Coated active material particle, current collector with active material layer, manufacturing method of electrode laminate, and manufacturing method of current collector with active material layer

Coated active material particles with a buffer portion and conductive network address gas generation and resistance issues in lithium-ion batteries, ensuring high reliability and capacity through uniform potential distribution and enhanced conductivity.

JP2024161660AInactive Publication Date: 2024-11-20KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023076487
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries face issues such as gas generation due to electrolyte decomposition, high resistance, and instability due to oxidative deterioration of solid electrolytes, particularly in high-voltage operations, leading to reduced reliability and capacity.

Method used

Coated active material particles with a buffer portion and a conductive network, forming a sea-island structure on the surface, which suppresses gas generation and ensures uniform potential distribution, enhancing Li ion conductivity and electron conductivity.

Benefits of technology

The solution results in highly reliable lithium-ion batteries with suppressed gas generation, improved Li ion conductivity, and reduced internal resistance, maintaining high capacity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161660000001_ABST
    Figure 2024161660000001_ABST
Patent Text Reader

Abstract

To provide: coated active material particles with which generation of gas due to decomposition of electrolytic media can be suppressed, which are excellent in characteristics, with which uniformalization of a potential in an active material layer including the coated active material particles can be achieved, and which can be used as materials of a highly reliable lithium ion secondary battery; a current collector with an active material layer; a manufacturing method of an electrode laminate; and a manufacturing method of a current collector with an active material layer.SOLUTION: There are provided coated active material particles 130 which each comprise an active material particle 30 coated with a film 35. The entire outer surface of the film on a side opposite to a side of the active material particles includes: a formation area where a cushioning portion 42 is formed; and a non-formation area where the cushioning portion is not formed and a conductive support member including a binder and a conductive network 80 is arranged. Further, an active material layer surface is an uneven surface including a protrusion of the non-formation area and a recess of the formation area, and a part of the conductive network is exposed on a non-formation area protrusion that is a protrusion of the non-formation area.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to coated active material particles, a current collector with an active material layer, a method for producing an electrode laminate, and a method for producing a current collector with an active material layer. [Background technology]

[0002] Lithium-ion secondary batteries (LIBs) are required to have high energy density so that they can be used as on-board power sources for electric vehicles. In addition, as a temporary storage system for electricity from solar cells and fuel cells, in addition to increasing capacity through the electrical series connection of multiple cells to increase voltage and parallel connection to increase capacity, there is a demand for high capacity cells themselves.

[0003] LIBs are classified into non-aqueous charged liquid LIBs and all-solid-state LIBs based on the electrolytic medium they contain. The electrolytic medium for all-solid-state LIBs includes solid electrolytes and polymer electrolytes.

[0004] Non-aqueous charged liquid LIBs have problems with leakage and combustion, and the design has the disadvantage of being complicated to address these issues.

[0005] Polymer LIBs are LIBs that use a solid polymer electrolyte or a gel polymer containing a liquid electrolyte as the electrolytic medium. They have excellent stability and flexibility and can be made into a variety of forms, such as small size and thin film.

[0006] There are two methods for manufacturing polymer LIBs:

[0007] One method is to mix a polymerization initiator and a monomer or oligomer with a non-aqueous electrolyte solution to prepare an electrolyte composition, which is then injected into a battery containing an electrode laminate and gelled (crosslinked). However, this method has the disadvantage that it is not easy to ensure the mechanical strength after gelling due to poor wettability inside the cell caused by the high viscosity of the composition before injection.

[0008] The other method involves coating one side of an electrode or separator with an electrolyte composition, hardening it using heat or UV light to form a gel polymer electrolyte, and then winding or stacking it to produce an electrode laminate. This is then stored in a battery case and the existing electrolyte is re-injected. However, heating or UV irradiation is required for gelation, and there is a concern that the gel-coated separator, etc. may absorb moisture, reducing the performance and stability of the battery, or if the separator has a high thermal shrinkage rate, a short circuit may occur between the electrodes due to temperature changes, resulting in a decrease in reliability.

[0009] All-solid-state LIBs are known to be susceptible to "solid electrolyte oxidative degradation," in which the solid electrolyte is easily oxidized and degraded by repeated charging and discharging when in direct contact with the active material, in particular the positive electrode active material. From the perspective of extending the lifespan (for example, improving cycle characteristics), measures are needed to prevent the degradation of the solid electrolyte. Solid electrolytes can be broadly divided into bulk and thin-film types, with the bulk type being advantageous from the perspective of increasing capacity, as it can increase the absolute amount of active material.

[0010] For these reasons, a material has been proposed as an electrode material for bulk-type all-solid-state LIBs in which secondary particles of a high conductivity active material (1 x 10-4 S / cm or more) are coated with a low conductivity first ion-conducting layer (1 x 10-6 S / cm or more) and the gaps between the primary particles that make up the secondary particles are filled, thereby allowing all primary particles to directly contribute to charging and discharging, and in which the secondary particles coated with the first ion-conducting layer are layered and coated with a medium conductivity second ion-conducting layer (1 x 10-5 S / cm or more) that is a different material from the first ion-conducting layer, thereby preventing the fracture of the secondary particles due to repeated charging and discharging ("active material secondary particle fracture").

[0011] Meanwhile, lithium nickel manganese oxide (hereinafter, also referred to as LNMO) has been conventionally known as a positive electrode active material for LIBs (for example, Patent Document 1).

[0012] The operating potential of LNMO is 4.7 V based on the deposition potential of Li metal, which is higher than that of conventional Li insertion materials used as positive electrode active materials (for example, lithium cobalt oxide has a potential of 4 V), and it is expected to contribute to achieving higher energy density.

[0013] In LIBs, the crystal structure of the active material changes when Li ions are inserted and removed, causing distortion, which can lead to instability (structural change, distortion, instability). As a result, the positive electrode active material undergoes dissolution of the transition metal ions that make up the crystal structure (transition metal dissolution), In the vicinity of the positive electrode, the bond with the transition metal is broken, resulting in "oxygen elimination", which generates oxygen gas, or reacts with the electrolytic medium to generate carbon dioxide gas, resulting in "gas generation". Even near the negative electrode, there is a problem of "reduced hydrogen gas generation" in which the electrolytic medium is reduced and hydrogen gas is generated. There is a demand to "suppress gas generation."

[0014] For example, in an LNMO positive electrode nonaqueous electrolyte LIB, which uses a nonaqueous electrolyte as the electrolytic medium and LNMO (described below) as the positive electrode active material, the operating voltage is high and the reaction proceeds in an oxidizing atmosphere near the positive electrode, resulting in the problem of significant "gas generation."

[0015] From the viewpoint of suppressing "oxygen desorption," it is conceivable to coat the positive electrode active material with a polyanion material such as LiFePO4 (LFP). This suppresses "oxygen desorption" as a result of "strengthening the polyanion transition metal-oxygen bond" which strengthens the bond between the transition metal in the material and oxygen. However, this gives rise to a new problem of "high polyanion resistance," which is an increase in resistance resulting from the low electrical conductivity of the polyanion.

[0016] In addition, the use of a positive electrode active material made of lithium transition metal composite oxide with a high nickel concentration results in a high-energy density LIB; however, it has been reported that output is reduced due to the inhibition of Li-ion conductivity by inactive NiO, which is generated by "oxygen desorption" due to charge-discharge cycles, etc., resulting in "inactive NiO conductivity inhibition." [Prior art documents] [Patent documents]

[0017] c [Patent Document 1] Patent Publication No. 2021-051987 Summary of the Invention [Problem to be solved by the invention]

[0018] Regarding the output reduction caused by "inactive NiO conductivity inhibition," when the active material surface is coated with a carbon-supported Li-based polyanion to reduce the direct contact area with the electrolyte and suppress the generation of inactive NiO, especially when LMP is used as the Li-based polyanion, Mn 3+ Mn in PO4 3+ It has been reported that the "mobile charge trap" caused by polaron holes due to the Jahn-Teller effect at the interface and the "interface mismatch" between MnPO4 and LMP cause the charge transfer potential barrier to rise, resulting in the high resistance at the interface leading to overvoltage application and, as a result, hastening the deterioration. As a countermeasure, a composite has been reported in which the surface of the first positive electrode active material of Ni-containing Li transition metal composite oxide is coated with a second positive electrode active material of an olivine type with surface carbon support and a coating layer containing CNT, but the ionic conductivity of the carbon-coated Li-based polyanion is considered to be insufficient as a distribution path for Li ions from the first positive electrode active material to the electrolytic medium.

[0019] Incidentally, polyanion materials not only have the above-mentioned "polyanion transition metal oxygen bond strengthening" effect, but also have a strong crystal structure that makes them less likely to release oxygen even at high temperatures and high voltages, making them a positive electrode active material. Polyanion-based positive electrode materials have the effect of "strongly crystalline low oxygen releasing polyanion", and for example, olivine-type Fe (LFP) and olivine-type Mn (LMP), which has a similar crystal structure, are being considered. LFP has a low energy density at a low operating potential, and LiMnPO4 has an operating potential of 4.1V and a theoretical capacity of 160mAh / g, and is expected to have a higher energy density than LiCoO2, the currently commonly used LIB positive electrode. However, it has been reported that the material itself has a high resistance, known as "high resistance of LMP", resulting in a low output density.

[0020] In order to solve this problem of "high resistance of polyanion positive electrode active material," an electrode material has been proposed in which the particle surface is covered with an organic compound that serves as a carbon source, and then this is carbonized to form a conductive carbonaceous coating on the active material particle surface. However, if there is an excess of carbonaceous coating that completely covers the particles, it becomes a barrier to the oxidation-reduction reaction and diffusion of Li ions, resulting in the problem of increased internal resistance. To solve this problem, a composite of a compound having Li-ion conductivity and a carbonaceous coating is formed as a coating with the intention of improving not only electronic conductivity but also Li-ion conductivity. A LIB has been proposed in which islands of minute oxide coatings exist in a sea of ​​carbonaceous coating on the surface of active material particles having LFP active material particles and oxide coatings and carbonaceous coatings on the surfaces of the particles, and the electrolyte is substantially free of a stabilizer for the SEI on the negative electrode surface. A carbonaceous coating containing an ion conductive material is formed on the particle surface, and at least a portion of the surface is exposed and not covered by the carbonaceous coating. An electron and Li-ion conductive electrode material has been proposed in which Li-ion conductivity is not impaired due to ion conduction in the exposed parts or in the thin parts of the carbonaceous coating. However, it is believed that the amount of Li-ion conductivity is drastically reduced through the carbonaceous coating, even if it is thin.

