Manufacturing method for parison for balloon catheter, manufacturing method for balloon catheter, and manufacturing device for parison for balloon catheter

By employing a controlled heating and cooling process on separated thermoplastic tubes, the method stabilizes the parison shape, addressing shape instability issues in balloon catheter manufacturing.

JP2024162784APending Publication Date: 2024-11-21TERUMO KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023078676
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The existing methods for manufacturing a parison for balloon catheters result in unstable shape formation due to unclear temperature differences between heated and unheated parts of the tube, affecting the stability of the balloon shape.

Method used

A method involving a pair of thermoplastic tubes separated in the longitudinal direction with fixed, heated, and cooled regions, followed by controlled stretching to create a clear temperature difference and stabilize the parison shape.

Benefits of technology

The method allows for stable formation of the parison shape by clearly defining temperature differences, ensuring consistent balloon catheter production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162784000001_ABST
    Figure 2024162784000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a parison for a balloon catheter, a manufacturing method for a balloon catheter, and a manufacturing device for a parison for a balloon catheter that can stably form a shape of a parison by lowering a heating temperature of a tube.SOLUTION: A manufacturing method for a parison 20 for a balloon catheter includes: a fixing step of fixing a thermoplastic tube 30 extending along a longitudinal direction with a pair of fixing areas 31, 31; a heating step of heating a pair of heating areas 32, 32 located between the pair of fixing areas 31, 31; a cooling step of cooling at least a part of the area between the pair of heating areas 32, 32 of the tube 30 during the heating step; and a stretching step of pulling the tube 30 in a direction in which the pair of fixing areas 31, 31 are separated and stretching the pair of heating areas 32, 32, wherein a large diameter portion 21 having an outer diameter larger than a portion stretched is formed between the pair of heating areas 32, 32 stretched in the stretching step.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a parison, which is an intermediate product in the manufacture of a balloon of a balloon catheter, a method for manufacturing a balloon catheter, and an apparatus for manufacturing a parison for a balloon catheter. [Background technology]

[0002] Balloon catheters are widely used to treat lesions (stenosis) that occur in biological lumens. A balloon catheter usually has a long shaft and a balloon that is provided at the tip of the shaft and can expand in the radial direction. The balloon is contracted and reaches a target location inside the body via a narrow biological lumen, and then expanded to expand the lesion.

[0003] The main components of a balloon catheter are the balloon and the shaft, as mentioned above. A balloon is formed by processing a tube formed by extrusion molding or the like into an intermediate product called a parison, and then biaxially stretching the parison in the radial and axial directions to finally form the balloon. The formed balloon is attached to the shaft and assembled. The manufacturing method for processing the tube, via the parison, into a balloon is disclosed in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 141382 Summary of the Invention [Problem to be solved by the invention]

[0005] The processing from a tube to a parison is performed by stretching a part of the tube in the longitudinal direction on both sides of the part to be processed into a balloon, while maintaining the original diameter of the part in the longitudinal direction. The part of the parison stretched in the longitudinal direction of the tube is oriented and has high strength. Therefore, when the parison is biaxially stretched, the part of the tube stretched in the longitudinal direction does not expand, and only the part of the tube that maintains its original diameter expands to form a balloon.

[0006] When producing a parison, both longitudinal sides of the tube to be processed into a balloon are heated and stretched in the longitudinal direction. The tube is heated by arranging the portion to be heated so that it is surrounded by the heating surface of a heating means having an internal space. However, when heat is transferred from the portion of the tube to the portion not heated by the heating means, the boundary between the heated portion and the non-heated portion becomes unclear, and the shape of the parison formed may become unstable. If the shape of the parison is unstable, it may affect the shape of the balloon formed from the parison.

