Aluminum-scandium composite, aluminum-scandium composite sputtering target and method of making

A non-equilibrium composite sputtering target with a ductile first phase and controlled scandium distribution addresses stoichiometry and porosity issues, enhancing film quality and target longevity in piezoelectric thin film production.

JP2024161587AActive Publication Date: 2024-11-19MATERION CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024144243
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-05
Filing Date
2024-08-26
Publication Date
2024-11-19
Estimated Expiration
2041-06-03

AI Technical Summary

Technical Problem

Conventional aluminum scandium alloys used in sputtering targets for producing piezoelectric thin films suffer from non-uniform stoichiometry, porosity, and microstructure defects, leading to poor performance, cracking, and reduced target life, which affects the quality and yield of thin films.

Method used

A non-equilibrium composite sputtering target comprising a ductile first phase and a brittle second phase, with controlled scandium distribution, is developed to enhance uniformity and minimize porosity, featuring a microstructure free of cracks and inclusions, and optimized scandium content exceeding equilibrium phase diagram expectations.

Benefits of technology

The composite target achieves improved film uniformity, reduced particle emissions, extended target life, and enhanced mechanical performance, resulting in higher wafer yields and lower costs by minimizing defects and maintaining consistent piezoelectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161587000002
    Figure 2024161587000002
  • Figure 2024161587000003
    Figure 2024161587000003
  • Figure 2024161587000004
    Figure 2024161587000004
Patent Text Reader

Abstract

To provide an Al-Sc alloy sputtering target that improves uniformity of stoichiometry and minimizes porosity, and to provide a method for making the same.SOLUTION: An Al-Sc alloy sputtering target. The target comprising from 1.0 at% to 65 at% scandium and from 35 at% to 99 at% aluminum and having a microstructure including a first aluminum matrix phase and a second phase dispersed uniformly therethrough. The second phase comprises one or more compounds corresponding to the formula ScxAly, where x is from 1 to 2 and y is from 0 to 3.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] cross reference

[0001] This application is related to and claims priority to U.S. Provisional Application No. 63 / 035,320, filed June 5, 2020, the entire contents of which are incorporated herein by reference.

[0002] This disclosure relates to alloys containing aluminum and scandium (Al-Sc alloys), and more particularly to the use of such Al-Sc alloys, and to articles and sputtering targets made from Al-Sc alloys. [Background technology]

[0003]

[0003] Aluminum scandium nitride (Al x Sc 1-x Sputtering (N) has been of interest for the purpose of producing thin film piezoelectric materials for various applications. Traditional methods produce these piezoelectric thin films by utilizing reactive sputter deposition. A sputtering target, usually a metal or metal alloy, is composed of the material to be sputtered. The sputtering target and substrate are placed in close proximity to each other in a chamber, and the target is bombarded with charged particles or ions. The energetic ions dislodge parts of the sputtering target and redeposit them on the substrate. Sputtering is beneficial because it allows control over the composition of the film, allows room for control over residual stress in the film, allows thin films to be deposited at high rates, and allows for easy controlled heating of the substrate. The use of this process in the production of thin films already has a well-established history.

[0004]

[0004] The properties of the resulting thin films are strongly dependent on the uniform deposition of the Al-Sc alloy. This places considerable demands on the sputtering target and alloy properties. The piezoelectric response of the thin films is strongly dependent on the scandium content of the film, so the overall stoichiometry and microdistribution of scandium in the sputtering target are important.

[0005]

[0005] In view of known alloys and sputtering targets, there is a need for alloys and sputtering targets that improve stoichiometric uniformity and minimize porosity. There is also a need for a microstructure that reduces target defects due to cracking and contamination from particulate emission during sputtering (not individual atoms / ions, but particles that are ejected from the surface of the sputtering target and land on the wafer, often referred to as particulation). These features can result in sputtering targets with better performance and life leading to higher wafer yields and lower cost of ownership. Summary of the Invention

[0006] In one embodiment, the present disclosure provides an Al-Sc composite or sputtering target comprising 1.0 at. % to 65 at. % scandium and 35 at. % to 99 at. % aluminum, having a microstructure comprising a first phase (5 vol. % to 99 vol. %, e.g., 20 vol. % to 99 vol. %) and a second phase (1 vol. % to 80 vol. %) dispersed therethrough, the second phase having the formula Al x Sc y where x is 0 to 3 and y is 1 to 2. The second phase may include ScAl3, ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof, or may include ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof. The second phase may include more than 25 atomic % scandium and / or more than 1 mole % Al2Sc, AlSc, AlSc2, or Sc , or combinations thereof, and / or less than 85 mol % aluminum, and / or 1.0 mol % to 70 mol % scandium nitride. The concentration of scandium in the second phase may exceed that predicted from an aluminum-scandium equilibrium phase diagram, for example by at least 1%. The composite or sputtering target may further comprise less than 1000 ppm oxygen, preferably less than 400 ppm, or more preferably less than 100 ppm oxygen. The grains of the first aluminum matrix phase may be characterized by a (110) crystallographic orientation or a random crystallographic orientation. The second phase may be characterized by a grain size ranging from 0.5 microns to 500 microns. The microstructure is substantially free of microcracks and fissures and / or oxide inclusions. The uniformity of scandium across the surface of the sputtering target may vary by less than ±0.5 atomic % scandium across the radius of the surface. The sputtering target may have a central axis through the thickness of the sputtering target and a diameter intersecting the central axis, and the uniformity of scandium across the central axis and diameter varies by less than ±0.5% by weight of scandium. The diameter may be greater than 300 mm.

[0007] In some embodiments, the present disclosure provides a method for preparing a non-equilibrium complex, comprising: x Sc y wherein x is 0 to 3 and y is 1 to 2; mixing the powder with a first phase comprising aluminum to form a composite precursor; applying at least one of heat or pressure to the composite precursor to solidify the material; and cooling the solidified composite precursor to form a non-equilibrium composite.