[0021] Therefore, an object of the present invention is to provide coated active material particles which can suppress the generation of gas due to decomposition of the electrolytic medium, have excellent properties, and can achieve uniform potential within an active material layer containing the coated active material particles, making them a component of highly reliable lithium ion secondary batteries. [Means for solving the problem]

[0022] One aspect of the present invention for solving the above problem is to The coated active material particles are active material particles coated with a coating film, The entire outer surface of the coating film opposite to the active material particles is A formation region in which a buffer portion is formed, and The buffer portion is not formed, and a binder, and a conductive network. A conductive support material is provided. a non-forming region; and the non-forming region being a convex portion and the forming region being a concave portion; The non-forming region is a convex portion. The coated active material particles have a part of the conductive network exposed at the non-forming region convex portion.

[0023] According to this aspect, a buffer section is formed in the formation region on the surface of the active material particle, which makes it possible to suppress the generation of gas due to decomposition of the electrolyte medium and results in a coated active material particle for LIBs with excellent characteristics. In the non-formation region where no buffer section is formed, a convex section is formed in which a conductive support material is arranged while ensuring exposure of the conductive network, which makes it possible to uniformize the potential within the active material layer including this, resulting in a highly reliable coated active material particle for LIBs.

[0024] One aspect of the present invention for solving the above problem is to a current collector with an active material layer, the current collector having an active material layer including the coated active material particles formed on the current collector, The active material layer is The cross-sectional shape is a sea-island structure, and includes an island portion and a sea-like portion, the islands include a permeable pore network leading to the formation region; The sea-like portion includes the conductive support material and the active material particles, and further includes The current collector with an active material layer has an active material layer surface, which is the surface opposite to the current collector side, that is an uneven surface having protrusions formed of the active material particles and recesses formed of the conductive support material.

[0025] According to this aspect, the surface of the active material layer, which is the surface opposite to the current collector, is an uneven surface consisting of convex portions formed from the active material particles and concave portions formed from the conductive support material, thereby enabling sufficient and smooth insertion and desorption of Li ions into and from the active material particles, resulting in a current collector with an active material layer for LIBs that has high capacity and low internal resistance.

[0026] One aspect of the present invention for solving the above problem is to A method for producing an electrode laminate including the current collector with an active material layer, comprising the steps of: a current collector A manufacturing process in which the different types of active material particles are used as positive electrode active material particles and negative electrode active material particles, respectively, to form an active material layer A containing the active material particles on the current collector, and form, as the current collector A with active material layer before forming the buffer section, a positive electrode current collector A with a positive electrode active material layer containing the positive electrode active material particles and a negative electrode current collector A with a negative electrode active material layer containing the negative electrode active material particles, respectively; a buffer portion B forming step of forming a buffer portion B as a part of the buffer portion in the active material particles of the active material layer A of at least one of the positive electrode current collector A with the positive electrode active material layer and the negative electrode current collector A with the negative electrode active material layer; and The method for producing an electrode laminate includes a step of producing an electrode laminate B, in which at least one pair of a positive electrode current collector B and / or a negative electrode current collector B, each including a current collector B with an active material layer B on which the buffer portion B is formed, are opposed to each other to form an electrode laminate B.

[0027] According to this aspect, since it is possible to form the buffer portion B according to the characteristics of the positive electrode, negative electrode, etc., it is possible to obtain a more excellent effect of suppressing gas generation and improving characteristics.

[0028] Preferably, the method further includes a buffer portion C formation step of forming a buffer portion C on the buffer portion B of at least one of the positive electrode current collector B and the negative electrode current collector B of the electrode laminate B as a part of the buffer portion.

[0029] Preferably, the buffer portion B is formed in a state in which the current collector A with the active material layer faces a metal plate.

[0030] Preferably, further comprising: an exposure expansion operation for expanding the exposure of the conductive network; and / or A protrusion formed of the active material particles. In the active material particle convex portion, a portion of the conductive support material, This includes a support material reduction operation, which reduces the area where the support material is present.

[0031] Preferably, the buffer portion B is formed by disposing a silicon-containing compound on the current collector B.

[0032] One aspect of the present invention for solving the above problem is to The method for producing the current collector with an active material layer includes the steps of: a current collector A manufacturing step of forming an active material layer A containing the active material particles on the current collector to form a current collector A with an active material layer before forming the buffer portion; a buffer portion B forming step of forming a buffer portion B as at least a part of the buffer portion in the active material particles of the active material layer A to form a current collector B; and a peeled product producing step of peeling the active material layer B from the current collector B to produce an active material layer B peeled product; and The method for producing a current collector with an active material layer includes a recycled current collector B formation step of forming a recycled material layer B, which includes a peeled-off material of the active material layer B, on the current collector to form a recycled current collector B with the recycled material layer B.

[0033] According to this aspect, it is possible to manufacture a current collector with an active material layer that includes coated active material particles in which a buffer portion is formed in an optimal state for various types and purposes of LIBs, including all-solid-state LIBs. Effect of the Invention

[0034] The coated active material particles for lithium ion secondary batteries of the present invention have a buffer section formed in the formation region on the surface of the active material particles, which makes it possible to suppress the generation of gas due to decomposition of the electrolyte medium and results in coated active material particles for LIBs with excellent characteristics. In the non-formation region where no buffer section is formed, a convex portion in which a conductive support material is arranged is formed while ensuring exposure of the conductive network, thereby making it possible to uniformize the potential within the active material layer including this, resulting in highly reliable coated active material particles for LIBs. [Brief description of the drawings]

[0035] [Figure 1]FIG. 1 is an explanatory diagram conceptually illustrating a lithium ion secondary battery according to a first embodiment of the present invention, where (a) is a perspective view of the lithium ion secondary battery, (b) is a cross-sectional view taken along line AA in (a), and (c) is a cross-sectional view taken along line BB in (a). [Diagram 2] FIG. 2 is an explanatory diagram of the electrode parts of the positive electrode part and the negative electrode part in FIG. 1, where (a) is a cross-sectional view of the electrode parts and (b) is a cross-sectional view of coated active material particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, an embodiment of the present invention will be described in detail.

[0037] (Lithium-ion secondary battery (LIB) 1) A lithium ion secondary battery (also simply referred to as LIB) 1 of a first embodiment of the present invention has a battery assembly in which an electrode stack 5 is housed in an outer casing 3, as shown in Figure 1, and an electrolytic medium 6 is filled and sealed inside the outer casing 3 of the battery assembly 2.

[0038] The lithium ion secondary battery 1 may be a nonaqueous electrolyte LIB in which the electrolytic medium 6 is a nonaqueous electrolyte solution, an all-solid-state LIB in which the electrolytic medium 6 is a solid electrolyte, or a polymer LIB in which the electrolytic medium 6 is a polymer electrolyte, and is preferably a nonaqueous electrolyte LIB.

[0039] In the following description, the lithium ion secondary battery 1 is a non-aqueous electrolyte LIB.

[0040] (Exterior body 3) The exterior body 3 can be appropriately selected as long as it is chemically stable to the electrolytic medium (electrolytic solution) 6, particularly stable to the nonaqueous electrolyte solution 6 and has sufficient water vapor barrier properties, and the electrode laminate 5 can finally form an enclosed internal space containing the electrolytic medium 6. It is preferable to use a laminate film exterior body 3 that can be opened and sealed multiple times so that the buffer part formation process according to the present invention can be performed under different conditions and the nonaqueous electrolyte solution can be injected and discharged multiple times. Examples of methods for opening the exterior body include making a hole, cutting a spare part, preparing a liquid injection port for the second and subsequent injections in advance and opening the liquid injection port, and so on.

[0041] Materials and forms used for the exterior body 3 include cans primarily made of aluminum, iron, or stainless steel, and laminate films containing laminate resin. For exterior bodies 3 using laminate resin, in the case of non-aqueous electrolyte secondary batteries, laminate films such as aluminum, silica-coated polypropylene, and polyethylene can also be used; however, from the standpoint of versatility, cost, and the like, it is preferable to use aluminum laminate films, and a preferred exterior body 3 is one formed by bonding two sheets of metal laminate films together.

[0042] (Electrode laminate 5) As shown in FIG. 1, the electrode laminate 5 has a positive electrode part 10, a negative electrode part 11, a separator 12, a positive electrode extraction member 13, and a negative electrode extraction member 14.

[0043] (Positive electrode part 10, negative electrode part 11) The positive electrode part 10 and the negative electrode part 11 are formed by laminating a positive electrode active material layer 21 and a negative electrode active material layer 121 on at least one of the main surfaces of a positive electrode current collector 20 and a negative electrode current collector 120, as shown in FIG. 1(b), and are intercalation electrodes capable of inserting and extracting Li ions.

[0044] In the positive electrode part 10 and the negative electrode part 11 of this embodiment, a positive electrode active material layer 21 and a negative electrode active material layer 121 are laminated on both main surfaces of a positive electrode current collector 20 and a negative electrode current collector 120, as shown in FIG. 2(a).

[0045] (Positive electrode current collector 20, negative electrode current collector 120) The positive electrode current collector 20 and the negative electrode current collector 120 are plate-like or film-like bodies having electrical conductivity, and are not particularly limited as long as they are electrically conductive. For example, aluminum or an aluminum alloy can be used. However, aluminum or an aluminum alloy is preferable because it is stable under the positive electrode reaction atmosphere and the negative electrode reaction atmosphere, and high-purity aluminum represented by JIS standards 1030, 1050, 1085, 1N90, 1N99, etc. is more preferable, and a coating in which a metal surface is coated with a metal that does not react at the positive electrode potential can be used.

