Battery, manufacturing method for battery, and using method for battery
The battery design addresses the issue of lithium depletion in lithium ion secondary batteries by incorporating a lithium alloy layer and controlled discharging to replenish lithium, thereby maintaining battery capacity.
Patent Information
- Application Number
- JP2023078611
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Lithium ion secondary batteries experience a decrease in battery capacity due to lithium depletion, and existing technologies do not effectively replenish depleted lithium, leading to a decrease in battery capacity that cannot be sufficiently suppressed.
A battery design with a negative electrode layer, an alloy layer containing a lithium alloy with a higher electrode potential than the negative electrode active material, and a positive electrode layer containing a lithium compound, along with a method to generate an alloy of metal and lithium by applying electricity, and a discharge strategy to replenish lithium when capacity decreases.
The battery design effectively suppresses the decrease in capacity by replenishing lithium, maintaining a stable discharge capacity through controlled discharging processes.
Smart Images

Figure 2024162748000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to batteries, methods of making batteries, and methods of using batteries. [Background technology]
[0002] Patent Document 1 discloses a sheet battery. The sheet battery described in Patent Document 1 includes a bipolar electrode unit having a positive electrode active material layer on one surface of a current collector and a negative electrode active material layer on the other surface of the current collector, and a solid electrolyte. The sheet battery described in Patent Document 1 uses a solid electrolyte as the electrolyte to prevent self-discharge between the positive electrode active material layer and the negative electrode active material layer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-100471 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, in a lithium ion secondary battery, which is a typical example of a sheet-type battery as described in Patent Document 1, it is known that the battery capacity gradually decreases due to repeated charging and discharging.
[0005] One of the causes of the decrease in the battery capacity of a lithium-ion secondary battery is the loss of lithium exchanged between the positive and negative electrodes. In conventional lithium-ion secondary batteries, there is no method for replacing lost lithium, and therefore, batteries that have experienced a decrease in battery capacity due to lithium loss must continue to be used in this state of reduced battery capacity.
[0006] In other words, the lithium ion secondary batteries according to the conventional technology have a problem in that the decrease in battery capacity cannot be sufficiently suppressed. Patent Document 1 does not disclose any technology capable of solving the above problems.
[0007] The present disclosure has been made to solve such problems, and has an object to provide a battery capable of suppressing a decrease in battery capacity, a method for manufacturing the battery, and a method for using the battery. [Means for solving the problem]
[0008] A battery according to one embodiment of the present disclosure comprises: a first negative electrode layer containing a negative electrode active material; an alloy layer that is located between the negative electrode layer and a current collector and contains a lithium alloy and has an electrode potential higher than that of the negative electrode active material; A positive electrode layer containing a lithium compound as a positive electrode active material. It's a battery.
[0009] A method for producing a battery according to one embodiment of the present disclosure includes: forming a metal layer containing a metal; forming a negative electrode layer containing a negative electrode active material; forming a positive electrode layer containing a lithium compound as a positive electrode active material; laminating the metal layer, the negative electrode layer, and the positive electrode layer; and generating an alloy of the metal and lithium in the metal layer by passing current through the laminated metal layer, the negative electrode layer, and the positive electrode layer. A method for manufacturing a battery.
[0010] A method for using a battery according to one embodiment of the present disclosure includes: A first discharge voltage and a second voltage smaller than the first voltage are determined for the battery, When the battery capacity of the battery is greater than a predetermined value, the battery is discharged so that a discharge voltage of the battery does not fall below a first discharge voltage; When the battery capacity of the battery is smaller than a predetermined value, the battery is discharged until a discharge voltage of the battery becomes a second discharge voltage. How to use the battery. Effect of the Invention
[0011] The present disclosure makes it possible to provide a battery capable of suppressing a decrease in battery capacity, a method for manufacturing a battery, and a method for using a battery. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view showing the configuration of a battery according to a first embodiment. [Diagram 2] 4 is a flowchart showing a method of using the battery according to the first embodiment. [Diagram 3] 4 is a flowchart showing a method for manufacturing a battery according to the first embodiment. [Figure 4] 1A to 1C are schematic cross-sectional views for illustrating a method for manufacturing a battery according to a first embodiment. [Diagram 5] 1 is a graph showing the results of performance tests in examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (First embodiment) <Battery configuration> Hereinafter, a first embodiment of the present disclosure will be described in detail with reference to the drawings. First, the configuration of the battery according to the present embodiment will be described in detail. Fig. 1 is a schematic cross-sectional view showing the configuration of the battery according to the first embodiment.
