Perlite malleable cast iron and method for producing perlite malleable cast iron
The described method stabilizes cementite in pearlitic malleable cast iron production using specific elemental compositions, addressing cost and efficiency issues in existing methods by enabling the production of both black-core and pearlite malleable cast iron with improved tensile strength and reduced costs.
Patent Information
- Application Number
- JP2023076800
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
AI Technical Summary
Existing methods for producing pearlitic malleable cast iron are costly due to multiple heat treatments and require large amounts of additional elements, leading to inefficiencies in molten metal management and operational costs.
A method using molten metal with specific carbon, silicon, manganese, nitrogen, and bismuth compositions to stabilize cementite, allowing for the production of both black-core and pearlite malleable cast iron without additional costly steps, utilizing manganese nitride and bismuth to inhibit graphitization and form pearlite.
Enables efficient production of pearlitic malleable cast iron with improved tensile strength and reduced manufacturing costs by utilizing the same molten metal for both types, enhancing operational efficiency and resource utilization.
Smart Images

Figure 2024161778000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to pearlitic malleable cast iron and a method for producing pearlitic malleable cast iron. [Background technology]
[0002] Cast iron is a general term for iron-carbon alloys suitable for casting. Cast iron can be classified into flake graphite cast iron, malleable cast iron, and spheroidal graphite cast iron, depending on the form of graphite present. Malleable cast iron can be further classified into whiteheart malleable cast iron, blackheart malleable cast iron, and pearlitic malleable cast iron. The carbon content of cast iron exceeds about 2.0 mass%, which is the carbon saturation solid solubility limit of austenite in the iron-carbon binary equilibrium diagram, and does not greatly exceed about 4.3 mass%, which is the eutectic point. During the solidification process of cast iron, graphite and / or cementite crystallize or precipitate first by a eutectic reaction and then by austenite eutectoid reaction.
[0003] In malleable cast irons, the constituent phase, i.e., the matrix, which occupies most of the alloy volume in whiteheart malleable cast iron and blackheart malleable cast iron, is basically composed of ferrite. In contrast, the matrix of pearlitic malleable cast iron is composed of pearlite in which ferrite and cementite are arranged in alternating layers, or pearlite in which granular cementite is dispersed in ferrite. This gives pearlitic malleable cast iron better tensile strength and wear resistance than other malleable cast irons.
[0004] One method for producing a matrix composed of pearlite in pearlite malleable cast iron is to heat treat white pig iron to precipitate graphite, and then further heat treat and rapidly cool it. For example, in the method described in Patent Document 1, white pig iron is first heated to 900°C or higher and subjected to primary annealing to precipitate graphite, and then subjected to secondary annealing at 300°C to obtain blackheart malleable cast iron. Next, the obtained blackheart malleable cast iron is heated to an austenite region above the A1 transformation point to dissolve carbon in the austenite matrix, and then removed from the heating furnace and forced air-cooled to transform the austenite matrix into pearlite. In this method, in order to increase toughness, further tempering may be performed after forced air-cooling.
[0005] Another method for producing pearlitic malleable cast iron is to add an element that inhibits the precipitation of graphite during annealing after casting, i.e., graphitization. For example, in the method described in Non-Patent Document 1, molten white pig iron for blackheart malleable cast iron melted in a cupola is transferred to a Herault-type electric furnace, and ferromanganese is added while the molten iron is heated to adjust the content of manganese, which has the effect of inhibiting graphitization, to 1.0%, and then the pearlitic malleable cast iron is obtained by heat treating it under the same heat treatment conditions as for blackheart malleable cast iron. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Utility Model Application Publication No. 5-40647 [Non-patent literature]
[0007] [Non-Patent Document 1] Matsuo Suzuki, Azuchi Hiramatsu, Nobuhisa Tsutsumi, "Melting Conditions of Manganese-Pearlite Malleable Cast Iron", Castings, Japan Foundry Association, September 25, 1960, Vol. 32, No. 9, pp. 625-635 Summary of the Invention [Problem to be solved by the invention]
[0008] The method using heat treatment described in Patent Document 1 requires two or three heat treatments in total to produce pearlitic malleable cast iron, which increases the manufacturing cost. The method using the addition of an element that inhibits graphitization described in Non-Patent Document 1 requires a relatively large amount of additive element to be added to the molten metal. For this reason, when adding additive element to molten metal dispensed into a ladle in continuous melting such as a cupola, it is not possible to add the required amount at once. In such a case, it is necessary to transfer the molten metal to a heating furnace for adjusting the composition and add the additive element there over a period of time, which also increases the manufacturing cost.
