Powder for lamination molding
A tailored powder blend with controlled particle size distributions addresses uneven material distribution in binder jet methods, achieving uniform layers and low shrinkage in additive manufacturing, enhancing the quality of three-dimensional products.
Patent Information
- Application Number
- JP2024153965
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-26
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
AI Technical Summary
The binder jet method in additive manufacturing often results in uneven distribution of constituent materials, leading to voids and uneven structures in the three-dimensional layered product, necessitating powders with improved spreading properties, uniformity, and low shrinkage rates during sintering.
A powder for additive manufacturing is formulated by controlling the volume ratio of particles with specific particle size distributions, using a blend of inorganic oxide powders with different particle sizes to achieve appropriate fluidity, bulk density, and shape stability, ensuring uniform layer formation and low shrinkage during sintering.
The solution provides a powder that forms uniform layers with good laying properties and shape stability, allowing the binder to penetrate between particles while maintaining low shrinkage rates during sintering, resulting in high-quality three-dimensional additively manufactured bodies.
Smart Images

Figure 2024161267000001 
Figure 2024161267000002 
Figure 2024161267000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a powder for additive manufacturing, a sintered body thereof, and a method for manufacturing a binder jet additive manufactured body. [Background technology]
[0002] In recent years, processing methods called additive manufacturing (AM) technology, 3D printing technology, etc., have been attracting attention. This is a technology in which a cross-sectional shape of a target object is created based on data of the three-dimensional shape and then laminated. As additive manufacturing technologies, processing methods such as a binder jet type (Patent Document 1) in which a binder is sprayed onto a powder material on a modeling stage to selectively model an object, a material jet type in which a photocurable resin or the like is sprayed from an inkjet nozzle to selectively model an object, a powder bed melting type in which a laser or electron beam is irradiated onto a powder bed covered with metal powder or the like to selectively melt and model an object, and a photolithography method (Patent Document 2) in which light is irradiated onto a slurry in which a liquid photocurable resin and an inorganic powder are mixed to form an object. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-117069 A [Patent Document 2] Patent Publication No. 2021-11050 Summary of the Invention [Problem to be solved by the invention]
[0004] The binder jet method is also known by the term "3D inkjet powder printing." This method includes, for example, a step of supplying powder material to a modeling stage using a roller to form a uniform powder layer, and a step of applying a liquid binder to the powder layer using an inkjet print head to selectively bond a part of the powder layer. By repeating these steps, the desired three-dimensional additive manufacturing object can be obtained. The three-dimensional additive manufacturing object is then subjected to a sintering process as necessary. In the binder jet method, a structure in which the distribution of constituent materials, such as voids, is uneven in the obtained three-dimensional additive manufacturing object may occur. In order to suppress this, it is desirable for the additive manufacturing powder to have good laying properties that allow it to be smoothly supplied to the modeling stage and to be laid out uniformly. In addition, it is believed that a highly uniform three-dimensional additive manufacturing object can be obtained by filling the additive manufacturing powder at a high density. In order to achieve good laying properties and high density filling, it is useful to increase the fluidity of the powder material. On the other hand, when applying the binder, it is also required that the powder layer is not disturbed and that the binder can penetrate between the powder materials. In addition, it is also desirable that the shrinkage rate during sintering is low.
[0005] The present disclosure provides a powder for additive manufacturing that has suitable fluidity to achieve both good spreadability to form a uniform powder layer and shape stability to maintain the shape from the application of the binder to the sintering process, and suitable bulk density to allow the binder to penetrate between the powder materials and to achieve a low shrinkage rate during sintering. [Means for solving the problem]
[0006] The present inventors have found that the flowability and bulk density of a powder for additive manufacturing can be controlled within an appropriate range by controlling the volume fraction of particles with a relatively large particle size within a specific range. Furthermore, the present inventors have found that the flowability and bulk density of a powder material can be controlled within an appropriate range by blending two types of inorganic oxide powders having different particle size distributions in a predetermined ratio.
[0007] The present disclosure relates to the following: [1] A powder for additive manufacturing which is an inorganic oxide powder, D10 is 1.0 to 4.0 μm, D50 is 5.5 to 9.0 μm, and D90 is 20.0 to 40.0 μm, Powder for additive manufacturing, with the volumetric ratio of particles with particle diameters of 16.8 to 60.0 μm being 15.0 to 22.0 volume %. [2] The powder for layered manufacturing according to [1], wherein the volume ratio of particles with a particle size of 2.0 μm or more is 90.0 to 100 volume %. [3] The ratio of D50 to D10 (D50 / D10) is 2.0 to 2.2; The ratio of D90 to D10 (D90 / D10) is 6.0 to 8.0. [1] or [2]. Powder for additive manufacturing. [4] BET specific surface area is 0.1 to 10.0 m 2 The powder for layered manufacturing according to any one of [1] to [3], wherein the powder has a molecular weight of 1.0 to 1.5 kg / g. [5] The powder for layered manufacturing according to any one of [1] to [4], which has a spherical shape. [6] The powder for additive manufacturing according to any one of [1] to [5], which is alumina. [7] Press molding under a pressure of 98 MPa. Bulk density is 2.52-2.54 g / cm 3 The powder for additive manufacturing according to [6], [8] The powder for additive manufacturing according to any one of [1] to [7], which is used in a binder jet method. [9] A sintered body of the powder for additive manufacturing according to any one of [1] to [7].
[10] A method for producing a binder jet type additive manufacturing object, comprising applying a liquid containing a binder to a powder for additive manufacturing according to any one of [1] to [7] to form a three-dimensional additive manufacturing object.
[11] Applying a liquid containing a binder to the powder for additive manufacturing according to any one of [1] to [7] to form a three-dimensional additive manufacturing object; and The three-dimensional laminated body is subjected to a sintering process. A method for producing a sintered body, comprising:
[12] A coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm; A fine inorganic oxide powder (B) having a D50 smaller than that of the coarse inorganic oxide powder (A). Including, The powder for layered manufacturing, wherein the volume ratio of the coarse-grained inorganic oxide powder (A) to the total volume of the coarse-grained inorganic oxide powder (A) and the fine-grained inorganic oxide powder (B) is 9.5 to 29.0 volume %.
[13] The powder for layered manufacturing according to
[12] , wherein a particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 0.26 to 1.15.
[14] D50 (D A 50) and the D50 of the fine inorganic oxide powder (B) (D B 50) D A 50-D B The powder for additive manufacturing according to
[12] or
[13] , which satisfies 50 ≧ 3.5 μm.
[15] A coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm; A fine inorganic oxide powder (B) having a D50 smaller than that of the coarse inorganic oxide powder (A). Including, The powder for layered manufacturing, wherein the particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 0.26 to 1.15.
[16] The powder for additive manufacturing according to
[15] , wherein the volume ratio of the coarse-grained inorganic oxide powder (A) to the total volume of the coarse-grained inorganic oxide powder (A) and the fine-grained inorganic oxide powder (B) is 9.5 to 29.0 volume %.
[17] D50 (D A50) and the D50 of the fine inorganic oxide powder (B) (D B 50) D A 50-D B The powder for additive manufacturing according to
[15] or
[16] , which satisfies 50 ≧ 3.5 μm.
[18] The powder for layered manufacturing according to any one of
[12] to
[17] , wherein the fine inorganic oxide powder (B) has a D50 of 5.0 to 8.0 μm.
