n-TYPE GaN CRYSTAL, GaN WAFER, AND GaN CRYSTAL, GaN WAFER AND NITRIDE SEMICONDUCTOR DEVICE PRODUCTION METHOD

Optimized n-type GaN crystals and wafers with controlled impurity concentrations and orientations address the quality issues in existing GaN growth methods, resulting in higher-quality nitride semiconductor devices with reduced manufacturing costs.

JP2024161234AActive Publication Date: 2024-11-15MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024153026
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-04-22
Filing Date
2024-09-05
Publication Date
2024-11-15
Estimated Expiration
2039-07-24

AI Technical Summary

Technical Problem

Existing methods for growing GaN crystals, particularly those doped with silicon or germanium, suffer from high full width at half maximum (FWHM) values in X-ray diffraction rocking curves, which affect the quality and efficiency of nitride semiconductor devices.

Method used

The development of n-type GaN crystals and wafers with specific impurity concentrations and orientations, such as Ge-doped GaN with resistivity below 0.03 Ω cm and (004) XRD rocking curve FWHM less than 20 arcsec, optimized for HVPE growth, to enhance crystal quality and reduce manufacturing costs.

Benefits of technology

The improved GaN crystals and wafers achieve reduced FWHM values, leading to higher quality nitride semiconductor devices with lower dislocation densities and enhanced electrical properties, thereby promoting cost-effective production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161234000001_ABST
    Figure 2024161234000001_ABST
Patent Text Reader

Abstract

To fulfill the following demand: if GaN crystals having a (004) XRD rocking curve FWHM of 20 arcsec or less, which is equivalent to that of GaN crystals grown by the ammonothermal method, can be grown by HVPE with high productivity, it is expected to contribute to promoting the development of nitride semiconductor devices produced using c-plane GaN wafers as substrates and a reduction in cost.SOLUTION: In this n-type GaN crystal, the donor dopant contained at the highest concentration is Ge. The n-type GaN crystal has a resistivity at room temperature of less than 0.03 Ω cm and has a (004) XRD rocking curve FWHM of less than 20 arcsec. The n-type GaN crystal has two principal surfaces each having an area of 3 cm2 or more, and one of the surfaces has Ga polarity and is inclined at an angle of 0 to 10 degrees relative to the (0001) crystal plane. Additionally, the n-type GaN crystal has a diameter of 20 mm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention primarily relates to n-type GaN crystals, GaN wafers, and methods for producing GaN crystals, GaN wafers, and nitride semiconductor devices. [Background technology]

[0002] GaN (gallium nitride) is a type of III-V compound semiconductor and has a wurtzite crystal structure belonging to the hexagonal crystal system. Representative growth techniques for bulk GaN crystals include HVPE (Hydride Vapor Phase Epitaxy), high pressure solution growth, ammonothermal, and Na flux methods (Non-Patent Document 1). HVPE has a significantly higher growth rate for GaN crystals than other techniques, and almost all GaN wafers currently on the market are grown by HVPE.

[0003] It has been reported that GaN crystals were grown by HVPE on a 1-inch diameter c-plane GaN seed wafer grown by the ammonothermal method, and then a c-plane GaN wafer with a diameter of 18 mm was cut from the GaN crystal (Non-Patent Document 2). It has been reported that GaN crystals were grown by HVPE on a c-plane GaN seed wafer grown by the ammonothermal method, and then GaN crystals doped with Si (silicon) were grown by HVPE on a c-plane seed wafer cut from the HVPE-grown GaN crystal (Non-Patent Document 3). The (002) XRD rocking curve FWHM of the Si-doped GaN crystal was reported to be 32 arcsec. It has been reported that GaN crystals doped with Ge (germanium) were grown by HVPE on a c-plane GaN seed wafer grown by the ammonothermal method (Non-Patent Document 4). The (002) XRD rocking curve FWHM of the Ge-doped GaN crystal was reported to be 67 arcsec.

[0004] It has been reported that a 5.6 mm thick GaN crystal was grown by HVPE on an m-plane GaN seed wafer grown by the acidic ammonothermal method, and a 2-inch diameter m-plane GaN wafer was cut out from the HVPE-grown GaN crystal (Non-Patent Document 5). A (200) XRD rocking curve FWHM of 13 arcsec was obtained at the center of the 2-inch HVPE wafer. A conductive c-plane GaN wafer is known, which is made of GaN crystals grown by the acidic ammonothermal method using NH4F (ammonium fluoride) and NH4I (ammonium iodide) as mineralizers, and has a (004) XRD rocking curve FWHM of approximately 10 arcsec (Patent Document 1). The above-mentioned XRD stands for X-Ray Diffraction, and FWHM stands for Full Width at Half Maximum. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO2018 / 030311A1 [Non-patent literature]

[0006] [Non-Patent Document 1] H. Amano, Japanese Journal of Applied Physics 52 (2013) 050001 [Non-Patent Document 2] JZ Domagala, et al., Journal of Crystal Growth 456 (2016) 80 [Non-Patent Document 3] M. Iwinska, et al., Journal of Crystal Growth 456 (2016) 91 [Non-Patent Document 4] M. Iwinska, et al., Journal of Crystal Growth 480 (2017) 102 [Non-Patent Document 5] Y. Tsukada, et al., Japanese Journal of Applied Physics 55 (2016) 05FC01 Summary of the Invention [Problem to be solved by the invention]

[0007] The inventors believed that if GaN crystals having a (004) XRD rocking curve FWHM of 20 arcsec or less, comparable to that of GaN crystals grown by the ammonothermal method, could be grown by HVPE, which has excellent mass productivity, it would contribute to promoting the development and reducing the cost of nitride semiconductor devices produced using c-plane GaN wafers as substrates. [Means for solving the problem]

[0008] The present invention relates to an n-type GaN crystal in one aspect, to a GaN wafer in another aspect, to a method for manufacturing a GaN wafer in yet another aspect, to a method for manufacturing an epitaxial wafer in yet another aspect, to an epitaxial wafer in yet another aspect, to a method for manufacturing a nitride semiconductor device, and to a method for manufacturing bulk GaN crystal in yet another aspect.

[0009] The embodiments of the present invention include, but are not limited to, the following [A1] to [A26]. [A1] An n-type GaN crystal characterized in that the donor impurity contained at the highest concentration is Ge, that it has a room temperature resistivity of less than 0.03 Ω cm, and that the (004) XRD rocking curve FWHM is less than 20 arcsec, less than 18 arcsec, less than 16 arcsec, less than 14 arcsec, or less than 12 arcsec. [A2] The n-type GaN crystal according to [A1] above, wherein the crystal has two principal surfaces facing in opposite directions, and each of the two principal surfaces has an area of ​​3 cm 2The n-type GaN crystal has the above structure, and one of the two main surfaces has Ga polarity and is inclined at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane. [A3] The n-type GaN crystal according to [A2] above, having a diameter of 20 mm or more, 45 mm or more, 95 mm or more, or 145 mm or more. [A4] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, the n-type GaN crystal being characterized in that the donor impurity contained at the highest concentration is Ge, the n-type GaN crystal has a room temperature resistivity of less than 0.03 Ω cm, and when a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less. [A5] The n-type GaN crystal according to [A4], wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [A6] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, the n-type GaN crystal being characterized in that the donor impurity contained at the highest concentration is Ge, the n-type GaN crystal has a room temperature resistivity of less than 0.03 Ω cm, and when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less. [A7] The average value of the (004) XRD rocking curve FWHM between all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 1 The n-type GaN crystal according to [A6] above, which has a thickness of 2 arcsec or less or 10 arcsec or less. [A8] An n-type GaN crystal according to any one of [A2] to [A7] above, which has a room temperature resistivity of less than 0.02 Ω·cm, less than 0.015 Ω·cm, or less than 0.010 Ω·cm. [A9] Carrier concentration is 1×10 18 cm -3 That's it, 2 x 10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The n-type GaN crystal according to any one of the above [A2] to [A7]. [A10] An n-type GaN crystal according to any one of the above [A2] to [A9], which satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [A11] An n-type GaN crystal according to the above [A10], which satisfies all of the above conditions (a) to (c) regarding impurity concentrations. [A12] O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The n-type GaN crystal according to any one of the above [A2] to [A11], which is as follows: [A13] Ge concentration is 1×10 18 atoms / cm 3 or more, and Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to any one of the above [A2] to [A12]. [A14] The concentration of each impurity except for Ge, Si, O and H is 5×10 15atoms / cm 3 An n-type GaN crystal according to any one of the above [A2] to [A13], which is: [A15] An n-type GaN crystal according to any one of the above [A2] to [A14], which is a GaN crystal grown by HVPE. [A16] A GaN wafer made of an n-type GaN crystal according to any one of the above [A2] to [A15]. [A17] A GaN wafer, comprising a first region made of an n-type GaN crystal according to any one of [A2] to [A15] above, provided on a Ga-polarity side, and a second region having a carrier concentration lower than that of the n-type GaN crystal, provided on an N-polarity side. [A18] The GaN wafer according to [A17], wherein the first region has a thickness of 5 μm or more and 250 μm or less. [A19] The GaN wafer according to [A17] or [A18], wherein the second region satisfies one or more conditions selected from the following (a) to (c) regarding an impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [A20] The GaN wafer according to [A19], wherein the second region satisfies all of the conditions (a) to (c) regarding impurity concentrations. [A21] The O concentration in the second region is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The GaN wafer according to any one of the above [A17] to [A20], which is as follows: [A22] In the second region, the concentration of each impurity other than Si, O and H is 5×10 15 atoms / cm 3The GaN wafer according to any one of the above [A17] to [A21], which is as follows: [A23] The GaN wafer according to any one of [A17] to [A22] above, which has a regrowth interface between the first region and the second region. [A24] A method for producing an epitaxial wafer, comprising the steps of: preparing a GaN wafer according to any one of [A16] to [A23] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer. [A25] A GaN wafer according to any one of [A16] to [A23] above, An epitaxial wafer comprising one or more nitride semiconductor layers epitaxially grown on a substrate. [A26] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a GaN wafer according to any one of [A16] to [A23] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

[0010] Further embodiments of the present invention include the following [B1] to [B29]. [B1] An n-type GaN crystal having a room temperature resistivity of less than 0.03 Ω cm, a (004) XRD rocking curve FWHM of less than 20 arcsec, and an impurity concentration satisfying one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [B2] The n-type GaN crystal according to [B1] above, wherein the crystal has two principal surfaces facing in opposite directions, and each of the two principal surfaces has an area of ​​3 cm 2 The n-type GaN crystal has the above structure, and one of the two main surfaces has Ga polarity and is inclined at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane. [B3] The n-type GaN crystal according to [B2] above, having a diameter of 20 mm or more, 45 mm or more, 95 mm or more, or 145 mm or more. [B4] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that it has a room temperature resistivity of less than 0.03 Ω cm, that when a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM between all measurement points is 20 arcsec or less, and that, regarding the impurity concentration, it satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [B5] The n-type GaN crystal according to [B4], wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, or 12 arcsec or less. [B6] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that it has a room temperature resistivity of less than 0.03 Ω cm, that when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less, and that, regarding the impurity concentration, it satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×1016 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [B7] The n-type GaN crystal according to [B6], wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, or 12 arcsec or less. [B8] An n-type GaN crystal according to any one of [B2] to [B7] above, which has a room temperature resistivity of less than 0.02 Ω·cm, less than 0.015 Ω·cm, or less than 0.010 Ω·cm. [B9] Carrier concentration is 1×10 18 cm -3 or more or 2×10 18 cm -3 The n-type GaN crystal according to any one of the above items [B2] to [B7]. [B10] An n-type GaN crystal according to any one of the above [B2] to [B9], which satisfies all of the above conditions (a) to (c) regarding impurity concentration. [B11]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The n-type GaN crystal according to any one of the above [B2] to [B10], which is as follows: [B12] The n-type GaN crystal according to any one of the above [B2] to [B11], wherein the donor impurity contained at the highest concentration is Si. [B13] The n-type GaN crystal according to the above [B12], wherein the total concentration of donor impurities excluding Si is 10% or less, 5% or less, or 1% or less of the Si concentration. [B14] The n-type GaN crystal according to [B13] above, wherein the carrier concentration is 90% or more of the Si concentration. [B15] The concentration of each impurity except for Si, O and H is 5×10 15 atoms / cm 3 An n-type GaN crystal according to any one of the above [B2] to [B14], which is: [B16] Ge concentration is 1×10 18 atoms / cm 3 or more, and Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to any one of the above [B2] to [B12]. [B17] The concentration of each impurity except for Ge, Si, O and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to the above [B16], which is as follows: [B18] An n-type GaN crystal according to any one of the above [B2] to [B17], which is a GaN crystal grown by HVPE. [B19] A GaN wafer made of an n-type GaN crystal according to any one of the above [B2] to [B18]. [B20] A GaN wafer, in which a first region made of an n-type GaN crystal according to any one of [B2] to [B18] above is provided on a Ga-polarity side, and a second region having a carrier concentration lower than that of the n-type GaN crystal is provided on an N-polarity side. [B21] The GaN wafer according to [B20], wherein the first region has a thickness of 5 μm or more and 250 μm or less. [B22] The GaN wafer according to [B20] or [B21], wherein the second region satisfies one or more conditions selected from the following (a) to (c) regarding an impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [B23] The GaN wafer according to [B22], wherein the second region satisfies all of the conditions (a) to (c) regarding impurity concentrations. [B24] The O concentration in the second region is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The GaN wafer according to any one of the above [B20] to [B23], which is as follows: [B25] In the second region, the concentration of each impurity other than Si, O and H is 5×10 15 atoms / cm 3 The GaN wafer according to any one of the above [B20] to [B24], which is as follows: [B26] A GaN wafer according to any one of [B20] to [B25] above, which has a regrowth interface between the first region and the second region. [B27] A method for producing an epitaxial wafer, comprising the steps of: preparing a GaN wafer according to any one of [B19] to [B26] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer. [B28] An epitaxial wafer comprising the GaN wafer according to any one of the above [B19] to [B26] and one or more nitride semiconductor layers epitaxially grown on the GaN wafer. [B29] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a GaN wafer according to any one of [B19] to [B26] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

[0011] Further embodiments of the present invention include the following [C1] to [C44]. [C1] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that the n-type GaN crystal has a diameter of 45 mm or more, a (004) XRD rocking curve FWHM of less than 20 arcsec, less than 18 arcsec, less than 16 arcsec, less than 14 arcsec, or less than 12 arcsec, and satisfies one or more conditions selected from the following (a) to (c) regarding the impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [C2] The n-type GaN crystal according to [C1] above, having a diameter of 95 mm or more or 145 mm or more. [C3] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that, when a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM between all measurement points is 20 arcsec or less, and the impurity concentration satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [C4] The n-type GaN crystal according to [C3], wherein an average value of the (004) XRD rocking curve FWHM between all of the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [C5] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that, when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the principal surfaces, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less, and the impurity concentration satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [C6] The n-type GaN crystal according to [C5], wherein the average value of the (004) XRD rocking curve FWHM between all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [C7] An n-type GaN crystal according to any one of [C1] to [C6] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentration. [C8] Si concentration is 5×10 17 atoms / cm 3 The n-type GaN crystal according to any one of the above [C1] to [C7], which is as follows: [C9] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3The n-type GaN crystal according to any one of the above [C1] to [C8], which is: [C10]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The n-type GaN crystal according to any one of the above [C1] to [C9], which is as follows: [C11]5×10 17 cm -3 The n-type GaN crystal according to any one of [C1] to [C10] above, having at least one of a carrier concentration of less than 0.05 and a room temperature resistivity of 0.04 Ω·cm or more. [C12] The n-type GaN crystal according to any one of [C1] to [C11] above, which is a GaN crystal grown by HVPE. [C13] A GaN wafer made of an n-type GaN crystal according to any one of [C1] to [C12] above. [C14] A semiconductor device comprising: a back layer made of an n-type GaN crystal according to any one of [C1] to [C12] above; and a front layer made of GaN and having a minimum thickness of 20 μm or more formed on a Ga-polarity main surface of the n-type GaN crystal via a regrowth interface, wherein at least a portion of the front layer within a distance of 5 μm from the top surface is included in a high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 This is the area of ​​double-layer GaN wafers. [C15] The bilayer GaN wafer according to [C14], wherein at least a portion within 20 μm from the top surface of the front layer is included in the high carrier concentration region. [C16] The high carrier concentration region has a lower limit of the carrier concentration of 2×10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The bi-layer GaN wafer according to [C14] or [C15] above, which is in the above region. [C17] The bi-layer GaN wafer according to any one of [C14] to [C16], wherein the front layer satisfies one or more conditions selected from the following (a) to (c) regarding an impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [C18] The bi-layer GaN wafer according to [C17], wherein the front layer satisfies all of the conditions (a) to (c) regarding impurity concentrations. [C19] The O concentration in the front layer is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The bi-layer GaN wafer according to any one of [C14] to [C18] above, which is: [C20] The bi-layer GaN wafer according to any one of [C14] to [C19] above, wherein the high carrier concentration region is doped with Si. [C21] The concentration of each impurity in the front layer, except for Si, O, and H, is 5×10 15 atoms / cm 3 The bi-layer GaN wafer according to [C20] above, which is as follows: [C22] The bi-layer GaN wafer according to any one of [C14] to [C20] above, wherein the high carrier concentration region is doped with Ge. [C23] The concentration of each impurity in the front layer, except for Ge, Si, O, and H, is 5×10 15 atoms / cm 3 The bi-layer GaN wafer according to [C22] above, which is as follows: [C24] A bi-layer GaN wafer according to any one of [C14] to [C23] above, wherein in the high carrier concentration region, the variation in carrier concentration or total concentration of donor impurities along the c-axis direction is within ±25%, ±20%, ±15%, or ±10% of the median. [C25] A bi-layer GaN wafer comprising a back layer made of an n-type GaN crystal according to any one of [C1] to [C12] above, and a front layer made of GaN and having a minimum thickness of 20 μm or more, formed on a Ga-polarity main surface of the n-type GaN crystal via a regrowth interface, wherein at least a portion of the front layer within a distance of 5 μm from the top surface is included in a carrier compensation region, and the carrier compensation region has a lower limit of a total compensation impurity concentration of 1×10 17 atoms / cm 3 This is the area of ​​double-layer GaN wafers. [C26] The bilayer GaN wafer according to [C25], wherein at least a portion of the front layer within 20 μm from the top surface is included in the carrier compensation region. [C27] The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 That's it, 5 x 10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3 or more than 5×10 18 atoms / cm 3 The bi-layer GaN wafer according to [C25] or [C26] above, [C28] The front layer has an impurity concentration selected from one or more of the following (a) to (c): The bi-layer GaN wafer according to any one of [C25] to [C27] above, which satisfies the following condition: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3The following is the result. [C29] The bilayer GaN wafer according to any one of [C25] to [C28], wherein in the carrier compensation region, the variation in the total concentration of compensation impurities along the c-axis direction is within ±25%, ±20%, ±15%, or ±10% of the median. [C30] The bi-layer GaN wafer according to any one of [C14] to [C29] above, wherein the bi-layer GaN wafer has a thickness greater than 300 μm, and the maximum thickness of the front layer is 300 μm or less, 250 μm or less, or 200 μm or less. [C31] The bi-layer GaN wafer according to any one of [C14] to [C30] above, wherein the minimum thickness of the front layer is 50 μm or more, 75 μm or more, or 100 μm or more. [C32] The bi-layer GaN wafer according to any one of [C14] to [C31] above, wherein the difference between the maximum thickness and the minimum thickness of the front layer is 200 μm or less, 100 μm or less, 50 μm or less, 25 μm or less, or 10 μm or less. [C33] A method for producing an epitaxial wafer, comprising the steps of: preparing a wafer according to any one of [C13] to [C32]; and epitaxially growing one or more nitride semiconductor layers on the prepared wafer. [C34] An epitaxial wafer comprising the wafer according to any one of [C13] to [C32] above, and one or more nitride semiconductor layers epitaxially grown on the GaN wafer. [C35] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a wafer according to any one of [C13] to [C32]; and epitaxially growing one or more nitride semiconductor layers on the prepared wafer. [C36] A method for producing a GaN wafer according to [C13], comprising the steps of: preparing a GaN wafer according to [C13]; and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga-polarity main surface of the prepared GaN wafer, the GaN layer having a high carrier concentration region or a carrier compensation region, the high carrier concentration region having a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×1017 atoms / cm 3 The above is the manufacturing method for double-layer GaN wafers. [C37] The manufacturing method according to [C36], wherein in the epitaxial growth step, the GaN layer is grown by HVPE. [C38] The manufacturing method according to [C36] or [C37], wherein the GaN layer has a thickness of 500 μm or less. [C39] The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The manufacturing method according to any one of [C36] to [C38] above, which is in the above range. [C40] The manufacturing method according to any one of [C36] to [C39], wherein the GaN layer is provided with the high carrier concentration, and the high carrier concentration region is doped with Ge. [C41] The manufacturing method according to any one of [C36] to [C40] above, wherein the GaN layer is provided with the high carrier concentration, and the high carrier concentration region is intentionally doped with Si. [C42] The GaN layer is provided with the carrier compensation region, and the carrier compensation region has a lower limit of a total concentration of compensation impurities of 5×10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3 or more than 5×10 18 atoms / cm 3 The manufacturing method according to any one of [C36] to [C38] above, which is in the above range. [C43] The manufacturing method according to any one of [C36] to [C42] above, further comprising a step of thinning the stack obtained in the epitaxial growth step. [C44] A method for producing a bulk GaN crystal, comprising the steps of preparing the GaN wafer according to [C13] above, and epitaxially growing GaN on the prepared GaN wafer.