[0014] FIG. 1(a) is a schematic cross-sectional view illustrating a portion of a battery according to a first embodiment. The battery 1 according to this embodiment is a lithium ion secondary battery having a laminated structure as shown in Fig. 1(a) . The battery 1 according to this embodiment includes a positive electrode layer PL, a negative electrode layer NL, an alloy layer AL, a current collector C, and an electrolyte layer EL.
[0015] For example, the battery 1 according to this embodiment may be a bipolar lithium ion secondary battery having a structure in which a plurality of bipolar electrodes are stacked with an electrolyte layer EL interposed therebetween. Fig. 1(b) is a schematic cross-sectional view showing an example of the configuration of an electrode used in the battery according to this embodiment. The bipolar electrode BE shown in Fig. 1(b) has a negative electrode layer NL and an alloy layer AL on one side of a current collector C. Furthermore, the bipolar electrode BE has a positive electrode layer PL on the other side of the current collector C. By stacking bipolar electrodes BE as shown in FIG. 1(b) with electrolyte layers EL interposed therebetween, a stacked structure as shown in FIG. 1(a) can be formed inside the battery 1.
[0016] However, the battery according to this embodiment is not limited to the bipolar type. 1(c) and 1(d) are schematic cross-sectional views showing other examples of the configuration of the electrodes used in the battery according to this embodiment. 1(c) includes a negative electrode layer NL and an alloy layer AL on both sides of a current collector C. Also, a positive electrode PE shown in FIG.
[0017] The battery according to the present disclosure may be, for example, a lithium secondary battery in which a negative electrode NE shown in FIG. 1(c) and a positive electrode PE shown in FIG. 1(d) are alternately stacked with an electrolyte layer EL interposed therebetween. Even with this configuration, the laminated structure shown in FIG. 1(a) can be formed in the battery 1.
[0018] Furthermore, the battery according to the present disclosure is not limited to a stacked type battery. For example, a battery according to the present disclosure may be constructed by immersing a current collector C having a positive electrode layer PL and a current collector C having a negative electrode layer NL and an alloy layer AL in an electrolyte.
[0019] In other words, the battery according to the present disclosure may have any configuration as long as it includes a positive electrode layer PL, a negative electrode layer NL, an alloy layer AL, and a current collector C, and the alloy layer AL is located between the negative electrode layer NL and the current collector C.
[0020] Returning to the explanation of Figure 1(a). The current collector C is an electric conductor. The current collector C has a positive electrode layer PL and an alloy layer AL on its surface. The current collector C also has a negative electrode layer NL on its surface, with the alloy layer AL interposed therebetween.
[0021] When the battery 1 is a bipolar battery, the current collector C is a plate-shaped conductor having a negative electrode layer NL and an alloy layer AL on one side and a positive electrode layer PL on the other side. Furthermore, when the battery 1 is a battery other than a bipolar type battery, some of the current collectors C have a negative electrode layer NL and an alloy layer AL on the surface, and some of the current collectors C have a positive electrode layer PL on the surface.
[0022] When the battery 1 is discharged, the current collector C receives electrons from the negative electrode layer NL through the alloy layer AL and supplies the electrons to the positive electrode layer PL. During charging of the battery 1, the current collector C receives electrons from the positive electrode layer PL and supplies the electrons to the negative electrode layer NL via the alloy layer AL.