[0008] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the drawings. [Brief description of the drawings]

[0009] [Figure 1]

[0009] Phase diagram for aluminum and scandium. The y-axis is temperature (°C), ranging from 0°C to 1600°C in intervals of 200°C. Also marked on the y-axis is the melting point of aluminum, 660°C. [Diagram 2]

[0010] FIG. 1 is a schematic cross-sectional view showing a conventional aluminum matrix. [Figure 3A]

[0011] FIG. 2 is a schematic cross-sectional view illustrating an exemplary microstructure of an Al—Sc alloy having a second phase. [Figure 3B]

[0012] FIG. 2 is a schematic cross-sectional view illustrating an exemplary microstructure of an Al—Sc alloy having a first second phase and a second phase. [Figure 4]

[0013] FIG. 4A is a diagram showing the microstructure of an Al-Sc alloy (multiple phases are displayed). FIG. 4B is a diagram showing the microstructure of an Al-Sc alloy (multiple phases are displayed). FIG. 4C is a diagram showing the microstructure of an Al-Sc alloy (multiple phases are displayed). FIG. 4D is a diagram showing the microstructure of an Al-Sc alloy (multiple phases are displayed). FIG. 4E is a diagram showing the microstructure of an Al-Sc alloy (multiple phases are displayed). [Diagram 5]

[0014] Figure 5A is a SEM image showing the microstructure of an Al-Sc alloy (distribution of elements is displayed), Figure 5B is a SEM image showing the microstructure of an Al-Sc alloy (distribution of elements is displayed), and Figure 5C is a SEM image showing the microstructure of an Al-Sc alloy (distribution of elements is displayed). [Figure 6]

[0015] FIG. 1 is a collection of X-ray diffraction plots showing the metallic content of each component of a conventional Al—Sc alloy and an Al—Sc alloy according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010]

[0016] As previously mentioned, aluminum-scandium alloys produced using many conventional methods do not meet the demands for uniform stoichiometry and minimal porosity, as well as defect-free microstructures. As a result, films and substrates formed therefrom suffer from inconsistent properties. The alloys have poor thin film uniformity. Targets containing the alloys also have poor physical / mechanical performance, such as defects that cause cracks that can lead to arcing or particulation during sputtering, resulting in yield loss and reduced target life. The industry requires targets that are defect-free, prevent target cracking, exhibit reduced particulate emissions during sputtering, and have extended target life.

[0011] Aluminum-Scandium Complex

[0017] Disclosed herein are non-equilibrium composites comprising a ductile first phase and a brittle second phase, for use, for example, as sputtering targets. A specific second phase, e.g., (brittle) intermetallic Al, is present (in a specific amount) in the non-equilibrium composite. x Sc y The use of the phase maximizes the amount of ductile aluminum phase and reduces the amount of brittle intermetallic Al while maintaining the overall composition ratio in the composite. x Sc y It has been found that this results in a microstructure that minimizes the amount of intermetallic Al phases that have higher scandium content and / or lower amounts of aluminum (outside the range of amounts expected from the aluminum-scandium equilibrium phase diagram). This results in a desirable combination of the aforementioned features, such as uniformity in the bulk composition of the aluminum-scandium alloy, and a microstructure that is free of defects and porosity, as well as prevention of target cracking and reduced casting defects and particle shedding. x Sc y The desired increase in ductile phase content is achieved by using less intermetallic Al phase. x Sc y Because a phase is used, a greater amount of the ductile aluminum phase is available, providing the advantages discussed above.

[0012]

[0018] As mentioned above, the addition of metastable ductile phases, such as "free aluminum", to the microstructure can reduce particulates and improve overall target performance. The added ductility provided by the ductile phase also facilitates thermomechanical processing of these materials. This allows for the repair of casting defects such as solidification pores and non-uniform microstructures. Arcing is also reduced, improving consistency of sputtering performance throughout the life of the target. Thin films made using the sputtering targets disclosed herein also advantageously exhibit reduced particulates during sputtering. Particles that are detrimentally expelled from the particle surface are considered contaminants, as these particles affect and reduce the overall device yield. In some embodiments, the (uniform) macroscopic distribution of the brittle second phase results in composites that have surprisingly been found to have a more uniform composition, and therefore result in sputtering targets that produce higher quality thin films. Additionally, the composites formed by the disclosed methods can advantageously produce larger diameter sputtering targets that, in some cases, are prone to cracking when produced by conventional methods.

[0013]

[0019] Previously, it has been difficult to achieve the desired amount (if any) of ductile aluminum phase in higher scandium containing alloys because conventional manufacturing (casting) methods yielded equilibrium microstructures with lower aluminum contents and phase volume ratios predicted from the aluminum-scandium equilibrium phase diagram. By utilizing the non-equilibrium phase distribution referred to herein, however, composites produced by the methods disclosed herein achieve the desired amount of ductile aluminum phase throughout the composition.

[0014]

[0020] By carefully designing the phases present in the composite target, the amount of ductile phase present can be beneficially increased compared to conventional balance alloys that have little, if any, free aluminum (alloys below 25% Sc) or no balance aluminum (alloys with Sc contents equal to or greater than 25% Sc), thereby increasing the ductility and strength of the material, improving chemical uniformity, and reducing the amount of particulate matter that occurs during sputtering.

[0015] Macroscopic structure

[0021] The present disclosure relates to composites containing aluminum and scandium (Al-Sc composites). The Al-Sc composites can be used to manufacture articles such as sputtering targets that, among other advantages, have high compositional uniformity with a uniform distribution of the second phase. In some embodiments, the Al-Sc composite contains 1.0 atomic % to 65 atomic % scandium and 35 atomic % to 99 atomic % aluminum (optionally with other elements). Further compositional details are provided below.

[0016]

[0022] Overall, the disclosed composites include 1.0 atomic % to 65 atomic % scandium in some embodiments, e.g., 5 atomic % to 55 atomic %, 5 atomic % to 45 atomic %, 10 atomic % to 50 atomic %, 15 atomic % to 45 atomic %, 20 atomic % to 40 atomic %, 1.0 atomic % to 5 atomic %, 5 atomic % to 10 atomic %, 10 atomic % to 15 atomic %, 15 atomic % to 20 atomic %, 20 atomic % to 25 atomic %, 25 atomic % to 30 atomic %, 30 atomic % to 35 atomic %, 35 atomic % to 40 atomic %, 40 atomic % to 45 atomic %, 45 atomic % to 50 atomic %, 50 atomic % to 55 atomic %, 55 atomic % to 60 atomic %, or 60 atomic % to 65 atomic %. [Confirm experimental data, if available, to be consistent with the examples.]