[0012] Further embodiments of the present invention include the following [D1] to [D19]. [D1] A c-plane GaN wafer characterized in that the donor impurity contained at the highest concentration is Ge, the conductivity type is n-type, the room temperature resistivity is less than 0.03 Ω cm, and the (004) XRD rocking curve FWHM is less than 20 arcsec, less than 18 arcsec, less than 16 arcsec, less than 14 arcsec, or less than 12 arcsec. [D2] Area 3cm 2 The c-plane GaN wafer according to [D1] above, comprising the above primary surface. [D3] The c-plane GaN wafer according to [D1] above, having a diameter of 20 mm or more, 45 mm or more, 95 mm or more, or 145 mm or more. [D4] A c-plane GaN wafer, characterized in that the donor impurity contained at the highest concentration is Ge, the conductivity type is n-type, and the room temperature resistivity is less than 0.03 Ω cm, and when the (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one main surface, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less. [D5] The c-plane GaN wafer according to [D4], wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [D6] A c-plane GaN wafer, characterized in that the donor impurity contained at the highest concentration is Ge, the conductivity type is n-type, and the room temperature resistivity is less than 0.03 Ω cm, and when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one main surface, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less. [D7] The c-plane GaN wafer according to [D6], wherein an average value of the (004) XRD rocking curve FWHM between all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [D8] The c-plane GaN wafer according to any one of [D1] to [D7] above, wherein the variation width of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x direction, and the variation width of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are 0.15 degrees or less, 0.1 degrees or less, or 0.08 degrees or less, respectively, within a 40 mm long section. [D9] The c-plane GaN wafer according to any one of [D1] to [D8] above, having a room temperature resistivity of less than 0.02 Ω cm, less than 0.015 Ω cm, or less than 0.010 Ω cm. [D10] A c-plane GaN wafer having a carrier concentration of 1×10 18 cm -3 That's it, 2 x 10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The c-plane GaN wafer according to any one of the above [D1] to [D8]. [D11] A c-plane GaN wafer according to any one of [D1] to [D10] above, which satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [D12] The c-plane GaN wafer according to [D11] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentrations. [D13]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The above [D1] to [D12] are as follows: 2. The c-plane GaN wafer according to claim 1 . [D14] Ge concentration is 1×10 18 atoms / cm 3 or more, and Si concentration is 4×10 17 atoms / cm 3 The c-plane GaN wafer according to any one of the above [D1] to [D13]. [D15] The concentration of each impurity except for Ge, Si, O and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to any one of the above [D1] to [D14], which is as follows: [D16] The c-plane GaN wafer according to any one of [D1] to [D15] above, which is made of a GaN crystal grown by HVPE. [D17] A method for manufacturing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of [D1] to [D16] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer. [D18] An epitaxial wafer comprising the GaN wafer according to any one of [D1] to [D16] above, and one or more nitride semiconductor layers epitaxially grown on the GaN wafer. [D19] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a GaN wafer according to any one of [D1] to [D16] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

[0013] Further embodiments of the present invention include the following [E1] to [E20]. [E1] A c-plane GaN wafer, characterized in that it has an n-type conductivity and a room temperature resistivity of less than 0.03 Ω cm, a (004) XRD rocking curve FWHM of less than 20 arcsec, and an impurity concentration that satisfies one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [E2] Area 3cm 2 The c-plane GaN wafer according to [E1] above, comprising the above primary surface. [E3] The c-plane GaN wafer according to [E1] above, having a diameter of 20 mm or more, 45 mm or more, 95 mm or more, or 145 mm or more. [E4] A c-plane GaN wafer having an n-type conductivity and a room temperature resistivity of less than 0.03 Ω cm, a maximum value of the (004) XRD rocking curve FWHM between all measurement points being 20 arcsec or less when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least one line on one main surface, and an impurity concentration satisfying one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [E5] The c-plane GaN wafer according to [E4], wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, or 12 arcsec or less. [E6] A c-plane GaN wafer, characterized in that it has an n-type conductivity and a room temperature resistivity of less than 0.03 Ω cm, that when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one main surface, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less, and that, regarding impurity concentration, it satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [E7] The c-plane GaN wafer according to [E6], wherein an average value of (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, or 12 arcsec or less. [E8] The c-plane GaN wafer according to any one of [E1] to [E7] above, wherein the variation width of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x direction, and the variation width of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are 0.15 degrees or less, 0.1 degrees or less, or 0.08 degrees or less, respectively, within a 40 mm long section. [E9] The c-plane GaN wafer according to any one of [E1] to [E8] above, having a room temperature resistivity of less than 0.02 Ω cm, less than 0.015 Ω cm, or less than 0.010 Ω cm. [E10] A c-plane GaN wafer having a carrier concentration of 1×10 18 cm -3 or more or 2×10 18 cm -3 The c-plane GaN wafer according to any one of the above items [E1] to [E8]. [E11] The c-plane GaN wafer according to any one of [E1] to [E10] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentrations. [E12]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The c-plane GaN wafer according to any one of the above [E1] to [E11], which is as follows: [E13] The c-plane GaN wafer according to any one of the above [E1] to [E12], wherein the donor impurity contained at the highest concentration is Si. [E14] The c-plane GaN wafer according to [E13] above, wherein a total concentration of donor impurities excluding Si is 10% or less, 5% or less, or 1% or less of the Si concentration. [E15] The c-plane GaN wafer according to [E14] above, wherein the carrier concentration is 90% or more of the Si concentration. [E16] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to any one of the above [E1] to [E15], which is as follows: [E17] The c-plane GaN wafer according to any one of [E1] to [E16], which is made of a GaN crystal grown by HVPE. [E18] A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of [E1] to [E17] above; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer. [E19] An epitaxial wafer comprising the c-plane GaN wafer according to any one of [E1] to [E17] above, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer. [E20] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a c-plane GaN wafer according to any one of [E1] to [E17] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

[0014] The embodiments of the present invention further include the following [F1] to [F25]. [F1] A c-plane GaN wafer characterized by having an n-type conductivity, a diameter of 45 mm or more, a (004) XRD rocking curve FWHM of less than 20 arcsec, less than 18 arcsec, less than 16 arcsec, less than 14 arcsec, or less than 12 arcsec, and an impurity concentration satisfying one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [F2] The c-plane GaN wafer according to [F1] above, having a diameter of 95 mm or more or 145 mm or more. [F3] The conductivity type is n-type. When the (004) XRD rocking curve is measured every 1 mm along at least one line on one main surface over a length of 40 mm, the entire measurement A c-plane GaN wafer characterized in that the maximum value of the (004) XRD rocking curve FWHM between fixed points is 20 arcsec or less, and that the impurity concentration satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [F4] The c-plane GaN wafer according to [F3], wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [F5] A c-plane GaN wafer, characterized in that the conductivity type is n-type, that when (004) XRD rocking curves are measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one main surface, the maximum value of the (004) XRD rocking curve FWHM between all measurement points on each line is 20 arcsec or less, and that the impurity concentration satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [F6] The c-plane GaN wafer according to [F5], wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less, 16 arcsec or less, 14 arcsec or less, 12 arcsec or less, or 10 arcsec or less. [F7] A c-plane GaN wafer according to any one of [F1] to [F6] above, wherein the variation width of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x direction, and the variation width of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are 0.15 degrees or less, 0.1 degrees or less, or 0.08 degrees or less, respectively, within a 40 mm long section. [F8] The c-plane GaN wafer according to any one of [F1] to [F7] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentrations. [F9] Si concentration is 5×10 17 atoms / cm 3 The c-plane GaN wafer according to any one of the above items [F1] to [F8], which is as follows: [F10] The concentration of each impurity except for Si, O and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to any one of the above [F1] to [F9], which is as follows: [F11] O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The c-plane GaN wafer according to any one of the above [F1] to [F10], which is as follows: [F12] 5×10 17 cm -3 The c-plane GaN wafer according to any one of [F1] to [F11] above, having at least one of a carrier concentration of less than 0.05 and a room temperature resistivity of 0.04 Ω·cm or more. [F13] The c-plane GaN wafer according to any one of [F1] to [F12] above, which is made of a GaN crystal grown by HVPE. [F14] A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of [F1] to [F13] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer. [F15] An epitaxial wafer comprising the c-plane GaN wafer according to any one of [F1] to [F13] above, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer. [F16] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a c-plane GaN wafer according to any one of [F1] to [F13] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer. [F17] A method for producing a c-plane GaN wafer according to any one of [F1] to [F13] above, and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga-polarity main surface of the prepared c-plane GaN wafer, the GaN layer having a high carrier concentration region or a carrier compensation region, the high carrier concentration region having a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is the manufacturing method for double-layer GaN wafers. [F18] The manufacturing method according to [F17], wherein in the epitaxial growth step, the GaN layer is grown by HVPE. [F19] The manufacturing method according to [F17] or [F18], wherein the GaN layer has a thickness of 500 μm or less. [F20] The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The manufacturing method according to any one of the above items [F17] to [F19]. [F21] The manufacturing method according to any one of [F17] to [F20], wherein the GaN layer is provided with the high carrier concentration region, and the high carrier concentration region is doped with Ge. [F22] The manufacturing method according to any one of [F17] to [F21] above, wherein the GaN layer is provided with the high carrier concentration region, and the high carrier concentration region is intentionally doped with Si. [F23] The GaN layer is provided with the carrier compensation region, and the carrier compensation region has a lower limit of a total concentration of compensation impurities of 5×10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3or more than 5×10 18 atoms / cm 3 The manufacturing method according to any one of the above items [F17] to [F19]. [F24] The manufacturing method according to any one of [F17] to [F23] above, further comprising a step of thinning the stack obtained in the epitaxial growth step. [F25] A method for producing a bulk GaN crystal, comprising the steps of preparing a c-plane GaN wafer according to any one of [F1] to [F13] above, and epitaxially growing GaN on the prepared c-plane GaN wafer.

[0015] Further embodiments of the present invention include the following [G1] to [G29]. [G1] The conductivity type is n-type, and the dislocation density on one of the main surfaces is 2×10 5 cm -2 Below, 1×10 5 cm -2 or less, or 5×10 4 cm -2 and, regarding impurity concentration, satisfying one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [G2] The c-plane GaN wafer according to [G1] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentrations. [G3]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The c-plane GaN wafer according to [G1] or [G2] above, which is as follows: [G4] A c-plane GaN wafer according to any one of [G1] to [G3] above, wherein the variation width of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x direction, and the variation width of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are 0.15 degrees or less, 0.1 degrees or less, or 0.08 degrees or less, respectively, within a 40 mm long section. [G5] 5×10 17 cm -3 and a room temperature resistivity of 0.04 Ω cm or more. aN wafer. [G6] Si concentration is 5×10 17 atoms / cm 3 The c-plane GaN wafer according to any one of the above [G1] to [G5], which is as follows: [G7] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to [G6] above, which is as follows: [G8] The c-plane GaN wafer according to any one of [G1] to [G4] above, having a room temperature resistivity of less than 0.03 Ω·cm, less than 0.02 Ω·cm, less than 0.015 Ω·cm, or less than 0.010 Ω·cm. [G9] Carrier concentration is 1×10 18 cm -3 That's it, 2 x 10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The c-plane GaN wafer according to any one of the above [G1] to [G4]. [G10] Ge concentration is 1×10 18 atoms / cm 3 or more, and Si concentration is 4×10 17 atoms / cm 3 The c-plane GaN wafer according to [G8] or [G9] above. [G11] The c-plane GaN wafer according to any one of [G8] to [G10] above, wherein the donor impurity contained at the highest concentration is Ge. [G12] The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to [G10] or [G11] above, which is: [G13] The c-plane GaN wafer according to either [G8] or [G9] above, wherein the donor impurity contained at the highest concentration is Si. [G14] The c-plane GaN wafer according to [G13] above, wherein the total concentration of donor impurities excluding Si is 10% or less, 5% or less, or 1% or less of the Si concentration. [G15] The c-plane GaN wafer according to [G14] above, wherein the carrier concentration is 90% or more of the Si concentration. [G16] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to any one of [G13] to [G15] above, which is: [G17] A c-plane GaN wafer according to any one of [G1] to [G16] above, which is made of a GaN crystal grown by HVPE. [G18] A method for manufacturing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of [G1] to [G17] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer. [G19] An epitaxial wafer comprising the c-plane GaN wafer according to any one of [G1] to [G17] above, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer. [G20] A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a c-plane GaN wafer according to any one of [G1] to [G17] above; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer. [G21] A method for producing a c-plane GaN wafer according to any one of [G1] to [G7] above, and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga-polarity main surface of the prepared c-plane GaN wafer, the GaN layer having a high carrier concentration region or a carrier compensation region, the high carrier concentration region having a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is the manufacturing method for double-layer GaN wafers. [G22] The manufacturing method according to [G21], wherein in the epitaxial growth step, the GaN layer is grown by HVPE. [G23] The manufacturing method according to [G21] or [G22], wherein the GaN layer has a thickness of 500 μm or less. [G24] The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The above-mentioned areas are described in any one of [G21] to [G23]. The manufacturing method described above. [G25] The manufacturing method according to any one of [G21] to [G24], wherein the GaN layer is provided with a high carrier concentration region, and the high carrier concentration region is doped with Ge. [G26] The manufacturing method according to any one of [G21] to [G25], wherein the GaN layer has a high carrier concentration region, and the high carrier concentration region is intentionally doped with Si. [G27] The GaN layer is provided with the carrier compensation region, and the carrier compensation region has a lower limit of a total concentration of compensation impurities of 5×10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm3 or more than 5×10 18 atoms / cm 3 The manufacturing method according to any one of the above items [G21] to [G23]. [G28] The manufacturing method according to any one of [G21] to [G27] above, further comprising a step of thinning the stack obtained in the epitaxial growth step. [G29] A method for producing a bulk GaN crystal, comprising the steps of preparing a c-plane GaN wafer according to any one of [G1] to [G7] above, and epitaxially growing GaN on the prepared c-plane GaN wafer.