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide a method and an apparatus for manufacturing a parison for a balloon catheter, which can clearly determine the temperature difference between heated and non-heated parts of a tube and stably form the shape of the parison. [Means for solving the problem]

[0008] To achieve the above object, (1) a method for producing a parison for a balloon catheter includes a fixing step of fixing a thermoplastic tube extending along a longitudinal direction at a pair of fixing regions spaced apart in the longitudinal direction, a heating step of heating a pair of heated regions of the tube between the pair of fixing regions and spaced apart in the longitudinal direction, a cooling step of cooling at least a part of the region of the tube between the pair of heated regions during the heating step, and a stretching step of pulling the tube in a direction in which the pair of fixing regions are separated, thereby stretching the pair of heated regions of the tube heated in the heating step, and forming a thick-diameter portion between the pair of heated regions stretched in the stretching step, the thick-diameter portion having an outer diameter larger than that of the stretched portion.

[0009] (9) A manufacturing apparatus for a parison for a balloon catheter that achieves the above-mentioned object includes a fixing mechanism that fixes a thermoplastic tube extending along a longitudinal direction at a pair of fixing regions spaced apart in the longitudinal direction, a heating mechanism that heats a pair of heating regions that are spaced apart in the longitudinal direction between the pair of fixing regions of the tube, a cooling mechanism that cools the region of the tube between the pair of heating regions, and a pulling mechanism that moves the fixing mechanism in a direction that increases the distance between the pair of fixing regions of the tube. Effect of the Invention

[0010] In the method for manufacturing a parison for a balloon catheter configured as described above, when the tube is heated, a clear temperature difference can be created between the region between the pair of heating regions and the heating region of the tube, so that the shape of the parison can be stably formed in the stretching process.

[0011] (2) In the method for producing a parison for a balloon catheter according to (1) above, in the cooling step, at least a part of a cooling means may be in contact with the surface of the tube, thereby making it possible to stably cool the tube by thermal conduction.

[0012] (3) In the method for producing a parison for a balloon catheter according to (1) above, in the cooling step, the cooling means may cool a space surrounded by walls having a rectangular cross section cut along a plane perpendicular to the longitudinal axis, thereby making it possible to stably cool the tube by a combination of radiant heat and convective heat transfer.

[0013] (4) In the method for producing a parison for a balloon catheter according to (2) or (3) above, the surface of the region between the pair of heating regions may be maintained at a temperature lower than the glass transition temperature of the tube in the cooling step, thereby suppressing a temperature rise in the portion that will become the large-diameter portion of the tube and enabling the shoulder of the produced parison to be clearly shaped.

[0014] (5) In any one of the above (2) to (4) methods for producing a parison for a balloon catheter, the surface of the heated region may be maintained at a temperature higher than the glass transition temperature of the tube in the heating step, thereby making it possible to reliably stretch the heated region of the tube in the stretching step and increase its strength.

[0015] (6) In the method for producing a parison for a balloon catheter according to any one of (1) to (5) above, the difference between the surface temperature of the tube in the heating step and the surface temperature of the tube in the cooling step can be 50° C. or more and 140° C. or less. This allows a sufficient temperature difference to be created between the heating region and the cooling region of the tube, allowing the shape of the large-diameter portion of the tube to be stably formed.

[0016] (7) In the method for producing a parison for a balloon catheter according to any one of (1) to (6) above, in the cooling step, the time from the start of cooling the tube to the state where the tube is maintained at a temperature lower than the glass transition temperature of the tube may be 5 seconds or more and 45 seconds or less, thereby ensuring that the unheated portion of the tube is cooled in accordance with the heating time of the tube.

[0017] (8) A method for producing a balloon catheter includes biaxially stretching the parison for a balloon catheter produced by any one of the production methods (1) to (7) above to form a balloon, and placing a shaft in the formed balloon. Since the shape of the parison for a balloon catheter is stably formed by any one of the production methods (1) to (10) above, a balloon catheter having a balloon with a stable shape can be produced.

