Electrode
By employing a binder particle group at the interface of the active material layer and current collector foil, the interfacial resistance is reduced and peel strength is maintained, addressing the resistive issues of conventional binder films in lithium ion battery electrodes.
Patent Information
- Application Number
- JP2024156517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-12-03
AI Technical Summary
The presence of a binder film between the current collector foil and the active material layer in lithium ion battery electrodes increases interfacial resistance due to its resistive nature.
The use of a binder particle group scattered at the interface between the active material layer and the current collector foil, instead of a continuous binder film, enhances the number of contact points and reduces interfacial resistance while maintaining high peel strength.
The binder particle group approach reduces interfacial resistance and maintains high peel strength with a smaller binder basis weight, achieving low interfacial resistance and improved adhesion.
Smart Images

Figure 2024161289000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to electrodes for lithium ion batteries and methods for making the same. [Background technology]
[0002] Japanese Patent Laid-Open Publication No. 2016-122631 (Patent Document 1) discloses forming a binder coat layer on a current collector. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-122631 A Summary of the Invention [Problem to be solved by the invention]
[0004] An electrode for a lithium ion battery (hereinafter, may be abbreviated as "electrode") may be manufactured by forming an active material layer on the surface of a current collector foil. In order to increase the peel strength between the active material layer and the current collector foil, it is considered to form a binder film between the active material layer and the current collector foil.
[0005] Conventionally, binder films are formed by a wet method. That is, a binder solution is applied to the surface of the current collecting foil to form the binder film. The binder film covers the surface of the current collecting foil. The binder is a resistive component. The presence of a binder film between the current collecting foil and the active material layer may increase the interfacial resistance (electronic resistance) between the current collecting foil and the active material layer.
[0006] An objective of the present disclosure is to mitigate the increase in interfacial resistance. [Means for solving the problem]
[0007] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.
[0008] 1. A lithium ion battery electrode includes a current collector foil, a binder particle group, and an active material layer. The binder particle group is attached to a surface of the current collector foil. The active material layer is disposed on the surface of the current collector foil. The active material layer includes an active material particle group. The binder particle group is scattered at the interface between the active material layer and the current collector foil.
[0009] In the electrode of "1" above, binder particle groups are scattered at the interface between the active material layer and the current collector foil. Because the binder is not in the form of a film but in the form of particles, a large number of active material particles can have contact with the current collector foil at the interface between the active material layer and the current collector foil. This can reduce the increase in interface resistance that accompanies the use of a binder.
[0010] When a binder film is formed on the surface of a current collector foil, it is believed that the number of contact points between the binder film (surface) and the active material particles is likely to be small. On the other hand, the binder particles may come into point contact with the active material particles. If the binder is particulate, the number of contact points between the binder and the active material particles may increase. By using binder particle groups instead of a binder film, it is expected that high peel strength can be obtained with a small binder basis weight.
[0011] 2. The ratio of the adhesion area of the binder particle group to the area of the current collecting foil may be, for example, 11.4 to 19.3%.
[0012] Hereinafter, "the ratio of the adhesion area of the binder particle group to the area of the current collecting foil" may be abbreviated as "area fraction." When the area fraction is 11.4% or more, an improvement in peel strength is expected. When the area fraction is 19.3% or less, a reduction in interface resistance is expected.
[0013] 3. The binder particles may have a smaller D50 than, for example, the active material particles.
[0014] When the size of the binder particles is smaller than the size of the active material particles, the number of contact points between the active material particles and the current collector foil can be increased, which is expected to reduce the interface resistance.
[0015] 4. The binder particle group is, for example, 0.010 to 0.017 mg / cm 2 The fiber may have a basis weight of
[0016] 5. A method for producing an electrode for a lithium ion battery includes the following steps (a) to (c): (a) Prepare a current collecting foil. (b) Binder particles are applied to the surface of the current collector foil by a dry method. (c) After the above (b), an active material layer is formed by applying an active material particle group onto the surface of the current collector foil.
[0017] When the binder particles are applied by a dry method, a binder film is not formed and the binder particles may become scattered.