[0016] Further embodiments of the present invention include the following [H1] to [H32]. [H1] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined from 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that at least one anomalous X-ray transmission image of a 10 mm x 10 mm square area can be obtained, and that the impurity concentration satisfies one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [H2] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined from 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that at least one anomalous X-ray transmission image of a 15 mm x 15 mm square area can be obtained, and that the impurity concentration satisfies one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [H3] An n-type GaN crystal having two principal surfaces facing in opposite directions, one of which has Ga polarity and is inclined at an angle of 0 to 10 degrees with respect to the (0001) crystal plane, characterized in that at least one anomalous X-ray transmission image of a square area of ​​20 mm x 20 mm can be obtained, and that the impurity concentration satisfies one or more conditions selected from the following (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is; (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. [H4] An n-type GaN crystal according to any one of [H1] to [H3] above, which satisfies all of the conditions (a) to (c) above regarding impurity concentration. [H5]O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The n-type GaN crystal according to any one of the above items [H1] to [H4], which is as follows: [H6]5×10 17 cm -3 The n-type GaN crystal according to any one of [H1] to [H5] above, having at least one of a carrier concentration of less than 0.01 and a room temperature resistivity of 0.04 Ω·cm or more. [H7]Si concentration is 5×10 17 atoms / cm 3 The n-type GaN crystal according to any one of the above items [H1] to [H6], which is as follows: [H8] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to the above [H7], which is as follows: [H9] The n-type GaN crystal according to any one of [H1] to [H5] above, having a room temperature resistivity of less than 0.03 Ω·cm, less than 0.02 Ω·cm, less than 0.015 Ω·cm, or less than 0.010 Ω·cm. [H10] Carrier concentration is 1×10 18 cm -3 That's it, 2 x 10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The n-type GaN crystal according to any one of the above items [H1] to [H5]. [H11] Ge concentration is 1×10 18 atoms / cm 3 or more, and Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to the above [H9] or [H10]. [H12] The n-type GaN crystal according to any one of the above [H9] to [H11], wherein the donor impurity contained at the highest concentration is Ge. [H13] The concentration of each impurity except for Ge, Si, O and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to [H11] or [H12] above, which is: [H14] The n-type GaN crystal according to [H9] or [H10] above, wherein the donor impurity contained at the highest concentration is Si. [H15] The n-type GaN crystal according to [H14], wherein a total concentration of donor impurities excluding Si is 10% or less, 5% or less, or 1% or less of the Si concentration. [H16] The n-type GaN crystal according to [H15] above, wherein the carrier concentration is 90% or more of the Si concentration. [H17] The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3The n-type GaN crystal according to any one of the above [H14] to [H16], which is: [H18] An n-type GaN crystal according to any one of [H1] to [H17], which is a GaN crystal grown by HVPE. [H19] The n-type GaN crystal according to any one of [H1] to [H18] above, which is a GaN wafer. [H20] The n-type GaN crystal according to [H19], wherein a variation width of an x-direction component of an offcut angle on a line passing through the center of the front surface and extending in the x direction, and a variation width of a y-direction component of an offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are 0.15 degrees or less, 0.1 degrees or less, or 0.08 degrees or less, respectively, within a 40 mm long section. [H21] A method for manufacturing an epitaxial wafer, comprising the steps of: preparing an n-type GaN crystal according to [H19] or [H20]; and epitaxially growing one or more nitride semiconductor layers on the prepared n-type GaN crystal. [H22] An epitaxial wafer comprising the n-type GaN crystal according to [H19] or [H20] above, and one or more nitride semiconductor layers epitaxially grown on the n-type GaN crystal. [H23] A method for manufacturing a nitride semiconductor device, comprising the steps of preparing an n-type GaN crystal according to [H19] or [H20] above, and epitaxially growing one or more nitride semiconductor layers on the prepared n-type GaN crystal. [H24] A method for producing an n-type GaN crystal according to any one of [H1] to [H8] above, comprising the steps of: preparing a GaN wafer which is an n-type GaN crystal according to any one of [H1] to [H8] above; and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga-polarity main surface of the prepared GaN wafer, wherein the GaN layer is provided with a high carrier concentration region or a carrier compensation region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is the manufacturing method for double-layer GaN wafers. [H25] The manufacturing method according to [H24], wherein in the epitaxial growth step, the GaN layer is grown by HVPE. [H26] The manufacturing method according to [H24] or [H25], wherein the GaN layer has a thickness of 500 μm or less. [H27] The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 That's it, 3 x 10 18 cm -3 or more than 4×10 18 cm -3 The manufacturing method according to any one of the above items [H24] to [H26], which is in the above range. [H28] The manufacturing method according to any one of [H24] to [H27], wherein the GaN layer has a high carrier concentration region, and the high carrier concentration region is doped with Ge. [H29] The manufacturing method according to any one of [H24] to [H28], wherein the GaN layer has a high carrier concentration region, and the high carrier concentration region is intentionally doped with Si. [H30] The GaN layer is provided with the carrier compensation region, and the carrier compensation region has a lower limit of a total concentration of compensation impurities of 5×10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3 or more than 5×10 18 atoms / cm 3 The manufacturing method described in [H24] above, which is in the above-mentioned range. [H31] The manufacturing method according to any one of [H24] to [H30] above, further comprising a step of thinning the stack obtained in the epitaxial growth step. [H32] A method for producing a bulk GaN crystal, comprising the steps of preparing a GaN wafer that is an n-type GaN crystal according to any one of [H1] to [H8] above, and epitaxially growing GaN on the prepared GaN wafer. Effect of the Invention

[0017] According to one preferred embodiment, a GaN crystal is provided that is grown by HVPE and has a (004) XRD rocking curve half-width of 20 arcsec or less. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a perspective view showing an n-type GaN crystal according to an embodiment. [Diagram 2] FIG. 2 is a plan view showing an n-type GaN crystal according to an embodiment. [Diagram 3] FIG. 3 is a plan view showing an n-type GaN crystal according to an embodiment. [Figure 4] FIG. 4 is a perspective view showing a GaN wafer according to the embodiment. [Diagram 5] FIG. 5 is a cross-sectional view showing a GaN wafer according to the embodiment. [Figure 6] FIG. 6 is a plan view showing a GaN wafer according to the embodiment. [Figure 7] FIG. 7 is a plan view showing a GaN wafer according to the embodiment. [Figure 8] FIG. 8 is a perspective view showing an example of a double-layer GaN wafer. [Figure 9] FIG. 9 is a schematic diagram showing the basic configuration of an HVPE apparatus. [Figure 10] FIG. 10(a) is a cross-sectional view showing a seed and an edge cover set on a susceptor, and FIG. 10(b) is a cross-sectional view showing a GaN crystal grown on the seed shown in FIG. 10(a). [Figure 11] FIG. 11 is a cross-sectional view showing the state where the seed and the edge cover are set on the susceptor. [Figure 12] FIG. 12 is a diagram showing the basic configuration of a crystal growth apparatus used for growing GaN crystals by the ammonothermal method. [Figure 13]FIG. 13 is a cross-sectional view showing a GaN crystal layer grown by an ammonothermal method on the N-polar surface of a first c-plane GaN wafer. [Figure 14] FIG. 14 is a diagram showing the configuration of the sample prepared in Experiment 6 and the observation direction of the three-photon excitation image in Experiment 6. [Figure 15] FIG. 15 is a diagram illustrating that the offcut angle of a c-plane GaN wafer can be resolved into components in two directions perpendicular to each other. [Figure 16] FIG. 16 is a transmission X-ray topography image of a square area of ​​20 mm×20 mm obtained from a c-plane GaN wafer (sample E-7) made of GaN crystals grown by HVPE in Experiment 7 (a photograph in place of a drawing). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In GaN crystals, the (0001) and (000-1) crystal planes are collectively called c-planes, the {10-10} crystal planes are called m-planes, and the {11-20} crystal planes are called a-planes. The crystal axis perpendicular to the c-plane is called the c-axis, the crystal axis perpendicular to the m-plane is called the m-axis, and the crystal axis perpendicular to the a-plane is called the a-axis. In this specification, when a crystal axis, a crystal plane, a crystal orientation, etc. are mentioned, unless otherwise specified, they mean the crystal axis, crystal plane, crystal orientation, etc. of a GaN crystal. The Miller indices of the hexagonal crystal (hkil) are sometimes written in three digits as (hkl) because of the relationship h+k=-i. For example, (0004) is written in three digits as (004). Hereinafter, the present invention will be described based on an embodiment with reference to the drawings as appropriate.

[0020] 1.n-type GaN crystal 1.1. Shape and dimensions A crystal 10 shown in FIG. 1 is an example of an n-type GaN crystal according to an embodiment. The crystal 10 has two main surfaces (large area surfaces) facing in opposite directions, i.e., a first main surface 11 and a second main surface 12. One of the first main surface 11 and the second main surface 12 has Ga polarity and the other has N polarity. The first main surface 11 and the second main surface 12 are preferably parallel to each other.

[0021] When the first main surface 11 has Ga polarity and the second main surface 12 has N polarity, the inclination of the first main surface 11 with respect to the (0001) crystal plane is 0 degrees or more and 10 degrees or less. The inclination may be 0.2 degrees or more, and may be less than 5 degrees, less than 2.5 degrees, less than 2 degrees, less than 1.5 degrees, less than 1 degree, or less than 0.5 degrees. The inclination of the first main surface 11 with respect to the (0001) crystal plane is, in other words, the angle between the

[0001] direction of the crystal 10 and the normal vector of the first main surface 11 . When the first main surface 11 is N-polar and the second main surface 12 is Ga-polar, the inclination of the first main surface 11 with respect to the (000-1) crystal plane is 0 degrees or more and 10 degrees or less. The inclination may be less than 5 degrees, less than 2.5 degrees, less than 2 degrees, less than 1.5 degrees, less than 1 degree, or less than 0.5 degrees.

[0022] The area of ​​the first main surface 11 and the second main surface 12 is 3 cm 2 More preferably, it is equal to or greater than this. Diameter D of crystal 10 C is usually 20 mm or more, and may be 45 mm or more, 95 mm or more, or 145 mm or more, and is typically 25 to 27 mm (about 1 inch), 50 to 55 mm (about 2 inches), 100 to 105 mm (about 4 inches), 150 to 155 mm (about 6 inches), etc. The shapes of the first main surface 11 and the second main surface 12 are not limited to a circle, but may be changed to a quadrilateral such as a square or a rectangle, a polygon such as a regular hexagon or a regular octagon, or any other shape.

[0023] Crystal 10 may be an ingot or a wafer, or it may be an epitaxial layer grown on another GaN crystal, or a film bonded to a support substrate, etc. In other words, crystal 10 may or may not be free-standing. When the crystal 10 is an ingot, its thickness t C is preferably 1.5 mm or more, more preferably 2 mm or more, and further preferably 3 mm or more. When the crystal 10 is a wafer, its thickness t C may be 200 μm or more and less than 500 μm, 500 μm or more and less than 750 μm, 750 μm or more and less than 1 mm, 1 mm or more and less than 2 mm, etc. When the crystal 10 is an epitaxial layer grown on another GaN crystal or a film bonded to a support substrate, its thickness t C can be 5 μm or more and less than 50 μm, 50 μm or more and less than 100 μm, 100 μm or more and less than 150 μm, 150 μm or more and less than 250 μm, etc.

[0024] 1.2. Properties The crystal 10 consists of HVPE grown GaN. GaN grown in a typical HVPE apparatus equipped with a quartz reactor usually satisfies one or more of the following conditions (a) to (c) regarding impurity concentration. (a) Si concentration is 5×10 16 atoms / cm 3 That's all. (b) O concentration is 3×10 16 atoms / cm 3 The following is the result. (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. The crystal 10 can satisfy all of the above conditions (a) to (c).

[0025] The crystal 10 is an n-type semiconductor containing a donor impurity. In one example, but not limited to, the room temperature resistivity (specific resistance at room temperature) of the crystal 10 may be less than 0.03 Ω·cm, preferably less than 0.02 Ω·cm, more preferably less than 0.015 Ω·cm, and even more preferably less than 0.010 Ω·cm. Donor impurities that the crystal 10 may contain include Group 14 elements such as Si (silicon) and Ge (germanium), and Group 16 elements such as O (oxygen) and S (sulfur). The donor impurity that crystal 10 contains in the highest concentration is preferably Si or Ge.

[0026] In one example, by making the total concentration of donor impurities excluding Si sufficiently lower than the Si concentration, the carrier concentration of crystal 10 can be controlled by adjusting the Si concentration. To achieve this, it is preferable to make the total concentration of donor impurities excluding Si 10% or less of the Si concentration, further 5% or less, and further 1% or less. When the total concentration of donor impurities excluding Si 10% or less of the Si concentration, the carrier concentration of crystal 10 can be 90% or more of the Si concentration. When adding Ge to the crystal 10, it is effective to increase the molar ratio of H2 contained in the carrier gas used during growth relatively in order to reduce unevenness in the Ge concentration. 17 atoms / cm 3 It could be more than one unit.

[0027] In order to sufficiently reduce the resistivity of the crystal 10, the carrier concentration of the crystal 10 at room temperature must be 1×10 18 cm -3 More than that, and even 2×10 18 cm -3 The carrier concentration is preferably 3×10 18 cm -3 More than that, and 4x10 18 cm -3 From the viewpoint of electrical properties, there is no particular upper limit to the carrier concentration, but in order not to deteriorate the productivity of the crystal 10, the carrier concentration is set to 1×10 19 cm -3 Can be set to 8×10 18 cm -3 Below, and further 5×10 18 cm -3 The doping concentration may be set to 0.1 or less because high concentration doping increases the frequency of abnormal growth.

[0028] 1.3.Crystal Quality The quality of the crystal 10 can be evaluated using the (004) XRD rocking curve FWHM measured by ω scan using CuKα1 radiation. The better the crystal quality, the narrower the (004) XRD rocking curve FWHM. In the (004) XRD rocking curve measurement, the X-ray tube was operated at a voltage of 45 kV and a current of 40 mA, and a monochromated CuK α X-rays are made incident on the first main surface 11. There are no particular limitations on the direction from which the X-rays are made incident on the first main surface 11, and for example, the incident plane of the X-rays may be perpendicular to the a-axis.

[0029] The size of the X-ray beam is as follows when the angle of incidence (the angle between the reflecting surface and the X-ray) is 90°: That is, when X-rays are incident perpendicularly on the (004) reflecting surface, the size of the irradiation area on the first main surface 11 is set to 5 mm in the direction parallel to the ω axis and 1 mm in the direction perpendicular to the ω axis. The ω axis is the rotation axis of the sample in rocking curve measurement. When the X-ray beam size is set in this way, in the (004) XRD rocking curve measurement of GaN, ω is about 36.5°, so the size of the irradiation area on the first main surface 11 is about 1.7 × 5 mm 2 It is. The (004) XRD rocking curve FWHM measured in this manner can be less than 20 arcsec, or even less than 18 arcsec, or even less than 16 arcsec, or even less than 14 arcsec, or even less than 12 arcsec.

[0030] When the diameter of the first main surface 11 exceeds 40 mm, as shown in FIG. 2, ω scanning is performed on the first main surface 11 along a line L having a length of 40 mm at 1 mm intervals under the above conditions, thereby obtaining 40 measurement points P arranged at 1 mm pitch on the line L. M The (004) XRD rocking curves at each measurement point P MIn the ω scan in , the ω axis is perpendicular to the line L. In other words, the X-ray is made incident on the crystal 10 so that the X-ray incidence plane and the line L are parallel to each other.

[0031] In a preferred embodiment, when such measurements are made along at least one line on the first main surface 11, the maximum value of the (004) XRD rocking curve FWHM among all measurement points may be 20 arcsec or less. The average value of the (004) XRD rocking curve FWHM among all the measurement points can be 18 arcsec or less, further 16 arcsec or less, further 14 arcsec or less, further 12 arcsec or less, or even 10 arcsec or less.

[0032] When the diameter of the first main surface 11 exceeds 40 mm, furthermore, by performing an ω-scan under the above conditions every 1 mm over a length of 40 mm along each of two mutually perpendicular lines L1 and L2 as shown in Fig. 3 on the first main surface 11, (004) XRD rocking curves at 40 measurement points arranged at a pitch of 1 mm can be obtained on each line L1, L2. In this case, in the ω-scan at each measurement point on line L1, the ω-axis is perpendicular to line L1, and in the ω-scan at each measurement point on line L2, the ω-axis is perpendicular to line L2.

[0033] In a preferred embodiment, when such measurements are made along at least two mutually perpendicular lines on the first main surface 11, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line may be 20 arcsec or less. That is, the maximum value among 40 measurement points on one of the two lines and the maximum value among 40 measurement points on the other of the two lines may both be 20 arcsec or less. The average (004) XRD rocking curve FWHM among all measurement points on each line can be 18 arcsec or less, or even 16 arcsec or less, or even 14 arcsec or less, or even 12 arcsec or less, or even 10 arcsec or less.

[0034] From the crystal 10, at least one anomalous X-ray transmission image of a 10 mm x 10 mm square area can be obtained in X-ray topography by the Lang method. In the Lang method, an X-ray source is placed on one main surface of a plate-shaped test piece, and an X-ray detector is placed on the other main surface. Anomalous transmission of X-rays, also known as the Borrmann effect, is a phenomenon in which X-rays penetrate a crystal with a thickness that would normally prevent them from penetrating due to absorption. For example, when a transmission image is obtained from a 344 μm-thick GaN crystal in X-ray topography using MoKα (wavelength 0.71073 Å) as the X-ray source, it is an anomalous transmission image. This is because the absorption coefficient μ of GaN is 290.40 cm when the X-ray source is MoKα. -1 When the wafer thickness t is 344 μm, μ t = 10.0. If there is no anomalous transmission, no transmission image can be obtained under the condition μ t ≧ 10. Since anomalous transmission images are not observed when the crystal perfection is low, GaN crystals that give anomalous transmission images in X-ray topography can be said to be of good quality. From the crystal 10, it is preferable to obtain at least one abnormal X-ray transmission image of a 15 mm×15 mm square area, and more preferably to obtain at least one abnormal X-ray transmission image of a 20 mm×20 mm square area.

[0035] 2. GaN wafers In this specification, a GaN wafer with an offcut of 10 degrees or less from the (0001) crystal plane or the (000-1) crystal plane is called a c-plane GaN wafer.

[0036] 2.1. Shape and dimensions The wafer 20 shown in FIG. 4 is an example of a GaN wafer according to the embodiment. Wafer 20 is a c-plane GaN wafer, and its two principal surfaces (large area surfaces) facing in opposite directions, i.e., first principal surface 21 and second principal surface 22, one of which is Ga polarity and the other is N polarity. The principal surface on the Ga polarity side is sometimes called a Ga polarity surface, and the principal surface on the N polarity side is sometimes called an N polarity surface. When the first main surface 21 has Ga polarity, the inclination of the first main surface 21 with respect to the (0001) crystal plane is 0 degrees or more and 10 degrees or less. The inclination may be 0.2 degrees or more, and may be less than 5 degrees, less than 2.5 degrees, less than 1.5 degrees, less than 1 degree, or less than 0.5 degrees. When the first main surface 21 is N-polar, the inclination of the first main surface 21 with respect to the (000-1) crystal plane is 0 degrees or more and 10 degrees or less. The inclination may be less than 5 degrees, less than 2.5 degrees, less than 1.5 degrees, less than 1 degree, or less than 0.5 degrees. The first main surface 21 and the second main surface 22 are preferably parallel to each other.

[0037] Diameter D of wafer 20 W is usually 45 mm or more, may be 95 mm or more, or 145 mm or more, and is typically 50 to 55 mm (about 2 inches), 100 to 105 mm (about 4 inches), 150 to 155 mm (about 6 inches), etc. The thickness t of the wafer 20 W is the diameter D W For example, the wafer 20 is designed to be self-supporting and handleable depending on the diameter D W When the thickness t is about 2 inches, W is preferably 250 to 500 μm, more preferably 300 to 450 μm, and the diameter D W When the thickness t is about 4 inches, W The diameter D of the wafer 20 is preferably 400 to 800 μm, and more preferably 500 to 650 μm. W When the thickness t is about 6 inches, W The thickness is preferably 500 to 850 μm, and more preferably 600 to 750 μm.

[0038] The offcut angle of the wafer 20 can be resolved into two mutually orthogonal components in the x-direction and y-direction within the first main surface 21. With reference to FIG. 15, when the normal direction of the first main surface 21 is the z-direction and a vector parallel to the c-axis is a vector Vc, the offcut angle of the wafer 20 is equal to the inclination θ of the vector Vc from the z-axis. This vector Vc is the x-direction component of the vector Vc xand the y-component of the vector Vc y The orthogonal projection of vector Vc on the xz plane is vector Vc x And the orthogonal projection of vector Vc on the yz plane is vector Vc y It is. When the vector Vc is decomposed in this way, the vector Vc x The inclination from the z-axis is the x-direction component θ of the offcut angle θ x and the vector Vc y The inclination from the z-axis is the y-axis component of the offcut angle θ y It is.

[0039] In the wafer 20, the fluctuation range of the x-direction component of the offcut angle on a line passing through the center of the first main surface 21 and extending in the x-direction and the fluctuation range of the x-direction component of the offcut angle on a line passing through the center of the first main surface 21 and extending in the y-direction are The fluctuation width of the y-direction component of the offcut angle may be 0.15 degrees or less, preferably 0.1 degrees or less, and more preferably 0.08 degrees or less within a section of 40 mm in length. In this evaluation, a portion that is less than 5 mm away from the outer periphery when the wafer 20 is viewed in plan may be excluded. The fluctuation range is the difference between the maximum value and the minimum value. For example, a fluctuation range of 0.15 degrees or less means that the fluctuation from the median value is within ±0.075 degrees. The x direction may be parallel to one of the a-planes, and then the y direction is parallel to one of the m-planes.