[19] The ratio (D50 / D10) of D50 to D10 of the coarse inorganic oxide powder (A) is 1.5 to 3.5; The ratio of D90 to D10 (D90 / D10) of the coarse inorganic oxide powder (A) is 4.0 to 7.0. The powder for additive manufacturing according to any one of
[12] to
[18] .
[20] The powder for layered manufacturing according to any one of
[12] to
[19] , wherein the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are both spherical in shape. [twenty one] The powder for layered manufacturing according to any one of
[12] to
[20] , wherein the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are both alumina. [twenty two] Press molding under a pressure of 98 MPa. Bulk density is 2.52-2.54 g / cm 3
[21] The powder for additive manufacturing according to
[21] . [twenty three] The powder for additive manufacturing according to any one of
[12] to
[22] , which is used in a binder jet method. [twenty four] A sintered body of the powder for additive manufacturing according to any one of
[12] to
[23] . [twenty five] A method for producing a binder jet type additive manufacturing object, comprising applying a liquid containing a binder to a powder for additive manufacturing according to any one of
[12] to
[23] to form a three-dimensional additive manufacturing object.
[26] Applying a liquid containing a binder to the powder for additive manufacturing according to any one of
[12] to
[23] to form a three-dimensional additive manufacturing object; and The three-dimensional laminated body is subjected to a sintering process. A method for producing a sintered body, comprising:
[27] D10 is 1.0 to 4.0 μm, D50 is 5.5 to 9.0 μm, and D90 is 20.0 to 40.0 μm, Alumina powder in which the volume ratio of particles having a particle diameter of 16.8 to 60.0 μm is 15.0 to 22.0 volume %.
[28] The alumina powder according to
[27] , wherein the volume ratio of particles having a particle diameter of 2.0 μm or more is 90.0 to 100 volume %.
[29] The ratio of D50 to D10 (D50 / D10) is 2.0 to 2.2; The ratio of D90 to D10 (D90 / D10) is 6.0 to 8.0.
[27] or
[28] . An alumina powder according to
[27] or
[28] .
[30] BET specific surface area is 0.1 to 10.0 m 2 The alumina powder according to any one of
[27] to
[29] , wherein the alumina powder has a molecular weight of 1 / g.
[31] The alumina powder according to any one of
[27] to
[30] , which has a spherical shape.
[32] Press molding under a pressure of 98 MPa. Bulk density is 2.52-2.54 g / cm 3 The alumina powder according to any one of
[27] to
[31] , Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a powder for additive manufacturing that has good spreadability to form a uniform powder layer, appropriate fluidity to achieve shape stability to maintain the shape from the application of the binder to the sintering process, and appropriate bulk density that allows the binder to penetrate between the powder materials and achieves a low shrinkage rate during sintering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present invention will be described. Note that the embodiments described below are representative examples of the present invention, and the present invention is not limited thereto.
[0010] In this specification, when "~" is used for a numerical range, the numerical values at both ends are the upper limit and the lower limit, respectively, and are included in the numerical range. When multiple upper or lower limits are listed, numerical ranges can be created from all combinations of the upper and lower limits. Similarly, when multiple numerical ranges are listed, separate numerical ranges can be created by individually selecting and combining the upper and lower limits from those numerical ranges.
[0011] In this specification, D10, D50, and D90 are the 10% particle size, 50% particle size, and 90% particle size, respectively, in the volume-based cumulative particle size distribution measured using an electrical resistance method particle size distribution measurement device (Beckman Coulter, Multisizer 4) with an aperture size of 100 μm.
[0012] In this specification, the press-molded bulk density means the density of a molded body obtained by filling a sample into a circular mold and pressing it under a predetermined pressure using a commercially available press. The press-molded bulk density is a value that serves as an index of the bulk density of a powder layer when a thin layer of powder is formed using a roller or the like.
[0013] In this specification, the angle of repose is a value measured and calculated according to JIS R 9301-2-2:1999 (alumina powder--Part 2: Measurement of physical properties--2: Angle of repose).
[0014] In this specification, the BET specific surface area is a value measured and calculated in accordance with "6.2 Fluidized method (3.5) Single point method" of JIS R 1626:1996 (Method of measuring specific surface area of fine ceramic powder by gas adsorption BET method). The measurement is performed by heating the sample to 180°C as a pretreatment, flowing nitrogen gas for 20 minutes, and then using nitrogen gas as the adsorbate.
[0015] In this specification, the circularity is the average value of values calculated for 5,000 particles according to the following formula (1), where S is the area of a projection of a particle and L is the perimeter. 4πS / L 2 (1)
[0016] In this specification, the volume ratios of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are values calculated from the charged mass and true density of the materials as follows. The volume VA of the coarse inorganic oxide powder (A) is calculated from the mass of the mixed coarse inorganic oxide powder (A) / the true density of the coarse inorganic oxide powder (A). The volume VB of the fine inorganic oxide powder (B) is calculated from the mass of the mixed fine inorganic oxide powder (B) / the true density of the fine inorganic oxide powder (B). Using these values, the volume ratio of the coarse inorganic oxide powder (A) is calculated from VA / (VA+VB), and the volume ratio of the fine inorganic oxide powder (B) is calculated from VB / (VA+VB).
[0017] In this specification, the particle size volume ratio is a value calculated by the following formula (2). (Volume ratio of coarse inorganic oxide powder (A) × D50 of coarse inorganic oxide powder (A)) / (Volume ratio of fine inorganic oxide powder (B) × D50 of fine inorganic oxide powder (B)) (2)
[0018] <Powder for additive manufacturing> The powder for additive manufacturing is an inorganic oxide powder, and its D10 is 1.0 to 4.0 μm, D50 is 5.5 to 9.0 μm, and D90 is 20.0 to 40.0 μm. In the powder for additive manufacturing, the volume ratio of particles having a particle size of 16.8 to 60.0 μm is 15.0 to 22.0 volume%. The present inventors have found that in the powder for additive manufacturing having a D50 of 5.5 to 9.0 μm, particles having a particle size of 16.8 to 60.0 μm contribute to improving the fluidity and bulk density of the powder for additive manufacturing. Therefore, it has been found that a good balance between the fluidity and bulk density of the powder material can be achieved by controlling the volume ratio of particles having a particle size of 16.8 to 60.0 μm to a specific range.
[0019] The D50 of the powder for additive manufacturing is 5.5 μm or more, preferably 6.0 μm or more, more preferably 6.5 μm or more. The D50 of the powder for additive manufacturing is 9.0 μm or less, preferably 8.5 μm or less, more preferably 8.0 μm or less. The D50 of the powder for additive manufacturing is 5.5 to 9.0 μm, preferably 6.0 to 8.5 μm, more preferably 6.5 to 8.0 μm. If the D50 of the powder for additive manufacturing is 5.5 μm or more, the shape stability of the powder layer formed by the powder for additive manufacturing is good, and the shrinkage rate during sintering can be reduced. If the D50 of the powder for additive manufacturing is 9.0 μm or less, the bulk density and flowability can be set to appropriate ranges.