[0009] In addition, the elements that inhibit graphitization are also present in large quantities in waste materials such as sprues and runners of castings that are cast using molten metal that contains large amounts of these elements. If these waste materials are returned to a cupola or electric furnace for melting, there is a risk that the components of the molten metal will exceed the control limits. This means that it is not possible to use the same molten metal to produce blackheart malleable cast iron and pearlitic malleable cast iron separately, which poses the problem of reduced operating efficiency of the melting furnace.
[0010] The present invention has been made in view of the above problems, and has as its object to make it possible to produce pearlitic malleable cast iron at low production costs by using molten metal produced for casting blackheart malleable cast iron in an acidic cupola. [Means for solving the problem]
[0011] In a first embodiment, the present invention is directed to pearlitic malleable cast iron having, all by mass percentage, carbon of 2.80% or more and 3.25% or less, silicon of 1.35% or more and 1.60% or less, manganese of 0.55% or more and 0.70% or less, nitrogen of 0.0160% or more and 0.0250% or less, bismuth of 0.008% or more and 0.020% or less, and the balance being iron and unavoidable impurities.
[0012] The pearlitic malleable cast iron according to the present invention can stabilize cementite and generate pearlite with less additive amounts than in the prior art by simultaneously adding manganese, nitrogen, and bismuth, which are elements that inhibit graphitization. As a result, even if the sprue and runner are remelted, the same molten metal can be used to produce blackheart malleable cast iron and pearlitic malleable cast iron, improving the yield of raw materials.
[0013] In a second embodiment, the present invention is an invention of a method for producing pearlitic malleable cast iron, which includes the steps of melting raw materials to produce a molten metal, adding manganese nitride and bismuth to the molten metal, pouring the molten metal to which manganese nitride and bismuth have been added into a mold to cast a casting, and heat treating the casting, and the final product contains, by mass percentage, 2.80% to 3.80% carbon, 1.35% to 1.60% silicon, 0.55% to 0.70% manganese, 0.0160% to 0.0250% nitrogen, 0.008% to 0.020% bismuth, and the balance being iron and unavoidable impurities. The tensile strength of the pearlitic malleable cast iron can be adjusted by appropriately adjusting the heat treatment temperature. Effect of the Invention
[0014] According to the present invention, it is possible to selectively cast either blackheart malleable cast iron or pearlitic malleable cast iron using the same molten metal without adding any costly processes, so that the molten metal produced in the foundry can be used up without waste according to fluctuations in demand. Also, according to the present invention, it is not necessary to prepare molten metals with different compositions for castings of different materials, so it is possible to contribute to reducing the total manufacturing cost and saving energy resources. [Brief description of the drawings]
[0015] [Figure 1] 1 is a flowchart showing a method for producing pearlitic malleable cast iron according to the present invention. [Diagram 2] 1 is an optical microscope photograph showing an example of the metal structure of pearlitic malleable cast iron according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The modes for carrying out the present invention will be described below by dividing them into different embodiments. Note that the embodiments and examples of the present invention shown here are merely illustrative of specific modes for carrying out the present invention, and the present invention is not limited to these embodiments. In this specification, when expressing the composition of a metal or alloy, it is expressed in mass percentage unless otherwise specified. The symbol "% (percent)" means that the numerical value to which this symbol is attached is a composition expressed in mass percentage.
[0017] <First embodiment> In a first embodiment, the present invention is an invention of pearlitic malleable cast iron containing, all by mass percentage, 2.80% or more and 3.25% or less of carbon, 1.35% or more and 1.60% or less of silicon, 0.55% or more and 0.70% or less of manganese, 0.0160% or more and 0.0250% or less of nitrogen, 0.008% or more and 0.020% or less of bismuth, and the balance being iron and unavoidable impurities.