[0040] The first main surface 21 of the wafer 20 is a main surface, i.e., a "front surface," that is intended to be used for epitaxial growth of a nitride semiconductor, for example, when a nitride semiconductor device is manufactured using the wafer 20 as a substrate. The first main surface 21 is mirror-finished, and its root-mean-square (RMS) roughness measured by AFM is preferably less than 2 nm in a measurement range of 2 μm×2 μm, and may be less than 1 nm or less than 0.5 nm. The second major surface 22 is the "back side" and may be mirror finished or matte finished.

[0041] The edges of the wafer 20 may be chamfered. The wafer 20 may be provided with various markings as necessary, such as an orientation flat or notch that indicates the crystal orientation, and an index flat that makes it easy to distinguish between the front and back surfaces. The main surface of the wafer 20 is circular, but is not limited to a circular shape and may be changed to a square, rectangle, hexagon, octagon, or any other shape.

[0042] 2.2. Properties Wafer 20 consists of a GaN crystal grown by HVPE. GaN grown in a typical HVPE apparatus equipped with a quartz reactor usually satisfies one or more of the following conditions (a) to (c) regarding impurity concentration. (a) Si concentration is 5×10 16 atoms / cm 3 That's all. (b) O concentration is 3×10 16 atoms / cm 3 The following is the result. (c) H concentration is 1×10 17 atoms / cm 3 The following is the result. The wafer 20 can satisfy all of the above conditions (a) to (c).

[0043] For reference, GaN grown by HVPE has an infrared absorption spectrum of 3150-3250 cm -1 The absorption coefficient is in the range of 0.5 cm -1 It can be distinguished from ammonothermally grown GaN in that it does not show any absorption peaks above 1000 nm, which are related to the high concentration of gallium vacancies in ammonothermally grown GaN [S. Suihkonen, et al., Applied Physics Letters 108, 202105 (2016); W. Jiang, et al., Applied Physics Express 10, 075506 (2017)].

[0044] The wafer 20 may be intentionally doped as desired. Thus, in one example, the wafer 20 may be formed entirely of unintentionally doped GaN (UID-GaN). Since unintentional donor impurity doping and the generation of nitrogen vacancies inevitably occur, the conductivity type of UID-GaN is n-type. In UID-GaN, the Si concentration is 5×10 17 atoms / cm 3 Below, the O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The following impurity concentrations are 5×10 except for Si, O, and H. 15 atoms / cm 3 It can be the following: In UID-GaN, the carrier concentration is 5×10 17 cm -3 and the room temperature resistivity may be 0.04 Ω·cm or more.

[0045] In one example, the room temperature resistivity of the wafer 20 can be reduced by intentional doping to less than 0.03 Ω·cm, or even less than 0.02 Ω·cm, or even less than 0.015 Ω·cm, or even less than 0.010 Ω·cm. To sufficiently reduce the resistivity, the wafer 20 can have a room temperature carrier concentration of less than 1×10 18 cm -3 More than that, and even 2×10 18 cm -3 The carrier concentration is preferably 3×10 18 cm -3 More than that, and 4x10 18 cm -3 From the viewpoint of electrical characteristics, there is no particular upper limit to the carrier concentration, but in order not to deteriorate the productivity of the wafer 20, the carrier concentration is set to 1×10 19 cm -3 Can be set to 8×10 18 cm -3Below, and further 5×10 18 cm -3 The reason is that high concentration doping increases the frequency of abnormal growth of GaN crystals.

[0046] The dopant added to the wafer 20 to reduce resistivity is preferably a donor impurity, and therefore the conductivity type of the wafer 20 when the resistivity is reduced by doping is preferably n-type. This is because donor impurities generally exhibit a higher activation ratio than acceptor impurities. The activation ratio is the ratio of the carrier concentration to the dopant concentration in doped GaN. Elements that can act as donor impurities include Group 14 elements such as Si (silicon) and Ge (germanium), and Group 16 elements such as O (oxygen) and S (sulfur).

[0047] When doped with a donor impurity, the donor impurity that the wafer 20 contains in the highest concentration is preferably Si or Ge, for two main reasons. First, Si and Ge are donor impurities that, like O, have high activation rates. Second, to obtain GaN highly doped with O, facet growth is required, whereas GaN highly doped with Si or Ge can be obtained by c-plane growth.

[0048] Facet growth is a technique in which a GaN film with a

[0001] orientation is grown with a pitted growth surface, in contrast to growing such a GaN film with a flat growth surface, known as c-plane growth. Threading dislocations have the tendency to gather at the bottom of pits, so the distribution of threading dislocations is non-uniform in GaN films formed by facet growth, and nitride semiconductor device manufacturers often do not like c-plane GaN wafers cut from such GaN films. GaN crystals with a (004) XRD rocking curve FWHM of 20 arcsec or less have a low density of threading dislocations, so when the c-plane is grown under appropriate conditions, the growth surface can be flat and hillock-free, with an extremely good morphology. Si and Ge can be said to be donor impurities that can take advantage of this characteristic.

[0049] In a preferred example, the total concentration of donor impurities excluding Si is made sufficiently lower than the Si concentration, so that the carrier concentration of the wafer 20 can be controlled by adjusting the Si concentration. To achieve this, it is preferable that the total concentration of donor impurities excluding Si is 10% or less of the Si concentration, more preferably 5% or less, and even more preferably 1% or less. When the total concentration of donor impurities excluding Si is 10% or less of the Si concentration, the carrier concentration of the wafer 20 can be 90% or more of the Si concentration. When Ge is intentionally added to the wafer 20, it is effective to relatively increase the molar ratio of H2 contained in the carrier gas used during growth in order to reduce unevenness in the Ge concentration. However, the Si concentration of the wafer 20 is accordingly increased by 10 17 atoms / cm 3 It could be more than one unit.

[0050] In one embodiment, only a portion of the wafer 20 may be intentionally doped. In the example shown in FIG. 5, the wafer 20 is made of intentionally doped GaN (ID-GaN). The first region R1 made of UID-GaN (nally doped GaN) is located on the Ga-polar first main surface 21 side, and the second region R2 made of UID-GaN is located on the N-polar second main surface 22 side. The first region R1 has a higher carrier concentration and a lower resistivity than the second region R2. Between the first region R1 and the second region R2, an intermediate region (not shown) having a carrier concentration intermediate between the first region R1 and the second region R2 may be provided, in which the carrier concentration may increase continuously or stepwise from the N-polarity side to the Ga-polarity side.

[0051] The thickness t1 of the first region R1 can be, for example, 5 μm or more and less than 50 μm, 50 μm or more and less than 100 μm, 100 μm or more and less than 150 μm, or 150 μm or more and 250 μm or less. A regrowth interface may exist between the first region R1 and the second region R2. That is, the wafer 20 shown in Fig. 5 may be manufactured by completing a c-plane GaN wafer made of UID-GaN, and then growing an ID-GaN layer on the Ga-polarity primary surface of the c-plane GaN wafer by HVPE.

[0052] 5, the room temperature resistivity in the first region R1 may be less than 0.03 Ω·cm, less than 0.02 Ω·cm, less than 0.015 Ω·cm, or less than 0.010 Ω·cm. The carrier concentration in the first region R1 at room temperature is preferably less than 1×10 18 cm -3 More preferably, 2×10 18 cm -3 That's 3 x 10. 18 cm -3 More than that, and 4x10 18 cm -3 It may be more than that. The intentional dopant contained in the first region R1 is preferably a donor impurity, and the donor impurity contained in the first region R1 at the highest concentration is Si or Ge. In a preferred embodiment, the total concentration of donor impurities other than Si in the first region R1 can be 10% or less, further 5% or less, or further 1% or less of the Si concentration. In the second region R2, the Si concentration is 5×10 17 atoms / cm 3 Below, the O concentration is 3×10 16 atoms / cm 3 Below, 2 x 10 16 atoms / cm 3 or less than 1×10 16 atoms / cm 3 The following impurity concentrations are 5×10 except for Si, O, and H. 15 atoms / cm 3 It can be the following: In the second region R2, the carrier concentration is 5×1017 and the room temperature resistivity may be 0.04 Ω·cm or more.

[0053] 2.3.Crystal Quality The crystalline quality of the wafer 20 can be evaluated using the (004) XRD rocking curve FWHM measured by ω scan using CuKα1 radiation as an index. The better the crystalline quality, the narrower the (004) XRD rocking curve FWHM. In the (004) XRD rocking curve measurement, the X-ray tube was operated at a voltage of 45 kV and a current of 40 mA, and a monochromated CuK α The ray is incident on the first major surface 21 .

[0054] The beam size of the X-ray is set so that when the angle of incidence (the angle between the reflecting surface and the X-ray) is 90°, that is, when the X-ray is made perpendicular to the (004) reflecting surface, the size of the irradiation area on the first main surface 21 is 5 mm in the direction parallel to the ω-axis and 1 mm in the direction perpendicular to the ω-axis. The ω-axis is the rotation axis of the sample in rocking curve measurement. When the X-ray beam size is set in this way, the ω is about 36.5° in the (004) XRD rocking curve measurement of GaN, so the irradiation area on the first main surface 21 is about 1.7 × 5 mm 2 It is.

[0055] As shown in FIG. 6, by performing ω scanning every 1 mm along a line L over a length of 40 mm on the first main surface 21 of the wafer 20, the following are arranged at a pitch of 1 mm on the line L: There are 40 measurement points P M The (004) XRD rocking curves at each measurement point P M In the ω scan at , the ω axis is set perpendicular to the line L. In other words, X-rays are made incident on the wafer 20 so that the X-ray incidence surface and the line L are parallel to each other.

[0056] When such measurements are made along at least one line on the first main surface 21 of the wafer 20, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less. The average value of the (004) XRD rocking curve FWHM among all the measurement points can be 18 arcsec or less, further 16 arcsec or less, further 14 arcsec or less, further 12 arcsec or less, and further 10 arcsec or less.

[0057] Furthermore, on the first main surface 21 of the wafer 20, by performing an ω-scan under the above conditions every 1 mm over a length of 40 mm along each of two mutually perpendicular lines L1 and L2 as shown in Fig. 7, (004) XRD rocking curves at 40 measurement points arranged at a pitch of 1 mm can be obtained on each line L1, L2. In this case, in the ω-scan at each measurement point on line L1, the ω-axis is perpendicular to line L1, and in the ω-scan at each measurement point on line L2, the ω-axis is perpendicular to line L2.

[0058] In a preferred embodiment, when such measurements are made along at least two mutually perpendicular lines on the first main surface 21, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line may be 20 arcsec or less. In other words, the maximum value among 40 measurement points on one of the two lines and the maximum value among 40 measurement points on the other of the two lines may both be 20 arcsec or less. The average (004) XRD rocking curve FWHM among all measurement points on each line can be 18 arcsec or less, or even 16 arcsec or less, or even 14 arcsec or less, or even 12 arcsec or less, or even 10 arcsec or less.

[0059] The dislocation density on the first main surface 21 of the wafer 20 is preferably 2×10 5 cm -2 Less than or equal to 1×10 5 cm -2 Less than 5×10, more preferably 4 cm -2In evaluating the dislocation density, a portion that is less than 5 mm away from the outer periphery when the wafer 20 is viewed in plan may be excluded.

[0060] 2.4.Applications The wafer 20 can be suitably used as a substrate in the manufacture of various nitride semiconductor devices. A nitride semiconductor device is a semiconductor device in which the main part of the device structure is formed from a nitride semiconductor. Nitride semiconductors are also called nitride III-V group compound semiconductors, group III nitride compound semiconductors, GaN-based semiconductors, etc., and include GaN as well as compounds in which part or all of the gallium in GaN is replaced with other group 13 elements of the periodic table (B, Al, In, etc.). Representative examples of nitride semiconductor devices that can be manufactured using wafer 20 include light-emitting devices such as light-emitting diodes (LEDs) and laser diodes (LDs), and electronic devices such as rectifiers, bipolar transistors, field-effect transistors, and HEMTs (High Electron Mobility Transistors), but are not limited to these.

[0061] When manufacturing a nitride semiconductor device, one or more nitride semiconductor layers are epitaxially grown on first main surface 21 of wafer 20 to form an epitaxial wafer having a semiconductor device structure. Preferred examples of epitaxial growth methods include, but are not limited to, gas phase methods such as MOCVD, MBE, pulsed deposition, sputtering, and HVPE. Semiconductor processing that may include etching, ion implantation, and the addition of structures such as electrodes and protective films. After the process is performed, the epitaxial wafer is thinned as necessary and cut into nitride semiconductor device chips. In the thinning process, the second main surface 22 of the wafer 20 is ground, polished, and / or etched.

[0062] When wafer 20 is made of only UID-GaN, typically no electrodes are formed on the surface of wafer 20. In one example, after an epitaxial wafer is formed using wafer 20 made of only UID-GaN, the entire wafer 20 may be removed from the epitaxial wafer by grinding, polishing, and / or etching. When wafer 20 has a first region R1 formed of ID-GaN on the first main surface 21 side and a second region R2 formed of UID-GaN on the second main surface 22 side, as shown in FIG. 5, in one example, after an epitaxial wafer is formed using wafer 20, second region R2 is removed from wafer 20 by grinding, polishing and / or etching, and an electrode can be formed on the surface of first region R1 exposed thereby. When wafer 20 is comprised solely of ID-GaN, in one example, after wafer 20 is used to form an epitaxial wafer, an electrode may be formed on second major surface 22 of wafer 20. This electrode may be formed after a thinning step of the epitaxial wafer.

[0063] Wafer 20 may also be used as a component material for a bilayer GaN wafer. The bilayer wafer 40 shown in FIG. 8 is an example of a bilayer GaN wafer, and includes a back layer L consisting of at least a portion of the wafer 20. b and a front layer L made of GaN epitaxially grown on the Ga polarity side of the wafer 20. f The front layer L f and the back layer L b There is a regrowth interface 43 between them.

[0064] The bilayer wafer 40 is intended to be used as a substrate in the manufacture of nitride semiconductor devices, similar to the wafer 20. Accordingly, the thickness thereof is the same as that of a normal GaN wafer, preferably 250 to 500 μm, more preferably 300 to 450 μm when the diameter is about 2 inches, preferably 400 to 800 μm, more preferably 500 to 650 μm when the diameter is about 4 inches, and preferably 500 to 850 μm, more preferably 600 to 750 μm when the diameter is about 6 inches.

[0065] Front layer L f In the bilayer wafer 40, when the regrowth interface 43 is inclined with respect to the Ga-polar main surface 41, the thickness of the front layer L f The thickness of the front layer L changes along the inclination direction. f The minimum thickness, ie the thickness at the location of the minimum thickness, is at least 20 μm, preferably 50 μm or more, such as 75 μm or more, 100 μm or more. When the thickness of the two-layer wafer 40 exceeds 300 μm, the front layer L f The maximum thickness, ie, the thickness at the location of maximum thickness, is preferably 300 μm or less, more preferably 250 μm or less, and even more preferably 200 μm or less. Front layer L f The difference between the maximum thickness and the minimum thickness is 200 μm or less, preferably 100 μm or less, more preferably 50 μm or less, even more preferably 25 μm or less, and even more preferably 10 μm or less.

[0066] Front layer L f In the case of the front layer L, at least a portion within a distance of 5 μm from the top surface is included in the high carrier concentration region or the carrier compensation region. f In other words, the upper surface is the Ga-polar main surface 41 of the bilayer wafer 40. In a preferred embodiment, the front layer L f The portion of the upper surface of the upper layer L within a distance Z is included in the high carrier concentration region or the carrier compensation region. f As long as the thickness does not exceed the minimum thickness, it may be 20 μm or more and less than 50 μm, 50 μm or more and less than 100 μm, 100 μm or more and less than 150 μm, 150 μm or more and 250 μm or less, etc.

[0067] The high carrier concentration region has a lower limit of 1×10 18 cm -3 The high carrier concentration region is where the lower limit of the carrier concentration is 2×10 18 cm -3 That's it, 3 x 10 18 cm -3or more, or 4×10 18 cm -3 It may be in the above area. Donor impurities preferably added to the high carrier concentration region are Si and Ge. The high carrier concentration region has a lower limit of 4×10 18 cm -3 or more, and the lower limit of the total concentration of donor impurities is 5 × 10 18 atoms / cm 3 That's it, 6 x 10 18 atoms / cm 3 or more, or 8 x 10 18 atoms / cm 3 It may be in the above area. The total concentration of donor impurities in the high carrier concentration region is limited to 5 × 10 to avoid significant degradation of the crystal quality. 19 atoms / cm 3 The following is further 2×10 19 atoms / cm 3 Below, and further 1×10 19 atoms / cm 3 It can be as follows. In the high carrier concentration region, the variation of the carrier concentration along the c-axis direction is preferably within ±25% of the median, more preferably within ±20%, even more preferably within ±15%, and even more preferably within ±10%. When it is difficult to measure the carrier concentration, it may be substituted with the total concentration of donor impurities.

[0068] The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The carrier compensation region is where the lower limit of the total concentration of compensation impurities is 5×10 17 atoms / cm 3 That's it, 1×10 18 atoms / cm 3 That's it, 2 x 10 18 atoms / cm 3 or more than 5×10 18 atoms / cm 3 It may be in the above area. The compensating impurity is an impurity that has the function of compensating for n-type carriers in a GaN crystal. Preferred compensating impurities are C (carbon) and transition metal elements, and preferred examples of the transition metal elements include Fe (iron), Mn (manganese), Co (cobalt), Cr (chromium), V (vanadium), Ni (nickel), and Cu (copper). The total concentration of the compensating impurities in the carrier compensation region is set to 5 × 10 in order to avoid a significant deterioration of the crystal quality. 19 atoms / cm 3 The following is further 2×10 19 atoms / cm 3 Below, and further 1×10 19 atoms / cm 3 It can be as follows. In the carrier compensation region, the variation in the total concentration of compensation impurities along the c-axis direction is preferably within ±25% of the median, more preferably within ±20%, even more preferably within ±15%, and even more preferably within ±10%.

[0069] When manufacturing the bilayer wafer 40, first the wafer 20 is prepared, and then a stack is obtained by epitaxially growing a GaN layer on the Ga-polarity primary surface of the wafer 20. The wafer 20 is preferably made of only UID-GaN. There is no limitation on the method for growing the GaN layer, and it may be MOCVD, but is preferably HVPE. The growth thickness of the GaN layer is preferably 500 μm or less. At least a part of the GaN layer is intentionally doped to provide a high carrier concentration region or a carrier compensation region. A thinning step is optionally provided for thinning the stack obtained by growing the GaN layer, in which either or both of the N-polarity side of the wafer 20 and the Ga-polarity side of the GaN layer are ground, polished, and / or etched.

[0070] The bilayer wafer 40 has an intentionally doped high carrier concentration region or carrier compensation region on the front layer L. fHowever, their function as substrates for nitride semiconductor device fabrication is not inferior to that of GaN wafers that are intentionally doped throughout, because the fabrication process for nitride semiconductor devices generally includes a thinning step of the epitaxial wafer, in which the GaN wafer used as the substrate is processed from the back side, and a significant portion of it is removed. In the two-layer wafer 40, the back layer L b Even if the layer is completely removed, the remaining surface layer L f serves as a substrate to support the structure of nitride semiconductor device chips The front layer L f The minimum thickness is at least 20 μm, preferably 50 μm or more.