[0023] In terms of the lower limit, the composite may contain more than 1.0 atomic %, e.g., more than 5 atomic %, more than 10 atomic %, more than 15 atomic %, more than 20 atomic %, more than 25 atomic %, more than 30 atomic %, more than 35 atomic %, more than 40 atomic %, more than 45 atomic %, more than 50 atomic %, more than 55 atomic %, or more than 60 atomic % scandium. In terms of the upper limit, the composite may contain less than 65 atomic %, e.g., less than 60 atomic %, less than 55 atomic %, less than 50 atomic %, less than 45 atomic %, less than 40 atomic %, less than 35 atomic %, less than 30 atomic %, less than 25 atomic %, less than 20 atomic %, less than 15 atomic %, less than 10 atomic %, or less than 5 atomic % scandium.

[0017]

[0024] The limitations "greater than" and "less than" used herein may be inclusive of the numbers attached thereto. In other words, "greater than" and "less than" may be interpreted as "greater than or equal to" and "less than or equal to." It is believed that this language may be modified in a later claim to include "or equal to." For example, "greater than 4.0" may be interpreted as "greater than or equal to 4.0" and may be modified in a later claim to "greater than or equal to 4.0."

[0018]

[0025] In some embodiments, the composite comprises 35 atomic % to 99 atomic %, e.g., 40 atomic % to 95 atomic %, 45 atomic % to 90 atomic %, 50 atomic % to 80 atomic %, 55 atomic % to 75 atomic %, 60 atomic % to 75 atomic %, 62 atomic % to 72 atomic %, 35 atomic % to 40 atomic %, 40 atomic % to 50 atomic %, 50 atomic % to 55 atomic %, 55 atomic % to 60 atomic %, 60 atomic % to 65 atomic %, 65 atomic % to 70 atomic %, 70 atomic % to 75 atomic %, 75 atomic % to 80 atomic %, 80 atomic % to 85 atomic %, 85 atomic % to 90 atomic %, 90 atomic % to 95 atomic %, or 95 atomic % to 99 atomic % aluminum. These amounts account for the aluminum present in the first phase (as free aluminum) and the aluminum present as a component in the second intermetallic phase.

[0019]

[0026] In terms of the lower limit, the composite may contain more than 35 atomic %, e.g., more than 40 atomic %, more than 45 atomic %, more than 50 atomic %, more than 55 atomic %, more than 60 atomic %, more than 65 atomic %, more than 70 atomic %, more than 75 atomic %, more than 80 atomic %, more than 85 atomic %, more than 90 atomic %, or more than 95 atomic % aluminum. In terms of the upper limit, the composite may contain less than 99 atomic %, e.g., less than 95 atomic %, less than 90 atomic %, less than 85 atomic %, less than 80 atomic %, less than 75 atomic %, less than 70 atomic %, less than 65 atomic %, less than 60 atomic %, less than 55 atomic %, less than 50 atomic %, less than 45 atomic %, or less than 40 atomic % aluminum.

[0020]

[0027] In some embodiments, the composite comprises 1.0 mol% to 70 mol%, e.g., 1 mol% to 5 mol%, 5 mol% to 10 mol%, 10 mol% to 15 mol%, 20 mol% to 25 mol%, 25 mol% to 30 mol%, 30 mol% to 35 mol%, 35 mol% to 40 mol%, 40 mol% to 45 mol%, 45 mol% to 50 mol%, 50 mol% to 55 mol%, 55 mol% to 60 mol%, 60 mol% to 65 mol%, or 65 mol% to 70 mol% scandium nitride. In terms of the lower limit, the alloy may contain more than 1 mol%, e.g., more than 5 mol%, more than 10 mol%, more than 15 mol%, more than 20 mol%, more than 25 mol%, more than 30 mol%, more than 35 mol%, more than 40 mol%, more than 45 mol%, more than 50 mol%, more than 55 mol%, more than 60 mol%, or more than 65 mol% scandium nitride. In terms of the upper limit, the alloy may contain less than 70 mol%, e.g., less than 65 mol%, less than 60 mol%, less than 55 mol%, less than 50 mol%, less than 45 mol%, less than 40 mol%, less than 35 mol%, less than 30 mol%, less than 25 mol%, less than 20 mol%, less than 15 mol%, less than 10 mol%, or less than 5 mol% scandium nitride.

[0021]

[0028] Nitride powders are useful in controlling oxygen absorption and can passivate powder components and stabilize them with the molten aluminum during processing.

[0022]

[0029] In some cases, the composite is of high purity and contains as little impurities as possible. For example, oxygen is extremely detrimental to the properties of piezoelectric films, both by selectively bonding to the substrate and stabilizing other non-piezoelectric phases. Therefore, the composite or sputtering target should contain as little oxygen as possible. In some embodiments, the composite contains less than 1500 ppm of oxygen, such as less than 1000 ppm, less than 900 ppm, less than 800 ppm, less than 700 ppm, less than 600 ppm, less than 500 ppm, less than 400 ppm, less than 300 ppm, less than 200 ppm, or less than 100 ppm. The presence of transition metal elements, such as iron, should also be minimized.

[0023]

[0030] In some embodiments, the uniformity of scandium across the surface of the composite, e.g., a sputtering target formed from the composite, varies by less than ±0.5 atomic % of scandium across the surface, e.g., less than ±0.4 atomic %, less than ±0.3 atomic %, less than ±0.2 atomic %, less than ±0.1 atomic %, or less than ±0.05 atomic %. In some embodiments, the uniformity of scandium across the central axis and diameter of a sputtering target formed from the composite and having a central axis and a diameter intersecting the central axis through the thickness of the sputtering target varies by less than ±0.5 atomic %, e.g., less than ±0.4 atomic %, less than ±0.3 atomic %, less than ±0.2 atomic %, less than ±0.1 atomic %, or less than ±0.05 atomic % of scandium.

[0024]

[0031] Sputtering targets made from the composites can be used to deposit thin films on substrates. The piezoelectric properties of individual devices on the substrate depend heavily on the local stoichiometry of the films contained within the individual devices. Therefore, the distribution of scandium on the Al-Sc sputtering target should be as uniform as possible, both in-plane (e.g., on the surface) and through the thickness of the sputtering target. Both chemical uniformity across the surface and through the thickness is required, because if the amount of scandium sputtered from the target varies over the life of the target, the piezoelectric properties of the deposited film will change over the life of the target, resulting in inconsistent device performance and loss of product yield. The properties and characteristics of the composites are described below.

[0025] Microstructure

[0032] In some embodiments, the composite comprises a first phase having ductility and a matrix. The composite may include a brittle second phase dispersed throughout the composite, the second phase may include aluminum and scandium. The scandium present throughout the composite is optionally provided by the second phase. Optionally, the second phase has the formula Al x Sc y where x is 0 to 3 and y is 1 to 2. The second phase may include Al3Sc, Al2Sc, AlSc, Sc2Al, or Sc, or combinations thereof.