[0018] The manufacturing apparatus for parisons for balloon catheters configured as described above can, when heating a tube, clearly create a temperature difference between the region between a pair of heating regions and the heating region of the tube, thereby stably forming the shape of the parison. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is an overall front view of the balloon catheter. [Diagram 2] FIG. 2 is an overall front view of the parison. [Diagram 3] FIG. 2 is an enlarged cross-sectional view of the central portion of the parison. [Figure 4] FIG. 2 is a front view of the parison manufacturing apparatus, showing a state in which a tube is fixed to a fixing mechanism portion. [Diagram 5] FIG. 2 is a front view of the parison manufacturing apparatus, showing the heating mechanism and the cooling mechanism in a closed state. [Figure 6] FIG. 13 is a cross-sectional view of a thermal mold in an open state with tubes in place. [Figure 7] FIG. 13 is a cross-sectional view of a thermal mold with tubes in a closed state. [Figure 8] FIG. 13 is a cross-sectional view of the open cooling mold with tubes in place. [Figure 9] FIG. 13 is a cross-sectional view of a cooling mold with tubes in a closed state. [Figure 10] FIG. 2 is a front view of the parison manufacturing apparatus, illustrating a state in which a tube is being stretched by a tension mechanism. [Figure 11]1A is an enlarged cross-sectional view of the vicinity of the center of the parison before biaxial stretching processing, and FIG. 1B is an enlarged cross-sectional view of the vicinity of the center of the parison after biaxial stretching processing. [Figure 12] FIG. 2 is an enlarged cross-sectional view of the vicinity of the balloon with a shaft installed in the manufactured balloon. [Figure 13] FIG. 1 is a cross-sectional view of a thermal mold in which multiple tubes are arranged. [Figure 14] FIG. 13 is a cross-sectional view of a cooling mold in which multiple tubes are arranged. [Figure 15] FIG. 13 is a cross-sectional view of a modified thermal mold in which a tube is disposed in an open state. [Figure 16] FIG. 13 is a cross-sectional view of a modified thermal mold in which a tube is disposed in a closed state. [Figure 17] FIG. 13 is a cross-sectional view of a modified cooling mold in which a tube is arranged in an open state. [Figure 18] FIG. 13 is a cross-sectional view of a cooling mold in a closed state according to a modified example in which a tube is arranged. [Figure 19] FIG. 13 is a cross-sectional view of a modified thermal mold in which multiple tubes are arranged in a closed state. [Figure 20] FIG. 13 is a cross-sectional view of a cooling mold in a closed state according to a modified example in which a plurality of tubes are arranged. [Figure 21] FIG. 13 is a cross-sectional view of a thermal mold according to a second modified example in which a tube is arranged in a closed state. [Figure 22] FIG. 11 is a cross-sectional view of a cooling mold according to a second modified example in which a tube is arranged, in a closed state. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the dimensional ratios in the drawings may be exaggerated for convenience of explanation and may differ from the actual ratios. In addition, in this specification, the side of the balloon catheter 10 that is inserted into a body lumen is referred to as the "distal end" or "distal side", and the side that is operated by the operator is referred to as the "base end" or "base side".

[0021] In the method for producing a parison for a balloon catheter according to the embodiment of the present invention, a part of a tube 30 made of a thermoplastic material is heated and stretched to produce a parison 20 in which the unheated part of the tube 30 is formed into a large diameter part 21 and the heated part of the tube 30 is formed into a small diameter part 22. A balloon 12 is formed from this parison 20, and the balloon catheter 10 is produced by placing the balloon 12 on the shaft 11.

[0022] 1, the manufactured balloon catheter 10 has a balloon 12 at the tip end of a long shaft 11, and a hub 13 is provided at the base end of the shaft 11. The balloon 12 can be expanded radially by an expansion fluid injected from the hub 13.

[0023] As shown in FIG. 2, the parison 20 extends along the long axis direction, has a large diameter portion 21 in the center in the long axis direction, and has thin diameter portions 22 on both sides of the large diameter portion 21 in the long axis direction, the thin diameter portions 22 having a smaller diameter than the large diameter portion 21.