[0023] The current collector C may be made of any material that is applicable to current collectors of lithium ion secondary batteries. The material used for the current collector C may be, for example, a metal or a conductive resin.
[0024] Specific examples of materials used for the current collector C include carbon-containing acrylic resins, polythiophene-based resins, polyacetylene-based resins, polyaniline-based resins, copper, and aluminum.
[0025] The positive electrode layer PL is a layer formed on the surface of the current collector C. The positive electrode layer PL contains a lithium compound as a positive electrode active material. The positive electrode layer PL accepts electrons from the current collector C and accepts lithium ions from the electrolyte layer EL when the battery 1 is discharged. When the battery 1 is charged, the positive electrode layer PL releases electrons to the current collector C and releases lithium ions to the electrolyte layer EL.
[0026] The positive electrode active material contained in the positive electrode layer PL may be any lithium compound that is applicable as a positive electrode active material for lithium ion secondary batteries. For example, the positive electrode active material contained in the positive electrode layer PL may be a material containing an oxide of cobalt, nickel, iron, manganese, aluminum, or the like, or may contain a phosphate compound of these metals.
[0027] Specific examples of the positive electrode active material contained in the positive electrode layer PL include LiCoO2, LiNiO2, LiMn2O4, LiNi x Co y O2, LiNi x Co y Al z O2, LiNi x Co y Mn z O2, LiFePO4, etc. In the above composition formula, x, y, and z are real numbers of 0 or more.
[0028] The negative electrode layer NL is a layer formed on the surface of the current collector C via the alloy layer AL. The negative electrode layer NL contains a negative electrode active material. When the battery 1 is discharged, the negative electrode layer NL releases electrons to the current collector C through the alloy layer AL and releases lithium ions to the electrolyte layer EL. When the battery 1 is charged, the negative electrode layer NL accepts electrons from the current collector C through the alloy layer AL and accepts lithium ions from the electrolyte layer EL.
[0029] More specifically, the negative electrode layer NL contains a negative electrode active material having an electrode potential lower than that of the lithium alloy contained in the alloy layer AL. However, the electrode potential referred to here may refer to, for example, a standard electrode potential. In this specification, the electrode potential may be used as an index for evaluating the difficulty of an electrode reaction occurring at the negative electrode during discharge. Therefore, a low electrode potential here means that an electrode reaction occurs more easily at the negative electrode during discharge.
[0030] In other words, the negative electrode active material having a lower electrode potential than the lithium alloy contained in the alloy layer AL refers to a negative electrode active material that is more likely to release lithium ions and electrons than the lithium alloy contained in the alloy layer AL when the battery is discharged. In addition, the negative electrode active material having an electrode potential lower than that of the lithium alloy contained in the alloy layer AL may be rephrased as a negative electrode active material that is more base than the lithium alloy contained in the alloy layer AL.
[0031] The negative electrode active material contained in the negative electrode layer NL may be any compound that is applicable as a negative electrode active material for lithium ion secondary batteries. The negative electrode active material contained in the negative electrode layer NL may be, for example, a graphite-based, silicon-based, or titanium oxide-based negative electrode active material. Specific examples of the negative electrode active material contained in the negative electrode layer NL include LiC6, Li 4.4 Si, Li4Ti5O 12 etc.
[0032] The electrolyte layer EL is a layer located between the positive electrode layer PL and the negative electrode layer NL, and contains an electrolyte capable of accepting lithium ions. When the battery 1 is discharged, the electrolyte layer EL receives lithium ions from the negative electrode layer NL and inserts lithium ions into the positive electrode layer PL. During charging of the battery 1, the electrolyte layer EL receives lithium ions from the positive electrode layer PL and inserts lithium ions into the negative electrode layer NL.
