and suppressing metal contact improves lubricity, improves writing feel, and reduces wear of the ball seat. Furthermore, pigments are preferable because they have excellent water resistance and light resistance, and can provide good handwriting fastness. In particular, the lubricating layer of the compound represented by the general formula (Chemical Formula 1), the nonionic surfactant or phosphate surfactant described later, and the synergistic effect of the pigment particles and the bearing action make it easier to maintain lubricity, suppress the wear of the ball seat, and improve the writing feel. In addition, taking into consideration the gap relationship inside the ballpoint pen tip, the average particle size is preferably 1 to 500 nm. More preferably, it is 30 to 350 nm, and even more preferably, it is 50 to 300 nm. Here, the average particle size can be determined by the laser diffraction method, specifically, the particle size (D50) at 50% cumulative volume of the particle size distribution measured based on the value calibrated using a standard sample or other measurement method using a laser diffraction type particle size distribution measuring instrument (product name "MicrotracHRA9320-X100", Nikkiso Co., Ltd.). In addition, since the pigment exerts the above-mentioned effects in a dispersed state in the ink composition for an oil-based ballpoint pen, it is preferable to obtain the particle size in the dispersed state. Furthermore, the pigment is preferable because it has excellent water resistance and light resistance and can obtain good color development.

[0023] In addition, when a dye is used, it is preferable to use a salt-forming dye in consideration of the stability over time due to the compatibility with the compound represented by the general formula (Chemical Formula 1), and further, in consideration of the stability over time due to the stable salt-forming bond, it is preferable to use a salt-forming dye made of a basic dye and an organic acid, a salt-forming dye made of an acidic dye and a basic dye, or a salt-forming dye made of an acidic dye and an organic amine. In consideration of the stability with the components in the ink, a salt-forming dye made of a basic dye and an organic acid is preferable.

[0024] Dyes used in the oil-based ink composition include oil-soluble dyes, acid dyes, basic dyes, metal-containing dyes, and various salt-forming dyes thereof, such as salt-forming dyes made of acid dyes and basic dyes, salt-forming dyes made of organic acids and basic dyes, salt-forming dyes made of acid dyes and organic amines, etc. Considering the stability of the compound represented by the general formula (Chemical Formula 1) used in the present invention, it is preferable to use salt-forming dyes. Dyes include Balifast Black 1802, Balifast Black 1805, Balifast Black 1807, Balifast Violet 1701, Balifast Violet 1704, Balifast Violet 1705, Balifast Blue 1601, Balifast Blue 1605, Balifast Blue 1613, Balifast Blue 1621, Balifast Blue 1631, Balifast Red 1320, Balifast Red 1355, Balifast Red 1360, Balifast Yellow 1101, Balifast Yellow 1151, Nigrosine Base EXBP, Nigrosine Base EX, BASE OF BASIC DYES ROB-B, BASE OF BASIC DYES RO6G-B, BASE OF BASIC DYES VPB-B, BASE OF BASIC DYES VB-B, BASE OF BASIC DYES MVB-3 (all manufactured by Orient Chemical Industry Co., Ltd.), Aizen Spiron Black GMH-Special, Aizen Spiron Violet C-RH, Aizenspiron Blue GNH, Aizenspiron Blue 2BNH, Aizenspiron Blue C-RH, Aizenspiron Red C-GH, Aizenspiron Red C-BH, Aizenspiron Yellow C-GNH, Aizenspiron Yellow C-2GH, SPT Blue 111, SPT Blue GLSH-Special, SPT Red 533, SPT Orange 6, SBN Yellow 510, SBN Yellow 530, SRC-BH (all manufactured by Hodogaya Chemical Co., Ltd.).

[0025] As the dye for use in the water-based ink composition, direct dyes, acid dyes, basic dyes, metal-containing dyes, various salt forming dyes, and the like can be used. (a) Direct dyes: Direct Yellow 4, 26, 44, 50, 85; Direct Red 1, 2, 4, 23, 31, 37, 39, 75, 80, 81, 83, 225, 226, 227; Direct Blue 1, 3, 15, 41, 71, 86, 106, 119; Direct Orange 6, etc.; (b) Acid dyes: The colors are Acid Black 1, 2, 24, 26, 31, 52, 107, Acid Orange 56, Acid Yellow 3, 7, 17, 19, 23, 42, 49, 61, 92, Acid Red 8, 9, 14, 18, 51, 52, 73, 87, 92, 94, Acid Blue 1, 7, 9, 22, 62, 90, 103, Acid Green 3, 9, 16, 25, 27, Acid Violet 15, 17, etc.; (c) Basic dyes include CI Basic Yellow 1, 2, 21, 7, 40, CI Basic Orange 2, 14, 32, CI Basic Red 1, 1:1, 2, 9, 14, CI Basic Violet 1, 3, 7, 10, 11:1, CI Basic Blue 3, 7, 26, Basic Green 4, CI Basic Brown 12, CI Basic Black 2, methyl violet, Victoria Blue FB, malachite green, rhodamine series, etc.; (d) Other dyes include disperse dyes such as Disperse Yellow 82, 121, Disperse Blue 7, etc.

[0026] The content of the colorant is preferably 5.0 to 30.0% by mass based on the total amount of the ink composition. If the content is less than 5.0% by mass, it tends to be difficult to obtain thick handwriting, and if the content exceeds 30.0% by mass, it tends to affect the solubility in the ink. Taking this tendency into consideration, the content is preferably 7.0 to 25.0% by mass, and further taking this into consideration, the content is more preferably 10.0 to 20.0% by mass.