[0020] The D10 of the powder for additive manufacturing is 1.0 μm or more, preferably 2.0 μm or more, and more preferably 3.0 μm or more. The D10 of the powder for additive manufacturing is 4.0 μm or less, preferably 3.8 μm or less, and more preferably 3.6 μm or less. The D10 of the powder for additive manufacturing is 1.0 to 4.0 μm, preferably 2.0 to 3.8 μm, and more preferably 3.0 to 3.6 μm. If the D10 of the powder for additive manufacturing is 1.0 μm or more, the shrinkage rate during sintering can be reduced. If the D10 of the powder for additive manufacturing is 4.0 μm or less, the bulk density and flowability can be set to appropriate ranges.
[0021] The D90 of the powder for additive manufacturing is 20.0 μm or more, preferably 20.5 μm or more, and more preferably 21.0 μm or more. The D90 of the powder for additive manufacturing is 40.0 μm or less, preferably 30.0 μm or less, and more preferably 25.0 μm or less. The D90 of the powder for additive manufacturing is 20.0 to 40.0 μm, preferably 20.5 to 30.0 μm, and more preferably 21.0 to 25.0 μm. If the D90 of the powder for additive manufacturing is 20.0 μm or more, the shape stability of the powder layer formed by the powder for additive manufacturing is good. If the D90 of the powder for additive manufacturing is 40.0 μm or less, the uniformity of the powder layer formed by the powder for additive manufacturing is good.
[0022] The volume ratio of particles having a particle size of 16.8 to 60.0 μm in the powder for additive manufacturing is 15.0 to vol.% or more, preferably 15.5 vol.% or more, and more preferably 16.0 vol.% or more. The volume ratio of particles having a particle size of 16.8 to 60.0 μm in the powder for additive manufacturing is 22.0 vol.% or less, preferably 21.0 vol.% or less, and more preferably 20.0 vol.% or less. The volume ratio of particles having a particle size of 16.8 to 60.0 μm in the powder for additive manufacturing is 15.0 to 22.0 vol.%, preferably 15.5 to 21.0 vol.%, and more preferably 16.0 to 20.0 vol.%. If the volume ratio of particles having a particle size of 16.8 to 60.0 μm is within the above range, the powder for additive manufacturing can be expected to have appropriate fluidity. The volume fraction of particles with particle sizes of 16.8 to 60.0 μm in the powder for additive manufacturing is determined by measurement using an electrical resistance particle size distribution measuring device (Beckman Coulter, Multisizer 4) with an aperture size of 100 μm.
[0023] The volume ratio of particles having a particle size of 2.0 μm or more in the powder for additive manufacturing is preferably 90.0 to 100 volume%, more preferably 93.0 to 100 volume%, and even more preferably 95.0 to 100 volume%. If the volume ratio of particles having a particle size of 2.0 μm or more is 90.0 volume% or more, the shrinkage rate during sintering can be reduced. The volume ratio of particles having a particle size of 2.0 μm or more in the powder for additive manufacturing is a value determined by a laser diffraction / scattering type particle size distribution measuring device (Microtrack Bell Co., Ltd., MT3300EXII).
[0024] The ratio of D50 to D10 (D50 / D10) of the powder for additive manufacturing is preferably 2.0 to 2.2. If D50 / D10 is in the above range, the powder for additive manufacturing can be expected to have a suitable fluidity that combines good spreadability that allows a uniform powder layer to be formed and shape stability that allows the shape to be maintained from the application of the binder to the sintering process.
[0025] The ratio of D90 to D10 (D90 / D10) of the powder for additive manufacturing is preferably 6.0 or more, more preferably 6.2 or more, and even more preferably 6.5 or more. The ratio of D90 to D10 (D90 / D10) of the powder for additive manufacturing is preferably 8.0 or less, more preferably 7.5 or less, and even more preferably 7.0 or less. The ratio of D90 to D10 (D90 / D10) of the powder for additive manufacturing is preferably 6.0 to 8.0, more preferably 6.2 to 7.5, and even more preferably 6.5 to 7.0. If D90 / D10 is 8.0 or less, the particle size distribution of the powder falls within a certain range, so that fine particles are appropriately arranged around the coarse particles, and the flowability can be made appropriate. If D90 / D10 is 6.0 or more, fine particles are appropriately arranged between the coarse particles, and the bulk density can be made appropriate.
[0026] The ratio of D90 to D50 (D90 / D50) of the powder for additive manufacturing is preferably 2.8 to 3.6, more preferably 2.9 to 3.5, and even more preferably 3.2 to 3.4. If D90 / D50 is 3.6 or less, the particle size distribution of the powder falls within a certain range, so that fine particles are appropriately arranged around coarse particles, and the flowability can be made appropriate. If D90 / D50 is 2.8 or more, fine particles are appropriately arranged between coarse particles, and the bulk density can be made appropriate.
[0027] The angle of repose of the powder for additive manufacturing is preferably 55 to 58 degrees, and more preferably 56 to 57 degrees. The angle of repose is one of the indicators of powder fluidity. If the angle of repose of the powder for additive manufacturing is 55 degrees or more, the powder layer formed by the powder for additive manufacturing has good shape stability. If the angle of repose of the powder for additive manufacturing is 58 degrees or less, the powder for additive manufacturing can be smoothly supplied to the modeling stage and evenly spread.
[0028] The BET specific surface area of the powder for additive manufacturing is preferably 0.1 m 2 / g or more, more preferably 0.2m 2 The BET specific surface area of the powder for additive manufacturing is preferably 10.0 m 2 / g or less, and more preferably 5.0m 2 / g or less, more preferably 2.0m 2 The BET specific surface area of the powder for additive manufacturing is preferably 0.1 to 10.0 m 2 / g, more preferably 0.1 to 5.0 m 2 / g, and more preferably 0.2 to 2.0 m 2 / g. The BET specific surface area is 0.1 m 2 If the BET specific surface area is 10.0 m / g or more, the powder layer formed by the powder for additive manufacturing has good shape stability. 2 If the powder density is 0.1 μm or less, the powder for additive manufacturing can be smoothly supplied to the modeling stage and spread evenly.
[0029] The shape of the powder for additive manufacturing is not particularly limited. For example, spherical, ellipsoidal, scaly, amorphous, etc. can be mentioned. Among them, spherical is preferable because it is easy to obtain an appropriate bulk density. From this viewpoint, the circularity of the powder for additive manufacturing is preferably 0.80 or more, more preferably 0.90 or more, and even more preferably 0.95 or more. The upper limit of the circularity of the powder for additive manufacturing is not particularly limited, but may be, for example, 1.00 or 0.99. If the circularity is 0.80 or more, the press molding bulk density can be increased.
[0030] The powder for additive manufacturing is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and more preferably spherical alumina. Alumina is preferable because it has high thermal conductivity, melting point, and hardness, is inexpensive, and is resistant to acids and alkalis. The volume ratio of alumina in the powder for additive manufacturing is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 80% by volume or more. The upper limit of the volume ratio of alumina in the powder for additive manufacturing is not particularly limited. For example, it may be 100% by volume, 98% by volume, or 95% by volume.
[0031] When the powder for additive manufacturing is alumina, the press molding bulk density of the powder for additive manufacturing under a pressure of 98 MPa is preferably 2.52 to 2.54 g / cm 3The press molding bulk density of the powder for additive manufacturing under a pressure of 98 MPa is 2.52 g / cm 3 If the powder for additive manufacturing has a press molding bulk density of 2.54 g / cm under a pressure of 98 MPa or more, the dimensional stability during sintering is good. 3 If the binder is below this value, it can easily penetrate between the powder materials when applied, and the strength of the shaped body and sintered body can be sufficient.