[0026]

[0033] In some embodiments, the composite comprises 5% to 99% by volume, e.g., 20% to 99% by volume, of the first phase (free aluminum) and 1% to 80% by volume of the second phase, based on the total volume of the composite. For example, the composite may comprise 5% to 95% by volume, e.g., 40% to 90% by volume, 5% to 50% by volume, 5% to 35% by volume, 5% to 25% by volume, 10% to 50% by volume, 10% to 40% by volume, 10% to 25% by volume, 7% to 50% by volume, 7% to 40% by volume, 7% to 30% by volume, 7% to 25% by volume, 45% to 85% by volume, 50% to 80% by volume, 55% to 75% by volume, or 60% to 70% by volume of the first phase. In terms of lower limits, the composite may comprise more than 5 vol%, e.g., more than 7 vol%, more than 10 vol%, more than 12 vol%, more than 15 vol%, more than 17 vol%, more than 20 vol%, more than 40 vol%, more than 45 vol%, more than 50 vol%, more than 55 vol%, more than 60 vol%, more than 65 vol%, or more than 70 vol% of the first phase. In terms of upper limits, the composite may comprise less than 99 vol%, e.g., less than 95 vol%, less than 90 vol%, less than 85 vol%, less than 80 vol%, less than 75 vol%, less than 70 vol%, less than 60 vol%, less than 50 vol%, less than 45 vol%, less than 40 vol%, less than 35 vol%, less than 30 vol%, less than 25 vol%, less than 20 vol%, less than 15 vol%, or less than 10 vol% of the first phase.

[0027]

[0034] The amounts of first and second phases present may be quantitatively measured by optical and SEM / EDS microscopy, EBSD, or other known techniques.

[0028]

[0035] Optionally, the first phase may contain small amounts of scandium, for example less than 1 wt.%, less than 0.5 wt.%, less than 0.2 wt.%, or less than 0.1 wt.%.

[0029]

[0036] In some embodiments, the composite comprises 1% to 80% by volume, e.g., 5% to 75% by volume, 10% to 70% by volume, 15% to 65% by volume, 20% to 60% by volume, 25% to 55% by volume, or 30% to 50% by volume of the second phase. At the lower end, the composite may comprise more than 20% by volume, e.g., more than 1% by volume, more than 5% by volume, more than 10% by volume, more than 15% by volume, more than 20% by volume, more than 25% by volume, more than 30% by volume, or more than 35% by volume of the second phase. At the upper end, the composite may comprise less than 80% by volume, e.g., less than 75% by volume, less than 70% by volume, less than 65% by volume, less than 60% by volume, less than 55% by volume, or less than 50% by volume of the first phase. Because the scandium content of the disclosed second phases is greater than conventional alloys using equilibrium phase distributions, as determined by equilibrium phase diagrams, these amounts are typically less than those used in conventional alloys. Thus, lesser amounts can be used to achieve the overall scandium concentration. Because lesser amounts of the second phases are used, it is possible to advantageously utilize a greater amount of the ductile aluminum phase.

[0030]

[0037] FIG. 1 is a phase diagram of aluminum and scandium. The x-axis shows the amount of scandium in atomic percent (at.%), with zero scandium / 100 at.% aluminum at the left end of the diagram. Examination of the Al-Sc phase diagram reveals that an equilibrium alloy with 0 to 25 at.% scandium may contain the intermetallic Al3Sc phase in a metallic aluminum matrix. At higher scandium contents, the composite may contain Al3Sc, Al It may contain one or more intermetallic phases selected from 2Sc, AlSc, AlSc2, or it may contain scandium, or it may contain any combination of an intermetallic phase and scandium.

[0031]

[0038] The second phase in the composite comprises a large amount / high concentration of scandium, e.g., outside of, e.g., greater than, the amount / concentration of scandium expected from an aluminum-scandium equilibrium phase diagram. For example, the second phase can comprise more than (or equal to), 25 atomic %, e.g., more than 28 atomic %, more than 30 atomic %, more than 33 atomic %, more than 35 atomic %, more than 40 atomic %, more than 45 atomic %, more than 50 atomic %, more than 55 atomic %, more than 65 atomic %, more than 66 atomic %, more than 70 atomic %, more than 75 atomic %, more than 80 atomic %, more than 85 atomic %, or more than 90 atomic % scandium relative to the total amount of the second phase.

[0032]

[0039] The second phase includes certain intermetallic phases, e.g., Al3Sc, Al2Sc, AlSc, AlSc2, in amounts outside the range of amounts / concentrations predicted, e.g., from an aluminum-scandium equilibrium phase diagram. For example, the second phase may include these intermetallic phases in amounts greater than 5 mol%, e.g., greater than 10 mol%, greater than 15 mol%, greater than 20 mol%, greater than 25 mol%, greater than 30 mol%, greater than 35 mol%, greater than 40 mol%, greater than 45 mol%, greater than 50 mol%, greater than 55 mol%, greater than 60 mol%, or greater than 65 mol% of the total amount of the second phase. In terms of upper limits, the second phase may contain these intermetallic phases in an amount of less than 95 mol%, e.g., less than 90 mol%, less than 85 mol%, less than 80 mol%, less than 75 mol%, less than 70 mol%, less than 65 mol%, less than 60 mol%, less than 60 mol%, less than 55 mol%, less than 50 mol%, less than 45 mol%, less than 40 mol%, less than 35 mol%, less than 30 mol%, or less than 25 mol%.

[0033]

[0040] In some embodiments, these amounts / concentrations are outside (eg, exceed) the range of amounts / concentrations predicted by the aluminum-scandium equilibrium phase diagram.

[0034]

[0041] In some embodiments, intermetallic phases having greater / higher amounts of scandium and / or less aluminum may be utilized. For example, the second phase may include Al3Sc, Al2Sc, AlSc, AlSc2, or Sc, or combinations thereof, in an amount greater than 1 mol%, e.g., greater than 2 mol%, greater than 5 mol%, greater than 10 mol%, greater than 15 mol%, greater than 20 mol%, greater than 25 mol%, greater than 30 mol%, greater than 35 mol%, greater than 40 mol%, greater than 45 mol%, greater than 50 mol%, greater than 55 mol%, greater than 60 mol%, or greater than 65 mol%, based on the total moles of the second phase. In some embodiments, these amounts / concentrations are outside (e.g., beyond) the ranges of amounts / concentrations predicted from an aluminum-scandium equilibrium phase diagram. These ranges and limits are applicable to the intermetallic phases collectively and to each intermetallic phase individually.

