Silicon clathrate electrode active material, negative electrode mixture, negative electrode active material layer, solid-state lithium-ion battery

A silicon clathrate electrode active material with controlled oxygen content and a clathrate type II structure, integrated with a solid electrolyte, addresses the issue of charging expansion, improving solid lithium ion battery performance.

JP2024162152APending Publication Date: 2024-11-21TOYOTA JIDOSHA KK +1

Patent Information

Application Number
JP2023077431
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Silicon clathrate electrode active materials, while suppressing expansion during charging, still require further reduction in expansion to enhance battery performance.

Method used

A silicon clathrate electrode active material containing a specific range of oxygen atoms (0% to 19.4% by mass, preferably 3.3% to 7.0% by mass) with a clathrate type II structure, combined with a solid electrolyte, conductive additives, and a binder, forms a negative electrode composite material that reduces charging expansion.

Benefits of technology

The solution results in a silicon clathrate electrode active material with significantly reduced expansion during charging, enhancing the performance of solid lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162152000001_ABST
    Figure 2024162152000001_ABST
Patent Text Reader

Abstract

To provide a silicon clathrate electrode active material that exhibits low expansion during charging, and a solid-state lithium ion battery having such a silicon clathrate electrode active material.SOLUTION: A silicon clathrate electrode active material according to the present disclosure contains more than 0 mass% and less than 19.4 mass% of oxygen atoms. A solid-state lithium ion battery according to the present disclosure includes a negative electrode active material layer according to the present disclosure. The negative electrode active material layer according to the present disclosure includes a negative electrode mixture according to the present disclosure. The negative electrode mixture according to the present disclosure includes the silicon clathrate electrode active material according to the present disclosure and a solid electrolyte.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a silicon class rate electrode active material, a negative electrode composite material, a negative electrode active material layer, and a solid lithium ion battery.

Background Art

[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Also, silicon is known as an electrode active material used in batteries, particularly lithium ion batteries.

[0003] The silicon electrode active material has a large theoretical capacity and is effective for increasing the energy density of the battery. On the other hand, the silicon electrode active material has a problem of large expansion during charging. In contrast, it is known that the use of a silicon class rate electrode active material as the silicon electrode active material suppresses the expansion during charging.

[0004] For example, Patent Document 1 discloses a silicon class rate electrode active material having a silicon class rate type II crystal phase and having a composition of Na x Si 136 (1.98 < x < 2.54). Patent Document 2 discloses a silicon class rate electrode active material having a silicon class rate type II crystal phase, having voids inside the primary particles, and having a void volume of voids with a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0006] Although silicon clathrate electrode active materials can suppress expansion during charging as compared with ordinary silicon electrode active materials, there is a demand for further suppression of the expansion of silicon clathrate electrode active materials during charging.

[0007] An object of the present disclosure is to provide a silicon clathrate electrode active material that exhibits small expansion during charging, and a solid-state lithium-ion battery having such a silicon clathrate electrode active material. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A silicon clathrate electrode active material containing more than 0 mass% and less than 19.4 mass% oxygen atoms. <Aspect 2> 2. The silicon clathrate electrode active material according to embodiment 1, comprising 2.0% by mass or more of oxygen atoms. <Aspect 3> 3. The silicon clathrate electrode active material of embodiment 2, comprising 3.3% by mass or more and 7.0% by mass or less of oxygen atoms. <Aspect 4> 2. The silicon clathrate electrode active material of embodiment 1, having at least partially a clathrate II type structure. <Aspect 5> 2. A negative electrode composite comprising the silicon clathrate electrode active material of embodiment 1 and a solid electrolyte. <Aspect 6> 6. The anode composite of claim 5, wherein the solid electrolyte is a sulfide solid electrolyte. Aspect 7 A negative electrode active material layer comprising the negative electrode mixture according to embodiment 5. <Aspect 8> A solid-state lithium ion battery having the anode active material layer of embodiment 7. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a silicon clathrate electrode active material that exhibits small expansion during charging, and a solid-state lithium ion battery having such a silicon clathrate electrode active material. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a graph showing the relationship between the oxygen atomic amount and the expansion amount of the silicon clathrate electrode active materials of Examples 1 to 5 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0012] Silicon clathrate electrode active material The silicon clathrate electrode active material of the present disclosure contains more than 0 mass % and less than 19.4 mass % of oxygen atoms.

[0013] The present inventors have unexpectedly discovered that a silicon clathrate electrode active material containing a predetermined amount of oxygen atoms exhibits small expansion during charging.

