Thermal recording medium
A heat-sensitive recording material with N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea and dimethyl terephthalate, combined with an undercoat layer, addresses heat resistance and printability issues, providing improved performance in high-temperature environments.
Patent Information
- Application Number
- JP2023077910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermal recording materials lack sufficient heat resistance, head matching properties, and printability, with existing technologies not adequately addressing these requirements, particularly in high-temperature environments.
A heat-sensitive recording material comprising a heat-sensitive recording layer with N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea as a color developer, dimethyl terephthalate as a sensitizer, and optionally ethylene bisstearamide as a wax, along with an undercoat layer containing hollow particles for improved heat insulation, is developed.
The material exhibits excellent heat resistance, head matching properties, and printability, with enhanced blank paper storage stability and reduced background fogging, even in high-temperature conditions.
Smart Images

Figure 2024162422000001 
Figure 2024162422000002 
Figure 2024162422000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosensitive recording medium. [Background technology]
[0002] Thermosensitive recording media that record color images by utilizing the thermal coloring reaction between colorless or light-colored leuco dyes and phenols or organic acids have been widely used. Such thermosensitive recording media have the advantages of being compact, easy to maintain, and quiet, because color images are formed simply by heating. For this reason, thermosensitive recording media are widely used as various information recording materials in issuing machines such as label printers, automatic ticket vending machines, CD / ATMs, order slip output machines for restaurants, data output machines for scientific research equipment, etc.
[0003] However, as the range of applications expands, the performance and quality required are becoming more diverse. For example, there is a demand for thermal recording media that are excellent in heat resistance, head matching properties and printability.
[0004] As a method for obtaining a thermal recording material having excellent thermal response and storage stability in the background and image areas, it has been proposed to use at least one salicylic acid derivative or a metal salt thereof as an electron accepting compound, and at least one compound selected from 2-benzyloxynaphthalene, 4-benzylbiphenyl, diphenyl adipate, dimethyl terephthalate, 1,2-bis(3,4-dimethylphenyl)ethane, bis(4-methylbenzyl)oxalate, and 1,2-bis(3-methylphenoxy)ethane, and an aliphatic amide compound having 18 or more carbon atoms in its molecule (Patent Document 1). However, in Patent Document 1, the condition for the heat resistance test of the background area is a low temperature of 60°C, and there is room for improvement in heat resistance. In addition, the head matching property and printability are not evaluated. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-108765 Summary of the Invention [Problem to be solved by the invention]
[0006] A primary object of the present invention is to provide a thermosensitive recording medium having excellent heat resistance, head matching properties and printability. [Means for solving the problem]
[0007] The present inventors have intensively studied the above-mentioned prior art and have come to solve the above-mentioned problems. That is, the present invention relates to the following thermosensitive recording medium.
[0008] Item 1: A thermal recording medium having a thermal recording layer containing at least a leuco dye, a developer and a sensitizer on a support, the thermal recording medium containing N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea as the developer and dimethyl terephthalate as the sensitizer. Item 2: The thermosensitive recording material according to Item 1, wherein the thermosensitive recording layer contains ethylene bisstearic acid amide as a wax. Item 3: The thermosensitive recording material according to item 1 or 2, wherein the thermosensitive recording layer contains clay as an inorganic pigment. Item 4: The thermosensitive recording material according to any one of Items 1 to 3, which has an undercoat layer between the support and the thermosensitive recording layer. Effect of the Invention
[0009] The thermal recording medium of the present invention is excellent in heat resistance, head matching property and printability. In addition, the blank paper storage stability is at a level that does not cause any practical problems. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In this specification, the expression "comprise" includes the concepts of "comprise", "consist essentially of" and "consist only of".
[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits.
[0012] The latex in the present invention includes a gel or a dried film state formed by drying a dispersion medium.
[0013] The present invention is characterized in that, in a thermosensitive recording medium having a thermosensitive recording layer on a support, which contains at least a leuco dye, a developer and a sensitizer, the developer is N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea and the sensitizer is dimethyl terephthalate.
[0014] [Support] The support in the present invention is not particularly limited in type, shape, size, etc., and can be appropriately selected from, for example, high-quality paper (acid paper, neutral paper), medium-quality paper, coated paper, art paper, cast-coated paper, glassine paper, resin-laminated paper, polyolefin-based synthetic paper, synthetic fiber paper, nonwoven fabric, synthetic resin film, and various transparent supports. The thickness of the support is not particularly limited, and is usually about 20 to 200 μm. The density of the support is not particularly limited, and is 0.60 to 0.85 g / cm. 3 degree is preferred.
[0015] [Thermal recording layer] (Leuco dye) The heat-sensitive recording layer of the heat-sensitive recording medium of the present invention may contain various known colorless or light-colored leuco dyes. Specific examples of such leuco dyes are given below.