[0018] The pearlitic malleable cast iron according to the first embodiment contains carbon of 2.80% or more and 3.25% or less. When the carbon content is 2.80% or more, the melting point of the molten metal used for casting is about 1300°C or less, so there is no need to heat the raw material to a high temperature to produce the molten metal, and there is a tendency that large-scale melting equipment is not required. At the same time, the viscosity of the molten metal is also reduced, so the molten metal tends to flow more easily and can be easily poured into a casting mold. When the carbon content is 3.25% or less, there is a tendency that mottle is less likely to be generated during the solidification process after casting. Therefore, the carbon content is preferably 2.80% or more and 3.25% or less. A more preferable carbon content is 2.85% or more and 3.20% or less.
[0019] The pearlitic malleable cast iron according to the first embodiment contains silicon in an amount of 1.35% or more and 1.60% or less. When the silicon content is 1.35% or more, the effect of promoting graphitization by silicon is obtained, and graphitization tends to be completed in a short time in the first stage annealing. When the silicon content is 1.60% or less, the effect of promoting graphitization by silicon is not excessive, and mottle tends not to be generated in the solidification process after casting, and pearlite tends to be stabilized without being decomposed during heat treatment. Therefore, the silicon content is preferably 1.35% or more and 1.60% or less. More preferably, the silicon content is 1.40% or more and 1.50% or less. The heat treatment including the first stage annealing will be described in detail in the description of the second embodiment of the present invention described later.
[0020] The pearlitic malleable cast iron according to the first embodiment contains manganese at 0.55% or more and 0.70% or less. When the manganese content is 0.55% or more, in the cooling process after the second stage annealing in which the temperature of the casting is maintained at a temperature equal to or higher than the A1 transformation point, graphitization is inhibited by the action of manganese, and pearlite structures consisting of ferrite and cementite are easily formed. When the manganese content is 0.70% or less, the inhibition effect of graphitization by manganese is not excessive, so the formation of lumpy graphite in the first stage annealing is not hindered. Therefore, the manganese content is preferably 0.55% or more and 0.70% or less. More preferably, the manganese content is 0.60% or more and 0.70% or less.
[0021] The pearlitic malleable cast iron according to the first embodiment contains nitrogen at 0.0160% or more and 0.0250% or less. When the nitrogen content is 0.0160% or more, graphitization is inhibited by the action of nitrogen in the cooling process after the second stage annealing, and pearlite structures consisting of ferrite and cementite are easily formed. When the nitrogen content is 0.0250% or less, the graphitization inhibition effect of nitrogen is not excessive, so the formation of lumpy graphite in the first stage annealing is not hindered. Therefore, the nitrogen content is preferably 0.0160% or more and 0.0250% or less. More preferably, the nitrogen content is 0.0180% or more and 0.0220% or less.
[0022] The pearlitic malleable cast iron according to the first embodiment contains bismuth at 0.008% or more and 0.020% or less. When the bismuth content is 0.008% or more, graphitization is inhibited by the action of bismuth in the cooling process after the second stage annealing, and pearlite structures consisting of ferrite and cementite are easily formed. When the bismuth content is 0.020% or less, the graphitization inhibition effect of bismuth is not excessive, so the formation of massive graphite in the first stage annealing is not hindered. Therefore, the bismuth content is preferably 0.008% or more and 0.020% or less. The bismuth content is more preferably 0.010% or more and 0.015% or less.
[0023] The pearlitic malleable cast iron according to the first embodiment contains iron and inevitable impurities as the balance in addition to the above elements. Iron is the main element of pearlitic malleable cast iron. In the present invention, the term "unavoidable impurities" refers to impurities that are self-evidently present in cast iron without being intentionally introduced in the manufacturing process until the desired final product as cast iron is obtained, and that are unnecessary to be present, but are present in a small amount and do not necessarily have a negative effect on the properties of the cast iron, and are therefore left present. Specifically, for example, elements such as oxygen, chromium, sulfur, and titanium that are originally contained in the raw materials in small amounts, compounds such as oxides that are mixed in from the furnace wall that contacts the molten metal in the manufacturing process, and compounds such as oxides that are generated by the reaction of the molten metal with the atmospheric gas correspond to the inevitable impurities in the present invention. Of these inevitable impurities, sulfur is contained in large amounts in coke used as a heat source when preparing molten metal using a cupola. These unavoidable impurities do not significantly change the properties of pearlitic malleable cast iron even if they are contained in a total amount of 1.0% or less. The preferred total content of unavoidable impurities is 0.5% or less.