[0071] In addition to the above, the wafer 20 can be used as a seed wafer when growing bulk GaN crystals by HVPE, THVPE (Tri-Halide Vapor Phase Epitaxy), OVPE (Oxide Vapor Phase Epitaxy), ammonothermal, Na flux, and other methods. Wafers 20 that are formed solely of UID-GaN are particularly suitable for this purpose.

[0072] 3. GaN crystal growth method Hereinafter, a GaN crystal growth method that can be preferably used in the manufacture of n-type GaN crystal or GaN wafers according to the embodiments, or in the manufacturing method of GaN wafers according to the embodiments, will be described. 3.1.HVPE Equipment FIG. 9 shows the basic configuration of an HVPE apparatus that can be used to produce n-type GaN crystals or GaN wafers according to the embodiments, or in the methods for producing GaN wafers according to the embodiments. 9, an HVPE apparatus 100 includes a hot-wall type reactor 101, a gallium reservoir 102 and a susceptor 103 disposed within the reactor, and a first heater 104 and a second heater 105 disposed outside the reactor. The first heater 104 and the second heater 105 each surround the reactor 101 in an annular shape.

[0073] The reactor 101 is a quartz tube chamber. Inside the reactor 101, there are a first zone Z1 that is heated mainly by a first heater 104, and a second zone Z2 that is heated mainly by a second heater 105. An exhaust pipe P E is connected to the reactor end on the second zone Z2 side. The gallium reservoir 102 located in the first zone Z1 is a quartz vessel having a gas inlet and a gas outlet. The susceptor 103 disposed in the second zone Z2 is made of, for example, graphite. A mechanism for rotating the susceptor 103 can be provided as desired.

[0074] On the susceptor 103, a seed is placed. Preferably, as shown in FIG. 10(a), an edge cover for covering the edge of the seed is placed on the susceptor together with the seed. The edge cover is formed, for example, from graphite, and its height h is set so that the position of the upper surface of the GaN thick film grown on the seed is not higher than the upper end of the edge cover when the growth is completed, as shown in Figure 10(b). As shown in FIG. 11, the edge cover may cover not only the edge of the seed but also the outer periphery of the main surface of the seed.

[0075] When growing a thick GaN crystal film on a large-area seed, the edge cover plays an important role. In the inventors' experience, when a circular GaN wafer with a diameter of 2 inches was used as a seed, the use of an edge cover was essential to grow a GaN layer thick enough to cut the wafer without cracking. On the other hand, when a GaN wafer with a rectangular main surface but an area larger than a 2-inch diameter circle was used as a seed, it was possible to grow a GaN film of a thickness that allowed the wafer to be cut out without cracking, even without an edge cover. However, the GaN thick film grown without an edge cover had poor surface morphology, with a ridge protruding in the c-axis direction formed along the outer edge, large pits densely occurring on the inner wall surface of the ridge, and fine cracks were observed on the surface of the ridge. When this GaN thick film was sliced ​​along the c-plane, cracks extending from the edge to the center were observed. A lock occurred and the desired wafer could not be obtained.

[0076] 9, when growing GaN crystals, the inside of the reactor 101 is heated by the first heater 104 and the second heater 105, NH3 (ammonia) diluted with a carrier gas is supplied to the second zone Z2 through the ammonia inlet pipe P1, and HCl (hydrogen chloride) diluted with a carrier gas is supplied to the gallium reservoir 102 through the hydrogen chloride inlet pipe P2. This HCl reacts with metallic gallium in the gallium reservoir 102, and the resulting GaCl (gallium chloride) is transported to the second zone Z2 through the gallium chloride inlet pipe P3. In the second zone Z2, NH3 and GaCl react with each other, and the resulting GaN crystallizes on the seed placed on the susceptor 103.

[0077] When the GaN crystal growing on the seed is doped with an impurity, a doping gas diluted with a carrier gas is introduced into the second zone Z2 in the reactor 101 through a dopant introduction pipe P4. The portions of the ammonia introduction pipe P1, the hydrogen chloride introduction pipe P2, the gallium chloride introduction pipe P3, and the dopant introduction pipe P4 that are disposed within the reactor 101 can be made of quartz.

[0078] In FIG. 9, the distance from the nozzle to the susceptor 103 is the same for the ammonia introduction pipe P1 and the gallium chloride introduction pipe P3, but this is not limited thereto, and the nozzle of the ammonia introduction pipe P1 may be opened at a position farther from the susceptor 103 (upstream) than the nozzle of the gallium chloride introduction pipe P3. Alternatively, the nozzle of the ammonia introduction pipe P1 and the nozzle of the gallium chloride introduction pipe P3, which are separate in FIG. 9, may be integrated to form a double-pipe nozzle with the former as an outer pipe and the latter as an inner pipe.

[0079] 9, the nozzles of the gallium chloride introduction tube P3 and the dopant introduction tube P4 are depicted as being independent, but this is not intended to be limiting. For example, the nozzle of the dopant introduction tube P4 may be opened into the gallium chloride introduction tube P3 so that GaCl and the doping gas are mixed and then released into the second zone Z2 through a common nozzle in order to uniformly dope the growing GaN crystal.

[0080] When doping the growing GaN crystal with Si, the doping gases are SiH4 (silane), SiH3Cl (monochlorosilane), SiH2Cl s (dichlorosilane), SiHCl3 (trichlorosilane) or SiCl4 (tetrachlorosilane) may preferably be used. When doping the growing GaN crystal with Ge, the doping gases include GeH4 (germane), GeH3Cl (monochlorogermane), and GeH2Cl. s (dichlorogermane), GeHCl3 (trichlorogermane) or GeCl4 (tetrachlorogermane) may preferably be used. Although the grown GaN crystals are not intentionally doped, they may contain O and Si. The unintentional Si probably comes from the quartz that constitutes the reactor or piping, and the unintentional O probably comes from either or both of the quartz and moisture that has infiltrated into the reactor from the outside.

[0081] The components arranged in the reactor 101, including those omitted in FIG. 9, are made of quartz and carbon, as well as silicon carbide (SiC), silicon nitride (SiN x(silicon nitride), BN (boron nitride), alumina, W (tungsten), Mo (molybdenum), etc. can be used. By doing so, the concentration of each impurity except for Si, O, and H in the GaN crystal grown on the seed is 5 × 10 unless intentionally doped. 15 atoms / cm 3 It can be the following:

[0082] 3.2.Seed A suitable example of a seed used for growing n-type GaN crystals or GaN wafers according to the embodiment is a c-plane GaN wafer grown by an acidic ammonothermal method using NH4F and NH4I as mineralizers, and the manufacturing method thereof can be referred to in the aforementioned Patent Document 1 (WO2018 / 030311A1). This c-plane GaN wafer is often 10 18 atoms / cm 3 Although the oxygen concentration is in the mid-level range, the oxygen concentration on the Ga-polar main surface is 3×10 16 atoms / cm 3 The following GaN crystals can be grown by HVPE with little strain: The inclination of the main surface with respect to the (0001) crystal plane is preferably within a range of 0 to 1 degree, more preferably 0 to 0.5 degrees.

[0083] 3.3. Growth conditions The preferred conditions for growing a GaN crystal on a seed by HVPE are as follows. The temperature of the gallium reservoir is, for example, 500 to 1000°C, preferably 700°C or higher, and preferably 900°C or lower. The susceptor temperature is, for example, 900 to 1100° C., preferably 930° C. or higher, more preferably 950° C. or higher, and preferably 1050° C. or lower, more preferably 1020° C. or lower.

[0084] The V / III ratio, which is the ratio of NH3 partial pressure to GaCl partial pressure in the reactor, can be, for example, 1 to 20, but is preferably 2 or more, more preferably 3 or more, and is preferably 10 or less. Too large or too small a V / III ratio can cause the surface morphology of the growing GaN to deteriorate, which in turn leads to a decrease in crystal quality and an increase in the concentration of oxygen unintentionally incorporated into the GaN crystal.

[0085] The incorporation efficiency of some impurities into GaN crystals strongly depends on the orientation of the facets exposed on the GaN surface during growth. The concentration of such impurities is less uniform inside GaN crystals that had poor surface morphology during growth, because the poor morphology surface has facets with various orientations. A typical example of such an impurity is O (oxygen), but the inventors have found that Ge (germanium) also has a similar tendency. As will be described later, this is related to the fact that when intentionally growing Ge-doped GaN crystals, it is better not to lower the molar ratio of H2 in the carrier gas too much.

[0086] In addition, using too low a V / III ratio increases the concentration of nitrogen vacancies in the growing GaN crystal. Although the effect of nitrogen vacancies on GaN wafers and nitride semiconductor devices formed on GaN wafers is not yet clear, their concentration should be as low as possible because they are point defects.

[0087] The growth rate of the GaN crystal can be controlled by using the product of the NH3 partial pressure and the GaCl partial pressure in the reactor as a parameter, and is, for example, 20 to 200 μm / h, preferably 30 μm / h or more, more preferably 40 μm / h or more, and preferably 120 μm / h or less, more preferably 100 μm / h or less, and even more preferably 80 μm / h or less. The inventors have discovered that when growing GaN crystals by HVPE on a high-quality seed consisting of a GaN crystal grown by the acidic ammonothermal method, if the growth rate is made too low, a problem occurs in which localized areas where growth has stopped are formed on the growth surface.

[0088] When a low growth rate of 20 μm / h to 50 μm / h is adopted, it is possible to preferably prevent the generation of new threading dislocations at the interface between a seed made of a GaN crystal grown by the acidic ammonothermal method and a GaN crystal grown on the seed by HVPE. In order to improve production efficiency, the growth rate may be increased during growth. When the initial growth rate is 40 μm / h and the growth rate is increased to 80 μm / h or 120 μm / h during the growth, the threading dislocation density of the GaN crystal grown at 80 μm / h is the same as that of a seed made of a GaN crystal grown by the acidic ammonothermal method, and the threading dislocation density of the GaN crystal grown at 120 μm / h is at most twice that of the seed. The growth rate should be increased within a range that does not deteriorate the surface morphology of the growing GaN crystal, as described above.

[0089] As a carrier gas for diluting NH3, HCl and the doping gas, H2 (hydrogen gas), N2 (nitrogen gas) or a mixed gas of H2 and N2 can be preferably used. The molar ratio of H2 in the carrier gas affects the impurity concentration of the growing GaN crystal. Note that the molar ratio of H2 in the carrier gas is calculated based on the flow rate of each gas species supplied as a carrier gas from outside the reactor to inside the reactor.

[0090] For reference, we investigated how the impurity concentrations of Si-doped GaN and Ge-doped GaN grown by HVPE at approximately the same growth rate using the same V / III ratio on the Ga polarity surface of a c-plane GaN wafer cut from a GaN crystal grown by HVPE on a sapphire substrate change depending on the molar ratio of H2 in the carrier gas. The doping gas used was SiH2Cl2 for Si doping and GeCl4 for Ge doping.

[0091] [Table 1]

[0092] As can be seen from Table 1, the O concentration of Si-doped GaN crystals can be 10% or less of the Si concentration when the H2 molar ratio of the carrier gas is 0 (zero). Since the donor impurity other than Si is essentially only O, this is equivalent to the total concentration of donor impurities other than Si being 10% or less of the Si concentration. If the H2 molar ratio in the carrier gas is increased, the O concentration of Si-doped GaN becomes even lower, and can be less than 1% of the Si concentration when the molar ratio is 0.7.

[0093] On the other hand, in Ge-doped GaN crystals, when the molar ratio of H2 in the carrier gas is 0 (zero), the Ge concentration is 10 times higher than when the molar ratio is 0.7, and the ratio of Ge concentration to Si concentration is also high. Therefore, at first glance, it seems that the lower the molar ratio of H2 in the carrier gas, the higher the Ge concentration. Although this seems like a desirable option, it is not necessarily so. When the molar ratio of H2 in the carrier gas is 0 (zero), the O concentration is one order of magnitude higher than when the molar ratio is 0.7. As can be seen from this, the surface morphology of the growing GaN is poor when the molar ratio is 0, and the inventors have confirmed that this is also the cause of the high Ge concentration. Since both O and Ge are donor impurities, problems such as reduced uniformity of the carrier concentration can occur in GaN crystals grown under conditions where the molar ratio of H2 in the carrier gas is too low. Therefore, it is preferable that the molar ratio of H2 in the carrier gas during Ge doping is about 0.3 to 0.7. In the Ge-doped GaN crystal grown under such conditions, the Ge concentration is 1×10 18 atoms / cm 3 When the Si concentration is 4×10 17 atoms / cm 3 That's all.

[0094] Regardless of whether the doping is with Si or Ge, the O concentration in GaN crystals grown by HVPE tends to decrease with increasing the molar ratio of H in the carrier gas, decreasing by 2×10 16 atoms / cm 3 Below, and further 1×10 16 atoms / cm 3 This is believed to be due to the improved surface morphology of the growing GaN crystal. The crystal quality of the c-plane GaN seed wafer also affects the surface morphology of the GaN crystal grown on it: GaN crystals with lower O concentrations can be grown on seeds with higher quality. When growing a GaN crystal on a seed, the doping gas may be supplied from the beginning, but it is preferable to start the supply after the growth thickness of the GaN layer reaches at least 10 μm. It is also preferable to gradually increase the supply rate of the doping gas to a predetermined value over a period of several minutes to several tens of minutes from the start of the supply.

[0095] 4. Experimental Results The experiments carried out by the present inventors are described below. In the experiment, a crystal growth apparatus with the basic configuration shown in Fig. 12 was used to grow GaN crystals by the ammonothermal method. This crystal growth apparatus includes an autoclave and a capsule made of Pt-Ir alloy placed inside it. The capsule has a melting zone and a growth zone separated from each other by a Pt baffle. When growing GaN crystals, a feedstock is placed in the melting zone together with a mineralizer (not shown), and a seed is suspended in the growth zone by a Pt wire. A gas line connected to a vacuum pump, an ammonia cylinder, and a nitrogen cylinder is connected to the autoclave and the capsule via a valve. When NH3 (ammonia) is put into the capsule, the amount of NH3 supplied from the ammonia cylinder can be checked with a mass flow meter.

[0096] The amount of NH3 put into the capsule determines the pressure inside the capsule when it is heated to a certain temperature. NH3 is sealed not only inside the capsule but also in the space between the autoclave and the capsule so that the pressure inside and outside the capsule are balanced. Once the seeds, feedstock and mineralizers are installed and the introduction of NH3 is complete, the capsule is sealed and heated from the outside of the autoclave with heaters (not shown) to achieve supercritical conditions inside. The top and bottom of the autoclave are heated separately by multiple heaters to provide a temperature gradient between the dissolution zone and the growth zone.

[0097] 4.1.Experiment 1 (1) Seed preparation First, a first c-plane GaN wafer having a thickness of 0.4 mm was prepared, which was grown by the ammonothermal method using NH4F and NH4I as mineralizers. On the mirror-finished N-polar surface of the first c-plane GaN wafer, a lift-off method is used, A stripe pattern selective growth mask was formed from a two-layer sputtered film in which a 100 nm thick Pt surface layer was laminated on a 100 nm thick TiW underlayer. The line width of the linear openings in the selective growth mask was 50 μm, and the pitch between the linear openings was 2 mm. The stripe direction was parallel to the a-plane of the GaN crystal constituting the wafer.

[0098] A first c-plane GaN wafer having such a selective growth mask formed on its N-polar surface was used as a seed to grow a GaN crystal by the ammonothermal method. The ammonothermal process used polycrystalline GaN as the feedstock and NH4F and NH4I as mineralizers. The polycrystalline GaN was produced by contacting elemental Ga with HCl gas under heating to generate gaseous GaCl, which was then reacted with NH3 gas. The amount of mineralizers, NH4F and NH4I, was 1.0% in terms of molar ratio to the NH3 solvent. The NH4I mineralizer was synthesized by reacting HI (hydrogen iodide) gas with NH3 in a Pt-Ir capsule, which was the reaction vessel.

[0099] In the ammonothermal process, the average values ​​of the temperature T1 of the melting zone and the temperature T2 of the growth zone were between 600°C and 620°C, the temperature difference between the two zones T1-T2 (T1>T2) was between 5°C and 10°C, and the pressure inside the capsule was between 200MPa and 230MPa. These conditions were maintained for more than 30 days. On the N-polarity surface of the first c-plane GaN wafer, as shown in FIG. 13, GaN crystals were grown in a layer with a thickness t of 3 mm. A void was formed in the portion adjacent to the selective growth mask, and the height h of the void, i.e., the distance from the top surface of the selective growth mask to the top end of the void, was between 0.5mm and 1mm. It should be noted that GaN crystals were also grown on the Ga-polarity surface of the first c-plane GaN wafer, but this is not shown in FIG. 13.

[0100] The grown GaN crystal layer was then processed to form a second c-plane GaN wafer with a thickness of 0.4 mm. The Ga polar surface of the second c-plane GaN wafer was mirror-flattened by grinding, and then finished by CMP to remove the damaged layer. When a c-plane GaN wafer produced by the same method as the second c-plane GaN wafer was measured, the full width at half maximum of the (004) XRD rocking curve was less than 10 arcsec.

[0101] (2) Preparation of Ge-doped c-plane GaN wafers The second c-plane GaN wafer is cut into pieces each having a Ga polar surface area of ​​about 7 cm 2Using a 0.4 mm thick c-plane GaN wafer as a seed, a GaN thick film was grown by HVPE on the Ga polarity surface using a vapor phase growth apparatus having the same basic configuration as the HVPE apparatus shown in Figure 9. The procedure is roughly as follows. First, the seeds were placed on the susceptor without using an edge cover. Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.25 atm, 0.73 atm and 0.02 atm, respectively, while the reactor was heated by a heater installed outside the reactor.

[0102] After the susceptor temperature reached 1002°C, the susceptor temperature was kept constant to grow GaN. The Ga reservoir temperature was set to 800°C. The carrier gas supplied to the reactor was 69% H2 by molar ratio, and the remainder N2. For 60 minutes after the start of growth, the partial pressures of GaCl and NH3 were 7.7×10 -3 atm and 2.3 × 10 -2 Atm was supplied into the reactor, and no doping gas was intentionally supplied.

[0103] 60 minutes after the start of growth, GeCl4 (tetrachlorogermane) was added to the reactor. The GeCl4 feed rate was gradually increased over a period of 5 min. After the supply rate of GeCl4 reached a predetermined value, GaCl, NH3, and GeCl4 were supplied at partial pressures of 7.7 × 10 -3 atm, 2.3×10 -2 atm and 1.7 × 10 -7 A Ge-doped GaN film was grown to a thickness of approximately 2.7 mm by supplying a Ge concentration of 1.0 atm to the reactor. The growth rate of the Ge-doped GaN thick film calculated from the thickness and growth time was about 33 μm / min.

[0104] Next, this Ge-doped GaN thick film was sliced ​​parallel to the c-plane, and the Ga polarity surface of the resulting wafer was flattened by grinding and then subjected to CMP finishing. Slicing damage on the N polarity surface side of the wafer was removed by etching. The wafer was then cut to a thickness of 335 μm and a main surface area of ​​approximately 7 cm2. 2 Thus, a Ge-doped c-plane GaN wafer (hereinafter also referred to as "sample E-1") was completed.