[0014] The reason for this is presumed to be as follows, without intending to be bound by any theory. That is, although the lithium ion conductivity of the silicon clathrate electrode active material is low, if a moderate amount of oxygen atoms are present in the silicon clathrate electrode active material, silicon oxide reacts with lithium to form an ion conductor such as lithium silicate, and the ion conductivity of the silicon clathrate electrode active material increases, so that the charging reaction proceeds uniformly and the expansion during charging is suppressed. In addition, since an excessive amount of oxygen atoms is not present in the silicon clathrate electrode active material, electrical conductivity is not hindered, and the charging reaction proceeds uniformly and the expansion during charging is suppressed.

[0015] In the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".

[0016] The silicon clathrate electrode active material of the present disclosure contains more than 0 mass % and less than 19.4 mass % of oxygen atoms. If the amount of oxygen atoms is within the above range, it is preferable for adequately suppressing expansion during charging.

[0017] The silicon clathrate electrode active material may contain oxygen atoms in an amount of 1.0 mass% or more, 2.0 mass% or more, 2.5 mass% or more, 2.7 mass% or more, 2.9 mass% or more, 3.0 mass% or more, 3.1 mass% or more, 3.2 mass% or more, or 3.3 mass% or more, or 15.0 mass% or less, 10.0 mass% or less, 9.0 mass% or less, 8.0 mass% or less, or 7.0 mass% or less. That is, it is particularly preferable that the silicon clathrate electrode active material contains oxygen atoms in an amount of 3.3 mass% or more and 7.0 mass% or less. When the amount of oxygen atoms is within the above range, the expansion during charging can be further reduced.

[0018] The method for measuring the amount of oxygen atoms is not particularly limited, but examples include elemental analysis using an oxygen / nitrogen / hydrogen analyzer, and calculation from analytical values ​​by EDX, XPS, etc. Specifically, for this measurement, EMGA-930 manufactured by Horiba, Ltd. can be used as the oxygen / nitrogen / hydrogen analyzer.

[0019] The silicon clathrate electrode active material of the present disclosure may at least partially have a clathrate II structure, which can further reduce expansion during charging.

[0020] In order to adjust the ratio of oxygen atoms in the silicon clathrate electrode active material, the silicon clathrate electrode active material can be subjected to an oxidation treatment and an oxygen removal treatment.

[0021] As a specific example of the oxidation treatment, the silicon clathrate electrode active material can be placed in an oxidizing atmosphere and optionally heated.

[0022] In addition, examples of the oxygen removal treatment include reduction treatment and silicon oxide removal treatment. The silicon oxide removal treatment can be performed by immersing the silicon clathrate electrode active material in a solution capable of dissolving and removing silicon oxide, for example, a hydrogen fluoride aqueous solution. In addition, when the silicon clathrate electrode active material has lithium silicate (Li2SiO3), it is also possible to convert the lithium silicate into soluble silicic acid (H2SiO3) using a hydrogen chloride aqueous solution (hydrochloric acid), and remove this silicic acid to reduce the oxygen atoms in the silicon clathrate electrode active material (Li2SiO3 + 2HCl → 2LiCl (dissolved) + H2SiO3 (dissolved)).

[0023] Furthermore, by carrying out an oxidation treatment before the silicon oxide removal treatment using a solution capable of dissolving and removing silicon oxide, it is possible to promote the removal of oxygen in the subsequent oxygen removal treatment.

[0024] 《Negative electrode mixture》 The negative electrode mixture of the present disclosure includes a silicon clathrate electrode active material and a solid electrolyte, and optionally includes a conductive additive and a binder.

[0025] In the present disclosure, the term "negative electrode mixture" refers to a composition that can form a negative active material layer as it is or by further containing other components. In the present disclosure, the term "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can be applied and dried to form a negative electrode active material layer.

[0026] <Silicon clathrate electrode active material> For the silicon clathrate electrode active material, reference may be made to the above description of the silicon clathrate electrode active material of the present disclosure.

[0027] <Solid electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte, an oxide solid electrolyte, a polymer electrolyte, or the like, and is preferably a sulfide solid electrolyte.

[0028] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0029] An example of an oxide solid electrolyte is Li7La3Zr2O 12 , Li 7-x La3Zr 1-x Nb x O 12 , Li 7-3x La3Zr2Al x O 12 , Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4, or Li 3+x PO 4-x N x (LiPON), but is not limited to these.

[0030] The sulfide solid electrolyte and the oxide solid electrolyte may be glass or crystallized glass (glass ceramic).

[0031] Examples of the polymer electrolyte include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.

[0032] The mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode mixture (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0033] <Conductive assistant> The conductive additive is not particularly limited. For example, the conductive additive may be a carbon material such as VGCF (Vapor Grown Carbon Fiber) and carbon nanofiber, a metal material, or the like, but is not limited thereto.