[0024] As shown in the examples described later, the content and the numerical range of each element contained in the pearlitic malleable cast iron according to the present invention are based on values measured by optical emission spectrometry. Optical emission spectrometry is a method for quantitatively analyzing the content of each element contained in a metal sample by applying electrical energy to the metal sample to cause a spark discharge and analyzing the intensity of the spectrum specific to each element contained in the light generated at that time. In the present invention, optical emission spectrometry is also applied to the analysis of molten metal obtained in the manufacturing process of pearlitic malleable cast iron.
[0025] In a preferred embodiment, the pearlitic malleable cast iron according to the first embodiment contains boron in mass percentage of 0.0030% or more and 0.0060% or less. By containing 0.0030% or more of boron simultaneously with nitrogen, the number of graphite grains crystallized at the grain boundaries of the austenite matrix in the first stage annealing increases, and the size of the massive graphite tends to become finer. When the number of graphite grains increases, the diffusion distance of carbon atoms required for graphite crystallization becomes shorter, so that the time required for graphitization in the first stage annealing can be shortened. When the boron content is 0.0060% or less, the action of nitrogen that inhibits graphitization is not hindered in the cooling process after the second stage annealing. Therefore, the boron content is preferably 0.0030% or more and 0.0060% or less. A more preferable boron content is 0.0040% or more and 0.0050% or less.
[0026] In the above preferred embodiment, the number of graphite particles increases due to the simultaneous inclusion of boron and nitrogen, and the mechanism is as follows. When cast iron is heated to a temperature of 800°C to 900°C, the boron and nitrogen dissolved in the cast iron are combined to form boron nitride. The boron nitride formed here is considered to be hexagonal boron nitride (h-BN), which is stable at normal pressure. Hexagonal boron nitride has a crystal structure similar to that of graphite. For this reason, it is considered that during graphitization, this boron nitride acts as a nucleus to cause a large number of graphite particles to precipitate finely. The above mechanism is speculated by the present inventor based on the experimental results obtained, and does not limit the technical scope of the present invention.
[0027] From the viewpoint of fully exerting the effects of boron and nitrogen, it is preferable to minimize the content of aluminum and / or titanium, which are more likely to bond with nitrogen than boron. For example, it is preferable to satisfy at least one of the conditions that the aluminum content is 0.10% or less and the titanium content is 0.020% or less.
[0028] In a preferred embodiment, the pearlitic malleable cast iron according to the first embodiment has a manganese-sulfur balance MS value expressed by the following formula, where Mn is the manganese content and S is the sulfur content, both expressed by mass percentage, of 0.30% or more and 0.60% or less.
[0029]
number
[0030] Manganese contained in the pearlitic malleable cast iron according to the present invention has the effect of inhibiting graphitization in the cooling process after the second stage annealing, and as a result, pearlite structures consisting of ferrite and cementite are easily formed. Sulfur is also an element that inhibits graphitization. As described above, when the molten metal is prepared using a cupola, the molten metal contains sulfur derived from the coke used as a heat source. In that case, the sulfur content in the molten metal is approximately 0.1%. However, when manganese is combined with sulfur to form manganese sulfide, the manganese and sulfur consumed thereby do not contribute to the inhibition of graphitization.
[0031] Therefore, in the above preferred embodiment, the manganese sulfur balance MS value, which corresponds to the remaining manganese content after subtracting the amount of manganese consumed by the formation of manganese sulfide, is set to 0.30% or more and 0.60% or less. In the above formula 1, the coefficient 1.7 related to the sulfur content S corresponds to the ratio of the atomic weight of manganese to the atomic weight of sulfur. When the manganese sulfur balance MS value is 0.30% or more, in the cooling process after the second stage annealing in which the temperature of the casting is maintained at a temperature equal to or higher than the A1 transformation point, graphitization is inhibited by the action of manganese, and pearlite structure consisting of ferrite and cementite is easily formed. When the MS value is 0.60% or less, the graphitization inhibition effect of manganese is not excessive, so the formation of lumpy graphite in the first stage annealing is not hindered. By adjusting the manganese content to 0.55% or more and 0.70% or less and adjusting the MS value to the above range, manganese can reliably exert its graphitization inhibition effect, and pearlite can be more reliably formed.