[0027] (Surfactant) In the present invention, it is preferable to use a surfactant. This is because it softens the coating formed by the resin contained in the ink, and it is easy to improve the writing performance, and further improves the lubricity and writing feel. As the surfactant, there are nonionic surfactants, anionic surfactants, cationic surfactants, etc., and it is preferable to use a nonionic surfactant. This is preferable because it is unlikely to show ionicity, and is unlikely to cause precipitation due to other components in the ink, and therefore the ink has good stability over time. Regarding the nonionic surfactant, in consideration of ink stability over time, the HLB value is preferably 16 or less. In consideration of ink stability over time, the HLB value is preferably 3 to 14, and more preferably 3 to 11. The HLB value can be determined by the Griffin method, etc. In particular, in retractable writing instruments such as knock-type writing instruments and rotary-type writing instruments, unlike cap-type writing instruments, the pen tip is always exposed to the outside, which tends to affect the writing performance when the writing tip dries, so it is more preferable to use a surfactant with the above HLB value.

[0028] Examples of nonionic surfactants include fatty acid esters, polyalkylene alkyl ethers, polyoxyethylene alkyl amines, alkyl imidazolines, alkyl alkanolamides, oxyethylene oxypropylene block copolymers, and surfactants having acetylene bonds. Among them, in consideration of the above-mentioned writing performance and ink stability over time, it is preferable to select one or more from fatty acid esters, polyalkylene alkyl ethers, polyoxyethylene alkyl amines, alkyl imidazolines, and alkyl alkanolamides, and in consideration of further improving writing performance, it is preferable to use fatty acid esters. These may be used alone or in combination of two or more.

[0029] Examples of the fatty acid esters include sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid esters, glycerin fatty acid esters, polyglycerin fatty acid esters, and polyoxyethylene fatty acid esters. Taking into consideration the interaction with polyoxyalkylene glyceryl ether, and the writing performance, it is preferable to select one or more from among sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, glycerin fatty acid esters, and alkyl imidazolines. Furthermore, it is preferable to use sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and alkyl imidazolines, which have a structure having a cyclic skeleton. From a more specific perspective, it is preferable to select one or more from sorbitan fatty acid esters that are sorbitan fatty acid esters or polyoxyethylene sorbitan fatty acid esters, which have multiple hydroxyl groups and are therefore more susceptible to moisture absorption.

[0030] Furthermore, among the above-mentioned sorbitan fatty acid esters, when taking into consideration the writing performance, it is preferable that the alkyl group of the sorbitan fatty acid esters contains 1 to 20 carbon atoms. Furthermore, when taking into consideration that the length is suitable for forming a lubricating layer, which makes it easier to improve the wear suppression of the ball seat under high writing pressure, it is preferable to use sorbitan fatty acid esters in which the alkyl group contains 10 to 20 carbon atoms, and from further consideration, it is preferable to use sorbitan fatty acid esters in which the alkyl group contains 12 to 18 carbon atoms. Specific examples of the sorbitan fatty acid esters include sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan monococoate, sorbitan dilaurate, sorbitan distearate, sorbitan dioleate, sorbitan trioleate, sorbitan tristearate, and composites thereof; and polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tristearate, and composites thereof.

[0031] The content of the nonionic surfactant is more preferably 0.1 to 15% by mass based on the total amount of the ink composition. This is because if it is less than 0.1% by mass, it is difficult to suppress the wear of the ball seat under the desired high writing pressure (writing load of 300 to 500 gf), improve the writing feel, and it is difficult to obtain the writing performance and ink tracking ability, and if it exceeds 15% by mass, the ink tends to become unstable over time. Taking this tendency into consideration, it is preferable that the content is 0.5 to 10% by mass based on the total amount of the ink composition, and more preferably, it is 1 to 5% by mass.

[0032] In the present invention, in order to improve the lubricity of the writing tip (ball and ball seat of a ballpoint pen), inhibit wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), improve the writing feel, and further improve the writing performance when the writing tip is left in the air and dries, it is preferable for the pen to contain a phosphate ester surfactant and a fatty acid, and in order to further improve lubricity, it is preferable for the pen to contain a phosphate ester surfactant. This is because it has a phosphoric acid group and a fatty acid group, so it is easily adsorbed to the metal surface, and in particular, it forms a lubricating film between the ball and the ball seat, so that the lubrication is improved, and the wear of the ball seat under high writing pressure (writing load 300 to 500 gf) can be suppressed and the writing feel can be improved. Therefore, when using a phosphoric acid ester surfactant, a fatty acid, and a compound represented by the general formula (Chemical Formula 1), the lubricating action of both works, and the lubrication between the ball and the ball seat can be further improved synergistically, and the wear of the ball seat under high writing pressure (writing load 300 to 500 gf) can be easily suppressed, so that a phosphoric acid ester surfactant is preferable. Furthermore, since the phosphate ester surfactant has a rust-preventing effect, when the ball is made of a metal material, it is preferable because it can suppress the corrosion of the ball, thereby improving the writing feel and suppressing the wear of the ball seat. Furthermore, when the ball material is used, cobalt, nickel, chromium, etc. are used as the binder, and since it is difficult to corrode over time with respect to metals such as cobalt, nickel, and chromium, it is preferable because it does not cause rotation resistance of the ball due to corrosion and can improve the writing feel and suppress the wear of the ball seat. In particular, in the case of a cemented carbide ball mainly composed of tungsten carbide, it is effective and preferable because cobalt, nickel, chromium, etc. are used as the binder. For this reason, in the present invention, it is effective and preferable to use a phosphate ester surfactant in combination with the compound represented by the general formula (Chemical Formula 1). Furthermore, in order to achieve a good balance between the writing feel and the wear inhibition of the ball seat, it is effective and preferable to use a nonionic surfactant, a phosphate ester surfactant, and the compound represented by the general formula (Chemical Formula 1) in combination. Furthermore, in the present invention, when polyvinyl butyral is used, the use of a phosphate-based surfactant is effective and preferable, since the lubricity is further improved by the lubricating layer made of polyvinyl butyral and the lubricating film made of the phosphate-based surfactant.