[0105] (3) Evaluation <(004) XRD rocking curve FWHM> A (004) XRD rocking curve measurement was performed on sample E-1 at a position on the Ga polar surface away from the edge. For the measurements, the line-focus CuKα source of the X-ray diffraction device [PANalytical X'Pert Pro MRD, Spectris, Inc.] was operated at 45 kV and 40 mA, and CuKα1 radiation was obtained using a Ge(440)4 crystal symmetric monochromator. The optical system used was a parallel optical system, with a 1 / 2 slit, an X-ray mirror, and a cross slit of w1 mm x h1 mm on the entrance side. The detector was a PIXcel semiconductor pixel detector. 3D The 0D mode of the NIRS (registered trademark) was used. The angular resolution was 5 to 6 arcsec.

[0106] The X-ray beam size was set so that when the incident angle was 90°, i.e., when the X-rays were incident perpendicularly to the Ga polar surface of the sample substrate, the size of the irradiation area on the Ga polar surface was 5 mm in the direction parallel to the ω axis and 1 mm in the direction perpendicular to the ω axis. In the rocking curve measurement, the X-ray was incident on the sample from a direction perpendicular to the a-axis of the GaN crystal. In other words, the incidence plane of the X-ray was parallel to the a-plane of the GaN crystal. The FWHM of the (004) XRD rocking curve was 8.5 arcsec.

[0107] <Electrical characteristics> The room temperature resistivity of sample E-1, and the carrier concentration and carrier mobility at room temperature obtained by Hall measurement are 0.012 Ω cm and 1.5 × 1018 cm -3 and 347 cm 2 / V s.

[0108] <Impurity concentration> The impurity concentration of sample E-1 was measured by dynamic SIMS and found to be 1.4×10 18 atoms / cm 3 , Si concentration is 7.0×10 17 atoms / cm 3 , O concentration is 6.8 × 10 15 atoms / cm 3 and the concentrations of H, Cl, and C were below the detection limit. The detection limit for this SIMS measurement is 1×10 15 atoms / cm 3 , Si is 5 × 10 14 atoms / cm 3 , O is 4 x 10 15 atoms / cm 3 , H(hydrogen) is 2×10 16 atoms / cm 3 , Cl (chlorine) is 1×10 14 atoms / cm 3 , C(carbon) is 3×10 15 atoms / cm 3 It was.

[0109] 4.2.Experiment 2 As a seed, a GaN wafer with a Ga polarity surface area of ​​approximately 6 cm2 and with the same crystal quality as the second c-plane GaN wafer prepared in experiment 1 was used. 2 A 0.4 mm thick c-plane GaN wafer was prepared using NH4 The seed was prepared from a GaN crystal grown by the ammonothermal method using F and NHI. A GaN thick film was grown by HVPE on the Ga polar surface of the seed using the same vapor phase epitaxy apparatus as that used in experiment 1. The procedure is roughly as follows. First, the seed was set on the susceptor of the vapor phase growth apparatus. No edge cover was used. Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.67 atm, 0.31 atm and 0.02 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor.

[0110] After the susceptor temperature reached 1000°C, the susceptor temperature was kept constant and GaN was grown. The Ga reservoir temperature was set to 900°C. The carrier gas supplied to the reactor during growth was 69% H2 by molar ratio, with the remainder being N2. For 60 minutes after the start of growth, the partial pressures of GaCl and NH3 were 7.9×10 -3 atm and 2.4 × 10 -2 Atm was supplied into the reactor, and no doping gas was intentionally supplied.

[0111] Sixty minutes after the start of growth, the supply of SiH2Cl2 into the reactor was started, and the supply rate of SiH2Cl2 was gradually increased over a period of 5 minutes. After the supply rate of SiH2Cl2 reached a predetermined value, GaCl, NH3, and SiH2Cl2 were fed at partial pressures of 7.9×10 -3 atm, 2.4×10 -2 atm and 1.9×10 -8 A Si-doped GaN film was grown to a thickness of approximately 2.38 mm by supplying nitrogen to the reactor at a pressure of 1.0 atm. The growth rate of the Si-doped GaN thick film calculated from the thickness and growth time was 40 μm / h.

[0112] Next, this Si-doped GaN thick film was sliced ​​parallel to the c-plane, and the Ga polarity surface of the resulting wafer was flattened by grinding and then CMP-finished. Slicing damage on the N polarity surface of the wafer was removed by etching. The wafer was then cut to a thickness of 335 μm and a main surface area of ​​approximately 6 cm2. 2 Thus, a Si-doped c-plane GaN wafer (hereinafter also referred to as "sample E-2") was completed.

[0113] The (004) XRD rocking curve of sample E-2 was measured at a position on the Ga polar surface away from the edge in the same manner as in experiment 1, and the FWHM was found to be 10.0 arcsec. The room temperature resistivity of sample E-2, and the carrier concentration and carrier mobility at room temperature obtained by Hall measurement are 0.013 Ω cm and 1.3 × 10 18 cm -3 and 391 cm 2 / V s.

[0114] The impurity concentration of sample E-2 was measured by dynamic SIMS, and the Si concentration was 1.4×10 18 atoms / cm 3 The concentrations of O (oxygen), H (hydrogen), Cl (chlorine) and C (carbon) were below the detection limit. The detection limit for this SIMS measurement was 5×10 14 atoms / cm 3 , O is 4 x 10 15 atoms / cm 3 , H is 2 × 10 16 atoms / cm 3 , Cl is 1×10 14 atoms / cm 3 , C is 3 × 10 15 atoms / cm 3 It was. In sample E-2, the total concentration of donor impurities excluding Si was less than 1% of the Si concentration, and the carrier concentration was 93% of the Si concentration.

[0115] 4.3.Experiment 3 As a seed, a GaN wafer with a Ga polarity surface area of ​​approximately 33 cm2 and with the same crystal quality as the second c-plane GaN wafer prepared in experiment 1 was used. 2 A 0.4 mm thick c-plane GaN wafer was prepared by nitriding with NH The seed was grown from a GaN crystal grown by the ammonothermal method using 4F and NHI. A GaN thick film was grown by HVPE on the Ga polar surface of the seed using the same type of vapor phase epitaxy apparatus as that used in experiment 1. The procedure is roughly as follows. First, a seed was placed on the susceptor of a vapor phase growth apparatus and was surrounded by a 6 mm high graphite edge cover that was attached closely to the edge of the seed.

[0116] Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.73 atm, 0.24 atm and 0.024 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor. After the susceptor temperature reached 1000°C, the susceptor temperature was kept constant and GaN was grown. The temperature of the Ga boat was set to 900°C. The carrier gas supplied to the reactor during growth was 75% H2 by molar ratio, and the remainder N2.

[0117] For 60 minutes after the start of growth, the partial pressures of GaCl and NH3 were 7.9×10 -3 atm and 2.4 × 10 -2 Atm was supplied into the reactor, and no doping gas was intentionally supplied. Sixty minutes after the start of growth, the supply of SiH2Cl2 into the reactor was started, and the supply rate of SiH2Cl2 was gradually increased over a period of 5 minutes. After the supply rate of SiH2Cl2 reached a predetermined value, GaCl, NH3, and SiH2Cl2 were fed at partial pressures of 7.9×10 -3 atm, 2.4×10 -2 atm and 1.6×10 -3 A Si-doped GaN thick film was grown to about 2 mm by supplying nitrogen to the reactor at a pressure of 1 atm. The growth rate of the Si-doped GaN thick film calculated from the thickness and growth time was 35 μm / h.

[0118] The grown GaN thick film was then sliced ​​parallel to the c-plane, and the Ga polarity surface of the resulting wafer was flattened by grinding, followed by CMP finishing. Slicing damage on the N polarity surface of the wafer was removed by etching. The wafer was then cut to a thickness of 360 μm and a main surface area of ​​approximately 30 cm.2 Thus, a Si-doped c-plane GaN substrate (hereinafter also referred to as "sample E-3") was completed.

[0119] The (004) XRD rocking curve was measured on the Ga polar face side of sample E-3. First, a line passing through the approximate center of the Ga polarity plane and perpendicular to the m-axis was scanned at ω-scan intervals of 1 mm over a length of 40 mm to obtain (004) XRD rocking curves at 40 measurement points arranged at 1 mm pitch on the line. The measurement conditions at each measurement point were the same as in Experiment 1, except that the X-ray was incident on the sample from a direction perpendicular to the m-axis of the GaN crystal. The maximum value of the (004) XRD rocking curve FWHM among 40 measurement points was 19.3 arcsec, and the average value was 10.5 arcsec.

[0120] Next, a line passing through the approximate center of the Ga polarity plane and perpendicular to the a-axis was scanned at ω-scan intervals of 1 mm over a length of 40 mm to obtain (004) XRD rocking curves at 40 measurement points arranged at 1 mm pitch on the line. The measurement conditions at each measurement point were the same as in Experiment 1. The maximum value of the (004) XRD rocking curve FWHM among 40 measurement points was 16.2 arcsec, and the average value was 10.4 arcsec. The carrier concentration of sample E-3 measured at the center of the Ga polar surface was 1.5×10 18 cm -3 It was.

[0121] 4.4.Experiment 4 As a seed, a GaN wafer with a Ga polarity surface area of ​​approximately 32 cm2 and with the same crystal quality as the second c-plane GaN wafer prepared in experiment 1 was used. 2 A 0.56 mm thick c-plane GaN wafer was prepared from a GaN crystal grown by ammonothermal method using NH4F and NHI as mineralizers. A GaN thick film was grown by HVPE on the Ga polar face of this seed using the same type of vapor phase epitaxy apparatus as that used in experiment 1. The procedure is roughly as follows. First, a seed was set on a susceptor of a vapor phase growth apparatus, and the edge of the seed and the outer periphery of the Ga polar surface were covered with a graphite edge cover having a height of 4 mm.

[0122] Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.30 atm, 0.65 atm and 0.052 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor. GaN growth was started when the susceptor temperature reached 960° C. Ten minutes after the start of growth, the supply of SiH2Cl2 into the reactor was started. The supply rate of SiH2Cl2 was gradually increased over 30 minutes.

[0123] The growth conditions from the start of growth until 3 hours later were: gallium reservoir temperature 800°C, susceptor temperature 960°C, GaCl partial pressure 6.0×10 -3 atm, NH3 partial pressure 4.1×10 -2 atm, SiH2Cl2 partial pressure 2.1×10 -8 Atm. After 3 hours had passed, the susceptor temperature was increased to 998° C. The carrier gas supplied to the reactor was 40% H2 by molar ratio, and the remainder N2. In this way, a Si-doped GaN thick film was grown to a thickness of about 2.2 mm at a growth rate of 37 μm / h.

[0124] The grown GaN thick film was then sliced ​​parallel to the c-plane, and the Ga polarity surface of the resulting wafer was flattened by grinding, followed by CMP finishing. Slicing damage on the N polarity surface of the wafer was removed by etching. The wafer was then cut to a thickness of 400 μm and a main surface area of ​​approximately 16 cm2. 2 Thus, a c-plane GaN wafer (hereinafter also referred to as "sample E-4") was completed.

[0125] The (004) XRD rocking curve was measured on the Ga polar face side of sample E-4. By performing ω-scans at 1 mm intervals along a line that passes through the center of the Ga polar plane and is perpendicular to the m-axis over a length of 40 mm, (004) XRD rocking curves were obtained at 40 measurement points arranged at 1 mm pitch on the line. The measurement conditions at each measurement point were the same as in experiment 1, except that the X-rays were incident on the sample from a direction perpendicular to the m-axis of the GaN crystal. The maximum value of the (004) XRD rocking curve FWHM among 40 measurement points was 17.8 arcsec, and the average value was 11.2 arcsec.

[0126] The carrier concentration of sample E-4 measured at the center of the Ga polar surface was 1.5×10 18 cm -3 It was. The crystal quality was equivalent to that of sample E-4, and the carrier concentration at the center of the Ga polarity plane was 2.8 × 10 18 cm -3 It was also possible to grow c-plane GaN substrates.

[0127] 4.5. Experiment 5 As a seed, a GaN wafer with a Ga polarity surface area of ​​approximately 33.8 cm2 and a crystal quality equivalent to that of the second c-plane GaN wafer prepared in Experiment 1 was used. 2 A 0.55 mm thick c-plane GaN wafer was prepared from a GaN crystal grown by ammonothermal method using NH4F and NHI as mineralizers. A GaN thick film was grown by HVPE on the Ga polar face of this seed using the same type of vapor phase epitaxy apparatus as that used in experiment 1. The procedure is roughly as follows. First, a seed was set on a susceptor of a vapor phase growth apparatus, and the edge of the seed and the outer periphery of the Ga polar surface were covered with a graphite edge cover having a height of 4 mm.

[0128] Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.30 atm, 0.65 atm and 0.052 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor. GaN growth was started when the susceptor temperature reached 1005°C. The growth conditions were gallium reservoir temperature 800°C, susceptor temperature 1005°C, GaCl partial pressure 9.0×10 -3 atm, NH3 partial pressure 4.1×10 -2 The carrier gas supplied to the reactor was 38% H2 in molar ratio and the remainder N2.

[0129] Furthermore, 5 hours after the start of growth, the supply of GeCl4 into the reactor was started. The GeCl4 partial pressure was gradually increased to 1.9×10 -7 atm and then kept constant. In this way, a Ge-doped GaN thick film was grown to a thickness of about 3 mm at a growth rate of 47 μm / h.

[0130] The grown GaN thick film was then sliced ​​parallel to the c-plane, and the Ga polarity surface of the resulting wafer was flattened by grinding, followed by CMP finishing. Slicing damage on the N polarity surface of the wafer was removed by etching. The wafer was then cut to a thickness of 400 μm and a main surface area of ​​approximately 19.5 cm2. 2 Thus, a c-plane GaN wafer (hereinafter also referred to as "Sample E-5") was completed.

[0131] The (004) XRD rocking curve was measured on the Ga polar face side of sample E-5. First, a (004) XRD rocking curve was obtained at 40 measurement points arranged at 1 mm pitch along a line passing through the center of the Ga polarity plane and perpendicular to the m-axis, by performing ω-scans every 1 mm over a length of 40 mm. The measurement conditions at each measurement point were the same as in Experiment 1, except that the X-rays were incident on the sample from a direction perpendicular to the m-axis of the GaN crystal. The maximum value of the (004) XRD rocking curve FWHM among 40 measurement points was 9.4 arcsec, and the average value was 7.5 arcsec.

[0132] Next, a line passing through the approximate center of the Ga polarity plane and perpendicular to the a-axis was scanned at ω-scan intervals of 1 mm over a length of 40 mm to obtain (004) XRD rocking curves at 40 measurement points arranged at 1 mm pitch on the line. The measurement conditions at each measurement point were the same as in Experiment 1. The maximum value of the (004) XRD rocking curve FWHM among 40 measurement points was 11.0 arcsec, and the average value was 7.9 arcsec. The carrier concentration of sample E-5 measured at the center of the Ga polar surface is 4.9×10 18 cm -3 It was.

[0133] Furthermore, the number of dark spots in the PL images observed within a square area of ​​230 μm × 230 μm was counted at multiple measurement points on the Ga polar surface of sample E-5 using a PL (photoluminescence) imaging device [PLI-200 manufactured by Photon Design Inc.]. The PL images were acquired using a mercury lamp as the excitation source, with an excitation wavelength of 313 nm and a detection wavelength of 365 ± 5 nm. The detector was a 2048 × 2048 pixel CMOS camera, so the pixel resolution was approximately 0.11 μm. The measurement points were located on the lattice points of a square lattice with each side being 2.88 mm, and the number of measurement points was 381. The average scotoma density among 381 measurement points was 3.3 × 10 4 cm -2 Then, a dark spot was observed. The number of measurement points where no scotoma was observed was 54% of the total. When calculating the average value, the scotoma density at the measurement points where no scotoma was observed was 0 cm -2 The dislocation density at the measurement point where only one dark spot was observed was 230 × 230 μm 2 Since there is one per unit, it is 1.9 x 10 3 cm -2 It was decided. After the above-mentioned measurement of the dark spot density by PL imaging, sample E-5 was etched for 1 hour with 89% sulfuric acid heated to 270°C, and the etch pits formed on the Ga polar surface corresponded one-to-one to the dark spots in the PL image. The inventors have separately confirmed that the etch pits formed by this method also correspond one-to-one to the dark spots appearing in the cathodoluminescence image.

[0134] This sample was sliced ​​from the Ge-doped GaN thick film with a thickness of about 3 mm at the same time as sample E-5, and processed in the same way as sample E-5 to a thickness of 400 μm and a main surface area of ​​about 20 cm. 2 We investigated the variation of the offcut angle in the primary surface of a c-plane GaN wafer. When the direction parallel to one of the a-planes was selected as the x direction and the direction perpendicular to the x direction was selected as the y direction, the variation range of the x-direction component of the offcut angle on a 4 cm long line passing through the center of the Ga polarity surface and extending in the x direction was 0.04 degrees (±0.02 degrees from the center value), and the variation range of the y-direction component of the offcut angle on a 4 cm long line passing through the center of the Ga polarity surface and extending in the y direction was 0.06 degrees (±0.03 degrees from the center value).

[0135] 4.6. Experiment 6 As a seed, a c-plane GaN wafer with the same crystal quality as the second c-plane GaN wafer produced in experiment 1 was prepared from a GaN crystal grown by the ammonothermal method using NH4F and NHI as mineralizers. Samples E-6a to E-6e were prepared by growing GaN crystals by HVPE on the Ga-polar primary surface of this seed under different conditions using the same type of vapor phase growth apparatus used in experiment 1.

[0136] When growing GaN crystals by HVPE, the susceptor temperature was about 1000°C, the Ga reservoir temperature was 800°C, and the carrier gas supplied to the reactor was 69% H2 by molar ratio, with the remainder being N2. For each of the samples E-6a to E-6e, the first layer grown on the seed was formed at a growth rate of about 40 μm / h.

[0137] Sample E-6a was grown with only the first layer on the seed. Sample E-6b was prepared by growing a first layer followed by a second layer having a thickness of 40 μm at a growth rate of 80 μm / h. Sample E-6c was prepared by growing a first layer followed by a second layer having a thickness of 40 μm at a growth rate of 120 μm / h. Sample E-6d was prepared by growing a first layer followed by a 21 μm thick second layer doped with SiH 2 Cl 2 (dichlorosilane). Sample E-6e was prepared by growing a first layer followed by a 21 μm thick second layer doped with GeCl 4 (tetrachlorogermane).

[0138] The GaN crystal growth conditions by HVPE when each sample was produced are shown in Table 2 below.

[0139] [Table 2]

[0140] In all of the samples E-6a to E-6e, the top surface of the GaN crystal grown on the seed by HVPE was mirror flat when observed with the naked eye. When the cross sections of samples E-6d and E-6e were observed with a fluorescent microscope, the flatness of the interface between the first layer and the second layer was found to be good. The carrier concentration in the second layer of samples E-6d and E-6e, as evaluated by Raman spectroscopy, was 1×10 18 cm -3 It was.