[0016] Specific examples of leuco dyes include blue-coloring dyes such as 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-methylphenyl)-3-(4-dimethylaminophenyl)-6-dimethylaminophthalide, and fluoran; green dyes such as 3-(N-ethyl-Np-tolyl)amino-7-N-methylanilinofluoran, 3-diethylamino-7-anilinofluoran, 3-diethylamino-7-dibenzylaminofluoran, and rhodamine B-anilinolactam; Color-forming dyes, such as 3,6-bis(diethylamino)fluoran-γ-anilinolactam, 3-cyclohexylamino-6-chlorofluoran, 3-diethylamino-6-methyl-7-chlorofluoran, and 3-diethylamino-7-chlorofluoran, red color-forming dyes such as 3-(N-ethyl-N-isoamyl)amino-6-methyl-7-anilinofluoran, 3-(N-methyl-N-cyclohexyl)amino-6-methyl-7-anilinofluoran, 3-diethyl ... -Di(n-butyl)amino-6-methyl-7-anilinofluoran, 3-di(n-pentyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isoamylamino)-6-methyl-7-anilinofluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-(N-isoamyl-N-ethylamino)-7-(o-chloroanilino)fluoran, 3-(N-ethyl-N-2-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3- (Nn-hexyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-ethylamino]-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-anilinofluoran, 3-diethylamino-7-(2-chloroanilino)fluoran, 3-di(n-butylamino)-7-(2-chloroanilino)fluoran, 4,4'-bis-dimethylaminobenzhydrin benzyl ether, N-2,4,5-Trichlorophenylleucoauramine, 3-diethylamino-7-butylaminofluoran, 3-ethyl-tolylamino-6-methyl-7-anilinofluoran, 3-cyclohexyl-methylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-chloro-7-(β-ethoxyethyl)aminofluoran, 3-diethylamino-6-chloro-7-(γ-chloropropyl)aminofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-(N-isopropyl)aminofluoran, Soamyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-dibutylamino-7-chloroanilinofluoran, 3-diethylamino-7-(o-chlorophenylamino)fluoran, 3-(N-ethyl-p-toluidino)-6-methyl-7-anilinofluoran, 3-(N-ethyl-p-toluidino)-6-methyl-7-(p-toluidino)fluoran, 3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-diethylamino -6-chloro-7-anilinofluoran, 3-dimethylamino-6-methyl-7-anilinofluoran, 3-pyrrolidino-6-methyl-7-anilinofluoran, 3-piperidino-6-methyl-7-anilinofluoran, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalido-3,9'-xanthene]-2'-ylamino]phenyl}propane, 3-diethylamino-7-(3'-trifluoromethylphenyl)aminofluoran, and other black pigments. Color dyes, 3,3-bis[1-(4-methoxyphenyl)-1-(4-dimethylaminophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-methoxyphenyl)-1-(4-pyrrolidinophenyl)ethylene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-p-(p-dimethylaminoanilino)anilino-6-methyl-7-chlorofluoran, 3-p-(p-chloroanilino)anilino-6-methyl-7-chlorofluoran, 3,Examples of the dyes include dyes having an absorption wavelength in the near infrared region, such as 6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide. Of course, the dyes are not limited to these, and two or more compounds can be used in combination as necessary.
[0017] The content of the leuco dye is not particularly limited, and is preferably about 3 to 30% by mass, more preferably about 5 to 25% by mass, and even more preferably about 7 to 25% by mass, based on the total solid content of the thermosensitive recording layer. By making it 3% by mass or more, the color development ability can be improved and the print density can be improved. By making it 30% by mass or less, the heat resistance can be improved.
[0018] (Developer) In the present invention, N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea is contained as a color developer. By combining this compound with dimethyl terephthalate as a sensitizer, it is possible to exhibit excellent heat resistance, head matching properties and printability. In addition, blank paper storage stability can be improved to a level that is practically problem-free, and color development ability can be maintained even after long-term storage in a blank state.
[0019] The content of N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea is not particularly limited and may be adjusted according to the leuco dye used. In general, it is preferably 0.5 parts by mass or more relative to 1 part by mass of the leuco dye, more preferably 0.8 parts by mass or more, even more preferably 1 part by mass or more, even more preferably 1.2 parts by mass or more, and particularly preferably 1.4 parts by mass or more. The content of N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea is preferably 10 parts by mass or less relative to 1 part by mass of the leuco dye, more preferably 5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 3.5 parts by mass or less. By making it 0.5 parts by mass or more, the recording performance can be improved. On the other hand, by making it 10 parts by mass or less, background fogging in a high-temperature environment can be effectively suppressed.
[0020] Other color developers may be contained as long as they do not impair the effects of the present invention. Specific examples of other color developers include 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidenediphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidenediphenol, 4,4'-cyclohexylidene diphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis (p-Tolylsulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, butyl bis(p-hydroxyphenyl)acetate, methyl bis(p-hydroxyphenyl)acetate, hydroquinone monobenzyl ether, bis(3-allyl-4-hydroxyphenyl)sulfone, 4-hydroxy-4' -Methyldiphenyl sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone, 3,4-dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxybenzophenone, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate ester, tolyl 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate, 4,Phenolic compounds such as 4'-dihydroxydiphenyl ether, or benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzylsalicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethyloxy]salicylic acid, 4-[3-(p-tolyl aromatic carboxylic acids such as zinc 4-[3-(p-tolylsulfonyl)propyloxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy)cumyl]salicylic acid, and 4-[3-(p-tolylsulfonyl)propyloxy]salicylic acid, and these phenolic compounds and salts of aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin, and nickel, as well as antipyrine complexes of zinc thiocyanate, and salts of terephthalaldehyde acid and other compounds. Examples of the acidic organic compounds include organic acidic compounds having a -SO2NH- bond in the molecule, such as N-(p-toluenesulfonyl)carbamoyl acid p-cumylphenyl ester, N-(p-toluenesulfonyl)carbamoyl acid p-benzyloxyphenyl ester, N-[2-(3-phenylureido)phenyl]benzenesulfonamide, and N-(o-toluoyl)-p-toluenesulfonamide. Examples of the acidic organic compounds include organic acidic compounds having a -SO2NH- bond in the molecule, such as N-(p-toluenesulfonyl)carbamoyl acid p-cumylphenyl ester, N-(p-toluenesulfonyl)carbamoyl acid p-benzyloxyphenyl ester, N-[2-(3-phenylureido)phenyl]benzenesulfonamide, and N-(o-toluoyl)-p-toluenesulfonamide. Examples of the acidic organic compounds include organic acidic compounds having a -SO2NH- bond in the molecule, such as N-(p-toluenesulfonyl)carbamoyl acid p-cumylphenyl ester, N-[2-(3-phenylureido)phenyl]benzenesulfonamide, and N-(o-toluoyl)-p-toluenesulfonamide. Examples of the acidic inorganic compounds include activated clay, attapulgite, colloidal silica, and aluminum silicate.
[0021] Further examples include urea urethane derivatives such as 4,4'-bis[(4-methyl-3-phenoxycarbonylaminophenyl)ureido]diphenyl sulfone, 4,4'-bis[(2-methyl-5-phenoxycarbonylaminophenyl)ureido]diphenyl sulfone, and 4-(2-methyl-3-phenoxycarbonylaminophenyl)ureido-4'-(4-methyl-5-phenoxycarbonylaminophenyl)ureidodiphenyl sulfone represented by the following general formula (1), diphenyl sulfone derivatives represented by the following general formula (2), 5-(N-3-methylphenyl-sulfonylamido)-(N',N''-bis-(3-methylphenyl)-isophthalic acid diamide, 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, and N,N'-di[3-(p-toluenesulfonyl)oxy]phenyl urea. Of course, the present invention is not limited to these, and two or more compounds may be used in combination as necessary.
[0022] [ka]
[0023] [ka] (In the formula, n represents an integer of 1 to 6.)