[0033] In the phosphoric acid ester surfactant, in order to further improve both the lubricity and writing performance due to the interaction with the compound represented by the general formula (Chemical Formula 1), the HLB value is preferably 6 to 18. This is because if the HLB value exceeds 18, the hydrophilicity is likely to be strong and the solubility in the ink is likely to be poor, so that the effect of the phosphoric acid ester surfactant due to the interaction with the compound represented by the general formula (Chemical Formula 1) is difficult to obtain, and in particular, the lubricating effect is difficult to obtain. In addition, if the HLB value is less than 6, the lipophilicity is too strong, which is likely to affect the compatibility with organic solvents, making it difficult to obtain ink stability over time, and further making it difficult to improve writing performance. Furthermore, in order to further consider the suppression of wear of the ball seat under high writing pressure, the HLB value is preferably 17 or less, and the HLB value is preferably 6 to 17, and in order to further consider the writing performance, the HLB value is preferably 7 to 17. In particular, in retractable ballpoint pens such as knock-type ballpoint pens and rotary-type ballpoint pens, the pen tip is always exposed to the outside, unlike cap-type ballpoint pens, and is therefore prone to affect the writing performance when the writing tip dries, so it is more preferable to use a phosphate ester surfactant with the above HLB value. The HLB can be determined by the Griffin method, the Kawakami method, etc.

[0034] Phosphate ester surfactants include those with alkoxy groups (C a H 2a+1 O), a phosphate ester having the formula (I) or (II), a phosphate monoester of a polyoxyethylene alkyl ether or a polyoxyethylene alkylaryl ether, a phosphate diester of a polyoxyethylene alkyl ether or a polyoxyethylene alkylaryl ether, a phosphate triester of a polyoxyethylene alkyl ether or a polyoxyethylene alkylaryl ether, an alkyl phosphate ester, an alkyl ether phosphate ester, or a derivative thereof. Among these, taking into consideration the suppression of wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), it is preferable to use a phosphate ester surfactant having an alkyl group, and in particular, the number of carbon atoms contained in the alkyl group is preferably 8 to 18, and even more preferably, the number of carbon atoms is 10 to 18, and even more preferably, the number of carbon atoms is 12 to 18. This is because if the number of carbon atoms in the alkyl group is too small, the lubricity tends to be insufficient, and if the number of carbon atoms is too large, the ink stability over time tends to be affected.

[0035] Furthermore, when a phosphate ester surfactant is used, the acid value is preferably 200 or less. This is to facilitate the improvement of lubricity due to the phosphate ester surfactant. Taking into consideration stability and lubricity in the ink, the acid value is preferably 30 to 170, and more preferably 40 to 160. The acid value is expressed as the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of sample.

[0036] In the present invention, the compounding ratio of the compound represented by the general formula (Chemical Formula 1) to the surfactant such as the nonionic surfactant or phosphate surfactant (compound represented by the general formula (Chemical Formula 1) / surfactant) is preferably 1 to 40 times by mass, more preferably 2 to 30 times, more preferably 1 to 25 times, and most preferably 1 to 15 times. This is because, within the above range, it is possible to suppress the wear of the ball seat, and improve the writing feel, writing performance, and ink tracking in a well-balanced manner.

[0037] (Stabilizer) In the present invention, when a surfactant such as a phosphate surfactant is used, neutralization is preferred because it is easy to obtain the effect of dissolving and stabilizing in the ink, improving the writing feel and writing performance. Examples of stabilizers include basic inorganic compounds such as ammonia, sodium carbonate, sodium phosphate, and sodium hydroxide, alkanolamines such as diethanolamine and triethanolamine, amines having ethylene oxide such as oxyethylene alkylamines and polyoxyethylene alkylamines, alkylamines such as laurylamine and stearylamine, aliphatic amines such as dimethyl alkylamines such as distearylamine, dimethyl laurylamine, dimethyl stearylamine, and dimethyl octylamine, basic organic compounds such as sodium acetate, lactic acid, and citric acid. Among them, amines having ethylene oxide, dimethyl alkylamines, and alkanolamines are preferred in terms of stability with the surfactant. In particular, in the case of an oil-based ink composition, amines having ethylene oxide and dimethylalkylamines are preferred, and further, in consideration of suppressing wear of the ball seat under high writing pressure (writing load of 300 to 500 gf), amines having ethylene oxide are preferred, and in the case of a water-based ink composition, alkanolamines are preferred, and it is preferable to use triethanolamine, which is weakly basic. These may be used alone or in combination of two or more kinds.