[0034] <binder> The binder is not particularly limited. For example, the binder may be, but is not limited to, a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), or styrene butadiene rubber (SBR), or a combination thereof.

[0035] 《Negative electrode active material layer》 The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. For the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referenced.

[0036] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.

[0037] Solid-state lithium-ion battery The solid-state lithium ion battery of the present disclosure has the negative electrode active material layer of the present disclosure. The solid-state lithium ion battery of the present disclosure may have, in this order, a negative electrode current collector layer, a negative electrode active material layer of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer. Furthermore, the lithium ion battery of the present disclosure may be restrained by restraining members such as end plates from both sides in the stacking direction of each of the layers.

[0038] In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Also, the solid-state battery of the present disclosure may be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.

[0039] In the lithium ion battery of the present disclosure, the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, and therefore expansion due to charging is reduced, thereby suppressing an increase in confining pressure due to charging.

[0040] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, the material may be stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, a resin current collector, or the like, but is not limited to these.

[0041] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0042] <Negative electrode active material layer> For the negative electrode active material layer, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.

[0043] <Solid electrolyte layer> The solid electrolyte layer includes at least a solid electrolyte. In addition to the solid electrolyte, the solid electrolyte layer may include a binder, etc., as necessary. For the solid electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.

[0044] The solid electrolyte layer may be impregnated with an electrolyte solution having lithium ion conductivity.

[0045] The electrolyte preferably contains an electrolyte supporting salt and a solvent. Examples of the electrolyte supporting salt (lithium salt) having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3. Examples of the solvent used in the electrolyte include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolyte preferably contains two or more solvents.

[0046] The thickness of the solid electrolyte layer is, for example, 0.1 to 1000 μm. The thickness of the solid electrolyte layer is preferably 0.1 to 300 μm, and particularly preferably 0.1 to 100 μm.

[0047] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.

[0048] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li1+x Mn 2-x-y M y The material may be, but is not limited to, a Li-Mn spinel substituted with a different element having a composition represented by O4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn).

[0049] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.

[0050] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0051] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.

[0052] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0053] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0054] <Positive electrode current collector layer> The material and shape of the positive electrode current collector layer are not particularly limited, and the above description of the negative electrode active material layer of the present disclosure can be referred to. In particular, the material of the positive electrode current collector layer is preferably aluminum. The shape is preferably a foil. EXAMPLES

[0055] 《Synthesis of silicon clathrate electrode active material》 <Alloying> Example 1 As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon alloy. The obtained lithium silicon alloy was reacted with ethanol in an argon atmosphere to obtain a powder having voids inside the primary particles, i.e., a Si powder having a porous structure.

[0056] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0057] <Clathrate formation> The obtained NaSi alloy and aluminum fluoride (AlF3) were weighed out to a molar ratio of 1:0.35, and the weighed NaSi alloy and AlF3 were mixed with a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 310 ° C for 60 hours to obtain a reaction product containing silicon clathrate. The obtained reaction product was placed in a device capable of reducing pressure and replacing gas, and the inside of the device was reduced in pressure at room temperature, and then the air was introduced to oxidize it. The oxidized reaction product was acid-washed using a mixed solvent of HNO3 and H2O mixed in a volume ratio of 10:90 to remove by-products in the reaction product. After washing, it was filtered, and the filtered solid was dried at 120 ° C for 3 hours or more to obtain a powdered silicon clathrate electrode active material. The obtained silicon clathrate electrode active material was further treated with a 3 wt % HF solution at 25° C. for 3 hours, filtered, and then dried at 120° C. for 3 hours or more to obtain the silicon clathrate electrode active material of Example 1.

[0058] Example 2 A silicon clathrate electrode active material of Example 2 was obtained in the same manner as in Example 1, except that oxidation in the clathrate formation was not carried out.

[0059] Example 3 A silicon clathrate electrode active material of Example 3 was obtained in the same manner as in Example 1, except that in the clathrate formation, air was introduced to oxidize the material so that the amount of air inflow was 1 / 100 of that in Example 1.

[0060] Example 4 A silicon clathrate electrode active material of Example 4 was obtained in the same manner as in Example 2, except that the silicon clathrate electrode active material was treated with a hydrogen chloride (HCl) solution.

[0061] Example 5 A silicon clathrate electrode active material of Example 5 was obtained in the same manner as in Example 2, except that the silicon clathrate electrode active material was treated with an HF solution at 0°C.

[0062] Comparative Example 1 A silicon clathrate electrode active material of Comparative Example 1 was obtained in the same manner as in Example 2, except that the silicon clathrate electrode active material was not treated with the HF solution.