[0024] (sensitizer) In the present invention, the heat-sensitive recording layer contains dimethyl terephthalate as a sensitizer, which not only enhances the recording sensitivity but also improves the heat resistance.
[0025] The content of dimethyl terephthalate as a sensitizer is not particularly limited, and is usually preferably about 2 to 40% by mass, more preferably about 5 to 25% by mass, of the total solid content of the heat-sensitive recording layer. By making it 2% by mass or more, the recording sensitivity can be increased. On the other hand, by making it 40% by mass or less, the heat resistance can be improved.
[0026] The content of dimethyl terephthalate is not particularly limited and may be adjusted according to the leuco dye used, and is generally preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 1 part by mass of leuco dye. The content of dimethyl terephthalate is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and particularly preferably 2.5 parts by mass or less, relative to 1 part by mass of leuco dye. By making it 0.1 parts by mass or more, recording performance can be improved. On the other hand, by making it 5 parts by mass or less, background fogging in a high-temperature environment can be effectively suppressed.
[0027] Other sensitizers may be contained as long as they do not impair the effects of the present invention.Specific examples of other sensitizers include stearic acid amide, methoxycarbonyl-N-stearic acid benzamyl, N-benzoylstearic acid amide, N-eicosanoic acid amide, ethylene bisstearic acid amide, behenic acid amide, methylene bisstearic acid amide, N-methylolstearic acid amide, dibenzyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, 1-hydroxy-2-naphthoic acid phenyl, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, oxalic acid di-p-chlorobenzyl ester, oxalic acid di-p-methylbenzyl ester, oxalic acid dibenzyl ester, p-tolyl biphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-di(3-methylphenoxy) ether, Examples of such compounds include ethane, 1,2-di(4-methylphenoxy)ethane, 1,2-di(4-methoxyphenoxy)ethane, 1,2-di(4-chlorophenoxy)ethane, 1,2-diphenoxyethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenylbenzyl ether, 1,4-di(phenylthio)butane, p-acetotoluidide, p-acetophenetidide, N-acetoacetyl-p-toluidine, 1,2-diphenoxymethylbenzene, di(β-biphenylethoxy)benzene, p-di(vinyloxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipate, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthoxy)propane, diphenyl, and benzophenone. These compounds can be used in combination as long as they do not cause any problems.
[0028] (Storage improver) In the present invention, the heat-sensitive recording layer can further contain a storage improver, mainly for the purpose of further improving the storage stability of the color image. Examples of such storage improvers include 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1-bis(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol, and 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol. At least one selected from phenol compounds such as 4-benzyloxyphenyl-4'-(2-methyl-2,3-epoxypropyloxy)phenylsulfone, epoxy compounds such as 4-(2-methyl-1,2-epoxyethyl)diphenylsulfone, and 4-(2-ethyl-1,2-epoxyethyl)diphenylsulfone, and isocyanuric acid compounds such as 1,3,5-tris(2,6-dimethylbenzyl-3-hydroxy-4-tert-butyl)isocyanuric acid can be used. Of course, the present invention is not limited to these compounds, and two or more compounds can be used in combination as necessary.
[0029] When a storage stability improver is used, the amount used should be an amount effective for improving storage stability, and is usually preferably about 1 to 30 mass %, more preferably about 5 to 20 mass %, of the total solid content of the thermosensitive recording layer.
[0030] (Waxes) Waxes can be contained in the thermosensitive recording layer in the present invention. This can improve sticking and head matching. Examples of waxes include paraffin wax, carnauba wax, microcrystalline wax, polyolefin wax, and polyethylene wax; higher fatty acid amides, higher fatty acid esters, and derivatives thereof, such as stearic acid amide and ethylene bisstearic acid amide; and higher fatty acid polyvalent metal salts, such as zinc stearate, aluminum stearate, calcium stearate, and zinc oleate. Among these, ethylene bisstearic acid amide is preferred from the viewpoint of improving head matching without impairing heat resistance. The wax content may be an amount effective for head matching, and is usually preferably about 1 to 20 mass % and more preferably about 2 to 15 mass % of the total solid content of the thermosensitive recording layer.
[0031] (Pigments) The thermosensitive recording layer of the present invention may contain a pigment. This can improve printability. Examples of pigments include inorganic pigments such as clay, calcined clay, diatomaceous earth, talc, kaolin, calcined kaolin, light or heavy calcium carbonate, precipitated calcium carbonate, magnesium carbonate, zinc oxide, aluminum oxide, aluminum hydroxide, magnesium hydroxide, titanium dioxide, barium sulfate, zinc sulfate, amorphous silica, amorphous calcium silicate, and colloidal silica, and organic pigments such as melamine resin, urea-formalin resin, polyethylene, nylon, styrene, acrylic, and hydrocarbon. Among these, clay is preferred from the viewpoint of particularly excellent printability. The content of the pigment may be an amount effective for printability, and is usually preferably about 10 to 40 mass % and more preferably about 15 to 35 mass % of the total solid content of the thermosensitive recording layer.
[0032] Other components constituting the heat-sensitive recording layer include an adhesive, and if necessary, auxiliary agents such as a crosslinking agent, a water-resistant agent, a dispersing agent, a coloring dye, and a fluorescent dye can be used.
[0033] (glue) The adhesive used in the coating liquid for the thermal recording layer may be, for example, a water-soluble adhesive or a water-dispersible adhesive. Examples of the water-soluble adhesive include modified polyvinyl alcohol such as polyvinyl alcohol, carboxy-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, diacetone-modified polyvinyl alcohol, and silicon-modified polyvinyl alcohol, starch and its derivatives, cellulose derivatives such as methoxycellulose, carboxymethylcellulose, hydroxyethylcellulose, hydroxypropylmethylcellulose, methylcellulose, and ethylcellulose, sodium polyacrylate, polyvinylpyrrolidone, polyamide, diisobutylene-maleic anhydride copolymer salt, styrene-acrylic acid copolymer salt, styrene-maleic anhydride copolymer salt, ethylene-maleic anhydride copolymer salt, acrylamide-acrylic acid ester copolymer, acrylamide-acrylic acid ester-methacrylic acid copolymer, polyacrylamide, sodium alginate, gelatin, casein, and gum arabic. Examples of water-dispersible adhesives include emulsions of polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylic acid ester, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate, ethylene-vinyl acetate copolymer, and the like, or latexes of water-insoluble polymers such as styrene-butadiene copolymer, styrene-butadiene-acrylic copolymer, and the like. The adhesives can be used alone or in combination of two or more. The content of the adhesive can be selected from a wide range, but is generally mixed in a range of preferably about 5 to 30 mass %, more preferably about 10 to 20 mass %, of the total solid content of the thermal recording layer.