[0038] Furthermore, the total amine value of the organic amine is preferably 100 to 300 (mgKOH / g) in consideration of the stability with the surfactant, phosphate ester surfactant, colorant and other components. If it exceeds 300 (mgKOH / g), it is highly reactive and easily reacts with the above components, so the ink stability over time is likely to be poor. If the total amine value is less than 100 (mgKOH / g), the stability of the surfactant and phosphate ester surfactant in the ink is likely to be affected, and if it is used as an oil-based ballpoint pen, the adsorption of metals such as the ball and tip body is likely to be poor, making it difficult to obtain lubricating performance. If the stability and lubricity with the above components are more considered, the range of 150 to 300 (mgKOH / g) is preferable, if the stability is more considered, 180 to 300 (mgKOH / g) is preferable, and if the stability is more considered, 230 to 270 (mgKOH / g) is preferable. The total amine value indicates the total amount of primary, secondary, and tertiary amines, and is expressed as the number of milligrams of potassium hydroxide equivalent to the amount of hydrochloric acid required to neutralize 1 g of sample.

[0039] The content of the stabilizer is preferably 0.1 to 10 mass% of the total amount of the ink composition, taking into consideration the neutralization stability with the surfactant, and more preferably 0.1 to 8 mass% when neutralization with the surfactant is further taken into consideration, and more preferably 0.5 to 6 mass%.

[0040] (resin) In the present invention, resins may be used as ink viscosity adjusters, ink leakage suppressants, pigment dispersants, and fixing agents. Examples of resins include polyvinyl butyral resins, ketone resins, polyacetal resins, polyvinyl alcohol resins, cellulose resins, terpene resins, alkyd resins, phenoxy resins, polyvinyl acetate resins, polyvinylpyrrolidone resins, ethylene oxide polymers, acrylic resins, styrene-acrylic resins, styrene-maleic acid resins, and resin particles such as olefin-based resin particles, acrylic acid ester resin particles, amino resin particles, acrylic resin particles, and styrene-butadiene-based resin particles. These may be used alone or in combination of two or more. Among these resins, in order to further improve ink leakage suppression, it is preferable that the resin contains polyvinyl butyral resin or ketone resin as an ink viscosity adjuster.

[0041] Polyvinyl butyral resin also easily forms a lubricating layer that provides a higher lubricating effect. This is because the polyvinyl butyral resin forms an elastic ink layer between the ball and the ball seat, making direct contact difficult, and therefore the writing feel is easily improved, and a higher lubricating effect is easily obtained due to the synergistic effect of the lubricating layer formed by using the polyvinyl butyral resin in combination with the compound represented by the general formula (Chemical Formula 1). Furthermore, the polyvinyl butyral resin is preferably used because the coating formed makes it easier to improve ink leakage, and when a pigment is used as a colorant, a pigment dispersion effect is also obtained, so that the polyvinyl butyral resin is preferably used. Here, the polyvinyl butyral resin is obtained by reacting polyvinyl alcohol (PVA) with butyraldehyde (BA), and has a structure having butyral groups, acetyl groups, and hydroxyl groups.

[0042] In addition, it is preferable that the polyvinyl butyral resin has a hydroxyl group content of 25 mol% or more. This is because polyvinyl butyral resins with a hydroxyl group content of less than 25 mol% do not have sufficient solubility in organic solvents, making it difficult to obtain sufficient lubrication effects and ink leakage suppression effects, and furthermore, considering the writing performance due to hygroscopicity, it is preferable to use polyvinyl butyral resins with a hydroxyl group content of 25 mol% or more. In addition, polyvinyl butyral resins with a hydroxyl group content of 30 mol% or more are preferable because they tend to improve the writing feel. This is because, during writing, frictional heat is generated by the rotation of the ball, which warms the ink at the tip of the tip and increases the temperature of the ink. However, unlike other resins, the polyvinyl butyral resin has a property that makes it difficult for the ink viscosity to decrease even when the ink temperature increases, and forms an ink layer that is always elastic between the ball and the ball seat, making it difficult for them to come into direct contact, which tends to improve the writing feel. When used in ballpoint pen ink, it is effective and preferable. In particular, it is assumed that oil-based ballpoint pens are used on copy paper, and writing pressure is higher than usual (high writing pressure writing), so it is desirable to have good high writing pressure (writing load 300 to 500 gf), so it is most effective and preferable to use it in ink for oil-based ballpoint pens. In addition, if a polyvinyl butyral resin with a hydroxyl group content of more than 40 mol% is used, the amount of moisture absorption tends to increase, which tends to affect the stability over time with the ink components, so a polyvinyl butyral resin with a hydroxyl group content of 40 mol% or less is preferable. Therefore, a polyvinyl butyral resin with a hydroxyl group content of 30 to 40 mol% is preferable, and a hydroxyl group content of 30 to 36 mol% is more preferable. The amount (mol %) of hydroxyl groups in the polyvinyl butyral resin refers to the content of hydroxyl groups (mol %) relative to the total molar amount of butyral groups (mol %), acetyl groups (mol %), and hydroxyl groups (mol %).