[0032] <Second embodiment> In a second embodiment, the present invention relates to a method for producing pearlitic malleable cast iron, which includes the steps of melting raw materials to produce a molten metal, adding manganese nitride and bismuth to the molten metal, pouring the molten metal to which manganese nitride and bismuth have been added into a mold to cast a casting, and heat treating the casting, and the final product contains, by mass percentage, 2.80% or more and 3.25% or less of carbon, 1.35% or more and 1.60% or less of silicon, 0.55% or more and 0.70% or less of manganese, 0.0160% or more and 0.0250% or less of nitrogen, 0.008% or more and 0.020% or less of bismuth, and the balance being iron and unavoidable impurities.
[0033] FIG. 1 is a flow chart showing a method for producing pearlitic malleable cast iron according to the second embodiment. The first step is a step (S1) of melting raw materials to produce molten metal. The raw materials used for melting can be a mixture of known raw materials such as pig iron produced in a blast furnace or scrap generated in a foundry or scrap iron collected from the market. Known means such as a continuous melting furnace represented by a cupola or a batch melting furnace represented by an electric furnace can be used to melt the raw materials. In general, it is more difficult to change the composition of the molten metal in a continuous melting furnace than in a batch melting furnace. According to the present invention, blackheart malleable cast iron and pearlitic malleable cast iron can be produced separately from the same molten metal, so that the effect of the present invention can be more effectively exerted in a continuous melting furnace than in a batch melting furnace. However, the means for melting the raw materials in the present invention is not limited to a continuous melting furnace.
[0034] The next step is the step (S2) of adding manganese nitride and bismuth to the molten metal. As described above, in the present invention, in order to inhibit the precipitation of graphite in the cooling process after the second annealing and form pearlite consisting of ferrite and cementite, a predetermined amount of manganese, nitrogen, and bismuth, which inhibit graphitization, are each contained. Among these elements, ferromanganese is often used in the prior art to add manganese. However, when only manganese is added as an element that inhibits graphitization, a very large amount of ferromanganese must be added to the molten metal. In this case, it takes time for the added ferromanganese to be uniformly dispersed in the molten metal, and there is a risk that the temperature of the molten metal will decrease during that time. Therefore, the molten metal must be once tapped into an electric furnace or the like, and manganese must be added while continuing to heat the molten metal so that the temperature does not decrease, which increases the production cost.
[0035] In the second embodiment, manganese nitride and bismuth are added to the molten metal. Manganese nitride is a compound containing manganese nitride. Manganese nitride is decomposed into manganese and nitrogen when heated in the molten metal. Both nitrogen and bismuth have a strong effect of inhibiting graphitization, so the amount of each of them to be added is smaller than when manganese is added alone. Therefore, it is possible to prepare a molten metal for casting with a desired composition by simply adding them to the molten metal tapped into a ladle.
[0036] Another method for adding nitrogen to the molten metal is to inject nitrogen gas into the molten metal through a gas injection tube or the like inserted into the molten metal. This method is suitable for adding nitrogen alone, but has the drawback that the temperature of the molten metal is lowered by injecting cold gas. In this regard, according to the method according to the second embodiment in which solid manganese nitride is added, it is possible to simultaneously add manganese and nitrogen, which are elements that inhibit graphitization, without lowering the temperature of the molten metal. It is preferable to use manganese nitride with as high a nitrogen content as possible for use in the second embodiment.
[0037] In the second embodiment, bismuth, which is added as an element that inhibits graphitization, can be added to the molten metal, for example, as a simple substance of bismuth. Manganese nitride and bismuth may be added to the molten metal simultaneously, or may be added separately at different times. The order in which manganese nitride and bismuth are added to the molten metal does not matter.
[0038] The next step is to pour the molten metal containing manganese nitride and bismuth into a mold to produce a casting (S3). In the present invention, the term "casting" refers to a block of cast iron that is cast as-cast using a mold and has not yet been heat-treated. Sand molds and other known molds can be used for casting.
[0039] The next and final step is a step (S4) of heat treating the casting. The heat treatment step in the second embodiment includes a first stage annealing step for decomposing free cementite contained in the casting to produce austenite and graphite, and a second stage annealing step that is performed following the first stage annealing step for decomposing pearlite cementite and crystallizing supersaturated carbon in the austenite as graphite.