[0032] The powder for additive manufacturing has good spreading property, shape stability of the powder layer, and appropriate bulk density, and is therefore suitable for use in the binder jet method. The powder for additive manufacturing can also be applied to the powder bed fusion method, in which a powder bed containing a powder material is selectively melted and shaped by irradiating it with a laser or electron beam, and other powder additive manufacturing methods.
[0033] The powder for additive manufacturing can be used for purposes other than additive manufacturing. The powder for additive manufacturing can be used, for example, as a filler in paints such as heat dissipation paints, heat-shielding paints, and abrasion-resistant paints, as a filler in thermally conductive resin compositions having adhesive properties, and as a filler in thermally conductive coating materials having the function of curing in the atmosphere.
[0034] One embodiment of the inorganic oxide powder is an alumina powder having a D10 of 1.0 to 4.0 μm, a D50 of 5.5 to 9.0 μm, a D90 of 20.0 to 40.0 μm, and a volume ratio of particles having a particle size of 16.8 to 60.0 μm of 15.0 to 22.0 volume %.
[0035] <Method of manufacturing powder for additive manufacturing> The powder for additive manufacturing can be produced, for example, by mixing a plurality of inorganic oxide powders having different particle size distributions so that the particle size distribution of the powder for additive manufacturing falls within a predetermined range. The particle size distribution of the powder for additive manufacturing may be adjusted by sieving or the like. The particle size distribution of the powder for additive manufacturing can be adjusted to an appropriate range by selecting the type (particle size distribution) and amount of the inorganic oxide powder to be mixed. The method of mixing the materials is not particularly limited, and examples of the method include a method of dry mixing or wet mixing the materials. The mixing may be performed manually or using a blender.
[0036] A more specific example of a method for producing powder for additive manufacturing is a method of mixing a coarse-grained inorganic oxide powder (A) shown below with a fine-grained inorganic oxide powder (B) having a D50 smaller than that of the coarse-grained inorganic oxide powder (A).
[0037] [Coarse inorganic oxide powder (A)] The D50 of the coarse inorganic oxide powder (A) preferably used is 9.0 to 25.0 μm, more preferably 12.0 to 20.0 μm, and even more preferably 14.0 to 18.0 μm. The D10 of the coarse inorganic oxide powder (A) is preferably 1.0 to 8.0 μm, more preferably 2.0 to 7.5 μm, and even more preferably 3.0 to 7.0 μm. The D90 of the coarse inorganic oxide powder (A) is preferably 28.0 to 40.0 μm, more preferably 28.5 to 38.0 μm, and even more preferably 29.0 to 36.0 μm.
[0038] The ratio of D50 to D10 (D50 / D10) of the coarse inorganic oxide powder (A) is preferably 1.5 to 3.5, more preferably 1.7 to 3.2, and even more preferably 2.0 to 3.0. The ratio of D90 to D10 (D90 / D10) of the coarse inorganic oxide powder (A) is preferably 3.5 to 9.0, more preferably 4.0 to 7.0, and even more preferably 4.5 to 6.0. The ratio of D90 to D50 (D90 / D50) of the coarse inorganic oxide powder (A) is preferably 1.7 to 2.3, more preferably 1.8 to 2.2, and even more preferably 1.9 to 2.0.
[0039] The shape of the coarse-grained inorganic oxide powder (A) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0040] The coarse inorganic oxide powder (A) is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the coarse inorganic oxide powder (A) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the coarse inorganic oxide powder (A) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0041] [Fine inorganic oxide powder (B)] The D50 of the fine inorganic oxide powder (B) is smaller than the D50 of the coarse inorganic oxide powder (A). The D50 of the fine inorganic oxide powder (B) preferably used is 5.0 to 8.0 μm, more preferably 5.5 to 7.8 μm, and even more preferably 6.0 to 7.5 μm. The D10 of the fine inorganic oxide powder (B) is preferably 1.0 to 4.0 μm, more preferably 2.0 to 3.8 μm, and even more preferably 2.5 to 3.5 μm. The D90 of the fine inorganic oxide powder (B) is preferably 9.0 to 25.0 μm, more preferably 12.0 to 24.0 μm, and even more preferably 14.0 to 23.0 μm.
[0042] The ratio (D50 / D10) of the fine inorganic oxide powder (B) between D50 and D10 is preferably 1.5 to 5.0, more preferably 1.7 to 4.0, and even more preferably 1.8 to 3.0. The ratio (D90 / D10) of the fine inorganic oxide powder (B) between D90 and D10 is preferably 3.5 to 9.0, more preferably 4.5 to 8.0, and even more preferably 5.5 to 7.0. The ratio (D90 / D50) of the fine inorganic oxide powder (B) between D90 and D50 is preferably 2.5 to 3.5, more preferably 2.8 to 3.2, and even more preferably 2.7 to 2.9.
[0043] The shape of the fine inorganic oxide powder (B) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0044] The fine inorganic oxide powder (B) is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the fine inorganic oxide powder (B) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the fine inorganic oxide powder (B) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0045] The volume ratio of the coarse-grained inorganic oxide powder (A) to the total volume of the coarse-grained inorganic oxide powder (A) and the fine-grained inorganic oxide powder (B) is selected so that the particle size distribution of the powder for additive manufacturing is in an appropriate range, and may be, for example, 9.5 to 29.0 volume %.
[0046] <Powder for additive manufacturing> In the powder additive manufacturing method in which the powder material is spread by a roller or the like, the press molding bulk density of the material is important. Inorganic oxide powders with a smaller D50 tend to have a lower bulk density and lower fluidity than inorganic oxide powders with a larger D50. The present inventors have found that a good balance between the fluidity and bulk density of the powder material can be achieved by blending a small amount of coarse inorganic oxide powder (A) with fine inorganic oxide powder (B) having a smaller D50 than coarse inorganic oxide powder (A). This is completely different from the design concept of conventional powder materials, which attempts to increase bulk density by filling the gaps between coarse particles with fine particles.
[0047] D50 of coarse inorganic oxide powder (A) (D A 50) and the D50 of fine inorganic oxide powder (B) (D B 50), powders for additive manufacturing are D A 50-D B It is preferable that the particle diameter satisfies 50≧3.5 μm. When the particle diameter is within this range, the excellent particle characteristics of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are effectively utilized, and a powder having a good balance between fluidity and bulk density is obtained. From the same viewpoint, D A 50-D B 50≧5.5 μm is more preferable, and D A 50-D B 50≧7.5 μm is more preferable. A 50-D B The upper limit of 50 may be 12.0 μm, 15.0 μm, or 19.0 μm.
[0048] In a first embodiment, the powder for additive manufacturing comprises a coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm and a fine-grained inorganic oxide powder (B) having a D50 smaller than that of the coarse-grained inorganic oxide powder (A), and the volume ratio of the coarse-grained inorganic oxide powder (A) to the total volume of the coarse-grained inorganic oxide powder (A) and the fine-grained inorganic oxide powder (B) is 9.5 to 29.0 volume %.