[0043] Regarding the average degree of polymerization of the polyvinyl butyral resin, if the average degree of polymerization is 200 or more, the ink leakage suppression performance is likely to be improved, and if the average degree of polymerization exceeds 2500, the ink viscosity tends to become too high and affect the writing feel, so the average degree of polymerization is preferably 200 to 2500. From a more detailed perspective, the average degree of polymerization is preferably 1500 or less, and from the perspective of the mutual lubricating effect with the compound represented by the general formula (Chemical Formula 1), the average degree of polymerization is preferably 200 to 1000. Here, the average degree of polymerization refers to the number of basic units constituting one molecule of the polyvinyl butyral resin, and a value measured based on the method specified in JIS K6728 (2001 edition) can be adopted.

[0044] The content of polyvinyl butyral resin is preferably 50% or more of the total resin content in the ink composition for oil-based ballpoint pens, and is preferably used as the main resin. This is because, if the content of polyvinyl butyral resin is less than 50% of the total resin content, other resins tend to inhibit the formation of an elastic ink layer, making it difficult to obtain the effect of improving the writing feel, and further, it tends to inhibit the formation of a resin coating at the tip end, making it impossible to suppress ink dripping, and further inhibiting the formation of an elastic ink layer, making it difficult to obtain the effect of improving the writing feel. Considering the tendency to further improve the writing feel and ink dripping performance, the content of polyvinyl butyral resin is preferably 70% or more of the total resin content, and preferably 90% or more.

[0045] If the content of the resin is less than 1% by mass relative to the total amount of the ink composition, the desired lubricity and ink leakage suppression performance are likely to be inferior, and if it exceeds 40% by mass, the solubility in the ink is likely to be inferior, so the content is preferably 1 to 40% by mass relative to the total amount of the ink composition.Furthermore, if the content is more than 5% by mass, it is preferable, and if it exceeds 30% by mass, the ink viscosity tends to become too high and affect the writing feel, so it is preferably 5 to 30% by mass, and more preferably 10 to 25% by mass.

[0046] In addition, as viscosity adjusters, pseudoplasticity imparting agents such as fatty acid amides and hydrogenated castor oil, colorant stabilizers, plasticizers, chelating agents, etc. may be appropriately used. These may be used alone or in combination of two or more kinds.

[0047] The ink viscosity of the ink composition for writing instruments of the present invention is not particularly limited. In the case of an oil-based ink composition, the ink viscosity is 20° C. at a shear rate of 5 sec -1 If the ink viscosity (at rest) exceeds 30,000 mPa s, the writing performance, writing feel, and ink tracking are likely to deteriorate. -1 The ink viscosity (at rest) is preferably 30,000 mPa·s or less. Also, at 20°C and a shear rate of 5 sec -1 If the ink viscosity (at rest) is less than 500 mPa·s, it is difficult to suppress ink leakage, so it is preferably 500 mPa·s or more. In consideration of further improving ink leakage suppression, writing feel, ink tracking performance, and writing start performance, the ink viscosity is more preferably 500 to 25,000 mPa·s, and more preferably 800 to 25,000 mPa·s, and further, in consideration of writing feel and writing start performance, 1000 to 20,000 mPa·s is preferable. In consideration of further improving the writing feel, increasing the ink consumption, and producing thicker handwriting, 500 to 10,000 mPa·s is preferable, and in consideration of these factors, 1000 to 5,000 mPa·s is preferable. For water-based ink composition, 20°C, shear rate 1.92 sec -1 The ink viscosity (at rest) is preferably 500 to 5000 mPa s, more preferably 500 to 3500 mPa s, and even more preferably 1000 to 3000 mPa s. The ink viscosity of the aqueous ink composition was measured using a Brookfield DV-II viscometer (CPE-42 rotor).

[0048] (Ballpoint pen) The ink composition for writing instruments according to the present invention can be applied to various ballpoint pens, but is preferably used in retractable ballpoint pens such as knock-type and rotary-type ballpoint pens. Such a ballpoint pen is provided with a housing tube containing the ink composition for writing instruments according to the present invention, and a ballpoint pen tip that rotatably holds a ball in a ball holding chamber disposed at the tip of the housing tube. The ballpoint pen tip is retractable from the tip opening of the barrel, and has a structure generally called a retractable ballpoint pen. In general, when the ink composition is used in a retractable ballpoint pen whose pen tip is not sealed, the tip tip is constantly left in the atmosphere, so that the tip tip dries out and smudges tend to occur when writing, but the use of the composition according to the present invention is preferable because such problems are improved.

[0049] (Ballpoint pen tip) In the case of a ballpoint pen, the movement amount in the vertical axis direction of the ball of the ballpoint pen tip is preferably 50 μm or less. In the case of an oil-based ballpoint pen, it is preferably 3 to 30 μm. This is because if it is less than 3 μm, it is difficult to obtain a good writing feel and suppression of handwriting smearing, and if it exceeds 30 μm, it is likely to affect ink leakage suppression, weeping smearing, and ink following performance. From a more careful consideration, it is preferable to set it to 3 to 25 μm, and more preferably, the movement amount in the vertical axis direction is 7 to 20 μm. In the case of a water-based ballpoint pen, it is preferably 15 to 50 μm. This is because if it is less than 15 μm, it is difficult to obtain a good writing feel and suppression of handwriting smearing, and if it exceeds 50 μm, it is likely to affect ink leakage suppression, weeping smearing, and ink following performance. From a more careful consideration, it is preferable to set it to 20 to 50 μm, and more preferably, the movement amount in the vertical axis direction is 25 to 45 μm. The amount of axial movement (clearance) of the ball of the ballpoint pen tip refers to the distance that the ball can move in the vertical axis direction of the ballpoint pen tip body.