[0018] 6. The above step (b) may include adhering the binder particles to the surface of the current collector foil by electrostatic force.
[0019] As an example of a dry method, it is possible to attach a binder particle group to a current collector foil by electrostatic force.
[0020] 7. The above (c) may include applying the active material particles by a dry method.
[0021] For example, when the active material particles are applied by a wet method, the arrangement of the binder particles may change. By applying the active material particles by a dry method, it is believed that the dispersed state of the binder particles is easily maintained.
[0022] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a conceptual cross-sectional view of a lithium ion battery electrode according to the present embodiment. [Diagram 2] FIG. 2 is a conceptual top view of the binder particles. [Diagram 3] FIG. 3 is a conceptual top view of the binder film. [Figure 4] FIG. 4 is a conceptual cross-sectional view of a binder film. [Diagram 5] FIG. 5 is a schematic flow chart of a method for producing an electrode for a lithium ion battery in this embodiment. [Figure 6] FIG. 6 is a conceptual diagram showing an example of a method for applying the binder particles. [Figure 7] FIG. 7 is a graph showing the relationship between the binder weight and the interface resistance. [Figure 8] FIG. 8 is a graph showing the relationship between the binder basis weight and the peel strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] <Definitions of terms, etc.> In this specification, the words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The word "consisting of" is closed-ended. However, even in the closed form, additional elements that are normally associated impurities or unrelated to the disclosed technology are not excluded. The word "consisting essentially of..." is semi-closed. In the semi-closed form, the addition of elements that do not substantially affect the basic and novel characteristics of the disclosed technology is permitted.
[0025] In this specification, expressions such as "may" and "can" are used in the permissive sense of "possibly" rather than in the obligatory sense of "must".
[0026] In this specification, a numerical range such as "m to n%" includes an upper limit and a lower limit unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". Furthermore, "m% or more and n% or less" includes "more than m% and less than n%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.
[0027] In this specification, all numerical values are modified by the term "about". The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values may be approximations that may vary depending on the application of the disclosed technology. All numerical values may be expressed in significant figures. Measurements may be average values of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are made, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limit of a measuring device.
[0028] In this specification, when a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may be allowed.
[0029] In this specification, the order of execution of multiple steps, operations, and the like included in various methods is not limited to the order described unless otherwise specified. For example, multiple steps may proceed simultaneously. For example, multiple steps may be performed in sequence.
[0030] In this specification, the term "electrode" is a general term for positive electrodes and negative electrodes. The electrode may be a positive electrode or a negative electrode.
[0031] In this specification, "D50" refers to the particle size at which the cumulative frequency from the smaller particle size reaches 50% in the volume-based particle size distribution. The volume-based particle size distribution is determined, for example, by a laser diffraction scattering method.
[0032] In this specification, the term "dry method" refers to a coating method in which the solid content of the paint is 90% or more. The solid content of the paint in the dry method may be, for example, 95 to 100%. The term "wet method" refers to a coating method in which the solid content of the paint is less than 90%. The solid content of the paint in the wet method may be, for example, 50 to 85%. The "solid content" refers to the mass fraction of solid components relative to the entire paint.
[0033] <Electrodes for lithium-ion batteries> FIG. 1 is a conceptual cross-sectional view of a lithium ion battery electrode in this embodiment. Hereinafter, the "lithium ion battery electrode in this embodiment" may be abbreviated as "the electrode". The electrode 10 is sheet-shaped. The electrode 10 includes a current collector foil 11, a binder particle group 12, and an active material layer 13. The binder particle group 12 and the active material layer 13 may be disposed on only one side of the current collector foil 11, or on both the front and back sides of the current collector foil 11.
[0034] The electrode 10 can have high peel strength. The peel strength between the active material layer 13 and the current collector foil 11 can be, for example, 1 N / m or more. The peel strength between the active material layer 13 and the current collector foil 11 can be, for example, 1 to 3.5 N / m. The electrode 10 can have low interface resistance. The interface resistance between the active material layer 13 and the current collector foil 11 can be, for example, 0.0033 Ω / cm 2 The interface resistance between the active material layer 13 and the current collecting foil 11 may be, for example, 0.0011 to 0.0033 Ω / cm 2 may be also possible.