[0046] (Active material layer 2 (positive electrode active material layer 21, negative electrode active material layer 121)) The active material layer 2 (positive electrode active material layer 21, negative electrode active material layer 121) is configured to contain particles 30 of a Li-ion conductive active material, and is also configured to contain a binder 70, a conductive network 80, and a permeable pore network 81. The active material layer 2 is formed on the current collector 20, 120, and preferably includes an SEI structure. As shown in the enlarged view of FIG. 2( a ), the active material layer 2 is preferably a sea-island film having a sea-island structure, and has a cross-sectional shape including sea-like portions 60 and island-like portions 61, which is a so-called bulk film.

[0047] In the positive electrode active material layer 21, the coated active material particles 130 occupy a large portion in terms of weight ratio, but in terms of volume ratio, the binder 70 and the conductive network 80 occupy such a portion that they can be confirmed even with an electron microscope.

[0048] (Coated active material particles 130) As shown in FIG. 2( b ), the coated active material particle 130 includes an active material particle 30 covered with a coating 35. The coating 35 is composed of, in order from the active material particle 30 side, a shell film 41 and / or a buffer portion 42. In this specification, a particle having a core-shell structure in which the active material particle 30 is the core and the shell film 41 is the shell may be referred to as a core-shell particle 36. Since the core-shell particle 36 and the active material particle 30 are treated as target particles and a buffer portion 42 is formed on them, the core-shell particle 36 and the active material particle 30, which are particles in which the buffer portion 42 is to be formed, are collectively referred to as “active material particles”. In other words, the “active material particle” is the core-shell particle 36 or the active material particle 30. For example, a positive electrode core-shell particle 36 in which the outer surface of a positive electrode active material particle 40 is covered with a shell film 41 may be expressed as a positive electrode “active material particle”.

[0049] Thus, coated active material particle 130 of the present embodiment, which is one of the preferred embodiments, further includes buffer portion 42 on a part or all of the outer surface of shell film 41. That is, coated active material particle 130 of the present embodiment has coating 35 covering the surface of positive electrode active material particle 40, and coating 35 is a multilayer film of shell film 41 and buffer portion 42.

[0050] From the viewpoint of obtaining a LIB with higher performance, it is preferable that the positive electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the positive electrode coated active material particle 130, is different from the negative electrode shell film Li ion concentration, which is the concentration of Li ions contained in the shell film 41 of the negative electrode coated active material particle 130. More preferably, LIBs that require high-speed charging and LIBs that require high-speed discharging are designed and manufactured separately. These concentrations are average concentrations in the film. Furthermore, in the above-mentioned shell film 41 / buffer section 42 multilayer film, the buffer section 42 contains an oxide and / or organic matter that does not contain Li ions and is composed of Li ions as a whole. Therefore, the positive electrode multilayer film Li By making a LIB with a different ion concentration and a negative electrode multilayer Li ion concentration, a LIB with higher performance can be obtained, which is preferable, and it is more preferable to separately design and manufacture LIBs for which high-speed charging is required and LIBs for which high-speed discharging is required.

[0051] (Active material particles 30 (40, 140) The active material particles 30 (40, 140) are lithium transition metal composite oxide particles, and are capable of inserting and extracting lithium ions.

[0052] The particle size is not particularly limited, but the median diameter d50 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 50 μm or less, and particularly preferably 30 μm or less. <Cathode active material particles 40> The positive electrode active material particles 40 have an average potential for desorption and insertion of Li relative to the deposition potential of Li metal (vs. Li + / Li) is preferably 4.5 V or more and 5.0 V or less. That is, the positive electrode active material particles 40 preferably have an operating potential of 4.5 V or more and 5.0 V or less relative to Li metal when used alone.

[0053] The potential (hereinafter referred to as voltage) of the Li ion insertion and desorption reaction (vs. Li + / Li) can be obtained, for example, by measuring the charge / discharge characteristics of a half cell with a working electrode using the positive electrode active material particles 40 and a Li metal counter electrode, and reading the voltage values ​​at the start and end of the plateau. When there are two or more plateaus, the plateau with the lowest voltage value is 4.5 V (vs. Li + / Li) or higher, and the highest voltage plateau is 5.0V (vs. Li + / Li) or less.

[0054] The positive electrode active material particles 40 are not particularly limited, but spinel-type lithium manganese-based oxides represented by the following formula (1) are preferred.

[0055] Li 1+x M y Mn 2-x-y O4···(1) In the above formula (1), x and y satisfy 0 ≤ x ≤ 0.2 and 0 < y ≤ 0.8 respectively, M is at least one selected from the group consisting of Al, Mg, Zn, Ni, Co, Fe, Ti, Cu, and Cr, and attention should also be paid to the "influence of promoting the reduction decomposition of acetonitrile eluted metal ion negative electrode deposited SEI damage" described later.

[0056] Among the above formula (1), lithium nickel manganese oxide (LNMO) in which M is Ni is preferred, but measures against the above-mentioned "oxygen desorption inactivation NiO diffusion inhibition" are required. <Negative electrode active material particles 140> From the viewpoint of being difficult for lithium precipitation to occur and improving safety, it is preferable to use lithium titanate (LTO) as the negative electrode active material particles 140.

[0057] Among LTO, spinel-structured LTO is particularly preferred because the expansion and contraction of the active material in the reaction of insertion / desorption of lithium ions are small.

[0058] LTO may contain trace amounts of elements other than lithium and titanium, such as Nb.

[0059] In a LIB containing LTO as the negative electrode active material, the oxidation / reduction potential of the negative electrode is relatively high, and it is difficult to form SEI with a normal non-aqueous electrolyte, and the generation of gas accompanying charge and discharge becomes a problem. Therefore, in such an "LTO negative electrode LIB", it is preferable to charge in a state where a non-aqueous electrolyte, that is, a "high potential SEI-forming non-aqueous electrolyte", which is a material capable of forming SEI even at such a high potential, is used to form a buffer portion 42 containing SEI.

[0060] Such a "high-potential SEI-forming nonaqueous electrolyte" is a nonaqueous electrolyte to which a phosphate compound or a sulfonate compound has been added, which is reduced at a relatively high potential to form a passivation film on the surface of a high-potential negative electrode, and this passivation film can be an SEI.

[0061] The phosphate compound is preferably Li difluorobisoxalatophosphate or Li tetrafluorophosphate.

[0062] (Shell Membrane 41) The shell film 41 is a film having a continuous layer structure that densely covers the surface shape of the active material particle 30, and is a coating composed of a Li-ion conductive compound containing phosphorus as an element, and is preferably composed of an intercalation material that functions as a positive electrode active material by itself.

[0063] Shell film 41 contains a phosphate ion-containing Li compound that further contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al.

[0064] Such phosphate ion-containing Li compounds are preferably lithium phosphate compounds such as lithium manganese phosphate (hereinafter also referred to as LMP) and Li iron phosphate (hereinafter also referred to as LFP) having an olivine type crystal structure, lithium titanium aluminum phosphate (hereinafter also referred to as LATP) having a NASICON type crystal structure, and lithium phosphate (hereinafter also referred to as LP), and lithium transition metal phosphates such as LMP, LFP, and LATP are preferred.

[0065] As for LP, Li3PO 4-a-b X a Y b(X is one selected from the group consisting of N, S, B, and Si, and Y is any halogen atom), which suppresses the consumption of Li present in the LIB and results in a high-capacity, low-resistance LIB. It has been reported that the compound has a structure in which some of the oxygen atoms are replaced by X and Y, and since the introduction of X improves the Li conductivity but reduces the electrical insulation, the introduction of an appropriate amount of Y ensures electrical insulation.

[0066] Among these, the shell film 41 is preferably a phosphate ion-containing lithium compound film containing manganese (Mn) element, and is more preferably an LMP having the characteristics of the "strongly crystalline low oxygen releasing polyanion" described above.

[0067] From the viewpoint of fully exerting the effects of the "strongly crystalline, low-oxygen releasing polyanion" and the effect as an "insertion destruction prevention" layer while suppressing the adverse effects of "high LMP resistance," "mobile charge traps," "elevated charge transfer potential barrier," and "interface mismatch," it is preferable that the shell film 41 has different metal components and / or compositions on both sides and has an LFP / LMP two-layer structure from the center of the active material particle 30 to the outside, more preferably, the shell film 41 has a constituent transition metal that is gradually changed from Fe to Mn, and even more preferably, the composition and / or ratio of the metal components of the "Li-based polyanion" is changed, including the buffer section 42 described later.

[0068] The thickness of shell film 41 is thinner than the particle diameter of the lithium ion conductive oxide, and is preferably 5 nm or more and 20 nm or less, and more preferably 5 nm or more and 15 nm or less.

[0069] Within this range, the amount of gas generated can be suppressed while suppressing the resistance loss in shell film 41.

[0070] The shell film 41 covers at least a portion of the surface of the positive electrode active material particle 40, more preferably covers 95% or more, and preferably covers the surface completely.

[0071] Shell film 41 is preferably amorphous from the viewpoint of “replenishment of consumed Li” for replenishing Li ions of positive electrode active material particles 40 consumed by the SEI structure of buffer section 42 described later.

[0072] (Buffer section 42) The buffer portion 42 is a silicon-containing compound film that contains lithium element and further contains silicon element.

[0073] The buffer section 42 has a solid electrolyte interface (hereinafter also referred to as SEI) structure generated by an electrochemical reaction between the core-shell particles 36 and the electrolyte for forming the buffer section, and is preferably a siloxane-modified coating layer containing silicon element.

[0074] The buffer section 42 is a selectively permeable membrane that passes only lithium ions but not electrons, and is an “insertion / destruction prevention” layer that prevents organic solvent molecules with a large molecular weight that move together with Li ions in the electrolytic medium 6 from being inserted into the core-shell particles 36, particularly into the Li ion insertion / desorption sites of the active material particles 30, thereby preventing the structure from being destroyed.

[0075] The buffer portion 42 preferably includes a modified region that is inseparably integrated with the SEI structure at the surface near the interface with the core-shell particle 36, particularly at the contact portion with the permeable pore network 81.