[0035]

[0042] It has been found that some second phase components are particularly brittle and can be detrimental to the composition as a whole. In some embodiments, the second phase includes a certain amount of an intermetallic phase, such as Al2Sc. For example, the second phase can include less than 60 mol%, such as less than 55 mol%, less than 50 mol%, less than 40 mol%, less than 30 mol%, less than 20 mol%, less than 10 mol%, or less than 5 mol% Al2Sc, based on the total moles of the second phase. In some embodiments, the second phase is free or substantially free of Al2Sc.

[0036]

[0043] The second phase, if present, contains small amounts / concentrations of aluminum, e.g., amounts / concentrations outside the range of amounts / concentrations predicted by the aluminum-scandium equilibrium phase diagram. The second phase may contain less than (or equal to) 75 atomic % aluminum, for example less than 70 atomic %, less than 66 atomic %, less than 65 atomic %, less than 60 atomic %, less than 55 atomic %, less than 50 atomic %, less than 45 atomic %, less than 40 atomic %, or less than 35 atomic % aluminum, relative to the total amount of the second phase.

[0037]

[0044] In some cases, the amount of scandium in the second phase is greater than that predicted by an aluminum-scandium equilibrium phase diagram, e.g., at least 1% more, at least 2% more, at least 5% more, at least 10% more, at least 15% more, at least 20% more, at least 25% more, at least 35% more, at least 50% more, at least 75% more, or at least 100% more.

[0038]

[0045] 3A and 3B depict schematic cross-sectional views of Al-Sc alloy microstructures, with FIG. 2 depicting a conventional aluminum alloy 100 with an aluminum-rich metal matrix 120 without the presence of a second phase. FIG. 3A depicts an Al-Sc alloy 200 according to the present disclosure, which may include a second phase 150 uniformly dispersed throughout the aluminum matrix 120. In some cases, said second phase may be dispersed a spatial distance d1 apart, which may include a range.

[0039]

[0046] The second phase may, in some embodiments, include multiple separate phases, such as a second phase, a third phase, and a fourth phase. Phases higher than the second phase, such as a third phase, a fourth phase, etc., are intended to have the same description and properties as those set forth above for the second phase. For example, the third phase may have a high scandium content, for example, outside the range of amounts expected from an aluminum-scandium equilibrium phase diagram.

[0040]

[0047] For example, Figure 3B shows another Al-Sc composite 300 according to the present disclosure including a second phase 150 and a third phase 160 uniformly dispersed throughout a first phase 120. Phases 150 and 160 can be as described herein. A composite according to the present disclosure, not shown, can include more than four phases, for example five or six phases, each phase dispersed throughout the first phase.

[0041]

[0048] In some embodiments, the first phase grains and the second phase grains each have an average grain size that may be measured according to ASTM E112 (this year).

[0042]

[0049] In some embodiments, the first phase is characterized by having an average particle size ranging from 2 μm to 200 μm, e.g., from 10 μm to 150 μm, from 15 μm to 125 μm, from 20 μm to 100 μm, from 25 μm to 75 μm, from 2 μm to 40 μm, from 2 μm to 20 μm, from 4 μm to 12 μm, from 10 μm to 100 μm, from 20 μm to 80 μm, from 30 μm to 70 μm, or from 40 μm to 70 μm.

[0043]

[0050] At the lower limit, the first phase may be characterized by having an average particle size of more than 2 μm, e.g., more than 4 μm, more than 10 μm, more than 20 μm, more than 25 μm, more than 30 μm, more than 40 μm, or more than 50 μm. At the upper limit, the first phase may be characterized by having an average particle size of less than 200 μm, e.g., less than 150 μm, less than 125 μm, less than 100 μm, less than 80 μm, less than 75 μm, less than 70 μm, less than 40 μm, less than 20 μm, or less than 12 μm.

[0044]

[0051] In some embodiments, the grains of the first aluminum matrix phase are characterized as having a (110) crystallographic orientation. In other embodiments, the grains of the first aluminum matrix phase are characterized as having no preferred crystallographic orientation or as having a random structure. In some cases, the structure may be quantified with XRD peak height ratios, EBSD volume ratios, EBSD structure analysis MRD values, and / or XRD pole figure MRD values.

[0045]

[0052] In some embodiments, the first phase grains are characterized as having a random crystallographic orientation.

[0046]

[0053] It may be desirable for the second phase to be as fine as possible, more particularly to have an average particle size of less than 100 microns (μm). In some embodiments, the second phase is characterized by having an average particle size ranging from 0.5 μm to 500 μm, such as from 1 μm to 450 μm, such as from 10 μm to 400 μm, 50 μm to 400 μm, 100 μm to 350 μm, or 200 μm to 300 μm. In terms of the lower limit, the second phase is characterized by having an average particle size of more than 0.5 μm, such as more than 1 μm, more than 10 μm, more than 50 μm, more than 100 μm, or more than 200 μm. In terms of the upper limit, the second phase is characterized by having an average particle size of less than 500 μm, such as less than 400 μm, less than 350 μm, less than 300 μm, or less than 250 μm.

[0047]

[0054] In some cases, the microstructure of a sputtering target is uniform across the surface area of ​​the target (usually a disk having a diameter of 5 to 18 inches, or about 125 to about 450 mm) and throughout its entire thickness (usually approximately one-quarter or one-quarter inch, or about 6 to about 7 mm). The dimensions of the microstructure in a sputtering target are also important. Defects such as microcracks and fissures, pores, refractory or dielectric inclusions, oxide inclusions, and large intermetallic phase grains should be avoided, as they are usually accompanied by undesirable phenomena such as micro-arcing and particulation, and have a very adverse effect on film properties.

[0048]

[0055] In some embodiments, the aluminum-scandium composite has a microstructure that is free or substantially free of microcracks and cracks, which can be measured using optical / SEM metallography.

[0049]

[0056] In some embodiments, the aluminum-scandium composite has a non-porous or substantially non-porous microstructure, the porosity of the composite being measured to be less than 3%, e.g., less than 2%, less than 1%, less than 0.9%, less than 0.8%, less than 0.7%, less than 0.6%, less than 0.5%, less than 0.4%, less than 0.3%, less than 0.2%, or less than 0.1%.

[0050]

[0057] In some embodiments, the aluminum-scandium alloy has a microstructure that is free or substantially free of oxide inclusions.