[0024] 3, the parison 20 is a hollow tube. The large diameter portion 21 of the parison 20 has a same diameter portion 21a having the same diameter along the long axis direction, and an inclined shoulder portion 21b connecting the same diameter portion 21a and the small diameter portion 22 at both ends of the same diameter portion 21a in the long axis direction.

[0025] The parison 20 is made of a thermoplastic material. In this embodiment, the material forming the parison 20 is polyamide. The material forming the parison 20 is not limited to this, and for example, polyolefins such as polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ionomer, or a mixture of two or more of these, and thermoplastic resins such as soft polyvinyl chloride resin, polyamide elastomer, polyester, polyester elastomer, polyurethane, and fluororesin can be used.

[0026] A manufacturing device 50 and a manufacturing method for the parison 20 will be described. As shown in Fig. 4, the manufacturing device 50 for the parison 20 has a fixing mechanism 51 for fixing the tube 30, a heating mechanism 52 for heating a part of the tube 30, a cooling mechanism 55 for cooling another part of the tube 30, a pulling mechanism 53 for moving the fixing mechanism 51 to pull the tube 30 along the longitudinal direction, and a moving mechanism 54 for opening and closing the heating mechanism 52 and the cooling mechanism 55.

[0027] The fixing mechanism 51 fixes the tube 30 extending along the longitudinal direction at a pair of fixing regions 31, 31 spaced apart in the longitudinal direction. The fixing mechanism 51 has a through space through which both ends of the tube 30 can be inserted, and has fixing means for radially pressing and holding the inserted tube 30.

[0028] The heating mechanism 52 can heat a pair of heating regions 32, 32 that are spaced apart in the longitudinal direction between a pair of fixing regions 31 of the tube 30. The heating mechanism 52 is composed of a pair of thermal molds 70, 70 that are heat sources disposed on both radial sides of the tube 30. The thermal molds 70, 70 can be opened and closed by moving them close to and away from each other along the radial direction of the tube 30 by the moving mechanism 54. In FIG. 4, the thermal molds 70, 70 are in an open state in which they are spaced apart from each other to expose the heating region 32 of the tube 30.

[0029] The cooling mechanism 55 can cool at least a part of the region between the pair of heating regions 32, 32 of the tube 30. The cooling mechanism 55 is composed of a pair of cooling dies 100, 100, which are cooling means respectively arranged on both radial sides of the tube 30. The cooling dies 100, 100 can be opened and closed by moving them close to and away from each other along the radial direction of the tube 30 by the moving mechanism 54. In FIG. 4, the cooling dies 100, 100 are in an open state.

[0030] Pulling mechanism 53 has an arm 81 connected to fixing mechanism 51, and a main body 80 that extends and retracts arm 81. By causing main body 80 to extend and retract arm 81, fixing mechanism 51 can be moved along the longitudinal direction of tube 30, and tube 30 fixed to fixing mechanism 51 can be pulled along the longitudinal direction.

[0031] The movement mechanism 54 has an arm 91 connected to the hot mold 70 or the cold mold 100, and a main body 90 that extends and retracts the arm 91. The main body 90 extends and retracts the arm 91, thereby moving the hot molds 70, 70 and the cold molds 100, 100 facing each other so as to open and close.

[0032] To manufacture the parison 20, first, as shown in FIG. 4, the fixing regions 31, 31 of the tube 30 are fixed to the fixing mechanism parts 51, 51 of the manufacturing apparatus 50, respectively (fixing step). Next, as shown in FIG. 5, the moving mechanism part 54 brings the mutually facing thermal molds 70, 70 of the heating mechanism part 52 close to each other to be in a closed state, and the pair of heating regions 32, 32 of the tube 30 are covered and heated (heating step). Also, the moving mechanism part 54 brings the cooling molds 100, 100 of the cooling mechanism part 55 close to each other to be in a closed state to cover the region between the pair of heating regions 32, 32 of the tube 30, and cools them during the heating step (cooling step). The timing of closing the cooling mold 100 to start cooling may be the same as the timing of closing the thermal mold 70 of the heating mechanism part 52 to heat it, or there may be a slight time difference, such as closing the cooling mold 100 to start cooling before closing the thermal mold 70. The cooling step continues while the heating step is being performed.