[0076] The SEI structure is formed on the surface of the electrode active material mainly when the battery is first charged, and is thought to be gradually damaged and deteriorated by repeated charging and discharging of the LIB. The deteriorated SEI is regenerated using the non-aqueous electrolyte near the surface of the electrode active material, but solutes, electrolyte, additives, etc. are consumed during this process, and the amount of Li ions and electrolyte decreases over long-term use, causing the battery characteristics to deteriorate. The speed of SEI deterioration is thought to be determined by the quality of the SEI, which is composed of components derived from the non-aqueous electrolyte, and is said to contain, for example, polymers linked with carbonate-derived components. If a structure derived from impurities such as flame retardants is introduced into the SEI, it is thought that the structure of the SEI will be disrupted and the quality will be low. An SEI that is initially formed with high quality is less likely to deteriorate and impurity uptake during regeneration is suppressed, making it a more effective SEI.

[0077] In other words, to improve the quality of the SEI, it is effective to carry out the SEI formation reaction in an electrolyte that does not contain additives, such as flame retardants. In addition, since the SEI is most largely formed during the first charge of the battery, it is believed to be effective to form a high-quality SEI during the first charge.

[0078] The buffer section 42 according to the present invention that includes such an SEI may include a metal oxide and / or a metal phosphate in addition to lithium and silicon elements.

[0079] Furthermore, it is preferable that the multilayer film of shell film 41 / buffer section 42 has different metal components and / or compositions on both sides and different concentrations of phosphate ions, from the viewpoint of fully exerting the effects of "strongly crystalline, low-oxygen-releasing polyanion" and "replenishment of consumed Li" while suppressing the adverse effects of high resistance due to Li-based polyanion coating, and it is preferable to decrease the concentration of phosphate ions and increase the concentration of oxides from the center to the outside of active material particle 30, and when shell film 41 contains LMP, it is more preferable to gradually change the composition and / or concentration in order to suppress "mobile charge traps" and "rise in charge transfer potential barrier", and to suppress "interface mismatch".

[0080] The buffer portion 42 covers at least a portion of the surface of the core-shell particle 36, more preferably covers 95% or more, and preferably covers the surface completely.

[0081] With regard to buffer section 42, in this specification, the "active material particles" before buffer section 42 is formed will be referred to as "active material particles A", the active material layer containing them will be referred to as active material layer A, the current collectors 20, 120 on which active material layer A is arranged will be referred to as current collector A with active material layer, the manufacturing process for producing them will be referred to as current collector A with active material layer manufacturing process, the electrode laminate in which positive and negative current collectors A with active material layers are opposed to each other will be referred to as electrode laminate A, and the manufacturing process for producing them will be referred to as electrode laminate A manufacturing process.

[0082] Similarly, with regard to buffer section 42, the present invention is characterized in that buffer section 42 is formed at least once, and preferably two or more times, on the "active material particles" of current collector A with an active material layer; however, the "active material particles" after buffer section 42 has been formed the first time, or in a previous one of the multiple times, will be referred to as "active material particles B", the active material layer containing them will be referred to as active material layer B, current collectors 20, 120 on which active material layer B is arranged will be referred to as current collector B with active material layer, the manufacturing process for producing them will be referred to as the current collector B with active material layer manufacturing process, an electrode laminate formed by opposing current collectors B with active material layers of the positive and negative electrodes will be referred to as electrode laminate B, and the manufacturing process for producing them will be referred to as the electrode laminate B manufacturing process.

[0083] Similarly, with regard to buffer section 42, the "active material particles" after formation of buffer section 42 in a later of multiple times will be referred to as "active material particles C", the active material layer containing them will be referred to as active material layer C, current collectors 20, 120 on which active material layer C is arranged will be referred to as current collector C with active material layer, the manufacturing process for producing this will be referred to as current collector C with active material layer manufacturing process, an electrode laminate formed by opposing current collectors C with active material layers of positive and negative electrodes will be referred to as electrode laminate C, and the manufacturing process for producing this will be referred to as electrode laminate C manufacturing process.

[0084] (Binder 70) The binder 70 is not particularly limited, but may be, for example, at least one selected from the group consisting of polyethylene glycol (PEG), polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber, polyimide, and derivatives thereof.

[0085] The binder 70 may include dispersants, thickeners, and conductive aids that are soluble in the binder material.

[0086] The amount of binder 70 is preferably 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of core-shell particles 36, which can impart to the active material layer 2 the strength necessary to support the active material particles 30 and the core-shell particles 36 as an integrated layer, can stably form a low-resistance conductive network 80, and can provide sufficient adhesive strength to the current collectors 20, 120.

[0087] Within this range, the positive electrode active material layer 21 can be formed in which the core-shell particles 36 are bonded with sufficient adhesive strength, and a stable low-resistance conductive network 80 can be configured. Furthermore, sufficient adhesive strength can be obtained with respect to the current collector 20.

[0088] (Conductive network 80) The conductive network 80 is composed of a conductive material, preferably a conductive carbon material, and more preferably at least one selected from natural graphite, artificial graphite, vapor-grown carbon fiber, carbon nanotubes, acetylene black, ketjen black, and furnace black.

[0089] The amount of the conductive network 80 is preferably 1 part by weight or more and 30 parts by weight or less with respect to 100 parts by weight of the core-shell particles 36 .

[0090] Within this range, the conductivity of the positive electrode part 10 can be ensured while maintaining the adhesiveness to the binder 70. In addition, the adhesiveness to the current collector 20 can be sufficiently obtained while the electrical conductivity with the current collector 20 can be sufficiently obtained.

[0091] The conductive network 80 is at least partially in contact with the core-shell particles 36 and extends outward from the region where it is formed with the core-shell particles 36 .

[0092] (Sea-like part 60) The sea-like portion 60 includes a conductive support material and "active material particles", the conductive support material including a binder 70 and a conductive network 80, and is composed of, for example, coated active material particles 130, a binder 70, and a conductive network 80, as shown in the enlarged view of Figure 2(a).

[0093] The sea-like portion 60 is longer than the conductive paths between adjacent coated active material particles 130, 30, and has a chain-like conductive network 80 as its main skeleton, with the binder 70 supporting the state in which multiple coated active material particles 130 are in contact with this conductive network 80.

[0094] It is presumed that the potential uniformity in the active material layer 2 is achieved not by the conductive paths between the coated active material particles 130 but by the conductive network 80, which is like a long chain mainly made of a conductive material.

[0095] The reason why a structure is formed in which the binder 70 supports the state in which multiple coated active material particles 130 are in contact with such a conductive network 80 is that, when produced by the manufacturing method described below, in the slurry formed in the application process, the coated active material particles 130 with hydrophilic surfaces are arranged in a hydrophobic medium containing a conductive material, binder, and solvent, and then, by drying and removing the solvent, the particles are supported by the binder 70.

[0096] (Island 61) The islands 61 are composed of a permeable pore network 81, as shown in FIG. 2(a).

[0097] The permeable pore network 81 has a plurality of pores which are interconnected to allow the electrolytic medium 6 to permeate therethrough.

[0098] It is preferable that some of the pores of the permeable pore network 81 reach and contact the surface formation region of the “active material particle”.

[0099] The permeable pore network 81 has a non-liquid lithium ion conductor having an SEI structure disposed at least in the formation region thereof.

[0100] The lithium ion conductor preferably contains one or more metal elements selected from Mn, Fe, Al and Si.

[0101] From another perspective, the permeable pore network 81 is a cavity formed by the contours of the coated active material particles 130, the binder 70, and the conductive network 80, and is three-dimensionally continuous from the positive electrode collector 20 side (inside) to the outside.

[0102] On the surface of the positive electrode active material particle 40 or "active material particle", the ratio of the total area of ​​pores to the area of ​​the surface is preferably 0.1% to 30%, and more preferably 1% to 10%.

[0103] The permeable pore network 81 is in contact with the positive electrode active material particles 40 or "active material particles", and at least a portion of the electrolytic medium 6 permeates therethrough during charging and discharging of the LIB1. It is preferable that an SEI structure-containing non-liquid Li ion conductor is formed in the formation region of the permeable pore network 81, and such an SEI structure-containing non-liquid Li ion conductor preferably contains one or more metal elements selected from the group consisting of Mn, Si, Fe, and Al, and more preferably contains Mn and Si. <Current collector with active material layer> The current collector with an active material layer is formed by forming an active material layer 2 containing coated active material particles 130 on a current collector 20, 120, and preferably, the surface of the active material layer, which is the surface opposite to the current collector 20, 120, is an uneven surface consisting of protrusions made of "active material particles" and recesses made of a conductive support material. <Coating 35> The entire outer surface of the coating 35 opposite the active material particles 30 side is composed of a formation region where the buffer section 42 is formed and a non-formation region other than the formation region, and the non-formation region is a region where the buffer section 42 is not formed and where a conductive support material including the binder 70 and the conductive network 80 is arranged.

[0104] Such a non-forming region is preferably an uneven surface with the non-forming region being the convex portion and the forming region being the concave portion, and part of the conductive network is exposed at the convex portion of the non-forming region. <Conductive materials> The conductive material constituting the conductive network 80 of the present invention can be any material that is generally used as a conductive assistant when preparing a paste, and is preferably a conductive carbon material, and is preferably at least one selected from natural graphite, artificial graphite, vapor-grown carbon fiber, carbon nanotubes, acetylene black, ketjen black, and furnace black.

[0105] The amount of the conductive material contained in the active material layer 2 is preferably 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of the (coated) active material particles 30, 130 and core-shell particles 36, and while ensuring the conductivity of the positive electrode portion 10 and the negative electrode portion 11, preferably the conductivity of the conductive network 80 according to the present invention is sufficiently ensured, adhesion to the binder 70 is maintained, and sufficient adhesion to the current collectors 20, 120 is obtained while ensuring sufficient conductivity with the current collectors 20, 120.

[0106] (Electrolytic medium 6) The electrolytic medium 6 is an electrolytic solution or a solid electrolyte, and in this embodiment is a non-aqueous electrolytic solution.

[0107] The electrolytic medium 6 is not particularly limited, but may be a non-aqueous electrolyte solution in which a solute is dissolved in a non-aqueous solvent, or a gel electrolyte in which a polymer is impregnated with a non-aqueous electrolyte solution in which a solute is dissolved in a non-aqueous solvent.