[0040] The temperature at which the first stage annealing is carried out is preferably 950° C. or more and 1100° C. or less. A more preferable temperature range is 980° C. or more and 1030° C. or less. As described above, in a preferred embodiment, the time for carrying out the first stage annealing in the method for producing pearlitic malleable cast iron according to the second embodiment can be significantly shortened compared to the conventional technology due to the effects of nitrogen and boron. Specifically, at most 3 hours, typically 1 hour or less, is sufficient.
[0041] The temperature for the second stage annealing is preferably a temperature near the A1 transformation point, and for example, the temperature can be slowly lowered over time from 760°C to 720°C. The preferred start temperature for the second stage annealing is 740°C or higher and 780°C or lower. The preferred end temperature is 680°C or higher and 720°C or lower. As shown in the examples described later, the temperature may be held at a constant temperature of 760°C or higher and 780°C or lower in order to increase the cooling rate after the second stage annealing. As with the time for the first stage annealing, the time for the second stage annealing can also be significantly shortened compared to the conventional technology due to the action of nitrogen and boron. Specifically, at most 3 hours, typically 1 hour or less, is sufficient.
[0042] In the second embodiment, the casting is quenched after the second stage annealing to form pearlite from austenite. The final form of the casting after this process is composed of massive graphite formed in the first stage annealing and the second stage annealing, and a matrix made of pearlite. Ferrite containing almost no carbon may be formed around the massive graphite. The cooling rate of the casting after the second stage annealing can be, for example, so-called air cooling, which is performed by forcibly blowing outside air. This is because cementite is preferentially crystallized instead of graphite even if the casting is not quenched so quickly, since the casting contains an element that inhibits graphitization.
[0043] In the second embodiment, after the second annealing and the subsequent cooling, a heat treatment for improving the material properties may be added as necessary. Specifically, for example, tempering may be performed to increase the toughness.
[0044] In the second embodiment, the final product contains, by mass percentage, 2.80% or more and 3.25% or less of carbon, 1.35% or more and 1.60% or less of silicon, 0.55% or more and 0.70% or less of manganese, 0.0160% or more and 0.0250% or less of nitrogen, 0.008% or more and 0.020% or less of bismuth, and the balance is iron and unavoidable impurities. In the present invention, the "final product" refers to a product at a stage where all manufacturing steps are completed and the product is put to practical use. The manufacturing process includes all steps from S1 to S4 described above, but other steps may also be included in the manufacturing process.
[0045] In principle, the content of each element in the final product can be known by analyzing the chemical composition of a sample taken from the final product. However, if the chemical composition of a sample taken from the molten metal or a sample taken from the casting before heat treatment is substantially the same as that of the final product, the analytical values of the chemical composition of these samples can be used instead of the analytical values of the final product. The effects of the inclusion of each element in the final product and the reasons for specifying the upper and lower limits of the content are the same as those in the explanation of the components of the pearlitic malleable cast iron according to the first embodiment described above, and therefore will not be explained here.
[0046] In a preferred embodiment, the manufacturing method of pearlitic malleable cast iron according to the second embodiment is such that the final product contains boron in mass percentage of 0.0030% or more and 0.0060% or less. In this preferred embodiment, the content of boron contained in the casting can be adjusted, for example, by adding ferroboron to the molten metal. The effect of containing boron and the reason for specifying the upper and lower limits of the content are the same as those described above in relation to the preferred components of the pearlitic malleable cast iron according to the first embodiment, and therefore will not be described here.
[0047] In a preferred embodiment, in the manufacturing method of pearlitic malleable cast iron according to the second embodiment, when the manganese content and sulfur content contained in the casting, expressed as mass percentage in the final product, are taken as Mn and S, respectively, the manganese-sulfur balance MS value, expressed by the following formula, is 0.30% or more and 0.60% or less.
[0048]
number
[0049] In this preferred embodiment, the manganese content in the casting can be adjusted, for example, by adding manganese nitride or the like to the molten metal according to the content of sulfur in the molten metal based on the mathematical formula 1. The reasons for specifying the upper and lower limits of the value of the manganese-sulfur balance MS are the same as those explained in the explanation of the preferred components of the pearlitic malleable cast iron according to the above-mentioned first embodiment, and therefore will not be explained here. EXAMPLES
[0050] <First Example> Raw materials and coke were alternately fed into the furnace from above, where an acidic cupola was used as the furnace material, and stacked. Hot air was blown into the furnace to burn the coke and continuously melt the raw materials. The molten metal obtained by melting was tapped into a ladle at regular intervals. The weight of the molten metal tapped into the ladle in one tapping run was approximately 700 kg. The temperature of the molten metal at the time of tapping was approximately 1500°C. The results of an analysis of the composition of the molten metal in the ladle are shown in Table 1. The molten metal contained 0.4% manganese derived from the iron raw material.