[0049] In this embodiment, the volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is 9.5 to 29.0 volume%, preferably 10.5 to 20.0 volume%, and more preferably 11.6 to 15.0 volume%. The volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is 9.5 volume% or more, preferably 10.5 volume% or more, and more preferably 11.6 volume% or more. The volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is 29.0 volume% or less, preferably 20.0 volume% or less, and more preferably 15.0 volume% or less. If the volume ratio is 9.5 volume% or more, the bulk density can be increased and the powder can be in a suitable range for layered manufacturing. If the volume ratio is 29.0% by volume or less, the flowability can be suppressed and it can be within an appropriate range for powder for layered manufacturing.
[0050] In this embodiment, the particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is preferably 0.26 to 1.15, more preferably 0.27 to 0.74, and even more preferably 0.29 to 0.32. The particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is preferably 0.26 or more, more preferably 0.27 or more, and even more preferably 0.29 or more. The particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is preferably 1.15 or less, more preferably 0.74 or less, and even more preferably 0.32 or less. If the particle size volume ratio is 0.26 or more, the bulk density can be increased and the powder can be in a suitable range for layered manufacturing. If the particle size volume ratio is 1.15 or less, the flowability can be suppressed and the powder can be in a suitable range for layered manufacturing.
[0051] In a second embodiment, the powder for additive manufacturing comprises a coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm and a fine-grained inorganic oxide powder (B) having a D50 smaller than that of the coarse-grained inorganic oxide powder (A), and the particle size volume ratio of the coarse-grained inorganic oxide powder (A) to the fine-grained inorganic oxide powder (B) is 0.26 to 1.15.
[0052] In this embodiment, the particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 0.26 to 1.15, preferably 0.27 to 0.74, and more preferably 0.29 to 0.32. The particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 0.26 or more, preferably 0.27 or more, and more preferably 0.29 or more. The particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 1.15 or less, preferably 0.74 or less, and more preferably 0.32 or less. If the particle size volume ratio is 0.26 or more, the bulk density can be increased and the powder can be in a suitable range for layered manufacturing. If the particle size volume ratio is 1.15 or less, the flowability can be suppressed and the powder can be in a suitable range for layered manufacturing.
[0053] In this embodiment, the volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is preferably 9.5 to 29.0 volume%, more preferably 10.5 to 20.0 volume%, and even more preferably 12.0 to 15.0 volume%. The volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is preferably 9.5 volume% or more, more preferably 10.5 volume% or more, and even more preferably 12.0 volume% or more. The volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is preferably 29.0 volume% or less, more preferably 20.0 volume% or less, and even more preferably 15.0 volume% or less. If the volume ratio is 9.5 volume% or more, the bulk density can be increased and the powder can be in a suitable range for layered manufacturing. If the volume fraction is 29.0% by volume or less, the flowability can be suppressed and it is possible to fall within the appropriate range for powder for layered manufacturing.
[0054] The D50 of the powder for additive manufacturing is preferably 5.5 to 9.0 μm, more preferably 6.0 to 8.5 μm, and even more preferably 6.5 to 8.0 μm. If the powder for additive manufacturing has a D50 of 5.5 μm or more, the powder layer formed by the powder for additive manufacturing has better shape stability and the shrinkage rate during sintering can be reduced. If the powder for additive manufacturing has a D50 of 9.0 μm or less, the bulk density and flowability can be set in appropriate ranges.
[0055] The powder for layered manufacturing has a D10 of preferably 1.0 to 4.0 μm, more preferably 2.0 to 3.8 μm, and even more preferably 3.0 to 3.6 μm. If the powder for layered manufacturing has a D10 of 1.0 μm or more, the shrinkage rate during sintering can be reduced. If the powder for layered manufacturing has a D10 of 4.0 μm or less, the bulk density and flowability can be kept within appropriate ranges.
[0056] The D90 of the powder for additive manufacturing is preferably 20.0 to 40.0 μm, more preferably 20.5 to 30.0 μm, and even more preferably 21.0 to 25.0 μm. If the D90 of the powder for additive manufacturing is 20.0 μm or more, the shape stability of the powder layer formed by the powder for additive manufacturing is better. If the D90 of the powder for additive manufacturing is 40.0 μm or less, the uniformity of the powder layer formed by the powder for additive manufacturing is better.
[0057] The volume ratio of particles having a particle size of 16.8 to 60.0 μm in the powder for additive manufacturing is preferably 15.0 to 26.0 volume%, more preferably 15.0 to 22.0 volume%, and even more preferably 16.0 to 20.0 volume%. If the volume ratio of particles having a particle size of 16.8 to 60.0 μm is within the above range, appropriate fluidity of the powder material can be expected. The volume ratio of particles having a particle size of 16.8 to 60.0 μm in the powder for additive manufacturing is a value determined by measuring with an electrical resistance type particle size distribution measuring device (Beckman Coulter, Multisizer 4) with an aperture size of 100 μm.
[0058] The volume ratio of particles having a particle size of 2.0 μm or more in the powder for additive manufacturing is preferably 90.0 to 100 volume%, more preferably 93.0 to 100 volume%, and even more preferably 95.0 to 100 volume%. If the volume ratio of particles having a particle size of 2.0 μm or more is 90.0 volume% or more, the shrinkage rate during sintering can be reduced. The volume ratio of particles having a particle size of 2.0 μm or more in the powder for additive manufacturing is a value determined by a laser diffraction / scattering type particle size distribution measuring device (Microtrack Bell Co., Ltd., MT3300EXII).
[0059] The ratio of D50 to D10 (D50 / D10) of the powder for additive manufacturing is preferably 2.0 to 2.2. If D50 / D10 is in the above range, the powder for additive manufacturing can be expected to have a suitable fluidity that combines good spreadability that allows a uniform powder layer to be formed and shape stability that allows the shape to be maintained from the application of the binder to the sintering process.
[0060] The ratio of D90 to D10 (D90 / D10) of the powder for additive manufacturing is preferably 6.0 to 8.0, more preferably 6.2 to 7.5, and even more preferably 6.5 to 7.0. If D90 / D10 is 8.0 or less, the particle size distribution of the powder falls within a certain range, so that fine particles are appropriately arranged around coarse particles, and the flowability can be made appropriate. If D90 / D10 is 6.0 or more, fine particles are appropriately arranged between coarse particles, and the bulk density can be made appropriate.
[0061] The ratio of D90 to D50 (D90 / D50) of the powder for additive manufacturing is preferably 2.8 to 3.6, more preferably 2.9 to 3.5, and even more preferably 3.2 to 3.4. If D90 / D50 is 3.6 or less, the particle size distribution of the powder falls within a certain range, so that fine particles are appropriately arranged around coarse particles, and the flowability can be made appropriate. If D90 / D50 is 2.8 or more, fine particles are appropriately arranged between coarse particles, and the bulk density can be made appropriate.
[0062] The angle of repose of the powder for additive manufacturing is preferably 55 to 58 degrees, and more preferably 56 to 57 degrees. The angle of repose is one of the indicators of powder fluidity. If the angle of repose of the powder for additive manufacturing is 55 degrees or more, the powder layer formed by the powder for additive manufacturing has good shape stability. If the angle of repose of the powder for additive manufacturing is 58 degrees or less, the powder for additive manufacturing can be smoothly supplied to the modeling stage and evenly spread.