[0034] (Crosslinking agent) A crosslinking agent that hardens the adhesive of the heat-sensitive recording layer or other layers can be contained in the heat-sensitive recording layer. This can improve the water resistance of the heat-sensitive recording layer. Examples of crosslinking agents include aldehyde compounds such as glyoxal, polyamine compounds such as polyethyleneimine, epoxy compounds, polyamide resins, melamine resins, glyoxylates, dimethylol urea compounds, aziridine compounds, and blocked isocyanate compounds; inorganic compounds such as ammonium persulfate, ferric chloride, magnesium chloride, sodium tetraborate, and potassium tetraborate; boric acid, boric acid triesters, boron-based polymers, hydrazide compounds, and glyoxylates. These may be used alone or in combination of two or more. The amount of the crosslinking agent used is preferably in the range of about 1 to 10 parts by mass relative to 100 parts by mass of the total solid content of the heat-sensitive recording layer. This can improve the water resistance of the heat-sensitive recording layer.
[0035] If necessary, various auxiliary agents such as an oil repellent, an antifoaming agent, a viscosity adjusting agent, etc. may be added to the heat-sensitive recording layer within the range that does not impair the effect of the present invention.
[0036] The thermal recording layer is generally formed on the base paper by dispersing a leuco dye, a developer, a sensitizer, and optionally a storage stability improver together or separately in water as a dispersion medium, together with water-soluble synthetic polymer compounds such as polyacrylamide, polyvinylpyrrolidone, polyvinyl alcohol, methyl cellulose, styrene-maleic anhydride copolymer salt, and other surfactants in various stirring and wet grinding machines such as ball mills, coball mills, attritors, and vertical and horizontal sand mills to prepare a dispersion, and then dispersing the dispersion to an average particle size of 2 μm or less, and mixing it with adhesives, wax, pigments, auxiliaries, etc. as necessary to prepare a coating liquid for the thermal recording layer. The coating amount of the thermal recording layer is not particularly limited, and is 1 to 12 g / m2 in terms of dry mass. 2 The preferred thickness is 2 to 10 g / m 2 More preferably, 2.5 to 8 g / m 2 More preferably, 3 to 5.5 g / m 2The heat-sensitive recording layer can be formed in two or more layers as required, and the composition and coating amount of each layer may be the same or different.
[0037] [Undercoat layer] The thermosensitive recording medium of the present invention may also have an undercoat layer between the support and the thermosensitive recording layer, if necessary. The undercoat layer preferably contains an adhesive.
[0038] (glue) Examples of adhesives include polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, and ethyl cellulose, water-soluble polymer materials such as sodium polyacrylate, polyvinylpyrrolidone, acrylamide-acrylic acid ester copolymers, acrylamide-acrylic acid ester-methacrylic acid ester copolymers, styrene-maleic anhydride copolymers, isobutylene-maleic anhydride copolymers, casein, gelatin, and their derivatives, as well as emulsions of polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylic acid esters, vinyl chloride-vinyl acetate copolymers, polybutyl methacrylate, and ethylene-vinyl acetate copolymers, or latexes of water-insoluble polymers such as styrene-butadiene copolymers and styrene-butadiene-acrylic copolymers. Among these, it is preferable to use an adhesive containing latex. The content of the adhesive can be selected from a wide range, but generally, it is preferably about 10 to 70 mass % of the total solid content of the undercoat layer, and more preferably about 15 to 60 mass %.
[0039] The adhesive preferably contains a binder resin with a glass transition temperature (Tg) of -10°C or lower. By making the glass transition temperature -10°C or lower, image quality can be improved even in a low energy region. Since the image quality can be further improved in a low energy region, the glass transition temperature is more preferably -30°C or lower. On the other hand, a glass transition temperature of -50°C or lower is undesirable because stickiness occurs, so a glass transition temperature of -40°C or higher is preferable.
[0040] (hollow particles) The undercoat layer may contain hollow particles. The hollow particles are preferably made of an organic resin from the viewpoint of improving cushioning properties. The undercoat layer, which has high heat insulating properties due to the inclusion of hollow particles, can prevent the diffusion of heat applied to the thermal recording layer and can increase the sensitivity as a thermal recording medium.
[0041] Hollow particles made of organic resins can be divided into expanded and non-expanded types depending on the manufacturing method. Of these two types, expanded hollow particles generally have a larger average particle size and a higher hollow ratio than non-expanded hollow particles. Therefore, expanded hollow particles can provide better sensitivity and image quality than non-expanded hollow particles.
[0042] Non-foamed hollow particles can be produced by polymerizing seeds in a solution, polymerizing other resins so as to encase the seeds, and then swelling and dissolving the internal seeds to remove them, thereby forming internal cavities. When swelling and dissolving the internal seeds to remove them, an alkaline aqueous solution or the like is used. Non-foamed hollow particles with a relatively large average particle size can also be obtained by subjecting core-shell particles, in which core particles having alkali swelling properties are covered with a shell layer not having alkali swelling properties, to an alkali swelling treatment.
[0043] Expanded hollow particles can be produced by preparing particles having a volatile liquid sealed inside a resin, softening the resin by heating, and vaporizing and expanding the liquid inside the particles.
[0044] The foamed hollow particles have a large hollow ratio and high heat insulating properties due to the heating and expansion of the liquid inside during the manufacturing process, which can increase the sensitivity of the thermosensitive recording medium and improve the recording density. The improvement in sensitivity is particularly important when coloring a halftone region where the thermal energy applied to the thermosensitive recording layer is small. In addition, if the thermosensitive recording layer is formed via a highly heat-insulating undercoat layer, the diffusion of heat applied to the thermosensitive recording layer is prevented, resulting in excellent image uniformity and improved image quality.