[0051] [Table 1]
[0052] Next, 2.2 kilograms of manganese nitride and 200 grams of bismuth were added to 700 kilograms of molten metal in the ladle as shown in Table 2, and the molten metal was stirred and then poured into a mold for test pieces to cast a number of test pieces. The nitrogen content of manganese nitride was 28%. The amount of manganese nitride added was a weight that could be added to the molten metal in the ladle. All of the cast test pieces were heated to 980°C and held for about two and a half hours to perform the first stage annealing, and then the temperature was lowered to 760°C, and the second stage annealing was performed while slowly cooling from there to 700°C over about two and a half hours, and then air-cooled to obtain the test piece of Example 1.
[0053] Next, as shown in Table 2, test pieces of Example 2 were prepared under the same conditions as in Example 1, except that the weight of bismuth charged into the ladle was changed to 310 grams.
[0054] [Table 2]
[0055] A sample for component analysis was taken from a part of the obtained test piece and analyzed. The analysis of chemical components was performed using a light emission analyzer (Shimadzu Corporation, model number: PDA-7000) using a sample whose surface had been polished in advance. The average value of two measurements was used as the analytical value. The results of the component analysis are shown in the columns for Example 1 and Example 2 in Table 3.
[0056] [Table 3]
[0057] Next, a sample for metal structure observation was prepared from a part of the obtained test piece, and an optical microscope image was taken to visually observe the ratio of pearlite in the matrix. In addition, the Rockwell hardness was measured using the surface of the same sample as a guide for the ratio of pearlite in the matrix. The higher the ratio of pearlite, the higher the Rockwell hardness value. The Rockwell hardness was measured using a B scale using a ball indenter. Furthermore, a sample for tensile testing was prepared from the remaining test piece, and the tensile strength, 2% proof stress, and elongation were measured. These results are shown in the columns for Example 1 and Example 2 in Table 4.
[0058] [Table 4]
[0059] Next, as a comparative example, as shown in Table 2, ferroboron was added in place of bismuth to the ladle, and the same amount of manganese nitride as in Example 1 was added, and casting and heat treatment were performed under the same conditions as in Example 1 to obtain a test piece of Comparative Example 1. The obtained test piece was evaluated under the same conditions as in Example 1, and the results are shown in the column of Comparative Example 1 in Tables 3 and 4. The content of boron contained in ferroboron was 18%. Also, as shown in Table 2, except that both bismuth 200 grams and ferroboron 160 grams were added, the same amount of manganese nitride as in Example 1 was added, and casting and heat treatment were performed under the same conditions as in Example 1 to obtain a test piece of Comparative Example 2. The obtained test piece was evaluated under the same conditions as in Example 1, and the results are shown in the column of Comparative Example 2 in Tables 3 and 4.
[0060] From the above results, it can be seen that according to the present invention, which adds manganese nitride and bismuth, pearlitization proceeds even with a small amount of manganese added compared to the conventional method of adding ferromanganese, and therefore it can be easily added to the molten metal in the ladle. This is thought to be because both manganese and nitrogen have the effect of stabilizing cementite and improving the pearlite ratio. As a result, the manganese content is reduced, making it possible to remelt and reuse the scraps.
[0061] It is also found that the pearlite ratio is highest and a tensile strength exceeding 500 Newtons per square millimeter is obtained in Examples 1 and 2, in which bismuth is added simultaneously with manganese nitride. This is believed to be because bismuth not only inhibits the precipitation of graphite during casting, but also contributes to the stabilization of cementite after solidification is complete.
[0062] On the other hand, in Comparative Example 1 and Comparative Example 2, in which ferroboron was added simultaneously with manganese nitride, it was found that the pearlite ratio estimated from the Rockwell hardness and the tensile strength also decreased compared to Example 1. This is believed to be because boron nitride, which is a combination of boron and nitrogen, is formed after solidification is complete, and this acts as a nucleus to promote the precipitation of graphite, while the amount of nitrogen, which dissolves in the matrix and inhibits graphitization, decreases, resulting in a decrease in the pearlite ratio.