[0108] The electrolytic medium 6 is not particularly limited, but may be a nonaqueous electrolyte, a polymer electrolyte, or a solid electrolyte. From the viewpoint of effectively achieving the effects of the present invention, it is preferable that the electrolytic medium 6 be a nonaqueous electrolyte having a solute dissolved in a nonaqueous solvent, or a polymer electrolyte having a polymer impregnated with a nonaqueous electrolyte having a solute dissolved in a nonaqueous solvent, and more preferably a nonaqueous electrolyte.

[0109] The electrolytic medium 6 may be previously contained in the positive electrode part 10 and the negative electrode part 11, and preferably in the separator 12 present in the electrolytic medium 6, or may be added after wrapping or laminating the separator 12 disposed between the positive electrode part 10 side and the negative electrode part 11 side.

[0110] The non-aqueous electrolyte is a liquid in which a Li salt is dissolved in a non-aqueous solvent, and various additives described below are added as necessary. In addition, other additives can be added for the purpose of improving charge / discharge cycle characteristics, high-temperature storage properties, safety, etc.

[0111] (Electrolyte for forming the buffer section, electrolyte for battery products at the time of shipment) Such nonaqueous electrolyte solutions include a buffer-forming electrolyte solution, which is used when forming the buffer section according to the present invention and contains the raw materials thereof, and a battery product-shipment electrolyte solution, which is injected into the battery product immediately before it is shipped and is used as the operating electrolyte solution when the battery is operated. One of the features of the present invention is that the components and / or composition of the buffer-forming electrolyte solution and the battery product-shipment electrolyte solution, and also of the buffer-forming electrolyte solution at each stage in the process, are different depending on the purpose.

[0112] For example, the electrolyte for forming the buffer section may have Li-ion conductivity and contain a silicon-containing compound that constitutes the buffer section 42, and such a silicon-containing compound is contained in the electrolyte as an additive. It is preferable that the electrolyte at the time of shipment of the battery product basically does not contain any raw material that may electrochemically generate the buffer section 42 and can stably exhibit Li-ion conductive function.

[0113] In this way, by using appropriate materials and amounts of additives required for buffer formation at each stage according to the purpose, the amount of expensive additives used can be reduced, generated gas can be easily released, and various electrolytes can be selectively used by injecting the electrolyte at each stage, resulting in a high-performance LIB that overcomes the limitations of the use of conventional Li salts and additives. <Polymers for polymer electrolytes> Polymers for polymer electrolytes include PEG, PEO, PAN, PVDF, fluoropolymers, and polymers obtained by grafting (meth)acrylic polymers onto these, and the like, and those having a weight average molecular weight of 5,000 to 20,000 are used.

[0114] For example, a (meth)acrylic polymer grafted fluoropolymer is an attempt to improve the problem of uniform distribution on the active material surface, which is caused by the low surface energy characteristics of a fluoropolymer, that is, the difficulty in injecting the fluoropolymer as an electrolyte composition and the difficulty in penetrating the electrolyte even if injected, and to utilize the characteristics of the fluoropolymer, such as electrochemical stability at high voltage and the ability to remove radicals by the fluorine group. <Solid electrolyte> As the solid electrolyte, any electrolyte having high ionic conductivity can be used. A ceramic electrolyte containing Li is preferable. For example, Li 10 GeP2S12, Li7P3S13, 70Li2S-30P2S5, La 0.1 Li 0.34 TiO 2.94 , Li 1.1 Al 0.7 Ti 1.5 (PO4)3, etc., and the preferred conductivity is 1×10 -4S / cm or more, more preferably 1×10 -3 S / cm or more, and a preferable thickness is 5 μm or more and 200 μm or less. If it is less than 5 μm, the mechanical strength of the solid electrolyte layer is insufficient and it is prone to short circuits, and a thickness of 10 μm or more and 100 μm or less is more preferable. <Non-aqueous solvent> The non-aqueous solvent preferably contains a cyclic aprotic solvent and / or a chain aprotic solvent.

[0115] Examples of cyclic aprotic solvents include cyclic carbonates, cyclic esters, cyclic sulfones, and cyclic ethers. From the viewpoint of forming a high-quality SEI, a cyclic carbonate-based compound containing an unsaturated bond or a halogen atom may be used.

[0116] As the chain aprotic solvent, a solvent generally used as a solvent for a nonaqueous electrolyte, such as a chain carbonate, a chain carboxylate, a chain ether, or acetonitrile, may be used. From the viewpoint of forming a high-quality SEI, a chain carbonate-based compound containing an unsaturated bond or a halogen atom may be used.

[0117] Here, acetonitrile is preferable because, when contained in the non-aqueous solvent, it can improve ionic conductivity and increase the diffusibility of Li ions within the battery. In particular, even when the active material layer is made thicker and the loading amount of the positive electrode active material is increased, Li ions can be sufficiently diffused even to the region near the current collector which is difficult for Li ions to reach during high-load discharge, resulting in a LIB having load characteristics and rapid chargeability that enable sufficient capacity to be discharged even during high-load discharge. However, since the nitrile group has a high metal coordination ability, it forms a complex with the transition metal in the positive electrode active material and stabilizes it, promoting metal elution. The eluted metal ions are reduced and precipitated on the negative electrode side, damaging the SEI of the negative electrode, promoting the reductive decomposition of the solvent at the negative electrode. In other words, "acetonitrile eluted metal ion negative electrode deposition SEI damage reductive decomposition promotion effect" occurs, and the irreversible capacity increases and the reductively decomposed solvent accumulates on the negative electrode. In addition, it has been reported that when the LIB is stored for a long period of time in a high temperature environment, physical peeling occurs between the positive electrode Al current collector and the positive electrode active material particles, and the internal resistance increases. In addition, acetonitrile is easily reduced and decomposed electrochemically, and when acetonitrile is used, it is necessary to use other solvents, for example, aprotic solvents other than acetonitrile, or to add an electrode protectant, so care must be taken. In addition, attention should also be paid to the "effect of suppressing the deterioration of the negative electrode SEI by containing a cyclic anion-containing Li salt and acetonitrile" described later.

[0118] More specifically, examples of aprotic solvents that can be used include dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, sulfolane, dioxolane, and methyl propionate.

[0119] These solvents may be used alone or in combination of two or more. However, it is preferable to use a mixture of two or more solvents in view of the ease of dissolving the solute described below and the high conductivity of Li ions.

[0120] When two or more types of aprotic solvents are mixed, it is preferable to mix one or more types of chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate, dipropyl carbonate, and methyl propyl carbonate with one or more types of cyclic compounds exemplified by ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone, because these have high stability at high temperatures and high Li conductivity at low temperatures.

[0121] A mixture of one or more chain carbonates exemplified by dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate and one or more cyclic carbonates exemplified by ethylene carbonate, propylene carbonate, and butylene carbonate is particularly preferred. <Solute> The solute is not particularly limited, but for example, LiClO4, LiBF4, LiPF6, LiAsF6, LiCF3SO3, LiBOB (Lithium Bis(Oxalato)Borate), LiN(SO2CF3)2, etc. are preferred because they are easily dissolved in the solvent.

[0122] Li salts containing cyclic anions are preferable as solutes for non-aqueous electrolytes containing acetonitrile from the viewpoint of improving long-term high-temperature durability. It has been reported that the cyclic anions dissociated from the Li ions electrically interact with acetonitrile, weakening the metal coordination ability of the nitrile group, and improving long-term high-temperature durability due to the "inhibition effect of the inclusion of Li salts containing cyclic anions and acetonitrile on the negative electrode SEI degradation," which occurs due to the reductive precipitation of metal complexes at the negative electrode caused by the inhibition of metal elution caused by the formation of a complex with a transition metal in the positive electrode active material by acetonitrile at high temperatures, which inhibits the migration of the metal complex to the negative electrode. <Additives for non-aqueous electrolyte 6> Examples of additives to the non-aqueous electrolyte 6 include an electrode protector, a gas generation inhibitor, an SEI forming agent, an SEI formation promoter, an SEI characteristic improver, a stabilizer, a metal elution inhibitor, and a flame retardant.

[0123] The electrode protecting agent is an additive for protecting the electrodes and may overlap with the non-aqueous solvent. Specific examples of the electrode protecting agent include fluoroethylene carbonate, unsaturated bond-containing cyclic carbonates, lactones, and cyclic sulfur compounds. The content of the electrode protecting agent in the non-aqueous electrolyte is preferably 0.1 to 30% by volume, and more preferably 0.3 to 15% by volume, based on the total amount of the non-aqueous solvent.

[0124] Vinylene carbonate, used as an electrode protectant, can suppress the reductive decomposition reaction of acetonitrile on the negative electrode surface, and is used in combination to prevent performance degradation at low temperatures due to excessive film formation. By keeping the interface resistance low, it contributes to suppressing deterioration of cycle characteristics at low temperatures.

[0125] The gas generation inhibitor has a function of suppressing gas generation mainly during high-temperature storage, Phosphate compounds are included.

[0126] An SEI forming agent is a material that is a raw material for the SEI that is formed on the electrode surface by decomposition through electrochemical redox reactions and the like as part of the non-aqueous electrolyte during charging. Normally, an SEI can be formed through an electrochemical redox reaction of an electrolyte containing a Li salt and a non-aqueous organic solvent, but such an SEI may be thick and have high resistance. By using an SEI forming agent, it may be possible to thin and densify the SEI that is formed, which may contribute to lowering the resistance of the SEI. Examples of such SEI forming agents include sulfonate compounds, sultone compounds, Examples of such compounds include acrylate-based compounds, six-membered aromatic heterocyclic compounds containing two or more nitrogen atoms in the molecule, cyclic anion-containing compounds, and various Li salts, such as oxalate complex negative ion Li salts, imide-based Li salts (e.g., Li bisfluorosulfonylimide (LiFSI)), fluorophosphate-based Li salts, and fluoroborate-based Li salts. For example, sulfonate compounds reduce internal resistance by forming a low-resistance SEI, and cyclic anion-containing compounds are reductively decomposed at the negative electrode, and the decomposition products generated thereby accumulate on the negative electrode to form an SEI.

[0127] The SEI property improver has a function of strengthening the SEI, and examples of the SEI property improver include acid anhydrides.

[0128] The SEI formation promoter has the function of promoting the formation of the SEI, and examples of such promoters include lactam compounds substituted with electron-withdrawing groups. By increasing the oxidation / reduction potential of the SEI raw materials, the SEI formation is promoted when the negative electrode active material is LTO.