[0035] Current-collecting foil The current collecting foil 11 is conductive. The current collecting foil 11 is in a sheet form. The current collecting foil 11 supports the active material layer 13. The current collecting foil 11 includes a metal foil. The current collecting foil 11 may include at least one type selected from the group consisting of, for example, aluminum foil, aluminum alloy foil, copper foil, copper alloy foil, nickel foil, titanium foil, and stainless steel foil. The current collecting foil 11 may have a thickness of, for example, 5 to 50 μm, or 10 to 25 μm.
[0036] <Binder particle group> The binder particle group 12 is scattered at the interface between the active material layer 13 and the current collector foil 11. FIG. 2 is a conceptual top view of the binder particle group. The binder particle group 12 is attached to the surface of the current collector foil 11. On the surface of the current collector foil 11, the binder particle group 12 is distributed in an island shape. Each island may be a single binder particle or an aggregate of a plurality of binder particles. The island may be distributed regularly or randomly. It is considered that the active material particles can come into contact with the current collector foil 11 in the gaps between the island portions. The gaps between the island portions may be, for example, the size of one binder particle or more.
[0037] On the surface of the current collecting foil 11, the binder particle group 12 has a density of, for example, 0.010 to 0.017 mg / cm 2 The binder particle group 12 may have a weight per unit area of, for example, 0.010 to 0.014 mg / cm. The weight per unit area indicates the mass (adhering amount) per unit area. 2 or 0.014 to 0.017 mg / cm 2 The fiber may have a basis weight of
[0038] On the surface of the current collecting foil 11, the binder particle group 12 may have an area fraction of, for example, 50% or less, 30% or less, or 20% or less. The binder particle group 12 may have an area fraction of, for example, 11.4 to 19.3%. When the area fraction is 11.4% or more, an improvement in peel strength is expected. When the area fraction is 19.3% or less, a reduction in interface resistance is expected. The binder particle group 12 may have an area fraction of, for example, 11.4 to 15.9%, or 15.9 to 19.3%.
[0039] The area fraction is calculated by the following formulas (I) to (IV). M = c × S0…(I) V = M ÷ ρ … (II) S1 = V÷T … (III) F = S1 ÷ S0 × 100 … (IV) "M" indicates the mass [mg] of the binder particle group. "c" is the weight of the binder particles [mg / cm 2 ] is indicated. "S0" is the area of the current collector foil [cm 2 ] is indicated. "V" is the volume of the binder particles [cm 3 ] is indicated. "ρ" is the density of the binder particles [g / cm 3 ] is indicated. "T" indicates the coating thickness [μm] of the binder particle group. "F" indicates the area fraction [%].
[0040] 3 is a conceptual top view of the binder film. Binder film 14 covers the surface of current collector foil 11. To form contact points between active material particles and current collector foil 11, binder film 14 may be arranged, for example, in stripes.
[0041] 4 is a conceptual cross-sectional view of a binder film. The active material particles come into contact with the current collector foil 11 in the gaps between the binder films 14. However, it is considered that the active material particles arranged on the binder film 14 are unlikely to come into contact with the current collector foil 11. Even if the binder film 14 is formed in a stripe pattern, it is considered that the desired interface resistance cannot be obtained.
[0042] The binder particle group 12 is an aggregate of a plurality of binder particles. The binder particle group 12 may have a D50 of, for example, 10 to 1000 nm, 50 to 500 nm, or 100 to 200 nm. The binder particle group 12 may have a smaller D50 than the active material particle group. Since the size of the binder particles is smaller than the size of the active material particles, the number of contact points between the active material particles and the current collector foil 11 may increase. This is expected to reduce the interface resistance. The D50 of the binder particle group 12 may be 1 / 10 or less, or 1 / 20 or less, of the D50 of the active material particle group. The D50 of the binder particle group 12 may be 1 / 100 or more of the D50 of the active material particle group.
[0043] The binder particles may include any component. For example, the binder particles may include at least one selected from the group consisting of polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyamideimide (PAI), and polyimide (PI).