[0063] The BET specific surface area of the powder for additive manufacturing is preferably 0.1 to 10.0 m 2 / g, more preferably 0.1 to 5.0 m 2 / g, and more preferably 0.2 to 2.0 m 2 / g. The BET specific surface area is 0.1 m 2 If the BET specific surface area is 10.0 m / g or more, the powder layer formed by the powder for additive manufacturing has good shape stability. 2 If the powder density is 0.1 μm or less, the powder for additive manufacturing can be smoothly supplied to the modeling stage and spread evenly.
[0064] The shape of the powder for additive manufacturing is not particularly limited. For example, spherical, ellipsoidal, scaly, amorphous, etc. can be mentioned. Among them, spherical is preferable because it is easy to obtain an appropriate bulk density. From this viewpoint, the circularity of the powder for additive manufacturing is preferably 0.80 or more, more preferably 0.90 or more, and even more preferably 0.95 or more. The upper limit of the circularity of the powder for additive manufacturing is not particularly limited, but may be, for example, 1.00 or 0.99. If the circularity is 0.80 or more, the press molding bulk density can be increased.
[0065] The powder for additive manufacturing is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and more preferably spherical alumina. Alumina is preferable because it has high thermal conductivity, melting point, and hardness, is inexpensive, and is resistant to acids and alkalis. The volume ratio of alumina in the powder for additive manufacturing is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 80% by volume or more. The upper limit of the volume ratio of alumina in the powder for additive manufacturing is not particularly limited. For example, it may be 100% by volume, 98% by volume, or 95% by volume.
[0066] When the powder for additive manufacturing is alumina, the press molding bulk density of the powder for additive manufacturing under a pressure of 98 MPa is preferably 2.52 to 2.54 g / cm 3 The press molding bulk density of the powder for additive manufacturing under a pressure of 98 MPa is 2.52 g / cm 3 If the powder for additive manufacturing has a press molding bulk density of 2.54 g / cm under a pressure of 98 MPa or more, the dimensional stability during sintering is good. 3 If the binder is below this value, it can easily penetrate between the powder materials when applied, and the strength of the shaped body and sintered body can be sufficient.
[0067] The powder for additive manufacturing has good spreading property, shape stability of the powder layer, and appropriate bulk density, and is therefore suitable for use in the binder jet method. The powder for additive manufacturing can also be applied to the powder bed fusion method, in which a powder bed containing a powder material is selectively melted and shaped by irradiating it with a laser or electron beam, and other powder additive manufacturing methods.
[0068] The powder for additive manufacturing can be used for purposes other than additive manufacturing. The powder for additive manufacturing can be used, for example, as a filler in paints such as heat dissipation paints, heat-shielding paints, and abrasion-resistant paints, as a filler in thermally conductive resin compositions having adhesive properties, and as a filler in thermally conductive coating materials having the function of curing in the atmosphere.
[0069] [Coarse inorganic oxide powder (A)] The coarse inorganic oxide powder (A) has a D50 of 9.0 μm or more, preferably 12.0 μm or more, and more preferably 14.0 μm or more. The coarse inorganic oxide powder (A) has a D50 of 25.0 μm or less, preferably 20.0 μm or less, and more preferably 18.0 μm or less. The coarse inorganic oxide powder (A) has a D50 of 9.0 to 25.0 μm, preferably 12.0 to 20.0 μm, and more preferably 14.0 to 18.0 μm. If the coarse inorganic oxide powder (A) has a D50 of 9.0 μm or more, the powder for layered manufacturing can be easily packed at a high density. If the coarse inorganic oxide powder (A) has a D50 of 25.0 μm or less, the angle of repose of the powder for layered manufacturing can be controlled within an appropriate range.
[0070] The D10 of the coarse-grained inorganic oxide powder (A) is preferably 1.0 to 8.0 μm, more preferably 2.0 to 7.5 μm, and even more preferably 3.0 to 7.0 μm. If the D10 of the coarse-grained inorganic oxide powder (A) is 1.0 μm or more, the shrinkage rate during sintering can be reduced. If the D10 of the coarse-grained inorganic oxide powder (A) is 8.0 μm or less, the powder material can be expected to have appropriate fluidity.
[0071] The D90 of the coarse-grained inorganic oxide powder (A) is preferably 28.0 to 40.0 μm, more preferably 28.5 to 38.0 μm, and even more preferably 29.0 to 36.0 μm. If the D90 of the coarse-grained inorganic oxide powder (A) is 28.0 μm or more, the density of the shaped body formed from the powder for additive manufacturing can be increased and the shape stability is better. If the D90 of the coarse-grained inorganic oxide powder (A) is 40.0 μm or less, the uniformity of the powder layer formed from the powder for additive manufacturing is better.
[0072] The ratio (D50 / D10) of D50 to D10 of the coarse inorganic oxide powder (A) is preferably 1.5 or more, more preferably 1.7 or more, and even more preferably 2.0 or more. The ratio (D50 / D10) of D50 to D10 of the coarse inorganic oxide powder (A) is preferably 3.5 or less, more preferably 3.2 or less, and even more preferably 3.0 or less. The ratio (D50 / D10) of D50 to D10 of the coarse inorganic oxide powder (A) is preferably 1.5 to 3.5, more preferably 1.7 to 3.2, and even more preferably 2.0 to 3.0. If D50 / D10 is in the above range, an improvement in press molding bulk density can be expected.
[0073] The ratio (D90 / D10) of D90 to D10 of the coarse inorganic oxide powder (A) is preferably 4.0 or more, more preferably 4.5 or more, and even more preferably 5.0 or more. The ratio (D90 / D10) of D90 to D10 of the coarse inorganic oxide powder (A) is preferably 7.0 or less, more preferably 6.0 or less, and even more preferably 5.5 or less. The ratio (D90 / D10) of D90 to D10 of the coarse inorganic oxide powder (A) is preferably 4.0 to 7.0, more preferably 4.5 to 6.0, and even more preferably 5.0 to 5.5. If D90 / D10 is in the above range, the particle size distribution falls within a certain range, making it easy to use as a base material for powder for additive manufacturing, and the bulk density and flowability can be improved in a well-balanced manner.
[0074] The ratio of D90 to D50 (D90 / D50) of the coarse-grained inorganic oxide powder (A) is preferably 1.7 to 2.3, more preferably 1.8 to 2.2, and even more preferably 1.9 to 2.0. When D90 / D50 is in the above range, the flowability of the powder for layered manufacturing can be set in an appropriate range.
[0075] The shape of the coarse-grained inorganic oxide powder (A) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0076] The coarse inorganic oxide powder (A) is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the coarse inorganic oxide powder (A) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the coarse inorganic oxide powder (A) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0077] [Fine inorganic oxide powder (B)] The D50 of the fine inorganic oxide powder (B) is smaller than the D50 of the coarse inorganic oxide powder (A). The D50 of the fine inorganic oxide powder (B) is preferably 5.0 μm or more, more preferably 5.5 μm or more, and even more preferably 6.0 μm or more. The D50 of the fine inorganic oxide powder (B) is preferably 8.0 μm or less, more preferably 7.8 μm or less, and even more preferably 7.5 μm or less. The D50 of the fine inorganic oxide powder (B) is preferably 5.0 to 8.0 μm, more preferably 5.5 to 7.8 μm, and even more preferably 6.0 to 7.5 μm. If the D50 of the fine inorganic oxide powder (B) is 5.0 μm or more, the powder for layered manufacturing can be easily packed at a high density. If the D50 of the fine inorganic oxide powder (B) is 8.0 μm or less, the angle of repose of the layered manufacturing powder can be increased and the flowability can be suppressed.