[0051]

[0058] Microscopy can be used to quantify the above measurements.

[0052]

[0059] In some embodiments, the aluminum-scandium composite sputtering target has a diameter or cross measurement of greater than 125 mm, eg, greater than 150 mm, greater than 200 mm, greater than 300 mm, greater than 350 mm, or greater than 400 mm.

[0053]

[0060] The aluminum-scandium composite sputtering target can have a thickness, eg, height, ranging from 1 mm to 50 mm, such as from 1 mm to 40 mm, 2 mm to 35 mm, 2 mm to 25 mm, 3 mm to 15 mm, or 5 mm to about 10 mm.

[0054] method

[0061] A method for producing a (non-equilibrium) aluminum-scandium complex as disclosed herein. In some embodiments, the method comprises the steps of: x Sc y(wherein x is 0 to 3 and y is 1 to 2), and mixing the powder with a first phase (powder) comprising aluminum to form a composite precursor. The method may further include applying at least one of heat or pressure to the composite precursor to consolidate the materials, e.g., the first phase powder and the second phase powder. The method further includes cooling the consolidated composite precursor to form a non-equilibrium composite.

[0055]

[0062] In some cases, temperatures in the range of 300° C. to 900° C., e.g., 350° C. to 850° C., 400° C. to 800° C., or 500° C. to 700° C., are used. For the lower limit, temperatures above 300° C., e.g., above 350° C., above 400° C., or above 500° C., may be used. For the upper limit, temperatures below 900° C., e.g., below 850° C., below 800° C., or below 700° C., may be used.

[0056]

[0063] In some cases, pressures in the range of 3000 kPa to 11000 kPa, such as 4000 kPa to 10000 kPa, 5000 kPa to 9000 kPa, or 6000 kPa to 8000 kPa, are used. For lower limits, pressures above 3000 kPa, such as above 4000 kPa, above 5000 kPa, or above 6000 kPa, may be used. For upper limits, pressures below 11000 kPa, such as below 10000 kPa, below 9000 kPa, or below 8000 kPa, may be used.

[0057]

[0064] In some embodiments, e.g., when rapid cooling is performed, e.g., in a squeeze casting process, the cooling of the composite may be performed at a rate of greater than 1°C / min, e.g., greater than 5°C / min, greater than 10°C / min, greater than 20°C / min, greater than 25°C / min, or greater than 35°C / min.

[0058]

[0065] In some cases, a cooling step is used to retain the amount of non-phase diagram intermetallic phase in the second phase in the matrix of the first phase without reverting to an equilibrium phase and / or amount. In some embodiments, a cooling step is used to maintain the non-equilibrium phase mixture without reverting to an equilibrium phase mixture.

[0059]

[0066] In some embodiments, the scandium-aluminum composites described herein can be formed through a casting process, preferably using aluminum (first phase) powder and intermetallic (second phase) powder. Melt processing, for example via a casting route, also produces composites with much lower oxygen content than powder processing, for example less than 1000 ppm, less than 800 ppm, less than 600 ppm, less than 400 ppm, less than 300 ppm, less than 200 ppm, or less than 100 ppm. Thus, casting of aluminum-scandium alloys is suitable for manufacturing the disclosed composites. In some cases, for example when using casting techniques, the free aluminum is increased / maintained by holding the temperature below a certain level. Holding the temperature within these ranges and extremes advantageously avoids / minimizes the formation of unwanted metallic phase components.

[0060]

[0067] In a typical casting process, the composite components are melted together at high temperature in a crucible and then poured into a mold where the molten composite solidifies into an ingot. Solidification typically proceeds from the bottom and walls of the mold toward the center, so the outermost regions of the casting are expected to cool much faster than the central region.

[0061]

[0068] In some cases, rapid cooling rates in castings with high intermetallic loading can cause large internal stresses to build up, potentially cracking the casting. Also, many cast composites have a tendency to destroy the characteristic structure associated with the casting, making it difficult to obtain a uniform microstructure throughout the thickness of the target. To obtain a desired strength, the casting is subjected to subsequent thermomechanical processing (e.g., plastic deformation and / or heat treatment). Brittle castings typically do not have much resistance to such thermomechanical processing steps. However, the disclosed composites, due to their composition, may be able to withstand this processing. EXAMPLES

[0062] Example 1

[0069] To produce the composite sputtering target of Example 1, an intermetallic (second phase) Al containing a plurality of intermetallic aluminum-scandium phases was prepared. 47 Sc 53 Powders were prepared. AlSc and Sc were mixed in a Turbula® mixer for 10 minutes to form a precursor. The precursor was loaded into a 5-inch graphite mold and compacted by hot pressing. The compacted precursor was heated and pressed at 600° C. and 1000 psi, respectively, for approximately 4 hours. The formed precursor was removed at room temperature and cooled. 200 grams of the cooled precursor was crushed with 50 grams of (free) aluminum powder to form a sputtering target composite precursor, which was further processed to produce a sputtering target composite. The total (free) aluminum content was approximately greater than 20 atomic % and the total scandium content was approximately 40 atomic %. These percentages are outside the range of amounts expected from the aluminum-scandium equilibrium phase diagram.

[0063] Comparative example A

[0070] A comparative intermetallic powder of Comparative Example A was prepared by alloying 145 grams of aluminum and 105 grams of scandium. These components were alloyed under vacuum at approximately 1450° C. to form a precursor. The precursor was cast using a mold in a conventional casting process and then cooled to room temperature.

[0064]

[0071] The total alloy aluminum and scandium contents were consistent with those predicted from the aluminum-scandium equilibrium phase diagram.

[0065] [Table 1]

[0072] As shown in Table 1, the target of Example 1 exhibited high (free) aluminum content and low intermetallic phase, e.g., Al2Sc content. Due to the high free aluminum / low ScAl2 content, the sputtering target should exhibit excellent ductility.

[0066]

[0073] 4A-4E are exemplary diagrams showing the microstructure of an Al-Sc alloy (multiple phases are displayed). The circular dots indicate scandium-containing second intermetallic phases, such as ScAl3, ScAl2, ScAl, Sc2Al, Sc, or combinations thereof, while the remaining areas represent the (first) free aluminum phase. Diagrams are shown for 10 at. %, 15 at. %, 20 at. %, 25 at. %, and 30 at. % scandium in the overall composition.