[0063] <Second Example> A test piece cast using a molten metal whose components were adjusted to the same composition as in Example 1 in Table 2 of the first embodiment was heated to 980°C and held for about 2 hours to perform the first stage annealing, and then the temperature was lowered to 760°C, and the second stage annealing was performed while slowly cooling from there to 720°C over about 2 hours, and then air-cooled to obtain a test piece of Example 3. In addition, annealing was performed under the same conditions as in Example 3 except that the second stage annealing was performed by holding at 760°C and 780°C for about 2 hours, to obtain test pieces of Examples 4 and 5. The results of measuring the Rockwell hardness evaluation, tensile strength, 2% proof stress, and elongation of these test pieces under the same conditions as in the first embodiment are shown in Table 5.
[0064] [Table 5]
[0065] FIG. 2 is an optical microscope image of the sample of Example 5. The black lumpy precipitates are free graphite formed during the first and second annealing stages. The lumpy graphite phases are approximately the same size and are uniformly dispersed in the matrix. The gray parts of the matrix are pearlite formed by a eutectoid reaction from austenite due to rapid cooling after the second annealing stage. The spacing between the lamellar layers in the pearlite is so fine that it cannot be seen at the magnification of this image. The white parts of the matrix are ferrite. The ferrite phase is present in large amounts around the graphite phase.
[0066] Next, as a comparative example, annealing was performed under the same conditions as in Example 3 except that the holding temperature in the second stage annealing was changed to 800°C, to obtain a test piece for Comparative Example 3. The Rockwell hardness evaluation, tensile strength, 2% proof stress, and elongation of this test piece were measured under the same conditions as in the first example, and the results are shown in the column for Comparative Example 3 in Table 5.
[0067] From the above results, it can be seen that in the present invention in which manganese nitride and bismuth are added, by increasing the temperature of the second stage annealing, a tensile strength exceeding 600 Newtons per square millimeter can be obtained. This is believed to be because the higher the temperature of the second stage annealing, the faster the cooling rate during the subsequent air cooling, and the narrower the spacing of the pearlite lamellar layers. On the other hand, in Comparative Example 3 in which the temperature of the second stage annealing was 800°C, it was found that there was almost no improvement in tensile strength compared to Example 3, and the elongation decreased and the toughness decreased. This is believed to be because residual stress was generated by rapid cooling from a high temperature that greatly exceeds the A1 transformation point. Therefore, it can be seen that the temperature range for performing the second stage annealing is preferably 760°C or higher and 780°C or lower.
Claims
1. All are mass percentages. Carbon: 2.80% or more, 3.25% or less; Silicon: 1.35% or more, 1.60% or less; Manganese: 0.55% or more, 0.70% or less; Nitrogen: 0.0160% or more, 0.0250% or less; Contains bismuth at 0.008% or more and 0.020% or less, The balance is iron and unavoidable impurities. Pearlitic malleable iron.
2. The boron content is 0.0030% or more and 0.0060% or less by mass percentage.
2. The pearlitic malleable cast iron according to claim 1.
3. When the manganese content expressed by mass percentage is Mn and the sulfur content is S, the manganese-sulfur balance MS value expressed by the following formula is 0.30% or more and 0.60% or less.
2. The pearlitic malleable cast iron according to claim 1. [0010]
4. A step of melting raw materials to produce a molten metal; adding manganese nitride and bismuth to the molten metal; A step of pouring the molten metal containing the manganese nitride and bismuth into a mold to cast a casting; and heat treating the casting, The final product is Carbon: 2.80% or more, 3.25% or less; Silicon: 1.35% or more, 1.60% or less; Manganese: 0.55% or more, 0.70% or less; Nitrogen: 0.0160% or more, 0.0250% or less; Contains bismuth at 0.008% or more and 0.020% or less, A method for producing pearlitic malleable cast iron, the balance being iron and unavoidable impurities.
5. The final product contains boron by mass percentage of 0.0030% or more and 0.0060% or less. The method for producing pearlitic malleable cast iron according to claim 4.
6. In the final product, when the manganese content expressed by mass percentage is Mn and the sulfur content is S, the manganese-sulfur balance MS value expressed by the following formula is 0.30% or more and 0.60% or less. A method for producing the pearlitic malleable cast iron according to claim 1. [0010]
Citation Information