[0050] The arithmetic mean roughness (Ra) of the ball surface of the ballpoint pen tip used in the present invention is preferably 0.1 to 12 nm. This is because if the arithmetic mean roughness (Ra) is less than 0.1 nm, the ink is difficult to sufficiently apply to the ball surface, it is difficult to obtain a thick handwriting during writing, and line skips and smears are likely to occur in the handwriting, and if the arithmetic mean roughness (Ra) exceeds 12 nm, the ball surface is too rough, the rotation resistance of the ball and the ball seat is large, and the ball seat is easily worn and the writing feel is easily deteriorated, and further, writing performance such as smears, line skips, and line unevenness is easily affected in the handwriting. In addition, if the arithmetic mean roughness (Ra) is 0.1 to 10 nm, it is more preferable because it improves the writing feel and makes it easier for ink to apply to the ball surface when using an ink composition such as the present invention, and 2 to 8 nm is preferable in consideration of the writing feel. The arithmetic mean roughness (Ra) of a ball surface is calculated by taking a reference length from a roughness curve measured with a surface roughness measuring device (Seiko Epson model SPI3800N) in the direction of the mean line, and adding up and averaging the absolute values ​​of the deviations from the mean line of this taken section to the measured curve.

[0051] The material used for the balls is not particularly limited, but examples include cemented carbide balls mainly composed of tungsten carbide, metal balls such as stainless steel, ceramic balls such as silicon carbide, silicon nitride, alumina, silica, and zirconia, and ruby ​​balls.

[0052] In addition, materials for ballpoint pen tips include metal materials such as stainless steel, nickel silver, brass, aluminum bronze, and aluminum, and resin materials such as polycarbonate, polyacetal, and ABS, but considering wear of the ball seat and stability over time, it is preferable to use a stainless steel tip body.

[0053] The ink consumption of the ballpoint pen per 100 m is preferably 20 to 120 mg. This is because if the ink consumption per 100 m is less than 20 mg, handwriting smears and uneven dots are likely to occur, making it difficult to obtain thick handwriting and a good writing feel, and if the ink consumption per 100 m exceeds 120 mg, the ink tracking performance is affected, ink is likely to leak from the gap between the ball and the tip end, and bleeding is also likely to occur. Taking the above effects into consideration, the ink consumption of the ballpoint pen per 100 m is preferably 25 to 100 mg, and more preferably 30 to 90 mg. Regarding ink consumption, a spiral writing test is conducted using five test samples at a writing speed of 4 m / min on JIS P3201 writing paper at a writing angle of 70° and a writing load of 200 g at 20°C. The average ink consumption per 100 m is defined as the ink consumption per 100 m.

[0054] In order to improve the darker handwriting, writing feel, ink tracking, and ink leakage prevention, it is effective to not only set the ink consumption but also to consider the relationship with the ball diameter. Specifically, the ratio of the ink consumption (mg) per 100 m of an oil-based ballpoint pen to the ball diameter (mm) (ball diameter: ink consumption) is preferably 1:40 to 1:140, which is a different relationship from the conventional one, and is therefore more likely to achieve darker handwriting, writing feel, ink tracking, and ink leakage prevention. Taking this into further consideration, it is preferable that the ratio is 1:50 to 1:130, and more preferably 1:60 to 1:120. Regarding ink consumption, a spiral writing test is conducted using five test samples at a writing speed of 4 m / min on JIS P3201 writing paper at a writing angle of 70° and a writing load of 200 g at 20°C. The average ink consumption per 100 m is defined as the ink consumption per 100 m.

[0055] (Example) The present invention will now be described with reference to examples. The ink composition for writing instruments (ink composition for oil-based ballpoint pens) of Example 1 was prepared by adding an organic solvent, a pigment, and a pigment dispersant in advance, and dispersing them with a three-roll disperser to prepare a pigment dispersion. Then, the pigment dispersion, the organic solvent, the compound (pentaerythritol polyoxyalkylene ether) in which R1 in the general formula (chemical formula 2) is a methyl group, a nonionic surfactant, polyvinylpyrrolidone, and a polyvinyl butyral resin were used, and a predetermined amount of these were weighed out, heated to 60°C, and then completely dissolved using a disperser stirrer to obtain an ink composition for writing instruments (ink composition for oil-based ballpoint pens). The specific blending amounts are as follows. In addition, the viscosity was measured using a Brookfield Viscometer RVDVII+Pro CP-52 spindle at a shear rate of 5 sec at 20°C. -1 When the ink viscosity of Example 1 was measured at a rotation speed of 2.5 rpm, the ink viscosity was 3000 mPa·s.