[0129] The stabilizer has the function of maintaining the state of the non-aqueous electrolyte itself and the state of the electrode parts in non-aqueous solvent liquid LIBs at the time of product shipment over a long period of time and over a large number of charge / discharge cycles, and examples of the stabilizer include silane-based compounds and phosphate esters, which are silicon-containing compounds according to the present invention.

[0130] The silane-based compound maintains the non-aqueous solvent liquid LIB in a state of low internal resistance and protects the non-aqueous electrolyte from the active sites of the positive electrode active material, which are the cause of oxidative deterioration of the non-aqueous electrolyte.

[0131] The phosphate ester stabilizes the non-aqueous electrolyte by suppressing side reactions during storage. <Silicon-containing compounds> Examples of the silicon-containing compound include siloxane compounds, silazane compounds, and silylamide compounds each containing one or more unsaturated groups. Preferred silicon-containing compounds include cyclic siloxanes having a vinyl group, such as 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane (4VC4S).

[0132] A siloxane-based compound containing one or more unsaturated groups contains a -Si-O-Si- bond (siloxane bond) and at least one carbon-carbon double bond. It is believed that the siloxane bond site can conduct Li ions and that this double bond can contribute to the formation of an SEI structure through cross-linking.

[0133] (Separator 12) As shown in FIG. 1, the separator 12 is disposed between the positive electrode part 10 and the negative electrode part 11, and has a structure that is insulating and can contain the electrolytic medium 6.

[0134] Examples of the separator 12 include woven fabrics, nonwoven fabrics, and microporous membranes made of nylon, cellulose, polysulfone, polyethylene, polypropylene, polybutene, polyacrylonitrile, polyimide, polyamide, polyethylene terephthalate, and composites of two or more of these.

[0135] The separator 12 may contain various plasticizers, antioxidants, and flame retardants, and may be coated with metal oxides or the like.

[0136] (Positive electrode extraction member 13, negative electrode extraction member 14) The extraction members 13 and 14 are terminals that are connected to one or more positive electrode parts 10 and one or more negative electrode parts 11 and can be connected to an external load, and are provided across the inside and outside of the exterior body 3.

[0137] (Manufacturing method of lithium ion secondary battery 1, etc.) Next, a method for producing the lithium ion secondary battery 1 etc. according to the present invention will be described.

[0138] The manufacturing method of the lithium ion secondary battery 1 etc. according to the present invention includes a manufacturing method for producing products such as coated active material particles, an active material layer, a current collector with an active material layer, a peeled product of an active material layer, an electrode laminate, a battery assembly, a battery product, etc., and these products can be produced at each step of the manufacturing method in which the battery 1 is the finished product.

[0139] The manufacturing method of battery 1 includes, in order, 1. active material particle preparation process, 2. current collector with active material layer manufacturing process, 3. electrode laminate manufacturing process, 4. battery assembly manufacturing process, and 5. battery product manufacturing process, and in some cases, preferably includes 2.5. peeled material manufacturing process, between 2. current collector with active material layer manufacturing process and 3. electrode laminate manufacturing process, as a peeled material manufacturing process for manufacturing a peeled material of the active material layer that is a raw material for reproducing the active material layer, in which at least a part of the active material layer is peeled off and recovered from the current collector, and these manufacturing processes include various processes as appropriate, and among them, the buffer part formation process, which is a process for forming the buffer part according to the present invention, is included in at least 5. battery product manufacturing process, and is preferably included in one or more manufacturing processes among 2 to 4.

[0140] In addition, these steps include, as operations that may be repeatedly performed in the manufacturing method of the present invention, an electrolyte injection operation, a voltage application operation, and a curing operation, and preferably also include a grinding operation, a rolling operation, an electrolyte immersion operation, an electrolyte discharge operation, an exposure expansion operation, and a support material reduction operation. (Manufacturing method of all-solid-state LIB) The manufacturing method for an all-solid-state LIB is to apply a solid electrolyte slurry to the current collectors with active material layers of both electrodes prepared in 2. Manufacturing process of current collectors with active material layers by using a doctor blade method in 3. Electrode laminate manufacturing process, volatilize the solvent to form a solid electrolyte layer, and then heat-dry (e.g., in air, at 150°C) the electrode laminate 5 in which the current collectors of both electrodes are laminated with this solid electrolyte layer between them, and then compression-molde it by a rolling operation to complete the basic structure of an all-solid-state LIB.

[0141] (Production method of non-aqueous electrolyte LIB) The above-mentioned manufacturing steps, steps, and operations will be described in detail below, focusing on the manufacturing method of the lithium ion secondary battery 1 of this embodiment, which is a method for manufacturing a nonaqueous electrolyte LIB. (1. Active material particle preparation process) In the active material particle preparation step, active material particles 30 are prepared, and preferably, core-shell particles 36 are prepared as coated active material particles 130 according to the present invention by the shell film formation step described later. (Shell film formation process) The shell film formation process is a process of forming a shell film 41 according to the present invention on the prepared active material particles 30, thereby preparing core-shell particles 36 having a core-shell structure in which the active material particles 30 form the core and the continuous shell film 41 forms the shell.

[0142] Specifically, in the shell film forming step, a phosphate ion-containing Li compound is first pulverized by a pulverizing device such as a ball mill to form phosphate ion-containing Li compound particles (pulverization operation). Here, the phosphate ion-containing Li compound is preferably a Li ion conductive oxide containing phosphorus, and the phosphate ion-containing Li compound before the pulverization step is preferably a phosphate-based compound having an olivine-type crystal structure. The phosphate ion-containing Li compound particles after pulverization may have a partially destroyed crystal structure and be entirely or partially amorphous (non-crystalline). When the particles are entirely amorphous, when the phosphate ion-containing Li compound particles are measured by X-ray diffraction (XRD), the inherent crystal peaks of the phosphate ion-containing Li compound particles that appeared before pulverization are not confirmed by a halo pattern.

[0143] In this case, the phosphate ion-containing Li compound particles have a BET specific surface area of ​​20 m2 / g or more and 80 m 2 / g or less, and the phosphate ion-containing Li compound particles preferably have a BET specific surface area equivalent diameter (dBET) of 30 nm or more, more preferably 50 nm or more, and preferably 500 nm or less, and more preferably 450 nm or less. Within these ranges, the surfaces of the active material particles 30 can be uniformly coated, and a dense shell film 41 can be formed.

[0144] The BET specific surface area equivalent diameter (dBET) is the particle size calculated by calculating the nitrogen adsorption BET specific surface area using the single-point nitrogen adsorption method in accordance with the method specified in JIS Z8830 (2013), and then using the formula dBET = 6 / (density × BET specific surface area).

[0145] Subsequently, the mixture is pulverized in a pulverization step, and the phosphate ion-containing Li compound particles are dispersed in a dispersion solvent to form a fine particle fluid (fine particle fluid formation step).

[0146] The dispersion solvent used in this case is preferably one or more alcohol solutions, and more preferably ethanol from the viewpoints of volatility and safety.

[0147] The fine particle fluid formed at this time is a transparent sol in a sol state and has fluidity.

[0148] Next, at least one type of energy of shear force, compression force, collision force, and centrifugal force is applied to the positive electrode active material particles 30 and / or the phosphate ion-containing Li compound particles constituting the shell film 41, while a mechanical coating method is used to mechanically contact the active material particles 30 with the phosphate ion-containing Li compound particles in the microparticle fluid, thereby forming a shell film 41 on the surface of the positive electrode active material particles 30.

[0149] In this embodiment, the microparticle fluid is ground into active material particles 30 by a grinding device such as a grinding mill to form a ground product (ground product forming step).

[0150] At this time, the amount of the phosphate ion-containing Li compound particles put into the grinding device is preferably 0.5 wt % or more.

[0151] At this time, the amount of the phosphate ion-containing Li compound particles put into the grinding device is preferably 2.5 wt % or less, more preferably 1.6 wt % or less, and particularly preferably 1 wt % or less.

[0152] The treatment temperature in the milling device is preferably 5°C or higher and 100°C or lower, more preferably 8°C or higher and 80°C or lower, and even more preferably 10°C or higher and 50°C or lower.

[0153] The treatment time in the milling device is preferably from 5 to 90 minutes, and more preferably from 10 to 60 minutes.

[0154] The atmosphere in the milling apparatus at this time is preferably an inert gas atmosphere or an air atmosphere.

[0155] The ground product is then subjected to a heat treatment to remove the dispersion solvent from the ground product, and a shell film 41 is formed.

[0156] The heat treatment temperature at this time is preferably 300° C. or higher, and more preferably 350° C. or higher.

[0157] If the heat treatment temperature is below 300° C., the adhesion between the active material particles 30 and the shell film 41 will be insufficient, and the shell film 41 may peel off during charging and discharging of the battery, which may lead to a decrease in the long-term reliability of the battery.

[0158] On the other hand, if the heat treatment temperature is too high, the crystal structure of shell film 41 may change, causing a decrease in Li-ion conductivity and preventing normal charging and discharging of the battery. Therefore, the heat treatment temperature is preferably 850°C or less, and more preferably 500°C or less from the viewpoint of suppressing crystallization of the amorphous portion of the partially formed shell film 41, which may be preferable.

[0159] The heat treatment time is preferably 30 minutes or more, more preferably 45 minutes or more, and is preferably 180 minutes or less, more preferably 150 minutes or less.

[0160] This concludes the description of the shell film forming step for forming shell film 41, which is a phosphate ion-containing Li compound film, on the surface of active material particle 30.

[0161] The shell film formation process of forming a shell film 41, which is a phosphate ion-containing Li compound film, on the surface of a positive electrode active material particle 40 and the shell film formation process of forming a shell film 41, which is a phosphate ion-containing Li compound film, on the surface of a negative electrode active material particle 140 are basically the same, except that the active material particles 30 to be coated are positive electrode active material particles 40 or negative electrode active material particles 140.