[0033] The solid electrolyte contained in the electrolyte layer EL may be any compound that can be used as a solid electrolyte for a lithium ion secondary battery. The electrolyte used as the main component of the electrolyte layer EL may be a sulfide-based electrolyte. A specific example is Li a S b P c S d Cl e , Li a Ge b P c S d , Li a P b S c Cl d , Li a P b S c In the above formula, a, b, c, d, and e are each a real number of 0 or more.
[0034] The alloy layer AL is a layer located between the negative electrode layer and the current collector, and contains a lithium alloy. More specifically, the alloy layer AL contains a lithium alloy having a higher electrode potential than the negative electrode active material contained in the negative electrode layer NL.
[0035] As described above, in this specification, the electrode potential may be used as an index for evaluating the difficulty of an electrode reaction occurring at the negative electrode during discharge. Therefore, the lithium alloy having a higher electrode potential than the negative electrode active material contained in the negative electrode layer NL refers to a lithium alloy that is less likely to release lithium ions and electrons than the negative electrode active material contained in the negative electrode layer NL when the battery is discharged. The "lithium alloy having a higher electrode potential than the negative electrode active material contained in the negative electrode layer NL" may be rephrased as a lithium alloy that is more noble than the negative electrode active material contained in the negative electrode layer NL.
[0036] When the battery 1 is discharged, the alloy layer AL transfers electrons released from the negative electrode layer NL to the current collector C. When the battery 1 is charged, the alloy layer AL transfers electrons received from the current collector C to the negative electrode layer NL.
[0037] In addition, in the step of discharging the battery 1 until the voltage reaches a second discharge voltage described below, the alloy layer AL releases lithium contained as a lithium alloy into the negative electrode layer NL in the form of lithium ions. Here, the step of discharging the battery 1 until the voltage reaches a second discharge voltage, which will be described later, is a step that is executed when the battery capacity of the battery 1 decreases.
[0038] That is, when the battery capacity of the battery 1 decreases, the alloy layer AL releases lithium contained as a lithium alloy to the negative electrode layer NL in the form of lithium ions. With this configuration, the battery 1 according to this embodiment can replenish lithium that moves between the positive electrode layer PL and the negative electrode layer NL when the battery capacity of the battery 1 decreases. As a result, the battery 1 according to this embodiment can suppress the decrease in battery capacity.
[0039] The alloy contained in the alloy layer AL may be, for example, an alloy of lithium and one or more metals selected from the group consisting of tin, aluminum, bismuth, indium, silver, and antimony.
[0040] A suitable combination of the negative electrode active material contained in the negative electrode layer NL and the alloy contained in the alloy layer AL is, for example, Li 4.4 A combination of Si and a lithium-tin alloy is given. However, the combination of the negative electrode active material contained in the negative electrode layer NL and the alloy contained in the alloy layer AL is not limited to this, and any combination may be used as long as the electrode potential of the lithium alloy is higher than that of the negative electrode active material contained in the negative electrode layer NL.
[0041] <How to use the battery> Next, a detailed description will be given of a method of using the battery according to the first embodiment. Fig. 2 is a flowchart for explaining the method of using the battery according to the first embodiment. In the following description, FIG. 1(a) will be referred to as appropriate.
[0042] In the method of using the battery according to this embodiment, a first discharge voltage and a second discharge voltage that is smaller than the first voltage value are defined for the battery 1. Here, the first discharge voltage is preferably a voltage greater than the discharge voltage at which lithium ions start to be released from the alloy layer AL. Moreover, the second discharge voltage is preferably a voltage lower than the discharge voltage at which lithium ions start to be released from the alloy layer AL.
[0043] In the method of using the battery according to this embodiment, first, a step of discharging the battery so that the voltage does not fall below a first discharge voltage (step ST101) is performed. The discharge performed in step ST101 may be a discharge for utilizing the power stored in the battery 1 for various purposes. In other words, step ST101 may be a step of utilizing the battery 1.
[0044] Note that step ST101 may be executed multiple times before executing step ST102. In this case, step ST101 may be a process of discharging and charging the battery so that the voltage does not fall below the first discharge voltage. For example, the user of the battery 1 may execute step ST102 after executing step ST101 a predetermined number of times.