[0033] As shown in Fig. 6, the pair of thermal molds 70, 70 have concave wall surfaces 72, 72 on the surfaces facing each other. The thermal mold 70 also has a heating section 71 inside. A heater can be used as the heating section 71. However, the heating section 71 may be provided on the outer surface of the thermal mold 70, or may be a heating means other than a heater. The heating section 71 heats the thermal mold 70, and the temperature of the wall surfaces 72 can be increased.

[0034] As shown in FIG. 7, the pair of thermal molds 70, 70 are in close proximity to each other in a closed state, thereby accommodating the tube 30 therein. The thermal molds 70, 70 in the closed state have a space 73 surrounded by wall surfaces 72 having a rectangular cross section cut along a plane perpendicular to the long axis direction. The wall surfaces 72 have a long wall 72a extending horizontally in the cross section cut along a plane perpendicular to the long axis direction, and a short wall 72b extending vertically, which is a different direction from the long wall 72a, and having a shorter length than the long wall 72a. The tube 30 disposed in the space 73 formed by the pair of thermal molds 70, 70 is in close proximity to the long wall 72a of the wall surfaces 72. The minimum distance Y between the wall surfaces 72 and the tube 30 is the distance between the long wall 72a and the tube 30, and is 0. <Y≦1.5mmである。

[0035] The temperature of the wall surface 72 is increased by the heating unit 71, and this generates radiant heat from the wall surface 72 and convective heat transfer within the space 73 heated by the wall surface 72, thereby heating the tube 30. The heating of the tube 30 is maintained for a certain period of time. In the heating process, the heat mold 70, which is a heat source, maintains the surfaces of the heating regions 32, 32 at a temperature higher than the glass transition temperature of the tube 30. In this embodiment, the heat mold 70 is heated to a temperature of 80° C. or higher and 160° C. or lower in the heating process. The heating process is performed for 1 second or higher and 30 seconds or shorter.

[0036] Since the wall surface 72 of the thermal mold 70 is close to the tube 30, the tube 30 can be stably heated by a combination of radiant heat and convective heat transfer. Therefore, even if the heating temperature of the thermal mold 70 is kept low, the tube 30 can be efficiently heated. In the heating process, by lowering the heating temperature of the thermal mold 70, so-called accidental heating of areas other than the heating area 32 of the tube 30 can be prevented, so that the temperature rise of the area can be suppressed. This allows the length of the parison 20 to be manufactured to be stably formed. Furthermore, the shape of the shoulder portion 21b of the parison 20 can be clearly formed, making it easier to identify the shape during inspection. Since the shape of the shoulder portion 21b of the parison 20 is clear, it can be determined that the large diameter portion 21 of the parison 20 has not been stretched. From the above, the parison 20 can be stably manufactured.

[0037] In this embodiment, the manufacturing apparatus 50 using the thermal mold 70 shown in FIGS. 6 and 7 has been described, but a conventional thermal mold may be used.

[0038] As shown in Fig. 8, a pair of cooling dies 100, 100 have concave wall surfaces 102, 102 facing each other. The cooling die 100 has a cooling part 101 therein, which can lower the temperature of the wall surface 102 and cool the tube 30 in the space 103. The cooling part 101 can be a heat transfer tube that flows cooling water. However, the cooling part 101 is not limited to a heat transfer tube as long as it is a means that can cool the cooling die 100.

[0039] 9, the cooling dies 100, 100 facing each other are brought close to each other to form a space 103 surrounded by walls 102, 102. The space 103 has a rectangular cross section cut along a plane perpendicular to the longitudinal direction, and can accommodate the tube 30.

[0040] When the pair of cooling dies 100, 100 are closed, the wall surface 102 has, in a cross section cut along a plane perpendicular to the long axis direction, a long wall 102a extending horizontally and a short wall 102b extending vertically, which is a different direction from the long wall 102a, and having a shorter length than the long wall 102a. The tube 30 disposed in the space 103 formed by the pair of cooling dies 100, 100 is adjacent to the long wall 102a of the wall surface 102.