[0056] Example 1 <Ink composition for oil-based ballpoint pens> Pigment dispersion (20% pigment, 20% polyvinyl butyral) 50.0% by mass Alcohol solvent (benzyl alcohol) 26.5% by mass R1 in the general formula (Chemical Formula 2) is a methyl group (pentaerythritol polyoxyalkylene ether) 20.0% by mass Nonionic surfactant (sorbitan fatty acid ester) 2.0% by mass Polyvinylpyrrolidone 0.5% by mass Polyvinyl butyral resin 1.0% by mass

[0057] Testing and Evaluation The ink compositions for oil-based ballpoint pens prepared in Examples 1 to 21 and Comparative Examples 1 to 3 were used to prepare an oil-based ballpoint pen. A ballpoint pen tip (having a coil spring in the tip that presses the ball directly against the inner wall of the tip end edge, axial movement of the ball: 12 μm) was attached to the tip of an ink holder (made of polypropylene) and a ball (φ0.7 mm, arithmetic mean roughness (Ra) of the ball surface) was rotatably held therein. The ink for oil-based ballpoint pens (0.2 g) of Example 1 was directly placed in the ink holder. The ballpoint pen refill was then placed in an oil-based ballpoint pen (product name: Acroball (registered trademark)) manufactured by Pilot Corporation to prepare an oil-based ballpoint pen. The following tests and evaluations were carried out using JIS P3201 writing paper as the writing test paper. The initial ink consumption per 100 m of Example 1 and Example 3 was 70 mg / 100 m and 75 mg / 100 m, respectively, when a spiral writing test was performed using an oil-based ballpoint pen.

[0058] Examples 2 to 21 As shown in the table, except for changing each component, inks were formulated in the same manner as in Example 1 to obtain ink compositions for writing instruments (ink compositions for oil-based ballpoint pens) of Examples 2 to 21. The evaluation results are shown in the table. The ink viscosity of Example 3 was measured using a Brookfield Viscometer RVDVII+Pro CP-52 spindle at a shear rate of 5 sec at a temperature of 20°C. -1 (Rotation speed 2.5 rpm), Example 3: Ink viscosity = 2000 mPa·s.

[0059] Comparative Examples 1 to 3 As shown in the table, except for changing each component, ink compositions for writing instruments (ink compositions for oil-based ballpoint pens) of Comparative Examples 1 to 3 were obtained in the same manner as in Example 1. The evaluation results are shown in the table.

[0060] Example 101 <Water-based ballpoint pen ink composition> As colorants, pigment dispersion, water, polyhydric alcohol, a compound in which R1 in the general formula (chemical formula 2) is a methyl group (pentaerythritol polyoxyalkylene ether), organic resin particles, stabilizer, phosphate ester surfactant, and rust inhibitor were used, and a predetermined amount of each was weighed out and heated to 60°C, and then completely dissolved using a dispersing stirrer to prepare a base ink. Thereafter, while heating the base ink prepared above, a shear thinning agent was added and thoroughly mixed and stirred using a homogenizer stirrer until it became uniform, thereby obtaining an aqueous ballpoint pen ink composition of Example 1. The specific blending amounts are as follows. The ink viscosity of Example 101 was measured at a shear rate of 1.92 sec at 20°C using a Brookfield DV-II viscometer (CPE-42 rotor). -1 When the ink viscosity was measured under the condition of rotation speed of 0.5 rpm, it was 1600 mPa·s.

[0061] Pigment dispersion (colored resin particles, solid content 34%) 20.0% by mass Water 66.2% by mass Polyhydric alcohol (glycerin) 10.0% by mass R1 in the general formula (Chemical Formula 2) is a methyl group (pentaerythritol polyoxyalkylene ether) 3.0% by mass Organic resin particles (olefin resin) 1.0% by mass Stabilizer (triethanolamine) 2.0% by mass Phosphate ester surfactant (HLB value: 11.5) 1.0% by mass Rust inhibitor (benzotriazole) 0.5% by mass Shear thinning agent (succinoglycan) 0.3% by mass

[0062] <Example 102> An aqueous ballpoint pen ink composition was obtained in the same manner as in Example 101, except that the amount of R1 in the general formula (Chemical Formula 2) added was changed to 5% methyl group (pentaerythritol polyoxyalkylene ether) and the amount of water was reduced accordingly.

[0063] The aqueous ballpoint pen ink compositions (1.0 g) prepared in Examples 101 and 102 were filled into ballpoint pen refills equipped with ballpoint pen tips (having a coil spring in the tip that presses the ball directly against the inner wall of the tip end edge, ball movement in the vertical axis direction: 30 μm, arithmetic mean roughness (Ra): 1 nm) that rotatably hold a ball with a ball diameter of φ0.7 mm in an ink storage tube (polypropylene) to prepare ballpoint pens. The following tests and evaluations were carried out using JIS P3201 writing paper as the writing test paper. [Table 1] [Table 2]

[0064] Abrasion resistance test (wear test of ball seat): Wear of the ball seat after the writing test was measured using a running test machine with a load of 400gf, a writing angle of 70°, and a speed of 4m / min. Ball seat wear is less than 5μm...◎ Ball seat wear is 5μm or more and less than 10μm. The wear of the ball seat is between 10μm and 20μm, but writing is possible. The ball seat is badly worn, causing poor writing.