[0141] Using a multiphoton excitation microscope (Nikon Corporation, High-Speed ​​Multiphoton Confocal Laser Microscope System A1R-MP+), three-photon excitation images (3PPL images) of each of samples E-6a to E-6e were observed from the surface side of the HVPE-GaN crystal (however, sample E-6a does not have a second layer) as shown in Fig. 14. A Ti-sapphire mode-locked laser with a wavelength of 800 nm was used as the excitation source, and it was driven with a pulse width of 140 fs and a repetition rate of 80 MHz.

[0142] The following was obtained from the 3PPL image observation. The only threading dislocations in the first layer of sample E-6a were those propagated from the seed, and no new threading dislocations were found to have been generated at the interface between the seed and the first layer, or anywhere in the first layer. In sample E-6b, the threading dislocations in the first layer propagated to the second layer without branching at the interface between the first and second layers, and no new threading dislocations were observed in the middle of the second layer. In sample E-6c, unlike sample E-6b, all threading dislocations propagating from the first layer to the second layer branched into two at the interface between the first and second layers, meaning that the number of threading dislocations in the second layer was twice that of the first layer.

[0143] In sample E-6d, some threading dislocations branched into two at the interface between the first and second layers as they propagated from the first layer to the second layer, but the ratio of such threading dislocations was about 1 in 100. No new threading dislocations were observed to occur in the second layer. In sample E-6e, some threading dislocations branched at the interface between the first and second layers when propagating from the first layer to the second layer, but the ratio of such threading dislocations was about 1 in 50. The generation of new threading dislocations in the middle of the second layer was not observed. The 3PPL observation results of samples E-6d and E-6e suggest that doping with Si or Ge has little effect on the threading dislocation density.

[0144] 4.7. Experiment 7 As a seed, a GaN wafer with a Ga polarity surface area of ​​approximately 24.8 cm2 and a crystal quality equivalent to that of the second c-plane GaN wafer prepared in Experiment 1 was used. 2 A 0.53 mm thick c-plane GaN wafer was prepared from GaN crystals grown by ammonothermal method using NH4F and NHI as mineralizers. A selective growth mask with 20 μm line width linear openings in a tilted square lattice pattern was used in the fabrication process of the GaN crystals. The tilted square lattice pattern was composed of two overlapping stripe patterns, each parallel to the a-plane and at an angle of 60 degrees to each other, one with a pitch of 2 mm and the other with a pitch of 15 mm. A GaN thick film was grown by HVPE on the Ga polarity surface of this seed using the same type of vapor phase growth apparatus as that used in experiment 1. The procedure is roughly as follows. First, a seed was set on a susceptor of a vapor phase growth apparatus, and the edge of the seed and the outer periphery of the Ga polar surface were covered with a graphite edge cover having a height of 4 mm.

[0145] Next, N2, H2 and NH3 were supplied into the reactor so that their partial pressures were 0.30 atm, 0.65 atm and 0.052 atm, respectively, while the inside of the reactor was heated by a heater installed outside the reactor. GaN growth was started when the susceptor temperature reached 1005°C. The growth conditions were gallium reservoir temperature 800°C, susceptor temperature 1005°C, GaCl partial pressure 9.2×10 -3 atm, NH3 partial pressure 4.2×10 -2 The pressure was adjusted to 100 atm, and the carrier gas supplied into the reactor was composed of 40% H2 in molar ratio and the remainder N2.

[0146] Furthermore, 5 hours after the start of growth, the supply of GeCl4 into the reactor was started. The GeCl4 partial pressure was gradually increased to 1.6×10 -7 At 5 hours after the start of growth, the GaCl partial pressure was gradually increased to 9.4 × 10 atm over a period of 4 hours. -3 It was an ATM. In this way, a Ge-doped GaN thick film was grown to a thickness of about 3 mm at a growth rate of 43 μm / h.

[0147] The grown GaN thick film was then sliced ​​parallel to the c-plane, and both main surfaces of the resulting wafer were flattened by grinding and then polished with CMP. The wafer was then cut to a thickness of 400 μm and a main surface area of ​​approximately 15.2 cm. 2 Thus, a c-plane GaN wafer (hereinafter also referred to as "sample E-7") was completed. The carrier concentration of sample E-7 measured at the center of the Ga polar surface was 2.0×10 18 cm -3 It was.

[0148] X-ray topography analysis of sample E-7 was performed using an X-ray diffraction apparatus [Rigaku Corporation High Throughput & High Resolution X-ray Topography Imaging System XRTmicron]. Figure 16 shows a transmission X-ray topography image of a 20 mm x 20 mm square area obtained using diffraction from the (110) crystal plane. The X-ray source used was MoKα, and the thickness of the sample was 400 μm, so μ·t = 11.6. Therefore, the X-ray topography image is an anomalous transmission image. In the past, there have been cases where anomalous X-ray transmission images were observed in m-plane GaN wafers made of GaN crystals grown by HVPE (WO2015 / 020161), but this is believed to be the first time that anomalous X-ray transmission has been reported in c-plane GaN wafers grown by HVPE. Referring to FIG. 16, a stripe of defect arrays extending in the left-right direction in the figure and the stripe The defect region is observed extending from the lower left to the upper right at an angle of 60 degrees from the stripe. The stripes are parallel to the a-plane and have a pitch of 2 mm, reflecting the pattern of the selective growth mask used in the production process of the seed c-plane GaN wafer. A transmission X-ray topography image of a 20 mm × 20 mm square area was also obtained for a 350 μm thick c-plane GaN wafer prepared in essentially the same manner except for changing the dopant from Ge to Si.

[0149] Although the present invention has been described above with reference to specific embodiments, each embodiment is presented as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be modified in various ways without departing from the spirit of the invention, and can be combined with features described in other embodiments within the scope of feasibility. [Explanation of symbols]

[0150] 10 crystals 11, 21 First principal surface 12, 22 Second principal surface 20 Wafers 40 Double-layer wafer 43 Regrowth interface 100 HVPE Equipment 101 Reactor 102 Gallium Reservoir 103 Susceptor 104 First Heater 105 Second Heater Z1 First Zone Z2 Second Zone P1 ammonia inlet tube P2 Hydrogen chloride inlet pipe P3 Gallium chloride introduction tube P4 dopant introduction tube P E Exhaust pipe

Claims

1. An n-type GaN crystal characterized in that the donor impurity contained therein at the highest concentration is Ge, the crystal has a room temperature resistivity of less than 0.03 Ω·cm, and the (004) XRD rocking curve FWHM is less than 20 arcsec.

2. 2. The n-type GaN crystal according to claim 1, wherein the crystal has two principal surfaces facing in opposite directions, each of the two principal surfaces having an area of ​​3 cm 2 The n-type GaN crystal has the above structure, and one of the two main surfaces has Ga polarity and is inclined at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane.

3. 3. The n-type GaN crystal according to claim 2, having a diameter of 20 mm or more.

4. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, The donor impurity contained at the highest concentration is Ge; having a room temperature resistivity of less than 0.03 Ω cm; and When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on said one main surface, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less. The n-type GaN crystal is characterized by:

5. 5. The n-type GaN crystal according to claim 4, wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less.

6. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, The donor impurity contained at the highest concentration is Ge; having a room temperature resistivity of less than 0.03 Ω cm; and When a (004) XRD rocking curve is measured every 1 mm along at least two mutually perpendicular lines on one of the main surfaces over a length of 40 mm, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less. The n-type GaN crystal is characterized by:

7. 7. The n-type GaN crystal according to claim 6, wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points on each line is 18 arcsec or less.

8. 8. The n-type GaN crystal according to claim 2, having a room temperature resistivity of less than 0.02 Ω·cm.

9. Carrier concentration is 1×10 18 cm -3 The n-type GaN crystal according to any one of claims 2 to 7.

10. The n-type GaN crystal according to any one of claims 2 to 9, which satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

11. 11. An n-type GaN crystal according to claim 10, which satisfies all of the conditions (a) to (c) regarding impurity concentrations.

12. O concentration is 3 x 10 16 atoms / cm 3 The n-type GaN crystal according to any one of claims 2 to 11, wherein:

13. Ge concentration is 1×10 18 atoms / cm 3 or more, and the Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to any one of claims 2 to 12.

14. The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to any one of claims 2 to 13, wherein:

15. The n-type GaN crystal according to any one of claims 2 to 14, which is a GaN crystal grown by HVPE.

16. A GaN wafer comprising an n-type GaN crystal according to any one of claims 2 to 15.

17. A GaN wafer, comprising a first region made of the n-type GaN crystal according to any one of claims 2 to 15, provided on a Ga-polar side, and a second region having a carrier concentration lower than that of the n-type GaN crystal, provided on an N-polar side.

18. 18. The GaN wafer according to claim 17, wherein the first region has a thickness of 5 μm or more and 250 μm or less.

19. The GaN wafer according to claim 17 or 18, wherein the second region satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

20. 20. The GaN wafer according to claim 19, wherein the second region satisfies all of the conditions (a) to (c) regarding impurity concentrations.

21. The O concentration in the second region is 3×10 16 atoms / cm 3 The GaN wafer according to any one of claims 17 to 20, wherein:

22. The concentration of each impurity in the second region, except for Si, O, and H, is 5×10 15 atoms / cm 3 The GaN wafer according to any one of claims 17 to 21, wherein:

23. 23. The GaN wafer according to claim 17, having a regrowth interface between the first region and the second region.

24. A method for producing an epitaxial wafer, comprising the steps of: preparing a GaN wafer according to any one of claims 16 to 23; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

25. 24. An epitaxial wafer comprising the GaN wafer according to claim 16 and one or more nitride semiconductor layers epitaxially grown on the GaN wafer.

26. A step of preparing a GaN wafer according to any one of claims 16 to 23, and epitaxially growing one or more nitride semiconductor layers on the GaN wafer.

27. An n-type GaN crystal having a room temperature resistivity of less than 0.03 Ω cm, a (004) XRD rocking curve FWHM of less than 20 arcsec, and an impurity concentration satisfying one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

28. 28. The n-type GaN crystal according to claim 27, wherein the crystal has two major surfaces facing in opposite directions, each of the two major surfaces having an area of ​​3 cm 2 The n-type GaN crystal has the above structure, and one of the two main surfaces has Ga polarity and is inclined at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane.

29. 30. The n-type GaN crystal of claim 28 having a diameter of 20 mm or greater.

30. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, having a room temperature resistivity of less than 0.03 Ω cm; When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on the one main surface, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

31. 31. The n-type GaN crystal according to claim 30, wherein an average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less.

32. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, having a room temperature resistivity of less than 0.03 Ω cm; when a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on said one main surface, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less; and An n-type GaN crystal characterized by satisfying one or more of the following conditions (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

33. 33. The n-type GaN crystal according to claim 32, wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less.

34. The n-type GaN crystal according to any one of claims 28 to 33, having a room temperature resistivity of less than 0.02 Ω·cm.

35. Carrier concentration is 1×10 18 cm -3 The n-type GaN crystal according to any one of claims 28 to 33.

36. 36. An n-type GaN crystal according to claim 28, which satisfies all of the conditions (a) to (c) with respect to impurity concentration.

37. O concentration is 3 x 10 16 atoms / cm 3 The n-type GaN crystal according to any one of claims 28 to 36, wherein:

38. The n-type GaN crystal according to any one of claims 28 to 37, wherein the donor impurity contained at the highest concentration is Si.

39. 39. The n-type GaN crystal according to claim 38, wherein the total concentration of donor impurities excluding Si is 10% or less of the Si concentration.

40. 40. The n-type GaN crystal according to claim 39, wherein the carrier concentration is 90% or more of the Si concentration.

41. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to any one of claims 28 to 40, wherein:

42. Ge concentration is 1×10 18 atoms / cm 3 or more, and the Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to any one of claims 28 to 38.

43. The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 43. The n-type GaN crystal of claim 42, wherein:

44. The n-type GaN crystal according to any one of claims 28 to 43, which is a GaN crystal grown by HVPE.

45. A GaN wafer comprising an n-type GaN crystal according to any one of claims 28 to 44.

46. A GaN wafer comprising a first region made of the n-type GaN crystal according to any one of claims 28 to 44, provided on a Ga-polar side, and a second region having a carrier concentration lower than that of the n-type GaN crystal, provided on an N-polar side.

47. 47. The GaN wafer of claim 46, wherein the first region has a thickness of 5 μm or more and 250 μm or less.

48. The GaN wafer according to claim 46 or 47, wherein the second region satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

49. 49. The GaN wafer according to claim 48, wherein the second region satisfies all of the conditions (a) to (c) regarding impurity concentration.

50. The O concentration in the second region is 3×10 16 atoms / cm 3 50. The GaN wafer according to claim 46, wherein:

51. The concentration of each impurity in the second region, except for Si, O, and H, is 5×10 15 atoms / cm 3 The GaN wafer according to any one of claims 46 to 50, wherein:

52. 52. The GaN wafer of any one of claims 46 to 51, having a regrowth interface between the first region and the second region.

53. A method for producing an epitaxial wafer, comprising the steps of: preparing a GaN wafer according to any one of claims 45 to 52; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

54. 53. An epitaxial wafer comprising the GaN wafer according to any one of claims 45 to 52, and one or more nitride semiconductor layers epitaxially grown on the GaN wafer.

55. A method for manufacturing a nitride semiconductor device, comprising the steps of: providing a GaN wafer according to any one of claims 45 to 52; and epitaxially growing one or more nitride semiconductor layers on the provided GaN wafer.

56. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, Having a diameter of 45 mm or more; (004) An n-type GaN crystal characterized in that the XRD rocking curve FWHM is less than 20 arcsec and the impurity concentration satisfies one or more of the following conditions (a) to (c): (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

57. 57. The n-type GaN crystal of claim 56, having a diameter of 95 mm or greater.

58. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on the one main surface, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

59. 59. The n-type GaN crystal according to claim 58, wherein the average value of the (004) XRD rocking curve FWHM among all the measurement points is 18 arcsec or less.

60. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

61. 61. The n-type GaN crystal of claim 60, wherein the average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less.

62. 62. An n-type GaN crystal according to any one of claims 56 to 61, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

63. Si concentration is 5×10 17 atoms / cm 3 The n-type GaN crystal according to any one of claims 56 to 62, wherein:

64. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to any one of claims 56 to 63, wherein:

65. O concentration is 3 x 10 16 atoms / cm 3 The n-type GaN crystal according to any one of claims 56 to 64, wherein:

66. 5×10 17 cm -3 The n-type GaN crystal according to any one of claims 56 to 65, having at least one of a carrier concentration of less than 0.01 and a room temperature resistivity of 0.04 Ω cm or more.

67. The n-type GaN crystal according to any one of claims 56 to 66, which is a GaN crystal grown by HVPE.

68. A GaN wafer comprising an n-type GaN crystal according to any one of claims 56 to 67.

69. A semiconductor device according to any one of claims 56 to 67, comprising a back layer made of the n-type GaN crystal and a front layer made of GaN with a minimum thickness of 20 μm or more formed on a main surface on the Ga polarity side of the n-type GaN crystal via a regrowth interface, wherein at least a portion of the front layer within a distance of 5 μm from the top surface is included in a high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The above area is a bilayer GaN wafer.

70. 70. The bilayer GaN wafer of claim 69, wherein at least a portion of the front layer within 20 μm from the top surface includes the high carrier concentration region.

71. The high carrier concentration region has a lower limit of the carrier concentration of 2×10 18 cm -3 71. The bilayer GaN wafer of claim 69 or 70, wherein the above region.

72. The bilayer GaN wafer according to any one of claims 69 to 71, wherein the front layer satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

73. 73. The bilayer GaN wafer of claim 72, wherein said front layer satisfies all of said conditions (a) to (c) regarding impurity concentration.

74. The O concentration in the front layer is 3×10 16 atoms / cm 3 69. The method of claim 69, 74. The bilayer GaN wafer according to any one of claims 1 to 73.

75. The bilayer GaN wafer of any one of claims 69 to 74, wherein the high carrier concentration region is doped with Si.

76. The concentration of each impurity in the front layer, except for Si, O, and H, is 5×10 15 atoms / cm 3 76. The bilayer GaN wafer of claim 75, wherein:

77. The bilayer GaN wafer of any one of claims 69 to 75, wherein the high carrier concentration region is doped with Ge.

78. The concentration of each impurity in the front layer, except for Ge, Si, O, and H, is 5×10 15 atoms / cm 3 78. The bilayer GaN wafer of claim 77, wherein:

79. The bilayer GaN wafer of any one of claims 69 to 78, wherein in the high carrier concentration region, the variation in carrier concentration or total concentration of donor impurities along the c-axis direction is within ±25% of the median value.

80. A semiconductor device according to any one of claims 56 to 67, comprising a back layer made of the n-type GaN crystal and a front layer made of GaN with a minimum thickness of 20 μm or more formed on a main surface on the Ga polarity side of the n-type GaN crystal via a regrowth interface, wherein at least a portion of the front layer within a distance of 5 μm from the top surface is included in a carrier compensation region, and the lower limit of the total concentration of compensation impurities in the carrier compensation region is 1×10 17 atoms / cm 3 The above area is a bilayer GaN wafer.

81. 81. The bilayer GaN wafer of claim 80, wherein at least a portion of the front layer within 20 μm from the top surface is included in the carrier compensation region.

82. The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 82. The bilayer GaN wafer of claim 80 or 81, wherein the above region.

83. The bilayer GaN wafer according to any one of claims 80 to 82, wherein the front layer satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

84. 84. The bilayer GaN wafer of claim 80, wherein in the carrier compensation region, the variation in total concentration of compensation impurities along the c-axis direction is within ±25% of the median value.

85. 85. The bilayer GaN wafer of any one of claims 69 to 84, wherein the bilayer GaN wafer has a thickness greater than 300 μm and the maximum thickness of the front layer is less than or equal to 300 μm.

86. The bilayer GaN wafer of any one of claims 69 to 85, wherein the front layer has a minimum thickness of 50 μm or greater.

87. The bilayer GaN wafer of any one of claims 69 to 86, wherein the difference between the maximum thickness and the minimum thickness of the front layer is 200 μm or less.

88. A method for producing an epitaxial wafer, comprising the steps of: preparing a wafer according to any one of claims 68 to 87; and epitaxially growing one or more nitride semiconductor layers on the prepared wafer.

89. 88. An epitaxial wafer comprising the wafer according to any one of claims 68 to 87 and one or more nitride semiconductor layers epitaxially grown on the GaN wafer.

90. A method for manufacturing a nitride semiconductor device, comprising the steps of: providing a wafer according to any one of claims 68 to 87; and epitaxially growing one or more nitride semiconductor layers on the provided wafer.

91. The method includes the steps of: preparing the GaN wafer according to claim 68; and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga-polarity main surface of the prepared GaN wafer, the GaN layer being provided with a high carrier concentration region or a carrier compensation region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is a method for manufacturing a bilayer GaN wafer.

92. 92. The method of claim 91, wherein the step of epitaxially growing includes growing the GaN layer by HVPE.

93. 93. The method of claim 91 or 92, wherein the GaN layer has a thickness of 500 μm or less.

94. The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 The manufacturing method according to any one of claims 91 to 93, wherein the region is the above region.

95. The method of any one of claims 91 to 94, wherein the GaN layer is provided with the high carrier concentration, and the high carrier concentration region is doped with Ge.

96. The method of any one of claims 91 to 95, wherein the GaN layer is provided with the high carrier concentration, and the high carrier concentration region is intentionally doped with Si.