[0044] 《Active material layer》 The active material layer 13 is disposed on the surface of the current collector foil 11. The active material layer 13 may have a thickness of, for example, 10 to 500 μm, or 50 to 200 μm. The active material layer 13 includes an active material particle group. The active material layer 13 may further include a conductive material, a binder, a solid electrolyte, and the like in addition to the active material particle group.
[0045] <Active material particle group> The active material particle group is an aggregate of a plurality of active material particles. The active material particle group may have a D50 of, for example, 1 to 30 μm, or may have a D50 of 3 to 10 μm.
[0046] The active material particles may include, for example, a positive electrode active material. The active material particles may include, for example, at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. Li(NiCoMn)O2 is, for example, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, Li(Ni 0.5 Co 0.2 Mn 0.3 )O2, Li(Ni 0.8 Co 0.1 Mn 0.1 ) O2, etc.
[0047] The active material particles may include, for example, a negative electrode active material, such as graphite, soft carbon, hard carbon, silicon, silicon oxide, a silicon-based alloy, tin, tin oxide, a tin-based alloy, and Li4Ti5O 12 may contain at least one selected from the group consisting of:
[0048] <Other Ingredients> The active material layer 13 may further contain a binder. The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material particle group. The binder contained in the active material layer 13 may be in the form of particles or a film. The binder may contain, for example, PVdF, CMC, SBR, etc.
[0049] The active material layer 13 may further contain a conductive material. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material particle group. The conductive material may contain, for example, conductive carbon particles, conductive carbon fibers, etc. The conductive material may contain, for example, at least one selected from the group consisting of carbon black, vapor-grown carbon fibers, carbon nanotubes, and graphene flakes. The carbon black may contain, for example, at least one selected from the group consisting of acetylene black, furnace black, channel black, and thermal black.
[0050] The active material layer 13 may further include a solid electrolyte. The solid electrolyte may include, for example, at least one selected from the group consisting of Li2S-P2S5, LiI-Li2S-P2S5, LiBr-Li2S-P2S5, and LiI-LiBr-Li2S-P2S5.
[0051] 〈Composition〉 For example, the active material particles may be composited with other solid materials (binders, conductive materials, etc.). For example, the active material particles may be mixed with other solid materials under conditions where a strong shearing force is applied to form composite particles. In the composite particles, for example, a binder and a conductive material may be attached to the surface of the active material particles.
[0052] <Method of manufacturing electrodes for lithium-ion batteries> 5 is a schematic flow chart of a method for manufacturing an electrode for a lithium ion battery in this embodiment. Hereinafter, "method for manufacturing an electrode for a lithium ion battery in this embodiment" may be abbreviated as "this manufacturing method". This manufacturing method includes "(a) preparation of a current collector foil", "(b) application of binder particles", and "(c) application of active material particles". This manufacturing method may further include, for example, "(d) fixing" or the like.
[0053] (a) Preparation of current collecting foil This manufacturing method includes preparing current collector foil 11. Details of current collector foil 11 are as described above.
[0054] (b) Coating of binder particles This manufacturing method includes applying, by a dry method, binder particles 12 (powder) to the surface of the current collector foil 11. For example, an electrostatic printing technique, an electrostatic painting technique, or a technique similar thereto may be used.
[0055] FIG. 6 is a conceptual diagram showing an example of a method for applying the binder particles. For example, the binder particles may be applied by electrostatic screen printing. The binder particles 12 are disposed on a screen 101. The screen 101 is conductive. A plurality of through holes are formed in the screen 101. The current collector foil 11 is disposed below the screen 101. The power source 102 applies a DC voltage between the current collector foil 11 and the screen 101. This forms an electric field (E) between the screen 101 and the current collector foil 11. An electric charge (q) is injected from the screen 101 to the binder particles 12. That is, the binder particles 12 are charged. The printing brush 103 smoothes the binder particles 12, so that the binder particles 12 are introduced into the electric field. In the electric field, an electrostatic force (F=qE) acts on the binder particles 12. The electrostatic force can cause the binder particles 12 to adhere to the surface of the current collector foil 11. For example, the application pattern can be controlled by the pattern of through holes in the screen 101. That is, a desired scattering state can be formed.