[0045] Next, a step of determining whether or not the battery capacity is smaller than a predetermined value (step ST102) is executed. If the battery capacity is not smaller than the predetermined value (NO in step ST102), the method of using the battery according to the first embodiment is completed.
[0046] If the battery capacity is smaller than the predetermined value (YES in step ST102), the step of discharging the battery until the battery voltage reaches the second discharge voltage (step ST103) is executed, and the method of using the battery according to the first embodiment is completed.
[0047] As described above, by performing step ST103, the alloy layer AL releases lithium ions to the negative electrode layer NL. When the alloy layer AL releases lithium ions to the negative electrode layer NL, the lithium moving between the positive electrode layer PL and the negative electrode layer NL is replenished.
[0048] That is, by performing step ST103, lithium that moves between the positive electrode layer PL and the negative electrode layer NL is replenished. As a result, by performing step ST103, a decrease in the battery capacity of the battery 1 caused by the loss of lithium that moves between the positive electrode layer PL and the negative electrode layer NL is suppressed.
[0049] <Battery manufacturing method> Next, a method for manufacturing the battery according to the first embodiment will be described in detail. Fig. 3 is a flow chart for explaining the manufacturing method of the battery according to the first embodiment. Fig. 4 is a schematic cross-sectional view for explaining the manufacturing method of the battery according to the first embodiment. More specifically, Fig. 4 is a schematic cross-sectional view showing the configuration of the battery 1 at the timing when step ST204 shown in Fig. 3 is completed.
[0050] In the method for manufacturing the battery according to the first embodiment, first, a step of forming a metal layer (step ST201) is performed. Here, the metal layer is a film containing a metal that is a precursor of the lithium alloy contained in the above-mentioned alloy layer AL. In other words, the metal layer is a film that corresponds to the alloy layer AL of the battery 1, but differs from the alloy layer AL in that it does not contain lithium.
[0051] In step ST201, the metal layer may be formed on the surface of the current collector C by, for example, ion sputtering. In step ST201, the metal layer may be formed on the surface of the plate-like member or film by, for example, ion sputtering, and then the metal layer may be peeled off from the plate-like member or film.
[0052] Next, a process of depositing a negative electrode layer (step ST202) is performed. For example, the negative electrode layer may be formed by applying a negative electrode slurry containing a negative electrode active material, a binder, and a solvent onto the surface of a plate-like member or a film, and drying the applied negative electrode slurry. Then, the negative electrode layer may be peeled off from the surface of the plate-like member or the film. Furthermore, for example, the negative electrode layer may be formed by applying a negative electrode slurry to the surface of the above-mentioned metal layer and drying the applied negative electrode slurry.
[0053] Next, a step of depositing a positive electrode layer (step ST203) is performed. For example, the positive electrode layer may be formed by applying a positive electrode slurry containing a positive electrode active material, a binder, and a solvent onto the surface of a plate-like member or a film, and drying the applied negative electrode slurry. The positive electrode layer may then be peeled off from the surface of the plate-like member or the film. Also, for example, the positive electrode layer may be formed by applying a positive electrode slurry to the surface of a current collector and drying the applied positive electrode slurry.
[0054] Note that steps ST201 to ST203 may be executed in an order different from the order described above. Also, steps ST201 to ST203 may be executed in parallel.
[0055] Next, the metal layer, the negative electrode layer, and the positive electrode layer formed in steps ST201 to ST203 are laminated (step ST204). More specifically, the metal layer, the negative electrode layer, and the positive electrode layer are laminated so as to be arranged as shown in FIG.
[0056] That is, in step ST204, the metal layer ML is laminated so as to be located between the negative electrode layer NL and the current collector C. In step ST204, the positive electrode layer PL and the negative electrode layer NL are laminated so as to face each other with the electrolyte layer EL interposed therebetween.