[0078] The fine inorganic oxide powder (B) has a D10 of preferably 1.0 to 4.0 μm, more preferably 2.0 to 3.8 μm, and further preferably 2.5 to 3.5 μm. If the fine inorganic oxide powder (B) has a D10 in the above range, the fine inorganic oxide powder (B) is expected to function as a bearing (bearing effect) and to keep the fluidity in an appropriate range.
[0079] The fine inorganic oxide powder (B) has a D90 of preferably 9.0 to 25.0 μm, more preferably 12.0 to 24.0 μm, and even more preferably 14.0 to 23.0 μm. When the fine inorganic oxide powder (B) has a D90 in the above range, the powder for layered manufacturing can be expected to have an appropriate fluidity.
[0080] The ratio of D50 to D10 (D50 / D10) of the fine inorganic oxide powder (B) is preferably 1.5 to 5.0, more preferably 1.7 to 4.0, and even more preferably 1.8 to 3.0. When D50 / D10 is within the above range, the effect of suppressing aggregation of the fine inorganic oxide powder (B) can be expected, and the bulk density of the powder for additive manufacturing can be improved.
[0081] The ratio of D90 to D10 (D90 / D10) of the fine inorganic oxide powder (B) is preferably 3.5 to 9.0, more preferably 4.5 to 8.0, and even more preferably 5.5 to 7.0. If D90 / D10 is within the above range, the particle size distribution falls within a certain range, making it easy to use as a base material for powder for additive manufacturing, and the bulk density and flowability can be improved in a well-balanced manner.
[0082] The ratio of D90 to D50 (D90 / D50) of the fine inorganic oxide powder (B) is preferably 2.5 to 3.5, more preferably 2.8 to 3.2, and even more preferably 2.7 to 2.9. When D90 / D50 is in the above range, the flowability of the powder for layered manufacturing can be set in an appropriate range.
[0083] The shape of the fine inorganic oxide powder (B) is not particularly limited. For example, it may be spherical, ellipsoidal, scaly, irregular, etc. Among them, the spherical shape is preferred because it is easy to obtain an appropriate bulk density.
[0084] The fine inorganic oxide powder (B) is preferably at least one selected from silica, alumina, zirconia, and titania, more preferably alumina, and even more preferably spherical alumina. The volume ratio of alumina in the fine inorganic oxide powder (B) is preferably 50 volume% or more, more preferably 60 volume% or more, and even more preferably 80 volume% or more. The upper limit of the volume ratio of alumina in the fine inorganic oxide powder (B) is not particularly limited. For example, it may be 100 volume%, 98 volume%, or 95 volume%.
[0085] <Method of manufacturing powder for additive manufacturing> The powder for additive manufacturing can be produced by mixing a coarse inorganic oxide powder (A) and a fine inorganic oxide powder (B). The method for mixing the materials is not particularly limited, and examples thereof include a method in which the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are dry-mixed or wet-mixed. The mixing may be performed manually or using a blender.
[0086] <Manufacturing method for 3D additive manufacturing> The three-dimensional additive manufacturing object can be manufactured by processing the additive manufacturing powder by a known powder additive manufacturing method. Examples of the powder additive manufacturing method include the binder jet method and the powder bed fusion method. The powder additive manufacturing method generally includes the following steps. (1) A process of supplying powder for additive manufacturing to the modeling stage of a powder additive manufacturing device (2) A process in which the supplied powder for additive manufacturing is spread evenly and thinly using a roller or the like to form a thin layer of powder for additive manufacturing. (3) A step of irradiating the formed thin layer of powder for additive manufacturing with a laser or an electron beam, or applying a liquid containing a binder to bind the powder for additive manufacturing. (4) A process of supplying new additive manufacturing powder on top of the solidified additive manufacturing powder. Thereafter, steps (2) to (4) are repeated to produce the desired three-dimensional layered object.
[0087] As a method for applying the binder-containing liquid, a method for ejecting the binder-containing liquid is preferred. The method for ejecting the binder-containing liquid is not particularly limited, and examples thereof include a dispenser method, a spray method, and an inkjet method. Among these, the inkjet method is preferred because it has good quantitation of droplets and can be applied over a large area.
[0088] When using the inkjet method, the liquid containing the binder can be applied by an inkjet head having a nozzle for ejecting the liquid. As the inkjet head, an inkjet head in a known inkjet printer can be suitably used, for example, an industrial inkjet RICOH MH / GH series (RICOH Co., Ltd.) can be mentioned.
[0089] The binder is not particularly limited, and known binders such as polyvinylpyrrolidone, polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, acrylic resins, polyamides, etc. The binder can be used by adjusting the viscosity with an appropriate solvent.
[0090] <Method of manufacturing sintered body> A sintered body can be produced by sintering the three-dimensional laminated body by a known sintering method. It is preferable to perform a degreasing treatment before the sintering treatment. A specific method for producing a sintered body is exemplified below.
[0091] The three-dimensional laminated model is placed in a sintering furnace, and the temperature inside the furnace is raised to a degreasing temperature. The degreasing temperature can be set appropriately within the range of, for example, 500 to 700°C. After that, the temperature inside the furnace is maintained at the degreasing temperature for 0.5 to 4 hours to burn off the organic components (degreasing). The degreasing time can be set according to the type of binder and the organic component ratio in the three-dimensional laminated model. Next, the temperature inside the furnace is raised to a sintering temperature. The sintering temperature can be set appropriately within the range of, for example, 900 to 1300°C. After that, the temperature inside the furnace is maintained at the sintering temperature for 1 to 7 hours to sinter the three-dimensional laminated model, thereby obtaining a sintered body (sintering). The sintering temperature and sintering time can be set according to the type of inorganic oxide powder. EXAMPLES
[0092] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0093] <Materials used> Coarse inorganic oxide powder (A): Spherical alumina (Showa Denko K.K. Alunabeads (trademark) / CB): True density 3.95g / m 3 Coarse inorganic oxide powder (B): Spherical alumina (Showa Denko K.K. Alunabeads (trademark) / CB): True density 3.95g / m 3
[0094] <Evaluation method> (bulk density) The bulk density was evaluated from the press-molded bulk density under a pressure of 98 MPa. Specifically, the sample was packed into a circular mold (inner diameter 30 mm) and a molded body was produced under a pressure of 98 MPa using a commercially available press. The density of the obtained molded body was determined as the press-molded bulk density under a pressure of 98 MPa. The press-molded bulk density was 2.52 g / cm 3 If the density is 2.54 g / cm or more, the density of the three-dimensional additive manufacturing body becomes high, so that the shrinkage rate during sintering becomes low, which is excellent. 3When the binder is applied, the binder can penetrate between the powder materials, which is excellent. That is, the press molding bulk density is 2.52 to 2.54 g / cm 3 In this case, the bulk density was evaluated as good.
[0095] (Circularity) The area S and perimeter L were measured using an FPIA-3000 manufactured by Malvern Panalytical. As a pretreatment, due to the measurement range of the device, about 10 g of the sample was placed in a 200 mm diameter gold sieve (25 μm mesh size) and shower water was used to remove particles larger than 25 μm. The sample that fell through the sieve was transferred to a plastic container and used as the measurement sample. The measurement conditions were LPF / HPF standard (20x lens) and bright field, and a particle sheath manufactured by the same company was used as the measurement solvent. 2 g of the measurement sample was weighed into a 50 mL beaker, and the sample was placed in the device using pure water and measured so that the effective number of analysis particles was 5000. As data processing after the measurement, particles with multiple particles on one screen were deleted and the average circularity was calculated.