[0056] The coating thickness (deposition thickness) of the binder particle group 12 may be, for example, 0.1 to 3 μm, or 0.1 to 1 μm.
[0057] (c) Coating of active material particles This manufacturing method includes coating the surface of the current collector foil 11 with the binder particles 12 and then coating the surface with active material particles (powder) to form the active material layer 13.
[0058] The active material particles may be applied by any method. For example, a slurry containing the active material particles may be prepared. For example, the slurry may be applied to the surface of the current collector foil 11 by a die coater or the like. For example, a wet powder containing the active material particles may be prepared. For example, the wet powder may be applied to the surface of the current collector foil 11 by a roll coater or the like. The wet powder may also be referred to as a granule.
[0059] Like the binder particles, the active material particles may also be applied by a dry method. It is believed that by applying the active material particles by a dry method, the dispersed state of the binder particles is easily maintained.
[0060] For example, composite particles may be formed by compounding active material particles, a conductive material, and a binder. By applying a composite particle group (powder) by a dry method, an active material layer 13 having a homogeneous composition can be formed. This is considered to be because the positional relationship between the active material particles, the conductive material, and the binder is unlikely to change during the formation process of the active material layer 13. In the wet method, for example, the binder moves together with the solvent (liquid) during the formation process of the active material layer 13, which tends to cause bias in the composition.
[0061] (d) Establishment The present manufacturing method may include applying at least one of heat and pressure to active material layer 13 to fix active material layer 13 to current collector foil 11. Fixing active material layer 13 to current collector foil 11 is expected to improve peel strength.
[0062] Pressure and heat may be applied separately. Pressure and heat may be applied substantially simultaneously. For example, active material layer 13 may be compressed by a heat roll, a heat plate, or the like. The heating temperature of active material layer 13 may be, for example, a temperature near the melting point of the binder. The heating temperature may be, for example, 80 to 200°C, 120 to 200°C, or 140 to 180°C.
[0063] The pressure can be adjusted according to, for example, the target thickness and the target density of the active material layer 13. For example, a pressure of 50 to 200 MPa may be applied to the active material layer 13.
[0064] In this manner, the present electrode 10 can be manufactured. The present electrode 10 may be cut into a predetermined planar shape according to the specifications of the battery. EXAMPLES
[0065] <Electrode manufacturing> Electrodes No. 1 to 5 were manufactured as follows.
[0066] No.1 The following materials were prepared: Active material particles: Li(NiCoMn)O2, particle size range = 3 to 10 μm Conductive material: Acetylene black Binder particle group: PVdF, D50=150nm, density=1.76g / cm 3 Current collecting foil: Aluminum foil, thickness = 12 μm
[0067] An electrostatic screen printer (manufactured by Berg Kogyo Co., Ltd.) was prepared. The distance between the screen 101 and the current collecting foil 11 was set to 1 cm. A DC voltage of 1.5 kV was applied between the screen 101 and the current collecting foil 11 to form an electric field. The binder particles 12 were applied to the surface of the current collecting foil 11 by electrostatic screen printing (see FIG. 6). That is, the binder particles 12 were applied by a dry method. The weight of the binder particles 12 was 0.007 mg / cm. 2 The coating thickness of the binder particle group 12 was 0.5 μm.
[0068] A mixing device called the "Multi-Purpose Mixer" manufactured by Nippon Coke & Engineering Co., Ltd. was prepared. The device includes a spherical tank (mixing vessel). The spherical tank's convection promotion effect generates strong shear forces, which can compound solid materials.
[0069] The active material particles, conductive material, and binder were placed in a spherical tank. The material mixing ratio was "active material particles / conductive material / binder = 90 / 5 / 5 (mass ratio)". The rotation speed of the stirring blade was set to 10,000 rpm. The materials were mixed for 10 minutes. Composite particles were formed by the conductive material and binder adhering to the surfaces of the active material particles.
[0070] The composite particle group was applied to the surface of the current collector foil 11 by electrostatic screen printing (dry method). This formed the active material layer 13. In other words, the present electrode 10 was manufactured.