[0063] The silicon clathrate electrode active material in each example had a clathrate II type crystal phase.

[0064] 《Making a lithium-ion battery》 Using the silicon clathrate electrode active material of each example, a lithium ion battery of each example was produced as follows.

[0065] <Preparation of negative electrode mixture> Butyl butyrate, a 5 wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, vapor grown carbon fiber (VGCF) as a conductive additive, the synthesized silicon clathrate electrode active material, and Li2S-P2S5 glass ceramic as a sulfide solid electrolyte were added to a polypropylene container, and the mixture was stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry).

[0066] <Formation of negative electrode active material layer> The obtained negative electrode composite slurry was applied onto a copper (Cu) foil serving as a negative electrode current collector layer by the blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C to form a negative electrode active material layer on the negative electrode current collector layer.

[0067] <Formation of solid electrolyte layer> Heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li2SP2S5-based glass ceramic as a sulfide solid electrolyte were added to a polypropylene container and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.

[0068] The obtained solid electrolyte slurry was applied onto an aluminum (Al) foil as a release sheet by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100°C to form a solid electrolyte layer. Three solid electrolyte layers were produced.

[0069] Preparation of Positive Electrode Mixture A polypropylene container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and VGCF as a conductive additive were added to a container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT).

[0070] Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), further stirred with an ultrasonic disperser for 30 seconds, and shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).

[0071] <Formation of Positive Electrode Active Material Layer> The obtained positive electrode mixture slurry was applied onto an Al foil serving as a positive electrode current collector layer by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C, thereby forming a positive electrode active material layer on the positive electrode current collector layer.

[0072] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.

[0073] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.

[0074] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.

[0075] The positive electrode laminate and the negative electrode laminate were laminated on top of each other so that the solid electrolyte layer of each laminate faced the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed at a pressure of 200 MPa and a press temperature of 120° C. for 1 minute, thereby obtaining an all-solid-state battery.

[0076] "evaluation" <Oxygen atomic weight> The amount of oxygen atoms was calculated from the analytical value by elemental analysis using an oxygen / nitrogen / hydrogen analyzer (Horiba, Ltd., EMGA-930).

[0077] <Expansion amount> The all-solid-state battery of each example was restrained at a predetermined restraining pressure using a restraining jig, and the amount of restraining pressure fluctuation was measured when constant current / constant voltage charging was performed up to 4.55 V at a 10-hour rate (1 / 10C). This amount of restraining pressure fluctuation was taken as the amount of expansion in this disclosure. The amount of restraining pressure fluctuation is the difference between the maximum and minimum values ​​of the restraining pressure, and the values ​​of the examples are shown as relative values ​​when the value of Comparative Example 1 is taken as 100.

[0078] "result" The amount of oxygen atoms in the silicon clathrate electrode active material and the amount of expansion of the silicon clathrate electrode active material for each example are shown in Table 1 and FIG.

[0079] [Table 1]

[0080] As shown in Table 1 and FIG. 1, the batteries of Examples 1 to 5, in which the oxygen atomic amount in the silicon clathrate electrode active material was within the range of the present disclosure, had smaller expansion amounts than the battery of Comparative Example 1.

Claims

1. A silicon clathrate electrode active material containing more than 0 mass% and less than 19.4 mass% oxygen atoms.

2. The silicon clathrate electrode active material according to claim 1 , containing 2.0 mass % or more of oxygen atoms.

3. The silicon clathrate electrode active material according to claim 2 , containing 3.3 mass % or more and 7.0 mass % or less of oxygen atoms.

4. 2. The silicon clathrate electrode active material of claim 1 having at least partially a clathrate II type structure.

5. A negative electrode mixture comprising the silicon clathrate electrode active material according to claim 1 and a solid electrolyte.

6. 6. The negative electrode mixture of claim 5, wherein the solid electrolyte is a sulfide solid electrolyte.

7. A negative electrode active material layer comprising the negative electrode mixture according to claim 5 .

8. A solid-state lithium ion battery comprising the negative electrode active material layer according to claim 7.

Citation Information

Patent Citations

  • Negative electrode active material containing silicon clathrate ii

    CN112447972A

  • Negative electrode active material including silicon clathrate ii

    JP2021034279A

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158004A

  • All-solid battery

    JP2022092723A

  • Porosity carbon-silicon composite microspheres for anode active material, Manufacturing method thereof and lithium secondary battery comprising the same

    KR101785064B1

Cited By

  • Method for manufacturing silicon clathrate electrode active material, and method for manufacturing lithium-ion battery

    JP2024165116A

  • Method for manufacturing silicon clathrate electrode active material and method for manufacturing lithium ion battery

    JP7782511B2