[0096] (Liquidity) Fluidity was evaluated from the angle of repose. If the angle of repose is 55 degrees or more, it has excellent shape stability (fluidity) that allows the shape to be maintained from the application of the binder to the sintering process. If it is 58 degrees or less, it has excellent laying ability (fluidity) that allows the material to be smoothly supplied to the modeling stage and spread evenly. In other words, if the angle of repose is 55 to 58 degrees, the fluidity was evaluated as good.
[0097] [Example 1] Coarse inorganic oxide powder (A) and fine inorganic oxide powder (B) having the particle size and particle size ratio shown in Table 1 were mixed using a rocking mixer in such a ratio that the volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) was 11.1 volume %, to obtain a powder for additive manufacturing. The particle size distribution, BET specific surface area, circularity, fluidity (angle of repose), and press molding bulk density of the obtained powder for additive manufacturing were evaluated. The results are shown in Table 2.
[0098] [Examples 2 to 6, Comparative Examples 1 to 16] Powder for additive manufacturing was obtained in the same manner as in Example 1, except that the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B), and the volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) were as shown in Table 1. The particle size distribution, BET specific surface area, circularity, flowability (angle of repose), and press molding bulk density of the obtained powder for additive manufacturing were evaluated. The results are shown in Table 2. Items that were not evaluated are marked with "-".
[0099] [Table 1-1] [Table 1-2]
[0100] [Table 2-1] [Table 2-2]
[0101] Examples 1 to 6 have angles of repose in the range of 55 to 58 degrees and have appropriate fluidity, so when used in the binder jet method, a uniform powder layer can be formed when forming a thin layer of powder for additive manufacturing, and it is believed that the shape can be maintained from the application of the binder to the sintering process. In addition, Examples 1 to 6 have press molding bulk densities of 2.52 to 2.54 g / cm 3 Since the bulk density is within the range of 0.1 to 1.0 μm and the press molding bulk density is appropriate, it is considered that when used in the binder jet method, the binder can penetrate between the powder materials and a low shrinkage rate can be achieved during sintering. [Industrial Applicability]
[0102] By using the powder for additive manufacturing in one embodiment, it is possible to create a molded body with few voids in an additive manufacturing method (binder jet method) in which a liquid binder is sprayed onto a spread powder material to solidify it, and this is expected to have the effect of reducing heat shrinkage during the sintering process of the molded body.
Claims
1. A powder for additive manufacturing which is an inorganic oxide powder, D10 is 1.0 to 4.0 μm, D50 is 5.5 to 9.0 μm, and D90 is 20.0 to 40.0 μm, A powder for additive manufacturing, in which the volume ratio of particles having a particle size of 16.8 to 60.0 μm is 15.0 to 22.0 volume %.
2. The powder for layered manufacturing according to claim 1, wherein the volume ratio of particles having a particle diameter of 2.0 μm or more is 90.0 to 100 volume %.
3. The ratio of D50 to D10 (D50 / D10) is 2.0 to 2.2; The ratio of D90 to D10 (D90 / D10) is 6.0 to 8.
0. The powder for additive manufacturing according to claim 1 .
4. BET specific surface area: 0.1 to 10.0 m 2 The powder for layered manufacturing according to any one of claims 1 to 3, wherein the powder has a molecular weight of 1000 or more and a molecular weight of 1000 or more.
5. The powder for layered manufacturing according to any one of claims 1 to 3, which has a spherical shape.
6. The powder for layered manufacturing according to any one of claims 1 to 3, which is alumina.
7. Press molding bulk density under a pressure of 98 MPa is 2.52 to 2.54 g / cm 3 The powder for additive manufacturing according to claim 6,
8. A coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm; A fine inorganic oxide powder (B) having a D50 smaller than that of the coarse inorganic oxide powder (A). Including, The powder for layered manufacturing, wherein the volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is 9.5 to 29.0 volume %.
9. The powder for layered manufacturing according to claim 8, wherein the particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) is 0.26 to 1.
15.
10. D50 (D A 50) and the D50 (D B 50), D A 50-D B The powder for additive manufacturing according to claim 8 or 9, which satisfies 50≧3.5 μm.
11. A coarse-grained inorganic oxide powder (A) having a D50 of 9.0 to 25.0 μm; A fine inorganic oxide powder (B) having a D50 smaller than that of the coarse inorganic oxide powder (A). Including, The powder for layered manufacturing has a particle size volume ratio of the coarse inorganic oxide powder (A) to the fine inorganic oxide powder (B) of 0.26 to 1.
15.
12. The volume ratio of the coarse inorganic oxide powder (A) to the total volume of the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) is 9.5 to 29.0 volume%. Powder for additive manufacturing according to claim 11.
13. D50 (D A 50) and the D50 (D B 50), D A 50-D B The powder for additive manufacturing according to claim 11 or 12, which satisfies 50≧3.5 μm.
14. The powder for additive manufacturing according to claim 8 or 11, wherein the fine inorganic oxide powder (B) has a D50 of 5.0 to 8.0 μm.
15. The ratio of D50 to D10 (D50 / D10) of the coarse inorganic oxide powder (A) is 1.5 to 3.5; The ratio of D90 to D10 (D90 / D10) of the coarse inorganic oxide powder (A) is 4.0 to 7.0; The powder for layered manufacturing according to claim 8 or 11.
16. The powder for layered manufacturing according to claim 8 or 11, wherein the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are both spherical in shape.
17. The powder for additive manufacturing according to claim 8 or 11, wherein both the coarse inorganic oxide powder (A) and the fine inorganic oxide powder (B) are alumina.
18. Press molding bulk density under a pressure of 98 MPa is 2.52 to 2.54 g / cm 3 The powder for additive manufacturing according to claim 17,
19. The powder for layered manufacturing according to any one of claims 1 to 3, 8, 9, 11 and 12, which is used in a binder jet method.
20. A sintered body of the powder for layered manufacturing according to any one of claims 1 to 3, 8, 9, 11 and 12.
21. A method for producing a binder jet type additive manufacturing object, comprising applying a liquid containing a binder to the powder for additive manufacturing according to any one of claims 1 to 3, 8, 9, 11, and 12 to form a three-dimensional additive manufacturing object.
22. Applying a liquid containing a binder to the powder for additive manufacturing according to any one of claims 1 to 3, 8, 9, 11 and 12 to form a three-dimensional additive manufacturing object; and The three-dimensional laminated body is subjected to a sintering process. A method for producing a sintered body, comprising:
23. D10 is 1.0 to 4.0 μm, D50 is 5.5 to 9.0 μm, and D90 is 20.0 to 40.0 μm, An alumina powder in which the volume ratio of particles having a particle diameter of 16.8 to 60.0 μm is 15.0 to 22.0 volume %.
Citation Information
Patent Citations
Material for laminate molding, method of manufacturing cast by powder fixing lamination method and casting mold
JP2016117069A
Powder for lamination molding, slurry for lamination molding, three-dimensional lamination molded body, sintered compact, method for producing slurry for lamination molding, lamination molding method and sintering method