97. The GaN layer is provided with the carrier compensation region, and the lower limit of the total concentration of compensation impurities in the carrier compensation region is 5×10 17 atoms / cm 3 The manufacturing method according to any one of claims 91 to 93, wherein the region is the above region.

98. The method according to any one of claims 91 to 97, further comprising a step of thinning the stack obtained in the epitaxial growth step.

99. 69. A method for producing a bulk GaN crystal, comprising the steps of: providing a GaN wafer as recited in claim 68; and epitaxially growing GaN on the provided GaN wafer.

100. The donor impurity contained at the highest concentration is Ge; The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; and (004) XRD rocking curve FWHM is less than 20 arcsec A c-plane GaN wafer characterized by:

101. Area 3cm 2 101. The c-plane GaN wafer of claim 100, comprising the above primary surface.

102. 101. The c-plane GaN wafer of claim 100 having a diameter of 20 mm or greater or greater.

103. The donor impurity contained at the highest concentration is Ge; The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; and When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all the measurement points is 20 arcsec or less. A c-plane GaN wafer comprising:

104. 104. The c-plane GaN wafer of claim 103, wherein the average value of the (004) XRD rocking curve FWHM among all measurement points is 18 arcsec or less.

105. The donor impurity contained at the highest concentration is Ge; The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; and When a (004) XRD rocking curve is measured every 1 mm along at least two mutually perpendicular lines on one of the main surfaces over a length of 40 mm, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less. A c-plane GaN wafer comprising:

106. 106. The c-plane GaN wafer of claim 105, wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less.

107. The c-plane GaN wafer according to any one of claims 100 to 106, wherein a fluctuation range of an x-direction component of an offcut angle on a line passing through the center of the front surface and extending in the x direction, and a fluctuation range of a y-direction component of an offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are each 0.15 degrees or less within a section having a length of 40 mm.

108. 108. The c-plane GaN wafer of any one of claims 100 to 107, having a room temperature resistivity of less than 0.02 Ω cm.

109. Carrier concentration is 1×10 18 cm -3 The above is a c-plane GaN wafer according to any one of claims 100 to 107.

110. The c-plane GaN wafer according to any one of claims 100 to 109, which satisfies one or more conditions selected from the following (a) to (c) regarding impurity concentration: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

111. 111. The c-plane GaN wafer according to claim 110, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

112. O concentration is 3 x 10 16 atoms / cm 3 The c-plane GaN wafer according to any one of claims 100 to 111, wherein:

113. Ge concentration is 1×10 18 atoms / cm 3 or more, and the Si concentration is 4×10 17 atoms / cm 3 The above is a c-plane GaN wafer according to any one of claims 100 to 112.

114. The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 The c-plane GaN wafer according to any one of claims 100 to 113, wherein:

115. The c-plane GaN wafer according to any one of claims 100 to 114, comprising a GaN crystal grown by HVPE.

116. A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 100 to 115; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

117. An epitaxial wafer comprising the GaN wafer according to any one of claims 100 to 115, and one or more nitride semiconductor layers epitaxially grown on the GaN wafer.

118. A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a GaN wafer according to any one of claims 100 to 115; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

119. The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; (004) XRD rocking curve FWHM is less than 20 arcsec; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer, characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

120. Area 3cm 2 120. The c-plane GaN wafer of claim 119, comprising the above primary surface.

121. 120. The c-plane GaN wafer of claim 119 having a diameter of 20 mm or greater.

122. The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer, characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

123. 123. The c-plane GaN wafer of claim 122, wherein the average value of the (004) XRD rocking curve FWHM among all measurement points is 18 arcsec or less.

124. The conductivity type is n-type and has a room temperature resistivity of less than 0.03 Ω cm; When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer, characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

125. 125. The c-plane GaN wafer of claim 124, wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less.

126. The c-plane GaN wafer according to any one of claims 119 to 125, wherein a fluctuation range of an x-direction component of an offcut angle on a line passing through the center of the front surface and extending in the x direction, and a fluctuation range of a y-direction component of an offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are each 0.15 degrees or less within a section having a length of 40 mm.

127. 127. The c-plane GaN wafer of any one of claims 119 to 126, having a room temperature resistivity of less than 0.02 Ω cm.

128. Carrier concentration is 1×10 18 cm -3 The above-mentioned c-plane GaN wafer according to any one of claims 119 to 126.

129. The c-plane GaN wafer according to any one of claims 119 to 128, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

130. O concentration is 3 x 10 16 atoms / cm 3 130. The c-plane GaN wafer according to any one of claims 119 to 129, wherein:

131. The c-plane GaN wafer of any one of claims 119 to 130, wherein the donor impurity contained at the highest concentration is Si.

132. 132. The c-plane GaN wafer of claim 131, wherein a total concentration of donor impurities excluding Si is less than or equal to 10% of the Si concentration.

133. 133. The c-plane GaN wafer of claim 132, wherein the carrier concentration is greater than or equal to 90% of the Si concentration.

134. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 134. The c-plane GaN wafer according to any one of claims 119 to 133, wherein:

135. The c-plane GaN wafer according to any one of claims 119 to 134, comprising a GaN crystal grown by HVPE.

136. A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 119 to 135; and epitaxially growing one or more nitride semiconductor layers on the prepared GaN wafer.

137. An epitaxial wafer comprising the c-plane GaN wafer according to any one of claims 119 to 135, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer.

138. 136. A method for manufacturing a nitride semiconductor device, comprising the steps of: providing a c-plane GaN wafer according to any one of claims 119 to 135; and epitaxially growing one or more nitride semiconductor layers on the provided c-plane GaN wafer.

139. The conductivity type is n-type; Having a diameter of 45 mm or more; (004) XRD rocking curve FWHM is less than 20 arcsec; and 、 Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

140. 140. The c-plane GaN wafer of claim 139 having a diameter of 95 mm or greater.

141. The conductivity type is n-type; When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least one line on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer, characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

142. 142. The c-plane GaN wafer of claim 141, wherein the average value of the (004) XRD rocking curve FWHM among all measurement points is 18 arcsec or less.

143. The conductivity type is n-type; When a (004) XRD rocking curve is measured every 1 mm over a length of 40 mm along at least two mutually perpendicular lines on one of the main surfaces, the maximum value of the (004) XRD rocking curve FWHM among all measurement points on each line is 20 arcsec or less; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer, characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

144. 144. The c-plane GaN wafer of claim 143, wherein an average value of the (004) XRD rocking curve FWHM among all measurement points on each line is 18 arcsec or less.

145. The c-plane GaN wafer according to any one of claims 139 to 144, wherein a variation width of an x-direction component of an offcut angle on a line passing through the center of the front surface and extending in the x direction, and a variation width of a y-direction component of an offcut angle on a line passing through the center of the front surface and extending in the y direction perpendicular to the x direction, are each 0.15 degrees or less within a section of 40 mm in length.

146. The c-plane GaN wafer according to any one of claims 139 to 145, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

147. Si concentration is 5×10 17 atoms / cm 3 147. The c-plane GaN wafer of any one of claims 139 to 146, wherein:

148. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 148. The c-plane GaN wafer of any one of claims 139 to 147, wherein:

149. O concentration is 3 x 10 16 atoms / cm 3 149. The c-plane GaN wafer of any one of claims 139 to 148, wherein:

150. 5×10 17 cm -3 The c-plane GaN wafer according to any one of claims 139 to 149, having at least one of a carrier concentration of less than 0.01 and a room temperature resistivity of 0.04 Ω cm or more.

151. The c-plane GaN wafer according to any one of claims 139 to 150, comprising a GaN crystal grown by HVPE.

152. A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 139 to 151; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

153. An epitaxial wafer comprising the c-plane GaN wafer according to any one of claims 139 to 151, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer.

154. A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 139 to 151; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

155. The method includes the steps of: preparing a c-plane GaN wafer according to any one of claims 139 to 151; and epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga polarity side main surface of the prepared c-plane GaN wafer, wherein the GaN layer is provided with a high carrier concentration region or a carrier compensation region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is a method for manufacturing a bilayer GaN wafer.

156. 156. The method of claim 155, wherein the step of epitaxially growing includes growing the GaN layer by HVPE.

157. 157. The method of claim 155 or 156, wherein the GaN layer has a thickness of 500 μm or less.

158. The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 The manufacturing method according to any one of claims 155 to 157, wherein the above region.

159. The method of any one of claims 155 to 158, wherein the GaN layer is provided with a high carrier concentration region, the high carrier concentration region being doped with Ge.

160. The method of any one of claims 155 to 159, wherein the GaN layer is provided with a high carrier concentration region, and the high carrier concentration region is intentionally doped with Si.

161. The GaN layer is provided with the carrier compensation region, and the lower limit of the total concentration of compensation impurities in the carrier compensation region is 5×10 17 atoms / cm 3 The manufacturing method according to any one of claims 155 to 157, wherein the above region.

162. The method further comprises a step of thinning the stack obtained in the epitaxial growth step. The method of any one of claims 155 to 161.

163. A method for producing a bulk GaN crystal, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 139 to 151; and epitaxially growing GaN on the prepared c-plane GaN wafer.

164. The conductivity type is n-type; The dislocation density on one of the main surfaces is 2×10 5 cm -2 and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: A c-plane GaN wafer characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

165. 165. The c-plane GaN wafer according to claim 164, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

166. O concentration is 3 x 10 16 atoms / cm 3 166. The c-plane GaN wafer of claim 164 or 165, wherein:

167. The c-plane GaN wafer according to any one of claims 164 to 166, wherein the variation width of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x-direction, and the variation width of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y-direction perpendicular to the x-direction, are each 0.15 degrees or less within a 40 mm long section.

168. 5×10 17 cm -3 The c-plane GaN wafer of any one of claims 164 to 167, having at least one of a carrier concentration of less than 0.01 and a room temperature resistivity of 0.04 Ω cm or more.

169. Si concentration is 5×10 17 atoms / cm 3 169. The c-plane GaN wafer of any one of claims 164 to 168, wherein:

170. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 170. The c-plane GaN wafer of claim 169, wherein:

171. 168. The c-plane GaN wafer of any one of claims 164 to 167, having a room temperature resistivity of less than 0.03 Ω cm.

172. Carrier concentration is 1×10 18 cm -3 The above-mentioned c-plane GaN wafer according to any one of claims 164 to 167.

173. Ge concentration is 1×10 18 atoms / cm 3 or more, and the Si concentration is 4×10 17 atoms / cm 3 The c-plane GaN wafer according to claim 171 or 172.

174. The c-plane GaN wafer of any one of claims 171 to 173, wherein the donor impurity present in the highest concentration is Ge.

175. The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 175. The c-plane GaN wafer of claim 173 or 174, wherein:

176. 173. The c-plane GaN wafer of claim 171 or 172, wherein the donor impurity present in the highest concentration is Si.

177. 177. The c-plane GaN wafer of claim 176, wherein a total concentration of donor impurities excluding Si is less than or equal to 10% of the Si concentration.

178. 178. The c-plane GaN wafer of claim 177, wherein the carrier concentration is greater than or equal to 90% of the Si concentration.

179. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 179. The c-plane GaN wafer of any one of claims 176 to 178, wherein:

180. The c-plane GaN wafer of any one of claims 164 to 179, comprising a GaN crystal grown by HVPE.

181. A method for producing an epitaxial wafer, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 164 to 180; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

182. 181. An epitaxial wafer comprising the c-plane GaN wafer according to any one of claims 164 to 180, and one or more nitride semiconductor layers epitaxially grown on the c-plane GaN wafer.

183. A method for manufacturing a nitride semiconductor device, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 164 to 180; and epitaxially growing one or more nitride semiconductor layers on the prepared c-plane GaN wafer.

184. The present invention includes a step of preparing a c-plane GaN wafer according to any one of claims 164 to 170, and a step of epitaxially growing a GaN layer having a thickness of 20 μm or more on a Ga polarity side main surface of the prepared c-plane GaN wafer, wherein the GaN layer is provided with a high carrier concentration region or a carrier compensation region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is a method for manufacturing a bilayer GaN wafer.

185. 185. The method of claim 184, wherein the step of epitaxially growing includes growing the GaN layer by HVPE.

186. 186. The method of claim 184 or 185, wherein the GaN layer has a thickness of 500 μm or less.

187. The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 The manufacturing method according to any one of claims 184 to 186, wherein the region is the above region.

188. The method of any one of claims 184 to 187, wherein the GaN layer is provided with the high carrier concentration region, and the high carrier concentration region is doped with Ge.

189. The method of any one of claims 184 to 188, wherein the GaN layer is provided with the high carrier concentration region, and the high carrier concentration region is intentionally doped with Si.

190. The GaN layer is provided with the carrier compensation region, and the carrier compensation region is a compensation impurity The lower limit of the total concentration of the substance is 5 x 10 17 atoms / cm 3 The manufacturing method according to any one of claims 184 to 186, wherein the region is the above region.

191. The method of any one of claims 184 to 190, further comprising a step of thinning the stack obtained in the epitaxial growth step.

192. A method for producing a bulk GaN crystal, comprising the steps of: preparing a c-plane GaN wafer according to any one of claims 164 to 170; and epitaxially growing GaN on the prepared c-plane GaN wafer.

193. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, At least one X-ray abnormal transmission image of a square area of ​​10 mm x 10 mm is obtained; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

194. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, At least one X-ray abnormal transmission image of a square area of ​​15 mm x 15 mm is obtained; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

195. An n-type GaN crystal having two principal surfaces facing in opposite directions, one of the two principal surfaces being Ga polar and tilted at an angle of 0 degrees or more and 10 degrees or less with respect to the (0001) crystal plane, Obtaining at least one X-ray abnormal transmission image of a square area of ​​20 mm x 20 mm; and Concerning impurity concentration, one or more of the following conditions (a) to (c) must be satisfied: An n-type GaN crystal characterized by: (a) Si concentration is 5×10 16 atoms / cm 3 That's it; (b) O concentration is 3×10 16 atoms / cm 3 Below is the result: (c) H concentration is 1×10 17 atoms / cm 3 The following is the result.

196. The n-type GaN crystal according to any one of claims 193 to 195, which satisfies all of the conditions (a) to (c) regarding impurity concentration.

197. O concentration is 3 x 10 16 atoms / cm 3 The n-type GaN crystal according to any one of claims 193 to 196, wherein:

198. 5×10 17 cm -3 The n-type GaN crystal according to any one of claims 193 to 197, having at least one of a carrier concentration of less than 0.01 and a room temperature resistivity of 0.04 Ω cm or more.

199. Si concentration is 5×10 17 atoms / cm 3 The n-type GaN crystal according to any one of claims 193 to 198, wherein:

200. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 200. The n-type GaN crystal of claim 199, wherein:

201. 198. The n-type GaN crystal according to any one of claims 193 to 197, having a room temperature resistivity of less than 0.03 Ω cm.

202. Carrier concentration is 1×10 18 cm -3 The n-type GaN crystal according to any one of claims 193 to 197.

203. Ge concentration is 1×10 18 atoms / cm 3 or more, and the Si concentration is 4×10 17 atoms / cm 3 The n-type GaN crystal according to claim 201 or 202.

204. The n-type GaN crystal according to any one of claims 201 to 203, wherein the donor impurity contained at the highest concentration is Ge.

205. The concentration of each impurity except for Ge, Si, O, and H is 5×10 15 atoms / cm 3 205. The n-type GaN crystal according to claim 203 or 204, wherein:

206. 203. The n-type GaN crystal according to claim 201 or 202, wherein the donor impurity contained at the highest concentration is Si.

207. The n-type GaN crystal according to claim 206, wherein a total concentration of donor impurities excluding Si is 10% or less of the Si concentration.

208. The n-type GaN crystal according to claim 207, wherein the carrier concentration is 90% or more of the Si concentration.

209. The concentration of each impurity except for Si, O, and H is 5×10 15 atoms / cm 3 The n-type GaN crystal according to any one of claims 206 to 208, wherein:

210. The n-type GaN crystal according to any one of claims 193 to 209, which is made of a GaN crystal grown by HVPE.

211. The n-type GaN crystal according to any one of claims 193 to 210, which is a GaN wafer.

212. The n-type GaN crystal according to claim 211, wherein the variation range of the x-direction component of the offcut angle on a line passing through the center of the front surface and extending in the x-direction, and the variation range of the y-direction component of the offcut angle on a line passing through the center of the front surface and extending in the y-direction perpendicular to the x-direction, are each 0.15 degrees or less within a 40 mm long section.

213. A method for manufacturing an epitaxial wafer, comprising the steps of: preparing an n-type GaN crystal according to claim 211 or 212; and epitaxially growing one or more nitride semiconductor layers on the prepared n-type GaN crystal.

214. 213. An epitaxial wafer comprising the n-type GaN crystal according to claim 211 or 212, and one or more nitride semiconductor layers epitaxially grown on the n-type GaN crystal.

215. A step of preparing an n-type GaN crystal according to claim 211 or 212, and epitaxially growing one or more nitride semiconductor layers on a type GaN crystal.

216. The method includes the steps of preparing a GaN wafer which is an n-type GaN crystal according to any one of claims 193 to 200, and epitaxially growing a GaN layer having a thickness of 20 μm or more on a main surface on the Ga polarity side of the prepared GaN wafer, and the GaN layer is provided with a high carrier concentration region or a carrier compensation region, and the high carrier concentration region has a carrier concentration lower limit of 1×10 18 cm -3 The carrier compensation region has a lower limit of the total concentration of compensation impurities of 2×10 17 atoms / cm 3 The above is a method for manufacturing a bilayer GaN wafer.

217. 217. The method of claim 216, wherein the step of epitaxially growing includes growing the GaN layer by HVPE.

218. 218. The method of claim 216 or 217, wherein the GaN layer has a thickness of 500 μm or less.

219. The GaN layer is provided with the high carrier concentration region, and the high carrier concentration region has a carrier concentration lower limit of 2×10 18 cm -3 The manufacturing method according to any one of claims 216 to 218, wherein the region is the above region.

220. The method of any one of claims 216 to 219, wherein the GaN layer is provided with a high carrier concentration region, and the high carrier concentration region is doped with Ge.

221. The method of any one of claims 216 to 220, wherein the GaN layer is provided with a high carrier concentration region, and the high carrier concentration region is intentionally doped with Si.

222. The GaN layer is provided with the carrier compensation region, and the lower limit of the total concentration of compensation impurities in the carrier compensation region is 5×10 17 atoms / cm 3 The manufacturing method according to any one of claims 216 to 218, wherein the region is the above region.

223. The method of any one of claims 216 to 222, further comprising a step of thinning the stack obtained in the epitaxial growth step.

224. A method for producing a bulk GaN crystal, comprising the steps of: preparing a GaN wafer that is an n-type GaN crystal according to any one of claims 193 to 200; and epitaxially growing GaN on the prepared GaN wafer.

Citation Information

Patent Citations

  • Epitaxial substrate for field-effect transistors

    JP2008227479A

  • Growing method of group iii nitride semiconductor crystal, fabrication method of group iii nitride semiconductor crystal substrate, and group iii nitride semiconductor crystal substrate

    JP2009126723A

  • III-V group substrate materials with specific crystallographic characteristics and methods for preparing them