[0045] Examples of resins that can be used for the expanded type hollow particles include thermoplastic resins such as styrene-acrylic resin, polystyrene resin, acrylic resin, polyethylene resin, polypropylene resin, polyacetal resin, chlorinated polyether resin, polyvinyl chloride resin, polyvinylidene chloride resin, acrylic resin (e.g., acrylic resin containing acrylonitrile as a constituent component), styrene resin, vinylidene chloride resin, and copolymer resin mainly composed of polyvinylidene chloride and acrylonitrile. The gas contained inside the expanded type hollow particles is generally propane, butane, isobutane, air, etc. Among the various resins mentioned above, the resin used for the hollow particles is preferably acrylonitrile resin and copolymer resin mainly composed of polyvinylidene chloride and acrylonitrile from the viewpoint of strength for maintaining the shape of the expanded particles.
[0046] The maximum particle diameter of the hollow particles in the present invention is preferably 10 to 30 μm, more preferably 10 to 25 μm. The maximum particle diameter is also called D100. When the maximum particle diameter of the hollow particles is 10 μm or more, the cushioning property of the undercoat layer is improved, so that the adhesion of the thermal recording medium to the thermal head during printing is improved, and a thermal recording medium with high image quality can be obtained. This high image quality can bring about an improvement in the recording density in intermediate tones that are developed with lower energy than that which gives the maximum recording density (Dmax). On the other hand, when the maximum particle diameter of the hollow particles is 30 μm or less, the smoothness of the undercoat layer is improved, so that the thermal recording layer provided via the undercoat layer can be made uniform, and a thermal recording medium with less white spots in the image can be obtained.
[0047] The average particle diameter of the hollow particles in the present invention is preferably 4.0 to 15 μm, more preferably 4.5 to 15 μm. Here, the average particle diameter is the diameter when the volume occupied by the larger particle and the smaller particle is equal when the particle diameter is divided into two, that is, the median diameter which is the particle diameter with a frequency of 50% by volume, and is also called D50. When the average particle diameter of the hollow particles is 4.0 μm or more, the cushioning property of the undercoat layer is improved, so that the adhesion of the thermal recording medium to the thermal head during printing is improved, and a thermal recording medium with high image quality can be obtained. This high image quality can bring about an improvement in the recording density in the intermediate tone which is developed with lower energy than that which gives the maximum recording density (Dmax). On the other hand, when the average particle diameter of the hollow particles is 15 μm or less, the smoothness of the undercoat layer is improved, so that the thermal recording layer provided through the undercoat layer can be made uniform, and a thermal recording medium with less white spots in the image can be obtained.
[0048] The maximum particle size (D100) and the average particle size (D50) of the hollow particles can be measured by a laser diffraction particle size distribution analyzer. Alternatively, the particle sizes can be measured from particle images (SEM images) using an electron microscope, and the average value of 10 particles can be used.
[0049] The ratio D100 / D50 of the maximum particle size (D100) to the average particle size (D50) of the hollow particles is an index showing the degree of particle size distribution. This ratio D100 / D50 is preferably 1.8 to 3.0, more preferably 2.0 to 2.8. When the D100 / D50 of the hollow particles is 1.8 or more, the hollow particles are sufficiently expanded, the maximum particle size is sufficiently large, the hollow ratio is high, and the heat insulation of the undercoat layer can be improved. On the other hand, when the D100 / D50 of the hollow particles is 3.0 or less, the size of the hollow particles is uniform, so that the smoothness of the undercoat layer is improved and white spots in the image can be suppressed.
[0050] In the particle size distribution obtained by a laser diffraction particle size distribution measuring device, the volume percentage of hollow particles having a particle diameter of 2.0 μm or less is preferably 1% or less. The volume percentage of hollow particles having a particle diameter of 2.0 μm or less is preferably 0.5% or less, and more preferably, no hollow particles are contained. Since hollow particles having a particle diameter of 2 μm or less are too small to have a sufficient hollow area, it is considered that their contribution to heat insulation is extremely small. By making the volume percentage of hollow particles having a particle diameter of 2 μm or less in the undercoat layer 1% or less, the recording density, image quality, etc. can be improved.
[0051] The hollow particles preferably have a hollow ratio of 80 to 98%, more preferably 90 to 98%. When the hollow ratio of the hollow particles is 80% or more, high heat insulation can be imparted to the undercoat layer containing the hollow particles. On the other hand, when the hollow ratio of the hollow particles is 98% or less, the strength of the film surrounding the hollow portion can be improved, so that the hollow particles do not collapse when the undercoat layer is formed.
[0052] The hollow ratio of hollow particles is determined by measuring the true specific gravity by the IPA method and calculating the true specific gravity value as follows. (1) Sample pretreatment Dry the sample at 60℃ overnight to prepare the sample. (2) Reagents Isopropyl alcohol (IPA: first-grade reagent) (3) Measurement method Accurately weigh the volumetric flask (W1). ·Put about 0.5 g of the dried sample into a measuring flask and weigh it accurately (W2). Add approximately 50 mg of IPA and shake thoroughly to completely remove any air outside the capsule. Add IPA up to the mark and measure (W3). As a blank, add only IPA to the measuring flask up to the mark and measure carefully (W4). (4) Calculation of true specific gravity True specific gravity = {(W2-W1)×((W4-W1) / 100)} / {(W4-W1)-(W3-W2)} (5) Calculation of hollow ratio Hollowness ratio (%)={1-1 / (1.1 / true specific gravity)}×100
[0053] The hollow ratio is expressed by the following formula (d 3 / D 3 ) × 100. In this formula, d represents the inner diameter of the hollow particle, and D represents the outer diameter of the hollow particle.
[0054] The content of hollow particles is preferably 5 to 40% by mass, more preferably 5 to 35% by mass, based on the total solid content of the undercoat layer. If the content of hollow particles is 5% by mass or more, the heat insulating properties of the undercoat layer can be improved. On the other hand, if the content of hollow particles is 40% by mass or less, problems are unlikely to occur in terms of coating properties, etc., a uniform undercoat layer can be easily formed, and the recording density can be improved. In addition, the coating strength of the undercoat layer can be increased.
[0055] The undercoat layer may contain, as a pigment, an oil-absorbing pigment having an oil absorption of 70 ml / 100 g or more, particularly about 80 to 150 ml / 100 g, and / or thermally expandable particles. Here, the oil absorption is a value determined according to the method of JIS K 5101.
[0056] As the oil-absorbing pigment, various types can be used, and specific examples include inorganic pigments such as calcined kaolin, amorphous silica, light calcium carbonate, and talc. The average particle size of the primary particles of these oil-absorbing pigments is preferably about 0.01 to 5 μm, and particularly preferably about 0.02 to 3 μm. The amount of the oil-absorbing pigment used can be selected from a wide range, but is generally preferably about 20 to 80 mass % of the total solid content of the undercoat layer, and more preferably about 25 to 75 mass %.