[0071] The electrode 10 was sandwiched between two heat plates (flat plates). The temperature of the heat plates was 160° C. A load of 15 tf was applied to the active material layer 13 by the heat plates. As a result, the active material layer 13 was fixed to the current collector foil 11.
[0072] No.2~4 As shown in Table 1 below, except that the basis weight of the binder particle group 12 was changed, the present electrode 10 was produced in the same manner as in No. 1, and the active material layer 13 was fixed.
[0073] No.5 A binder solution was prepared by dissolving the binder particles in a solvent. The binder solution was applied in stripes to the surface of the current collector foil 11 (see Figs. 3 and 4). This formed a binder film 14. Except for this, an electrode was manufactured in the same manner as No. 1.
[0074] <Electrode evaluation> The peel strength between the active material layer 13 and the current collector foil 11 was measured by a 90-degree peel test.
[0075] The interface resistance between the active material layer 13 and the current collecting foil 11 was measured using an electrode resistance measuring system (model name "RM2610", manufactured by HIOKI Corporation).
[0076] [Table 1]
[0077] 7 is a graph showing the relationship between the binder weight and the interface resistance. There is a tendency that the interface resistance increases as the binder weight increases.
[0078] FIG. 8 is a graph showing the relationship between the binder weight and peel strength. By applying the binder particles in a dry manner, there is a tendency that high peel strength can be obtained with a small binder weight. In other words, the dry method can reduce the binder weight compared to the wet method. Therefore, it is considered that the increase in interface resistance can be reduced by applying the binder particles in a dry manner (see FIG. 7).
[0079] <Additional Notes> This specification also supports a lithium ion battery. The lithium ion battery includes the present electrode. The lithium ion battery is expected to have a low battery resistance. This is because the interface resistance between the active material layer and the current collector foil is low in the present electrode. The lithium ion battery may be a liquid battery or an all-solid-state battery.
[0080] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]
[0081] 10 electrode (lithium ion battery electrode), 11 current collecting foil, 12 binder particle group, 13 active material layer, 14 binder film, 101 screen, 102 power supply, 103 printing brush.
Claims
1. A current collecting foil; an active material layer including a plurality of binder particles and a plurality of active material particles; Equipped with the plurality of binder particles are attached to a surface of the current collecting foil and are randomly distributed on the surface of the current collecting foil; The interface resistance between the current collecting foil and the active material layer is 0.004 Ω / cm 2 Below is the electrode.
2. The binder particles have a smaller D50 than the active material particles.
2. The electrode of claim 1.
3. The interface resistance is 0.0011 Ω / cm 2 0.0033Ω / cm or more 2 Below is the 3. The electrode according to claim 1 or 2.
4. The peel strength between the current collecting foil and the active material layer is 0.6 N / m or more and 3.5 N / m or less.
4. The electrode according to claim 1 .
5. The plurality of active material particles are Li(NiCoMn)O 2 Including particles, 5. An electrode according to any one of claims 1 to 4.
6. The plurality of active material particles are Li(NiCoAl)O 2 Including particles, 5. An electrode according to any one of claims 1 to 4.
7. The plurality of active material particles include graphite particles.
5. An electrode according to any one of claims 1 to 4.
8. The plurality of active material particles include graphite particles and silicon oxide particles.
5. An electrode according to any one of claims 1 to 4.
9. The plurality of binder particles include PVdF particles.
7. The electrode according to claim 5 or claim 6.
10. The plurality of binder particles include at least one of SBR particles and CMC particles, 9. The electrode according to claim 7 or claim 8.
11. The plurality of binder particles include SBR particles and CMC particles.
9. The electrode according to claim 7 or claim 8.
Citation Information
Patent Citations
Method for manufacturing electrode for battery and capacitor
JP2001216956A
Modified Guarane Binder for Lithium-ion Batteries
JP2017506800A
Method for manufacturing electrodes for all-solid-state batteries and electrodes for all-solid-state batteries manufactured by the same
JP2022512483A
Method of manufacturing electrode for lithium ion secondary battery
JP2016122631A