[0067]

[0074] 5A-5C are SEM images showing the microstructure of an Al-Sc alloy. FIG. 5A shows a microstructure mapped with EDS (energy dispersive x-ray spectroscopy) to show aluminum content, e.g., free aluminum and / or aluminum-containing intermetallics (see speckled areas). FIG. 5B shows a microstructure mapped with EDS to show scandium content, e.g., scandium-containing intermetallic phases (see hatched areas). FIG. 5C shows a microstructure mapped with EDS to show free aluminum content. Areas showing both the presence of aluminum and the presence of scandium indicate intermetallic (second phase) content. The free aluminum content (first phase) is represented in FIG. 5C by areas containing aluminum but not scandium (the presence of scandium is shown in FIG. 5B) (see speckled areas in FIG. 5C). The free aluminum (first phase) areas were analyzed and calculated to represent approximately 15% to 40% by volume of the total alloy.

[0068]

[0075] FIG. 6 is an X-ray diffraction plot showing the metal content for each component of the comparative Al-Sc alloy and the examples. As shown in the top comparative plot, the peaks shown are for intermetallic phases, e.g., Al2Sc and Al3Sc, and no peaks related to free aluminum peaks are shown. Meanwhile, the middle plot for the examples shows free aluminum peaks at approximately 38 and 45 degrees. These peaks show significant free aluminum content, which is advantageous. The bottom plot shows individual peaks for all components for the examples, including the peaks shown in the middle plot and the intermetallic phases. The peaks were analyzed and extrapolated to calculate volume percentages. The volume percentage of free aluminum (first phase) in the examples was calculated to be approximately 15% to 40% by volume of the total composition.

[0069] Embodiment

[0076] The following embodiments are contemplated: All combinations of features and embodiments are contemplated.

[0070]

[0077] Embodiment 1: An Al-Sc composite comprising 1.0 at.% to 65 at.% scandium and 35 at.% to 99 at.% aluminum, the Al-Sc composite having a microstructure comprising a first phase and a second phase dispersed throughout the first phase, the second phase having the formula Al x Sc y wherein x is 0 to 3 and y is 1 to 2.

[0071]

[0078] Embodiment 2: An Al-Sc composite sputtering target comprising 1.0 at.% to 65 at.% scandium and 35 at.% to 99 at.% aluminum, the Al-Sc composite sputtering target having a microstructure comprising a first phase and a second phase dispersed throughout the first phase, the second phase having the formula Al x Sc y wherein x is 0 to 3 and y is 1 to 2.

[0072]

[0079] Embodiment 3: The embodiment of embodiment 1 or 2, wherein the second phase comprises ScAl3, ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof.

[0073]

[0080] Embodiment 4: The embodiment of any of embodiments 1-3, wherein the second phase comprises ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof.

[0074]

[0081] Embodiment 5: Any of the embodiments of embodiments 1-4, wherein the microstructure comprises 5 vol.% to 99 vol.%, such as 20 vol.% to 99 vol.% of a first phase and 1 vol.% to 80 vol.% of a second phase as determined by quantitative image analysis.

[0075]

[0082] Embodiment 6: Any of embodiments 1-5, wherein the concentration of scandium in the second phase is greater than would be expected from an aluminum-scandium equilibrium phase diagram.

[0076]

[0083] Embodiment 7: Any of embodiments 1-6, wherein the concentration of scandium in the second phase is at least 1% higher than would be expected from an aluminum-scandium equilibrium phase diagram.

[0077]

[0084] Embodiment 8: The embodiment of any of embodiments 1-7, wherein the second phase comprises greater than 25 atomic % scandium.

[0078]

[0085] Embodiment 9: The embodiment of any of embodiments 1-8, wherein the second phase comprises greater than 1 mol% Al2Sc, AlSc, AlSc2, or Sc, or a combination thereof.

[0079]

[0086] Embodiment 10: Any of embodiments 1-9, wherein the second phase comprises less than 85 mole % aluminum.

[0080]

[0087] Embodiment 11: The embodiment of any of embodiments 1-10, wherein the second phase further comprises 1.0 mol % to 70 mol % scandium nitride.

[0081]

[0088] Embodiment 12: Any of embodiments 1 to 11, wherein the grains of the first aluminum matrix phase have a crystallographic orientation of (110).

[0082]

[0089] Embodiment 13: Any of embodiments 1 to 12, wherein the grains of the first aluminum matrix phase are characterized by random crystallographic orientation.

[0083]

[0090] Embodiment 14: Any of embodiments 1-13, wherein the second phase is characterized by a particle size ranging from 0.5 microns to 500 microns.

[0084]

[0091] Embodiment 15: Any of embodiments 1-14, wherein the microstructure is substantially free of microcracks and fissures.

[0085]

[0092] Embodiment 16: Any of embodiments 1-15, wherein the microstructure is substantially free of oxide inclusions.

[0086]

[0093] Embodiment 17: The embodiment of any of embodiments 1-16, wherein the composite or sputtering target further comprises less than 1000 ppm oxygen, preferably less than 400 ppm, or more preferably less than 100 ppm oxygen.

[0087]

[0094] Embodiment 18: Any of embodiments 1-17, wherein the uniformity of scandium across the surface of the sputtering target varies by less than ±0.5 atomic % of scandium across the radius of the surface.

[0088]

[0095] Embodiment 19: Any of embodiments 1-18, wherein the sputtering target has a central axis through a thickness of the sputtering target and a diameter intersecting the central axis, and the uniformity of scandium across the central axis and diameter varies by less than ±0.5% by weight of scandium.

[0089]

[0096] Embodiment 20: Any of the embodiments of embodiments 1-19, wherein the sputtering target has a diameter of greater than 300 mm.

[0090]

[0097] Embodiment 21: A method for preparing a non-equilibrium complex comprising the steps of: x Sc y wherein x is 0 to 3 and y is 1 to 2; and mixing the powder with the first phase comprising aluminum to form a composite precursor. applying at least one of heat or pressure to the composite precursor to solidify the material; and cooling the solidified composite precursor to form a non-equilibrium composite.

[0091]

[0098] Embodiment 22: The embodiment of embodiment 21, wherein the compound comprises Al2Sc, AlSc, AlSc2, or Sc, or a combination thereof, present in an amount greater than 1 mol %.