[0065] Writing feel: Evaluation was performed by a sensory test using handwriting. Very smooth...◎ Something that is smooth Smoothness at a level that does not cause any problems in practical use... △ Heavy objects ×

[0066] Writing performance test: After handwriting, the pen was left in an environment of 20°C and 65% RH for 24 hours with the tip extended, and then a running test was performed under the writing conditions listed below, and the length of the smudged handwriting at the start of writing was measured. <Writing conditions> The pen was evaluated by writing a straight line using a running test machine under the following conditions: writing load 200gf, writing angle 70°, writing speed 4m / min. The length of the smudged handwriting is less than 5mm. The length of the smudged handwriting is 5mm or more but less than 10mm. The length of the smudged handwriting is 10mm or more but less than 20mm...△ The length of the smudged handwriting is 20mm or more. ×

[0067] Ink tracking performance test: After one month in a 50°C environment, continuous, rapid handwriting was performed for 10 seconds. No smudges or skipped lines...◎ There was some smudged writing or skipped lines, but it was not a problem for practical use. Those with smudged handwriting or skipped lines...△ The handwriting was smudged and the lines were skipped... ×

[0068] In Examples 1 to 21 (oil-based ballpoint pens), good performance was obtained in the abrasion resistance test (abrasion test of the ball seat), writing feel, writing start performance test, and ink following performance test. In Examples 1 to 21 and 101 to 102, the ink compositions for writing instruments containing a pigment as a colorant had good pigment dispersibility and were stable. For Examples 101 to 102 (water-based ballpoint pens), abrasion resistance tests (load 100 gf, writing angle 70°, writing speed 4 m / min), writing feel and writing start performance tests (load 100 gf, writing angle 70°, writing speed 4 m / min), and ink following performance tests were conducted, and good performance was obtained in each test.

[0069] In addition, as Example 22, an oil-based ballpoint pen was produced using the writing instrument ink composition (ink composition for oil-based ballpoint pens) of Example 1, but with a ball (φ0.7 mm, arithmetic mean roughness (Ra): 2 nm) changed to an oil-based ballpoint pen. As Example 23, an oil-based ballpoint pen was produced using the writing instrument ink composition (ink composition for oil-based ballpoint pens) of Example 1, but with a ball (φ0.7 mm, arithmetic mean roughness (Ra): 3 nm) changed to an oil-based ballpoint pen. As Example 24, a ballpoint pen tip (a ball was directly inserted into the tip) was produced using the writing instrument ink composition (ink composition for oil-based ballpoint pens) of Example 1. As Example 25, an oil-based ballpoint pen modified to have a ballpoint pen tip (having a coil spring within the tip that presses the ball directly against the inner wall of the tip edge, axial movement of the ball: 7 μm) was tested and evaluated using the ink composition for writing instruments (ink composition for oil-based ballpoint pens) of Example 1.As a result, good performance was obtained in the abrasion resistance test (abrasion test of the ball seat), writing feel, writing performance test, and ink following performance test, as in Example 1.

[0070] In Comparative Examples 1 to 3, since the compound represented by the general formula (Chemical Formula 1) was not used, the abrasion resistance test (ball seat abrasion test) was poor, and further the ink followability test was poor.

[0071] In addition, when using a retractable writing instrument such as a knock-type writing instrument or a rotary-type writing instrument, writing performance is one of the important performance characteristics, so it is effective to use an ink composition such as that of the present invention.

[0072] In addition, in this embodiment, a writing instrument (oil-based ballpoint pen) in which a ballpoint pen refill containing an ink composition for a writing instrument (ink composition for an oil-based ballpoint pen) in an ink containing tube is disposed in a barrel has been exemplified, but the writing instrument (oil-based ballpoint pen) of the present invention may be a direct-loading type writing instrument (ballpoint pen) in which the barrel itself is the ink containing tube and the ink composition for a writing instrument (ink composition for an oil-based ballpoint pen) is directly contained in the barrel, or may have a structure in which an ink composition for a writing instrument (ink composition for an oil-based ballpoint pen) contained in an ink containing tube (ballpoint pen refill) is used as it is as a writing instrument (ballpoint pen). [Industrial Applicability]

[0073] The present invention can be used as an oil-based ink composition for a writing instrument and a water-based ink composition for a writing instrument. More specifically, the present invention can be widely used as a cap-type, knock-type or other writing instrument filled with the ink composition for a writing instrument, such as a ballpoint pen, a marking pen or a felt-tip pen.

Claims

1. An ink composition for an oil-based ballpoint pen, comprising a colorant, an organic solvent, and a compound represented by the general formula (Chemical Formula 1). [Formula 1]

2. The ink composition for oil-based ballpoint pens according to claim 1, characterized in that the hydroxyl value (mgKOH / g) of the general formula (Chemical Formula 1) is 100 to 1000 (mgKOH / g).

3. 3. The ink composition for an oil-based ballpoint pen according to claim 1, further comprising a polyvinyl butyral resin or a ketone resin.

4. 4. The ink composition for an oil-based ballpoint pen according to claim 1, further comprising a nonionic surfactant.

5. 5. The ink composition for an oil-based ballpoint pen according to claim 1, further comprising a phosphate ester surfactant or a fatty acid.

6. 20℃, shear rate 5sec -1 6. The ink composition for oil-based ballpoint pens according to claim 1, wherein the ink viscosity at 2000 g / ml is 30,000 mPa·s or less.

7. 7. An oil-based ballpoint pen, comprising an ink holder having a ballpoint pen tip at the tip of the ink holder that rotatably holds a ball, and an ink composition for an oil-based ballpoint pen according to claim 1 contained in the ink holder.

Citation Information

Patent Citations

  • Water-base pigment ink composition for ball-point pen

    JP1993186730A

  • Aqueous ink composition for ball-point pen

    JP1996302267A

  • Oil-base ink for ball-point pen

    JP1998204368A

  • Ink composition for oil base ball point pen and oil base ball point pen using the ink

    JP2004115611A

  • Water-based ballpoint pen

    JP2004291632A