[0057] The undercoat layer is formed on the support by, for example, applying a coating liquid for the undercoat layer prepared by mixing an adhesive, hollow particles, pigments, auxiliaries, etc., with water as a medium, and then drying the coating liquid. The amount of the coating liquid for the undercoat layer to be applied is not particularly limited, but is preferably 2 to 20 g / m2 in terms of dry mass. 2 The preferred thickness is 2 to 12 g / m 2 degree is more preferable.
[0058] Examples of auxiliaries contained in the coating liquid for the undercoat layer include dispersants such as sodium dioctyl sulfosuccinate, sodium dodecylbenzenesulfonate, sodium lauryl alcohol sulfate, and fatty acid metal salts; waxes such as zinc stearate, calcium stearate, polyethylene wax, carnauba wax, paraffin wax, and ester wax; water-resistant agents such as hydrazide compounds, boric acid, dialdehyde starch, glyoxylates, and epoxy compounds; antifoaming agents, coloring dyes, and fluorescent dyes.
[0059] [Protective layer] In the thermal recording medium, a protective layer may be provided on the thermal recording layer on the side opposite to the resin layer, if necessary. The protective layer preferably contains mainly an adhesive. Furthermore, the protective layer preferably contains a lubricant such as polyolefin wax or zinc stearate for the purpose of preventing sticking to the thermal head, and may also contain an ultraviolet absorber and a pigment. Furthermore, by providing a glossy protective layer, the added value of the product can be increased.
[0060] The pigment contained in the protective layer is not particularly limited, and examples thereof include inorganic pigments such as amorphous silica, kaolin, clay, light calcium carbonate, heavy calcium carbonate, calcined kaolin, titanium oxide, magnesium carbonate, aluminum hydroxide, colloidal silica, and synthetic layered mica, and plastic pigments such as urea-formaldehyde resin filler.
[0061] The adhesive contained in the protective layer is not particularly limited, and a water-soluble or water-dispersible aqueous adhesive can be used. The adhesive can be appropriately selected from those that can be used in the thermal recording layer. Among these adhesives, various modified polyvinyl alcohols such as acetoacetyl-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, and diacetone-modified polyvinyl alcohol are more preferably used.
[0062] The protective layer is formed on the thermosensitive recording layer by, for example, applying a coating liquid for the protective layer, which is prepared by mixing a pigment, an adhesive, and, if necessary, an auxiliary, etc., in water as a dispersion medium, and then drying the coating liquid. The amount of the coating liquid for the protective layer is not particularly limited, and is preferably 0.3 to 15 g / m2 in terms of dry mass. 2 The preferred range is 0.3 to 10 g / m 2 The preferred range is 0.5 to 8 g / m 2 More preferably, the thickness is 1 to 8 g / m 2 The preferred range is 1 to 5 g / m 2 The protective layer may be formed in two or more layers as required, and the composition and coating amount of each layer may be the same or different.
[0063] [Other layers] In the present invention, it is preferable that the support has an adhesive layer on at least one side. This can increase the added value of the thermal recording medium. For example, the adhesive layer can be made into adhesive paper, remoistened adhesive paper, delayed tack paper, etc. by applying coating processing with an adhesive, remoistened adhesive, delayed tack type adhesive, etc. on one side. In addition, the surface of the support opposite to the thermal recording layer can be given the function of thermal transfer paper, inkjet recording paper, carbonless paper, electrostatic recording paper, xeography paper, etc., to make a recording paper capable of double-sided recording. Of course, it can also be made into a double-sided thermal recording medium. In addition, a back layer can be provided to suppress the penetration of oil and plasticizer from the back side of the thermal recording medium, to control curling, and to prevent static electricity. It is also possible to make a linerless label that does not require a release paper by coating processing a release layer containing silicone on the protective layer and coating processing a pressure sensitive adhesive on one side.
[0064] [Thermal recording medium] The thermosensitive recording medium can be manufactured by forming each of the above layers on a support. As a method for forming each of the above layers on a resin layer, any of known coating methods such as an air knife method, a blade method, a gravure method, a roll coater method, a spray method, a dip method, a bar method, a curtain method, a slot die method, a slide die method, and an extrusion method may be used. In addition, each coating material may be applied and dried one by one to form each layer, or the same coating material may be applied in two or more layers. Furthermore, simultaneous multi-layer coating in which two or more layers are applied simultaneously may be performed. In addition, after each layer is formed or in any process after all layers are formed, a smoothing treatment can be performed using a known method such as a super calendar or a soft calendar.
[0065] The method of recording an image on the thermal recording medium of the present invention is not particularly limited and can be appropriately selected according to the purpose. For example, a thermal head printer, laser light (e.g., carbon dioxide laser, UV laser, semiconductor laser light, YAG laser light, fiber laser light, solid laser light, dye laser light, etc.) can be used as the image recording method. When using laser light, the wavelength of the laser light is not particularly limited and can be appropriately selected according to the purpose. EXAMPLES
[0066] The present invention will be described in more detail with reference to examples, but the present invention is not limited thereto. In addition, unless otherwise specified, "parts" and "%" respectively indicate "parts by mass" and "% by mass".
[0067] Example 1 (1) Preparation of coating solution for undercoat layer A coating liquid for an undercoat layer was obtained by mixing and stirring 52.8 parts of hollow particles (trade name: Ropeic SN-1055, manufactured by Dow, solids concentration 26.5%), 67 parts of calcined kaolin (trade name: Ansilex 93, manufactured by BASF), 31.3 parts of styrene-butadiene copolymer latex (trade name: L-1571, manufactured by Asahi Kasei Corporation, solids concentration 48%), 12 parts of a 25% solution of oxidized starch (trade name: Petrocoat C-8, manufactured by Nippon Starch Chemical Co., Ltd.), 5 parts of a 20% solution of polyvinyl alcohol (trade name: Kuraray Poval 5-98, manufactured by Kuraray Co., Ltd.), and 200 parts of water.
[0068] (2) Preparation of leuco dye dispersion (liquid A) 40 parts of 3-di-(n-butyl)amino-6-methyl-7-anilinofluoran, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by Imex Co., Ltd.) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) was 0.5 μm, thereby obtaining a leuco dye dispersion liquid (Liquid A).