[0057] Finally, a step of passing current through the metal layer, the negative electrode layer, and the positive electrode layer (step ST205) is performed, completing the method for manufacturing the battery according to this embodiment. More specifically, in step ST205, an alloy of the metal contained in the metal layer and lithium is generated in the metal layer by passing current through the metal layer, the negative electrode layer, and the positive electrode layer. That is, by performing step ST205, the metal layer ML is converted into the alloy layer AL. Note that step ST205 may be executed as a step of charging the battery 1.
[0058] By using the manufacturing method as described above, the battery 1 according to this embodiment can be manufactured. EXAMPLES
[0059] Hereinafter, the negative electrode for secondary batteries according to the first embodiment will be described in more detail by way of examples. However, the negative electrode for secondary batteries according to the first embodiment is not limited to only the following examples.
[0060] (Example) <Preparation of positive electrode layer> LiNi 0.8 Co 0.15 Al 0.05 O2, Li2S-P2S5, vapor grown carbon fiber, PVDF (Polyvinylidene Difluoride) binder, and butyl butyrate were mixed in a weight ratio of 88.2:9.8:1.3:0.7 and stirred with an ultrasonic disperser. The obtained mixture was applied onto an aluminum foil and a stainless steel foil as a positive electrode slurry, and these were heated and dried using a hot plate to prepare a positive electrode layer.
[0061] <Preparation of negative electrode layer> Powdered silicon, Li2S-P2S5, PVDF binder, and vapor grown carbon fiber were mixed in a weight ratio of 100:77.6:2:15 and stirred with an ultrasonic disperser. The obtained mixture was applied onto nickel foil and stainless steel foil as a negative electrode slurry, and these were heated and dried on a hot plate to prepare a negative electrode layer.
[0062] <Preparation of solid electrolyte layer> Li2S-P2S5:PVDF-based binder were mixed in a weight ratio of 99.4:0.4 and stirred with an ultrasonic dispersing device. The resulting mixture was applied as an electrolyte layer slurry onto the positive electrode layer to prepare an electrolyte layer.
[0063] <Preparation of current collector> Carbon, acrylic resin, and a solvent were mixed to obtain a paste-like mixture. The resulting mixture was applied onto a PET (PolyEthylene Terephthalate) film and then dried by heating. The PET film was peeled off from the resulting thin film to obtain a foil-shaped current collector.
[0064] <Preparation of metal layer> A tin metal layer was formed on one surface of a foil-shaped current collector by ion sputtering.
[0065] <Battery Construction> A stainless steel foil having a negative electrode layer formed on its surface and an aluminum foil having a positive electrode layer and a solid electrolyte layer formed on its surface were laminated in the order of stainless steel foil, negative electrode layer, solid electrolyte layer, positive electrode layer, and aluminum foil. The resulting laminate was pressed while being heated by a roll press. The stainless steel foil was peeled off from the pressed laminate to obtain a first laminate.
[0066] A nickel foil having a negative electrode layer formed on its surface and a stainless steel foil having a positive electrode layer and a solid electrolyte layer formed on its surface were laminated in the order of nickel foil, negative electrode layer, solid electrolyte layer, positive electrode layer, and stainless steel foil. The obtained laminate was pressed while being heated by a roll press. The stainless steel foil was peeled off from the pressed laminate to obtain a second laminate.
[0067] The first laminate, the second laminate, and the current collector having a metal layer formed on the surface were laminated in the following order: nickel foil, anode layer, solid electrolyte layer, cathode layer, current collector, metal layer, anode layer, solid electrolyte layer, cathode layer, and aluminum foil. The obtained laminate was pressed while being heated by a roll press. A circular laminate of 1 cm2 was punched out from the pressed laminate to obtain a third laminate. The third laminate was sandwiched between two restraining plates to prepare a battery according to this example.
[0068] (Comparative Example) A battery was produced in the same manner as in the example, except that no metal layer was formed.