[0162] (2. Manufacturing process of current collector with active material layer) The process for producing a current collector with an active material layer is a process for producing a current collector with an active material layer that can function as an electrode by forming an active material layer 2 on a current collector 20, 120, and includes, in order, a coating process of coating the current collector with an active material layer paste, which will be described later, and active material layering, which converts the applied active material layer paste into a layer that can function as an active material layer, and preferably includes a buffer section formation process, which will be described later.Furthermore, by using coated active material particles 130 derived from the peeled material produced in the peeled material production process of the present invention, which will be described later, as the active material particle-containing material of the active material layer paste, the process also serves as a process for producing a current collector with an active material layer in which an active material layer is reproduced. (Coating process) The coating process is a process in which active material particles, i.e., active material particles 30, core-shell particles 36, and optionally coated active material particles 130, are mixed with a conductive assistant and a binder, dispersed in a solvent to form a paste, forming a slurry which is an active material layer paste, and the slurry is applied to the current collectors 20, 120 to form a paste-coated current collector.

[0163] The solvent used in this step is not particularly limited as long as it can dissolve or disperse the active material particles 30, the conductive assistant, and the binder, and examples of the solvent that can be used include N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, methyl ethyl ketone, methyl acetate, ethyl acetate, and tetrahydrofuran. A dispersant and a thickener may be added to these. (Active material layering process) The active material layer process is a process in which the active material layer paste applied onto the current collectors 20, 120 is dried or otherwise processed, and the paste-applied current collectors are fired, for example, for a predetermined firing time and at a predetermined firing temperature, to form a work-in-progress positive electrode part containing positive electrode active material particles 40 and a work-in-progress negative electrode part containing negative electrode active material particles 140, respectively.

[0164] The firing temperature is not particularly limited as long as the paste-coated current collector is fired and the slurry is solidified at the temperature, but is preferably, for example, 80° C. or higher and 200° C. or lower.

[0165] The current collectors each including the in-process positive electrode part and the in-process negative electrode part thus formed can be used as current collectors with active material layers that function as electrodes, but it is preferable to subsequently carry out a rolling operation or a buffer part formation step described below to form a current collector with a more highly functional active material layer. <Rolling operation> The rolling operation is a step of rolling the current collector on which the active material layer has been formed. (Buffer forming process) The buffer section forming step according to the present invention is a step that mainly involves a voltage application process (described later) for forming the buffer section 42 according to the present invention in the formation region over the entire surface of the outer surface of the "active material particle", including the non-formation region where the buffer section 42 is not formed. As described above, such a buffer portion forming step is included at least in 5. Battery Product Manufacturing Steps, and preferably in one or more of manufacturing steps 2 to 4. Each case will be explained below as appropriate.

[0166] 2. In the process for producing a current collector with an active material layer, the buffer section formation step is carried out by placing a buffer section formation electrolyte and a current collector with an active material layer in a container, immersing the active material layer in the buffer section formation electrolyte (electrolyte immersion operation), and then using a metal electrode, for example Li metal foil, as a counter electrode and applying a voltage between the current collector and the metal electrode (voltage application operation) to cause an electrochemical reaction. <Electrolyte immersion operation> The electrolyte immersion operation is an operation of immersing both electrodes facing each other in an electrolyte. The electrodes here are a current collector with an active material layer of one electrode and a metal electrode, for example, a metal plate, and also are both electrodes of the electrode laminate 5, that is, a current collector with an active material layer of one electrode and a current collector with an active material layer of the other electrode. <Voltage application operation> The voltage application operation is an operation of applying a voltage between opposing electrodes, for example, an operation of applying a voltage between the positive electrode take-out member 13 and the negative electrode take-out member 14 of the in-progress electrode laminate, where the electrodes are a current collector with an active material layer of one electrode and a current collector with an active material layer of the other electrode or a metal electrode, for example, a metal plate, and are also both electrodes in the electrode laminate 5, and further, both electrodes in the electrode laminate 5 included in the battery assembly in the exterior body 3. By such a voltage application operation, for example, a silicon-containing compound in the buffer part-forming electrolyte is layered on the "active material particles" of the in-progress electrode laminate to form a buffer part 42, and an electrode laminate 5 including, for example, a positive electrode part 10 and a negative electrode part 11 is formed.

[0167] In such a buffer section formation process, the voltage application operation involves applying a voltage between both electrodes to obtain a predetermined constant current (CC), for example a constant current of 0.05 C, and once the predetermined voltage value is reached, current is allowed to flow under constant voltage (CV) conditions until the current reaches a predetermined current value, for example 0.005 C.

[0168] When such a voltage application operation is carried out in the buffer section formation process in the battery assembly manufacturing process described below, it is preferable to carry out the operation without sealing the electrolyte injection port of the outer casing 3, as this makes it possible to exhaust gas generated in the electrochemical reaction and to carry out the electrolyte exhaust operation described below.

[0169] In addition, when LNMO particles are used as the positive electrode active material particles, and a silicon-containing compound in the electrolyte for forming the buffer portion is precipitated as the buffer portion 42 on the surface of the “active material particles”, preferably via a shell film 41, the potential is preferably 4.5 V or more and 5 V or less relative to the lithium dissolution deposition potential.

[0170] 3. In the electrode laminate manufacturing process, the buffer section formation process involves subjecting the in-progress electrode laminate in the electrode laminate manufacturing process described below to an electrolyte immersion operation, followed by a voltage application operation to cause an electrochemical reaction.

[0171] In the 4. Battery Assembly Manufacturing Process, the buffer section formation process involves carrying out an electrolyte injection operation on the in-progress battery assembly in the 4. Battery Assembly Manufacturing Process described below, followed by a voltage application operation to cause an electrochemical reaction. <Electrolyte injection operation> The electrolyte injection operation is an operation of injecting electrolyte into the outer casing 3 after the electrode laminate or the in-progress electrode laminate has been placed inside the outer casing 3 so that both opposing electrodes of the electrode laminate or the in-progress electrode laminate are immersed. For example, the in-progress electrode laminate is placed inside the outer casing 3, the internal pressure of which has been reduced to 0.1 atmospheres or less using a vacuum packaging machine, and the outer casing 3 is sealed except for the injection port, etc., and then the interface electrolyte is injected into the outer casing 3 of the in-progress battery assembly. This operation can be preferably performed multiple times in combination with the (electrolyte discharge operation) described below via the (voltage application operation) described above. Furthermore, such an electrolyte injection operation can also be performed, if necessary, simultaneously in parallel with the (electrolyte discharge operation) described below, in which the electrolyte for forming the buffer section is discharged from the outer casing 3 while the electrolytic medium 6 is injected into the outer casing 3 of the battery assembly. <Electrolyte drain operation> The electrolyte draining operation is an operation for draining, to the outside of the exterior body 3, the electrolyte that has immersed both of the opposed electrodes of the electrode laminate or in-progress electrode laminate after placement within the exterior body 3.

[0172] The buffer formation process in the 5. Battery product manufacturing process is a process in which, after injecting the battery product's factory-set electrolyte, which is the electrolyte at the time of shipment, in the (electrolyte injection operation) in the 5. Battery product manufacturing process described below, and optionally sealing the electrolyte injection port and gas exhaust port, a (voltage application operation) is performed as initial product charging to form a typical SEI structure by an electrochemical reaction.

[0173] (2.5. Peeling manufacturing process) The exfoliated material manufacturing process according to the present invention is a process for manufacturing an exfoliated material including coated active material particles 130 including buffer portions 42 formed on the outer surfaces of the "active material particles". This exfoliated material is crushed as necessary to form coated active material particles 130 according to the present invention. The coated active material particles 130, which are composed of the coating 35 including buffer portions 42, the "active material particles", and a conductive support material according to the present invention, can be used as positive and negative active material layer materials for various types of LIBs, including not only nonaqueous charged liquid LIBs but also all-solid-state LIBs including polymer LIBs, by selecting not only the active material particles 30 and shell film 41 but also the buffer portions 42 and conductive support materials according to the respective characteristics. Therefore, the conductivity of electricity and Li ions can be increased while maintaining the capacity, and gas generation, etc. can be suppressed, making it a raw material for manufacturing LIBs with excellent characteristics according to each characteristic. <Exposure expansion operation> The exposure expansion operation is an operation for expanding the exposed area of ​​the conductive network 80 that is preferably exposed in the convex non-forming region convex portions of the uneven surface that is the outer surface of the coating 35, where the buffer portion 42 is not formed and the conductive support material is arranged; specifically, it is an operation for partially removing the binder 70 material that supports the conductive network 80 and together with the conductive support material, while maintaining the support, or changing it into a conductive material by a chemical reaction; when the peeled material of the present invention is reproduced as the coated active material particle 130 of the present invention, its conductivity can be improved. <Support material reduction operation> The support material reduction operation is an operation for reducing the support material present portion, which is the portion where the conductive support material is present, in the active material particle convex portion, which is the convex portion composed of "active material particles" on the uneven surface, which is the active material layer surface, which is the surface opposite to the current collectors 20, 120 of the active material layer 2. Since the area of ​​the surface of the "active material particle" that is not covered by the conductive support material that is in direct contact with the electrolytic medium 6 becomes larger, it is possible to achieve high capacity and low internal resistance. Specifically, it is an operation for partially removing the binder 70 material, which supports the conductive network 80 and together with the binder 70 constitutes the conductive support material, while maintaining the support, or changing it into a conductive material by a chemical reaction. When the peeled material of the present invention is reproduced as the coated active material particle 130 of the present invention, its conductivity can be improved.

[0174] (3. Electrode laminate manufacturing process) 3. The electrode laminate manufacturing step is a step of sandwiching a separator 12 between a work-in-progress positive electrode part and a work-in-progress negative electrode part to form a work-in-progress electrode laminate or an electrode laminate.

[0175] Although the above-mentioned buffer portion forming process can also be carried out on the in-progress electrode stack in this electrode stack manufacturing process, it is preferable to carry it out on the in-progress battery assembly in the battery assembly manufacturing process described below from the viewpoint of forming a buffer portion simply and at low cost. However, from the viewpoint of forming a buffer portion of higher quality, it is preferable to carry out the buffer portion forming process before placing the electrode stack 5 in the outer casing 3.

[0176] (4.Battery assembly manufacturing process) 4. The battery assembly manufacturing process is a process in which a part-time electrode laminate is placed inside the exterior housing 3 to produce a part-time battery assembly or a battery assembly.