[0069] (3) Preparation of developer dispersion liquid (liquid B) 40 parts of Np-tolylsulfonyl-N'-3-(p-tolylsulfonyloxy)phenylurea, 40 parts of a 10% aqueous solution of polyvinyl alcohol (degree of polymerization 500, degree of saponification 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by Imex) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) was 1.0 μm, thereby obtaining a color developer dispersion (Liquid B).
[0070] (4) Preparation of sensitizer dispersion (liquid C) 40 parts of dimethyl terephthalate (manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder manufactured by Imex Co., Ltd.) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) was 1.0 μm, thereby obtaining a sensitizer dispersion liquid (Liquid C).
[0071] (5) Preparation of coating liquid for thermal recording layer 40.9 parts of solution A, 50.0 parts of solution B, 18.2 parts of solution C, 30 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: Kuraray Poval 22-88, manufactured by Kuraray Co., Ltd.), 46.7 parts of a 15% aqueous solution of polyvinyl alcohol (trade name: Kuraray Poval 11-98, manufactured by Kuraray Co., Ltd.), 8 parts of a 25% solution of oxidized starch (trade name: Petrocoat C-8, manufactured by Nippon Starch Chemical Co., Ltd.), paraffin wax (trade name: Hydrin P-7, manufactured by Chukyo Yushi Co., Ltd., solids concentration 30%)3. A coating liquid for a thermal recording layer was obtained by mixing and stirring 3 parts of ethyl acetate, 8.8 parts of polyethylene wax (trade name: Chemipearl W-400, manufactured by Mitsui Chemicals, solids concentration 40%), 16.7 parts of zinc stearate (trade name: Hydrin Z-9, manufactured by Chukyo Yushi, solids concentration 36%), 16.5 parts of aluminum hydroxide (trade name: Hidilite H-42, manufactured by Resonac Corporation), 13 parts of silica (trade name: Nipsil E-743, manufactured by Tosoh Silica Corporation), and 180 parts of water.
[0072] (6) Preparation of thermal recording medium Basis weight 60g / m 2 The coating liquid for the undercoat layer and the coating liquid for the thermal recording layer were applied on one side of the high-quality paper in an amount of 4.5 g / m2 after drying. 2 , 4.0g / m 2 After the undercoat layer and the thermosensitive recording layer were successively formed, the surface was smoothed by a supercalender to obtain a thermosensitive recording medium.
[0073] Example 2 A thermal recording medium was obtained in the same manner as in Example 1, except that in preparing the coating liquid for the thermal layer of Example 1, 18.5 parts of ethylene bisstearic acid amide (product name: High Micron G-110, manufactured by Chukyo Yushi Co., Ltd., solid content concentration 27%) was added, the amount of aluminum hydroxide (product name: Higilite H-42, manufactured by Resonac Corporation) was changed from 16.5 parts to 13.5 parts, and the amount of silica (product name: Nipsil E-743, manufactured by Tosoh Silica Corporation) was changed from 13 parts to 11 parts.
[0074] Example 3 A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in the preparation of the coating liquid for the thermosensitive layer in Example 1, 18.5 parts of ethylene bisstearic acid amide (product name: High Micron G-110, manufactured by Chukyo Yushi Co., Ltd., solid content concentration 27%) and 4 parts of clay (product name: HG90, manufactured by Kamin Co., Ltd.) were added, the amount of aluminum hydroxide (product name: Higilite H-42, manufactured by Resonac Co., Ltd.) was changed from 16.5 parts to 11.5 parts, and the amount of silica (product name: Nipsil E-743, manufactured by Tosoh Silica Co., Ltd.) was changed from 13 parts to 9 parts.
[0075] Comparative Example 1 (7) Preparation of sensitizer dispersion (liquid D) 40 parts of di-p-methylbenzyl oxalate (product name: HS-3520, manufactured by DIC Corporation), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by Imex Corporation) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) reached 1.0 μm, thereby obtaining a sensitizer dispersion liquid (Liquid D).
[0076] A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in the preparation of the coating liquid for the thermosensitive layer in Example 1, Liquid D was used instead of Liquid C.
[0077] Comparative Example 2 (8) Preparation of sensitizer dispersion (E solution) 40 parts of di-p-chlorobenzyl oxalate (product name: HS-3519, manufactured by DIC Corporation), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by Imex Corporation) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) was 1.0 μm, thereby obtaining a sensitizer dispersion (Liquid E).
[0078] A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in the preparation of the coating liquid for the thermosensitive layer in Example 1, 13.6 parts of Liquid D and 4.5 parts of Liquid E were used instead of 18.2 parts of Liquid C.
[0079] Comparative Example 3 (9) Preparation of sensitizer dispersion (liquid F) 40 parts of 1,2-di(3-methylphenoxy)ethane (product name: KS-232, manufactured by Sankosha), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by Imex Co., Ltd.) until the median diameter measured with a laser diffraction particle size measuring device SALD2200 (manufactured by Shimadzu Corporation) was 1.0 μm, thereby obtaining a sensitizer dispersion liquid (Liquid F).
[0080] A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in the preparation of the coating liquid for the thermosensitive layer in Example 1, Liquid F was used instead of Liquid C.
[0081] Comparative Example 4 (10) Preparation of sensitizer dispersion (liquid G) 40 parts of diphenyl sulfone (trade name: DPS, manufactured by NICCA Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree 500, saponification degree 88%), and 20 parts of water were mixed and ground using a sand mill (sand grinder, manufactured by IMEX Co., Ltd.) until the median diameter measured with a laser diffraction particle size analyzer SALD2200 (manufactured by Shimadzu Corporation) was 1.0 μm, thereby obtaining a sensitizer dispersion liquid (Liquid G).
[0082] A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in the preparation of the coating liquid for the thermosensitive layer in Example 1, Liquid G was used instead of Liquid C.
[0083] Comparative Example 5 A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in preparing the coating liquid for the thermosensitive layer in Example 1, 32 parts of stearic acid amide (product name: Himicron L-271, manufactured by Chukyo Yushi Co., Ltd., solids concentration 25%) was used instead of 18.2 parts of Liquid C.