[0069] (Charge / discharge test) The fabricated battery was subjected to constant current charging at a current of 1 / 10 C until the control voltage reached 8.10 V. The fabricated battery was then subjected to constant voltage charging at a control voltage of 8.10 V until the current reached 1 / 100 C. Hereinafter, the above process will be referred to as the charging process.
[0070] The unit of current, C, is the C rate, and this also applies to the steps described below. 1C is defined as the magnitude of the constant current when a battery is completely discharged in one hour when it is discharged from a fully charged state at a constant current.
[0071] Next, the fabricated battery was subjected to constant current discharge at a current of 1 / 10 C until the control voltage reached 5.0 V. Then, the fabricated battery was subjected to constant voltage discharge at a control voltage of 5.0 V until the current reached 1 / 100 C. Hereinafter, the above process is referred to as the discharge process. The discharging step corresponds to step ST103 in FIG. 2, that is, the step of discharging the battery until the battery voltage reaches the second discharge voltage.
[0072] Next, a process of constant current charging at a current of 2 C until the control voltage reached 8.10 V and a process of constant current discharging at a current of 2 C until the control voltage reached 5.0 V were alternately repeated 20 times each. Hereinafter, the above process will be referred to as a cycle charge / discharge process. The step of performing constant current discharge in the cyclic charge / discharge process corresponds to step ST101 in FIG. 2, that is, the step of discharging the battery so that the voltage does not fall below the first discharge voltage.
[0073] The charging step, the discharging step, and the cyclic charging / discharging step were repeated three times in the order described above, and the discharge capacity was measured at the end of the discharging step and at the end of the constant current discharge performed in the cyclic charging / discharging step.
[0074] FIG. 5 shows the measurement results of the discharge capacity in the charge-discharge test. Fig. 5 is a graph showing the results of a charge / discharge test. More specifically, Fig. 5(a) is a graph showing the results of a charge / discharge test of a battery according to an embodiment, Fig. 5(b) is a graph showing the results of a charge / discharge test of a battery according to a comparative example, and Fig. 5(c) is a graph showing the results of the charge / discharge test of a battery according to an embodiment and the results of the charge / discharge test of a battery according to a comparative example superimposed on each other.
[0075] As shown in Figures 5(a) and 5(c), the discharge capacity of the battery according to the embodiment gradually decreases with each repetition of charging and discharging in the cycle charging and discharging process. However, the discharge capacity of the battery according to the embodiment is restored by performing the discharging process. As a result, the battery according to the embodiment maintains a discharge capacity of 1.2 mAh or more even at the end of the third cycle charging step.
[0076] In contrast, in the battery according to the comparative example, as shown in FIG. 5(b) and FIG. 5(c), the battery capacity does not recover even when the discharging process is performed. As a result, the comparative battery was unable to maintain a discharge capacity of 1.2 mAh or more at the end of the third cycle charging step.
[0077] Thus, the battery according to this embodiment, that is, the battery produced in the Examples, exhibits clearly superior charge / discharge cycle characteristics compared to the battery produced in the Comparative Examples.