[0177] (5.Battery product manufacturing process) 5. The battery product manufacturing process is a manufacturing process in which the electrolyte is injected into the battery product at the time of shipment, followed by the aging process described below, to prepare the battery product for shipment. (Aging process) The aging process is a process in which a voltage application operation as an initial product charge and a curing operation are performed on the battery assembly after the electrolyte is injected at the time of shipment of the battery product. This initial product charge can include the voltage application operation in the buffer section formation process described above and electrical characteristic confirmation tests such as initial deterioration of the battery product. The curing operation is an operation in which the outer casing 3 is cured to seal the electrode stack 5 and the electrolytic medium 6, and the electrolyte injection port and gas exhaust port of the outer casing 3 are sealed.

[0178] (Effects brought about by the implementation of the invention) According to the lithium ion secondary battery 1 of this embodiment, the coating 41, 141 covering the active material particle 30 contains a phosphate ion-containing Li compound, and preferably the shell film 41 contains one or more metals selected from the group consisting of Fe, Mn, Si, and Al, more preferably the shell film 41 uniformly covers the active material particle 30 (40, 140), and even more preferably, since the active material particle 30 has an active material layer 2, the area of ​​contact between the active material particle 30 and the nonaqueous electrolyte 5 is reduced, and gas generation due to decomposition of the electrolytic medium 6 can be suppressed.

[0179] Preferably, the positive electrode active material particles 40 are made of a LiMn-based oxide, and are covered with a shell film 41 of a phosphate-based compound that can also be used as a positive electrode active material, so that the insertion and desorption reaction of Li ions can occur smoothly. More preferably, the positive electrode active material particles 40 are made of a LiMn-based oxide containing nickel, for example a LiMn-based oxide having a spinel-type crystal structure, so that a high-capacity secondary battery capable of generating high voltage can be constructed. Also, preferably, the positive electrode active material particles 40 are made of a LiMn-based oxide having a layered rock-salt type, and particularly preferably a Li-excess layered rock-salt type structure, so that an even higher-capacity secondary battery can be constructed.

[0180] Preferably, the negative electrode active material particles 140 are made of Li-titanium oxide, which allows the construction of a secondary battery with excellent safety and reliability. Furthermore, since this is covered with a shell film 41 of a phosphate-based compound that can also be used as a positive electrode active material, the insertion and desorption reactions of Li ions are likely to occur smoothly, allowing the construction of a secondary battery with excellent characteristics.

[0181] Preferably, the vicinity of the interface between shell film 41 and active material particle 30 is amorphous, so that even if a volume change occurs in active material particle 30 as charging and discharging progresses, the amorphous portion of shell film 41 functions as a buffer, making shell film 41 and, ultimately, coating film 41, 141 less likely to crack or peel off. Preferably, a fine particle fluid in which fine particles, the raw material of shell film 41, are dispersed in a dispersion solvent is ground into active material particle 30, and heat treatment is preferably performed at a temperature of 100°C or higher and 500°C or lower, so that a high-quality, thin shell film 41 can be formed on the surface of active material particle 30 while maintaining its amorphous nature.

[0182] According to the lithium ion secondary battery 1 of this embodiment, the active material layer 2 preferably has a conductive network 80 and a permeable pore network 81, which facilitates the exchange of charges and Li ions between the electrolytic medium 6 and the active material particles 30, making it easier for the electrode reaction to occur.

[0183] According to the lithium ion secondary battery 1 of this embodiment, the permeable pore network 81 preferably has a Li ion conductor provided from the formation region of the active material particles 30 or the "active material particles" toward the pores, so that the exchange of charges and Li ions between the electrolytic medium 6 and the active material particles 30 becomes smoother, making it easier for the electrode reaction to occur.

[0184] According to the lithium ion secondary battery 1 of this embodiment, the active material layer 2 has a silicon-containing compound film containing elemental silicon, so that the binding property of the active material layer 2 is improved and cracks and the like are less likely to occur.

[0185] According to lithium ion secondary battery 1 of the present embodiment, shell film 41 contains Li element, and the Li in shell film 41 can be used to replenish Li consumed for some reason, so that performance is less likely to deteriorate.

[0186] According to the lithium ion secondary battery 1 of this embodiment, the elution of Mn from the positive electrode active material particles 40 into the electrolytic medium 6 can be suppressed, and therefore the performance is less likely to deteriorate.

[0187] In the above-described embodiment, the active material layer 2 is formed by injecting the buffer section forming electrolyte solution in the buffer section forming electrolyte injection step and applying a voltage between the positive electrode extraction member 13 and the negative electrode extraction member 14 in the voltage application step, but the present invention is not limited to this.

[0188] For example, a silicon-containing compound containing elemental silicon may be added to the slurry in the coating step, and active material layer 2 may be formed in the active material layer forming step.

[0189] Alternatively, after the active material layering step, a paste containing a silicon-containing compound may be applied to the in-progress positive electrode part and the in-progress negative electrode part, and then solidified by heating, ultraviolet light, or the like, to form the active material layer 2.

[0190] After the electrode laminate manufacturing process, the active material layer 2 may be formed by applying a paste containing a silicon-containing compound to the in-progress electrode laminate and solidifying it by heating, ultraviolet light, or the like.

[0191] In the above embodiment, the buffer portion 42 is formed, but the present invention is not limited to this, and the buffer portion 42 does not necessarily have to be formed.

[0192] According to the present invention, for example, by forming the buffer section 42 with an electrolyte for forming the buffer section that is substantially free of flame retardants, it is possible to form the buffer section 42 that is substantially free of flame retardants, and therefore it is possible to suppress the decrease in battery capacity due to repeated charge / discharge cycles. In addition, by making the electrolyte at the time of shipment of the battery product contain a flame retardant, it is possible to increase the flash point of the electrolyte, i.e., it is possible to improve both the characteristics and safety of the battery.

[0193] In the above-described embodiments, each component may be freely substituted or added between the respective embodiments as long as it falls within the technical scope of the present invention. [Explanation of symbols]

[0194] 1. Lithium-ion secondary battery 2 Active material layer 21 Positive electrode active material layer 3 Exterior body 5 Electrode laminate 6 Electrolytic medium (electrolyte) 10 Positive electrode 11 Negative electrode 12 Separator 13 Positive electrode removal member 14 Negative electrode removal member 20 Positive electrode current collector 120 Negative electrode current collector 30 Active material particles 130 Coated active material particles (coated active material particles for lithium ion secondary batteries) 35 Coating 36 Core-shell particles 40 Positive electrode active material particles 140 Negative electrode active material particles 41 Shell Membrane 42 Buffer section 60 Marine part 61 Island 70 Binder 80 Conductive Network 81 Permeable Pore Network

Claims

1. The coated active material particles are active material particles coated with a coating film, The entire outer surface of the coating film opposite to the active material particles is A formation region in which the buffer portion is formed, and The buffer portion is not formed, and a binder, and a conductive network. A conductive support material is provided. a non-forming region; and the non-forming region being a convex portion and the forming region being a concave portion; The non-forming region is a convex portion. The coated active material particles have a part of the conductive network exposed at the non-forming region convex portion.

2. A current collector with an active material layer, comprising an active material layer including the coated active material particles according to claim 1 formed on a current collector, The active material layer is The cross-sectional shape is a sea-island structure, and includes an island portion and a sea-like portion, the islands include a permeable pore network leading to the formation region; The sea-like portion includes the conductive support material and the active material particles, and further includes a current collector with an active material layer, the surface of the active material layer opposite to the current collector side being an uneven surface having protrusions formed of the active material particles and recesses formed of the conductive support material.

3. The current collector with an active material layer according to claim 2, A method for producing an electrode stack, comprising the steps of: a current collector A manufacturing process in which an active material layer A containing different types of the active material particles as positive electrode active material particles and negative electrode active material particles is formed on the current collector, and a current collector A with an active material layer before the buffer section is formed is formed as a positive electrode current collector A with a positive electrode active material layer containing the positive electrode active material particles and a negative electrode current collector A with a negative electrode active material layer containing the negative electrode active material particles, respectively; a buffer portion B forming step of forming a buffer portion B as a part of the buffer portion in the active material particles of the active material layer A of at least one of the positive electrode current collector A with the positive electrode active material layer and the negative electrode current collector A with the negative electrode active material layer; and The method for producing an electrode laminate includes an electrode laminate B production step of forming an electrode laminate B by opposing at least one pair of a positive electrode current collector B and / or a negative electrode current collector B, the pair including a current collector B with an active material layer B on which the buffer portion B is formed.

4. The method for producing an electrode stack according to claim 3, further comprising: a buffer portion C forming step of forming a buffer portion C on the buffer portion B of at least one of the positive electrode current collector B and the negative electrode current collector B as a part of the buffer portion of the electrode stack B.

5. The method for producing an electrode stack according to claim 3 or 4, further comprising: the buffer portion B is formed in a state in which the active material layer-attached current collector A faces a metal plate.

6. The method for producing an electrode stack according to claim 3 or 4, further comprising: an exposure expansion operation for expanding the exposure of the conductive network; and / or A protrusion formed of the active material particles. In the active material particle convex portion, a portion of the conductive support material, A method for producing an electrode stack comprising a support material shrinking operation, whereby a portion of the support material is reduced.

7. A method for producing the electrode stack according to claim 3 or 4, the buffer portion B is formed by disposing a silicon-containing compound on the current collector B.

8. A method for producing a current collector with an active material layer according to claim 2, comprising the steps of: a current collector A manufacturing step of forming an active material layer A containing the active material particles on the current collector to form a current collector A with an active material layer before forming the buffer portion; a buffer portion B forming step of forming a buffer portion B as at least a part of the buffer portion in the active material particles of the active material layer A to form a current collector B; and a peeled product producing step of peeling the active material layer B from the current collector B to produce an active material layer B peeled product; and A method for manufacturing a current collector with an active material layer, comprising a recycled current collector B formation step of forming a recycled material layer B including the active material layer B peeled off material on the current collector to form a recycled current collector B with the recycled material layer B.

Citation Information

Patent Citations

  • Electrode group, nonaqueous electrolyte secondary battery, battery pack and vehicle

    JP2021051987A