[0084] Comparative Example 6 A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in preparing the coating liquid for the thermosensitive layer in Example 1, 13.6 parts of Solution D and 4.5 parts of Solution E were used instead of 18.2 parts of Solution C, the amount of paraffin wax (product name: Hydrin P-7, manufactured by Chukyo Yushi Co., Ltd., solid content concentration 30%) was changed from 3.3 parts to 15 parts, the amount of aluminum hydroxide (product name: Higilite H-42, manufactured by Resonac Co., Ltd.) was changed from 16.5 parts to 14.5 parts, and the amount of silica (product name: Nipsil E-743, manufactured by Tosoh Silica Co., Ltd.) was changed from 13 parts to 11.5 parts.
[0085] Comparative Example 7 A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in preparing the coating liquid for the thermosensitive layer in Example 1, 13.6 parts of Solution D and 4.5 parts of Solution E were used instead of 18.2 parts of Solution C, the amount of polyethylene wax (product name: Chemipearl W-400, manufactured by Mitsui Chemicals, Inc., solid content concentration 40%) was changed from 8.8 parts to 17.5 parts, the amount of aluminum hydroxide (product name: Higilite H-42, manufactured by Resonaq) was changed from 16.5 parts to 14.5 parts, and the amount of silica (product name: Nipsil E-743, manufactured by Tosoh Silica Corporation) was changed from 13 parts to 11.5 parts.
[0086] Comparative Example 8 A thermosensitive recording medium was obtained in the same manner as in Example 1, except that in preparing the coating liquid for the thermosensitive layer in Example 1, 13.6 parts of Solution D and 4.5 parts of Solution E were used instead of 18.2 parts of Solution C, the amount of zinc stearate (product name: Hydrin Z-9, manufactured by Chukyo Yushi Co., Ltd., solid content concentration 36%) was changed to 26.4 parts instead of 16.7 parts, the amount of aluminum hydroxide (product name: Higilite H-42, manufactured by Resonac Co., Ltd.) was changed to 14.5 parts instead of 16.5 parts, and the amount of silica (product name: Nipsil E-743, manufactured by Tosoh Silica Co., Ltd.) was changed to 11.5 parts instead of 13 parts.
[0087] The above examples and comparative examples were evaluated by the following methods. The results are shown in Table 1.
[0088] [90℃ heat resistance] A blank sample of each thermal recording medium was left to stand in a chamber at 90° C. for 1 hour, and the optical density of the blank portion after processing was measured with a spectrodensitometer (X-Rite504, manufactured by X-Rite Corporation). The evaluation criteria were as follows. Density of blank areas after processing: 0.20 or less: No problem in practical use. Density of blank area after processing exceeds 0.20: background fogging is severe and is problematic in practical use.
[0089] [Blank storability] Untreated samples of each thermal recording medium and blank samples of each thermal recording medium were left to stand for 3 days in a chamber at 40°C and 90% RH, and then recorded on each thermal recording medium using a thermal recording evaluation machine (product name: TH-PMD, manufactured by Okura Electric Co., Ltd.) with an applied energy of 0.16 mJ / dot (medium to high gradation color development density), and the resulting printed area was measured with a spectrodensitometer (X-Rite504, manufactured by X-Rite Co., Ltd.). The recording density difference was calculated using the following formula, and the evaluation criteria were as follows. Thermal recording mediums with a large negative value have a problem of reduced color development ability during long-term storage. Formula: (Recording density difference) = (Processed recording density) - (Unprocessed recording density) Recording density difference ≧−0.10: Blank paper preservation property is high and is very excellent. -0.10> Recording density difference ≧-0.20: Blank paper preservation property is high and excellent. -0.20>Recording density difference ≧-0.30: The sensitivity is slightly low, but there is no problem in practical use. -0.30> Recording density difference: The blank paper preservation property is low, which is problematic in practical use.
[0090] [Head matching] (Head waste) Using a thermal printer (product name: Respri T-408v-ex, manufactured by Sato Corporation), 18 cm of solid black was printed six times with an applied energy of 5A, and the amount of head residue adhering to the thermal head was evaluated according to the following criteria.
[0091] (stick) At an ambient temperature of 5°C, a thermal printer (product name: Respri T-408v-ex, manufactured by Sato Corporation) was used to repeatedly print 8 dots of solid black and 8 dots of blank space with an applied energy of 3A, and skipped prints over a printing length of 10 cm were evaluated according to the following criteria. ◎: The amount of head residue is extremely small, to the point where sticking such as skipped prints does not occur. ◯: A small amount of head residue adheres or slight printing skips occur, but at a level that does not cause any problems in practical use. ×: Printing problems caused by head residue or clear printing skips occurring to a level that is problematic in practical use.
[0092] [Suitable for offset printing] The offset printing suitability of each thermal recording medium was evaluated using an RI printing machine. 0.25 g of UV ink (product name: Bestcure UV NVR Red, manufactured by T&K Co.) was mixed with an ink mixing roller for 1 minute, and then a printing test was performed. After UV irradiation, the solid uniformity of the printed area was evaluated as follows. ◎: The print density is high and there are no defects such as whiteouts or picking, and the print is clean. ◯: The print density is slightly low and very small blank areas are observed, but this does not cause any problems in practical use. ×: Large white spots or picking occurred in the printed area, which is problematic for practical use.
[0093] [Table 1]
[0094] As can be seen from Table 1, the thermal recording materials of Examples 1 to 3 have superior heat resistance at 90°C compared to Comparative Examples 1 to 5, which use other sensitizers. In addition, by using ethylene bisstearic acid amide as the wax, head matching was improved without impairing heat resistance (Example 2). Furthermore, by using clay as the inorganic pigment, printability was improved (Example 3).
Claims
1. The thermal recording medium has a thermal recording layer on a support, the thermal recording layer containing at least a leuco dye, a color developer and a sensitizer, and is characterized in that the color developer is N-(p-toluenesulfonyl)-N'-3-(p-toluenesulfonyloxyphenyl)urea and the sensitizer is dimethyl terephthalate.
2. 2. The thermosensitive recording material according to claim 1, wherein the thermosensitive recording layer contains ethylene bisstearic acid amide as a wax.
3. 3. The thermosensitive recording material according to claim 1, wherein the thermosensitive recording layer contains clay as an inorganic pigment.
4. 3. The thermosensitive recording medium according to claim 1, further comprising an undercoat layer between the support and the thermosensitive recording layer.
Citation Information
Patent Citations
Thermal recording material
JP1995108765A
Cited By
Rotary compressor and refrigeration apparatus
WO2026063175A1