[0092]

[0099] Although the present invention has been described in detail, modifications within the spirit and scope of the present invention will be readily apparent to those skilled in the art. In view of the relevant knowledge and references in the art set forth above in connection with the foregoing description, background and detailed description, the disclosures of which are incorporated herein by reference in their entirety. It should also be understood that aspects of the present invention and various embodiments and various features described below and / or in the appended claims may be combined or substituted in whole or in part. In the foregoing description of various embodiments, an embodiment that refers to another embodiment may be combined with other embodiments as appropriate, as understood by those skilled in the art. Furthermore, those skilled in the art will appreciate that the foregoing description is by way of example only and is not intended to be limiting. [Mode of the invention] [1] An Al-Sc composite containing 1.0 atomic % to 65 atomic % scandium (Sc) and 35 atomic % to 99 atomic % aluminum (Al), having a microstructure including a first phase and a second phase dispersed throughout the first phase, the second phase having the formula Alx Sc y wherein x is 0 to 3 and y is 1 to 2. [2] The composite of claim 1, wherein the second phase comprises ScAl3, ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof. 3. The composite of claim 1, wherein the second phase comprises less than 60 mol% AlSc, based on the total moles of the second phase. [4] The composite of claim 1, wherein the second phase comprises ScAl2, ScAl, Sc2Al, or Sc, or a combination thereof. 5. The composite of claim 1, wherein the microstructure comprises 5 vol. % to 99 vol. % of the first phase and 1 vol. % to 80 vol. % of the second phase, as determined by quantitative image analysis. [6] The composite of claim 1, wherein the concentration of scandium in the second phase is greater than that predicted by an aluminum-scandium equilibrium phase diagram. [7] The composite of claim 1, wherein the concentration of scandium in the second phase is at least 1% higher than the concentration predicted by an aluminum-scandium equilibrium phase diagram. [8] The composite of claim 1, wherein the second phase comprises greater than 25 atomic % scandium. [9] The composite of claim 1, wherein the second phase comprises greater than 1 mol% Al2Sc, AlSc, AlSc2, or Sc, or a combination thereof.

[10] The composite of claim 1, wherein the second phase comprises less than 85 mol % aluminum.

[11] The composite of claim 1, wherein the second phase further comprises 1.0 mol% to 70 mol% scandium nitride (ScN).

[12] The composite of claim 1, wherein the grains of the first aluminum matrix phase are characterized by a (110) crystallographic orientation.

[13] The composite of claim 1, wherein the grains of the first aluminum matrix phase are characterized by random crystallographic orientation.

[14] The composite of claim 1, wherein the second phase has a particle size in the range of 0.5 microns to 500 microns.

[15] The composite of 1, wherein the microstructure is substantially free of microcracks and fissures and / or oxide inclusions.

[16] The composite of 1, wherein the composite or sputtering target further comprises less than 1000 ppm oxygen, preferably less than 400 ppm, or more preferably less than 100 ppm oxygen.

[17] A method for producing a non-equilibrium complex, comprising: Formula Al x Sc y providing a second phase powder comprising a compound corresponding to the formula: mixing the powder with a first phase comprising aluminum to form a composite precursor; applying at least one of heat and pressure to the composite precursor to solidify the material; cooling the solidified complex precursor to form the non-equilibrium complex; A method comprising:

[18] The method of claim 17, wherein the compound comprises Al2Sc, AlSc, AlSc2, or Sc, or a combination thereof, present in an amount greater than 1 mol%.

[19] An Al-Sc composite sputtering target comprising 1.0 atomic % to 65 atomic % scandium (Sc) and 35 atomic % to 99 atomic % aluminum (Al), having a microstructure comprising a first phase and a second phase dispersed throughout the first phase, the second phase having the formula Al x Sc y wherein x is 0 to 3 and y is 1 to 2.

[20] The sputtering target of claim 19, wherein the uniformity of scandium across the surface of the sputtering target varies by less than ±0.5 atomic % of scandium across the radius of the surface.

Claims

1. A sputtering target comprising aluminum and scandium, 25 atomic % to 50 atomic % scandium (Sc), A 2 Al exists in a larger amount than Sc intermetallic compounds 3 Sc intermetallic compounds, and a microstructure containing 15% to 40% by volume of free aluminum; Sputtering target.

2. 10. The sputtering target of claim 1 comprising at least 20% by volume of free aluminum.

3. 2. The sputtering target of claim 1, wherein the free aluminum grains have a (110) crystallographic orientation; or wherein the free aluminum grains have a random crystallographic orientation.

4. 10. The sputtering target of claim 1, wherein the sputtering target comprises less than 1000 ppm oxygen, preferably less than 400 ppm oxygen, and more preferably less than 100 ppm oxygen.

5. The microstructure is Al 2 The sputtering target of claim 1 , which is free of Sc.

6. 10. The sputtering target of claim 1, wherein the microstructure is free of microcracks and fissures and / or oxide inclusions.

7. The Al 3 2. The sputtering target of claim 1, wherein Sc intermetallic compounds are dispersed throughout the free aluminum.

8. A method for producing a sputtering target, the method comprising: mixing an aluminum and scandium intermetallic powder with scandium powder to form a precursor; solidifying the precursor with at least one of heat or pressure to form a solidified precursor; crushing the consolidated precursor together with free aluminum powder and processing to form the sputtering target; Including, The microstructure of the sputtering target is Aluminum and scandium, having 25 atomic % to 50 atomic % scandium; A 2 Al exists in a larger amount than Sc intermetallic compounds 3 Sc intermetallic compounds, and 15% to 40% by volume of free aluminum having method.

9. 9. The method of claim 8, further comprising cooling the solidified precursor at a rate greater than 1° C. / min to form the sputtering target.

10. The method of claim 8, wherein solidifying the precursor comprises heating to a temperature of between 400°C and 900°C.

11. The method of claim 8, wherein consolidating the precursor comprises pressing to a pressure of 5000 kPa to 9000 kPa.

12. 9. The method of claim 8, wherein consolidating the precursor comprises heating to a temperature of 400° C. to 900° C. and pressing to a pressure of 5000 kPa to 9000 kPa.

13. The method of claim 8 , wherein consolidating the precursor comprises hot squeezing.

14. The method of claim 9 , wherein the solidifying and cooling comprises squeeze casting.

15. The method of claim 8 , wherein the sputtering target comprises at least 20% by volume of free aluminum.

Citation Information

Patent Citations

  • Alloy target of aluminum and rare earth element and manufacturing method of the same

    JP2015096647A

  • Scandium-containing aluminum alloy for powder metallurgical technologies

    JP2017186646A

  • Aluminum-scandium alloys with high uniformity and elemental content and articles thereof

    JP2020514551A

  • Sputtering target and production method therefor

    WO2017213185A1