[0078] A part or all of the above-described embodiments can be described as, but is not limited to, the following supplementary notes. (Appendix 1) a negative electrode layer containing a negative electrode active material; an alloy layer that is located between the negative electrode layer and a current collector and contains a lithium alloy and has an electrode potential higher than that of the negative electrode active material; A positive electrode layer containing a lithium compound as a positive electrode active material. battery. (Appendix 2) an electrode including the negative electrode layer and the alloy layer on one surface of the current collector and the positive electrode layer on the other surface of the current collector, the electrode being laminated with an electrolyte interposed therebetween; 2. A battery as described in Appendix 1. (Appendix 3) a first current collector having the negative electrode layer and the alloy layer on both sides thereof; a second current collector having the positive electrode layer on both sides thereof; The first and second current collectors are alternately stacked with an electrolyte interposed therebetween. 2. A battery as described in Appendix 1. (Appendix 4) The lithium alloy is an alloy of lithium and one or more metals selected from the group consisting of tin, aluminum, bismuth, indium, silver, and antimony. 4. The battery according to claim 1. (Appendix 5) The negative electrode active material is LiC6, Li 4.4 Si and Li4Ti5O 12 One or more selected from the group consisting of: 5. The battery according to claim 1. (Appendix 6) the lithium alloy is an alloy of tin and lithium; The negative electrode active material is silicon. 6. The battery according to any one of claims 1 to 5. (Appendix 7) a negative electrode layer containing a negative electrode active material; an alloy layer that is located between the negative electrode layer and a current collector and contains a lithium alloy and has an electrode potential higher than that of the negative electrode active material, on one surface of the current collector; a positive electrode layer containing a lithium compound as a positive electrode active material on the other surface of the current collector; electrode. (Appendix 8) a negative electrode layer containing a negative electrode active material; an alloy layer containing a lithium alloy and having an electrode potential higher than that of the negative electrode active material, the alloy layer being located between the negative electrode layer and a current collector and provided on both sides of the current collector; electrode. (Appendix 9) For the battery according to any one of claims 1 to 6, a first discharge voltage and a second voltage lower than the first voltage are defined; When the battery capacity of the battery is greater than a predetermined value, the battery is discharged so that a discharge voltage of the battery does not fall below a first discharge voltage; When the battery capacity of the battery is smaller than a predetermined value, the battery is discharged until a discharge voltage of the battery becomes a second discharge voltage. How to use the battery. (Appendix 10) forming a metal layer containing a metal; forming a negative electrode layer containing a negative electrode active material; forming a positive electrode layer containing a lithium compound as a positive electrode active material; laminating the metal layer, the negative electrode layer, and the positive electrode layer; and generating an alloy of the metal and lithium in the metal layer by passing current through the laminated metal layer, the negative electrode layer, and the positive electrode layer. How batteries are manufactured.
[0079] While the present invention has been described above with reference to the above-described embodiment, the present invention is not limited to the configuration of the above-described embodiment, and of course includes various modifications, alterations, and combinations that may be made by a person skilled in the art within the scope of the invention as defined in the claims of the present application. [Explanation of symbols]
[0080] 1. 1M battery, C current collector, PL positive electrode layer, NL negative electrode layer, EL electrolyte layer AL alloy layer, ML metal layer
Claims
1. a negative electrode layer containing a negative electrode active material; an alloy layer that is located between the negative electrode layer and a current collector and contains a lithium alloy and has an electrode potential higher than that of the negative electrode active material; A positive electrode layer containing a lithium compound as a positive electrode active material. battery.
2. The lithium alloy is an alloy of lithium and one or more metals selected from the group consisting of tin, aluminum, bismuth, indium, silver, and antimony.
10. The battery of claim 1.
3. the lithium alloy is an alloy of tin and lithium; The negative electrode active material is silicon.
3. The battery of claim 2.
4. A method for producing a battery according to any one of claims 1 to 3, comprising: determining a first discharge voltage and a second voltage that is smaller than the first voltage; Discharging the battery so that the discharge voltage of the battery does not fall below a first discharge voltage; When the battery capacity of the battery is smaller than a predetermined value, the battery is discharged until a discharge voltage of the battery becomes a second discharge voltage. How to use the battery.
5. forming a metal layer containing a metal; forming a negative electrode layer containing a negative electrode active material; forming a positive electrode layer containing a lithium compound as a positive electrode active material; laminating the metal layer, the negative electrode layer, and the positive electrode layer; and generating an alloy of the metal and lithium in the metal layer by passing current through the laminated metal layer, the negative electrode layer, and the positive electrode layer. How batteries are manufactured.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP2004063394A
Nonaqueous electrolyte secondary battery
JP2004213946A
All-solid type secondary battery, and manufacturing method thereof
JP2021068706A
Polymer secondary battery and method for producing same
WO2011102453A1
Lithium ion secondary battery
WO2014128905A1