[0041] By cooling the wall surface 102 by the cooling section 101, radiation cooling to the wall surface 102 and convection heat transfer within the space 103 cooled by the wall surface 102 occur, and the tube 30 can be cooled.

[0042] In the cooling step, the surface of the region between the pair of heating regions 32, 32 of the tube 30 is maintained below the glass transition temperature of the tube 30. In the cooling step, the time from the start of cooling of the tube 30 to the state where the temperature is maintained below the glass transition temperature of the tube 30 is 5 seconds or more and 45 seconds or less. In addition, the difference between the surface temperature of the tube 30 in the heating step and the surface temperature of the tube 30 in the cooling step is 50°C or more and 140°C or less. In the cooling step, the region that will become the large diameter portion 21 of the tube 30 is cooled while the region that will be stretched in the stretching step is heated, and the temperature difference between the two regions can be clearly created. This suppresses the temperature rise of the portion that will become the large diameter portion 21 of the tube 30, and the shape of the shoulder portion 21b of the parison 20 to be manufactured can be clearly formed, and the parison 20 can be stably manufactured.

[0043] After the heating step heats the heating region 32 of the tube 30 while cooling a part of the tube 30 in the cooling step, the heating and cooling of the tube 30 are stopped, and as shown in FIG. 10, the tube 30 is pulled by the pulling mechanism 53 in a direction in which the pair of fixed regions 31, 31 are separated, and the pair of heated regions 32, 32 heated in the heating step of the tube 30 are stretched (stretching step). During the stretching step, the moving mechanism 54 opens the heating mold 70 and the cooling mold 100, thereby separating the heating mold 70 and the cooling mold 100 from the surface of the tube 30. The heating mold 70 and the cooling mold 100 may be opened at the same time as the start of the stretching step after the heating step, or may be opened during the stretching step. When the cooling step is performed with the cooling mold 100 whose wall surface 102 is close to the surface of the tube 30, the stretching step may be performed after the cooling step with the cooling molds 100, 100 closed.

[0044] The stretching process stretches the heated region 32 of the tube 30 in the longitudinal direction, and the stretched portion is oriented and strengthened. The stretching process forms a thick-diameter portion 21 having an outer diameter larger than that of the thin-diameter portion 22 between a pair of heated regions 32, 32 that have been stretched to form the thin-diameter portion 22 in the tube 30.

[0045] The balloon 12 is formed by biaxially stretching the large diameter portion 21 of the parison 20 shown in FIG. 11(a) and expanding it as shown in FIG. 11(b). The biaxial stretching of the large diameter portion 21 is performed by blow molding so as to expand the large diameter portion 21 in two axial directions, the longitudinal direction and the radial direction. During the biaxial stretching, only the portion of the large diameter portion 21 of the tube 30 that is not stretched expands, forming the intermediate portion 12c and the distal end portion 12a and the proximal end portion 12b extending before and after it. After the parison 20 is biaxially stretched, both ends in the longitudinal direction are cut so that a predetermined length remains as the distal end portion 12a and the proximal end portion 12b, and the balloon 12 can be obtained. Details of the biaxial stretching process can be appropriately adopted by known methods. The intermediate portion 12c of the balloon 12 has the function of pushing open a narrowed portion or the like when it is expanded. The distal end portion 12a and the proximal end portion 12b are liquid-tightly joined to the shaft 11, as described later.

[0046] Once the balloon 12 is formed, a shaft 11 having a hub 13 is placed on the formed balloon 12. Specifically, as shown in Fig. 12, an inner tube shaft 11a is fixed to a tip end 12a of the balloon 12 by a known method such as fusion, an outer tube shaft 11b disposed outside the inner tube shaft 11a is fixed to a base end 12b of the balloon 12 by a similar method, and the shaft 11 is placed on the balloon 12, thereby manufacturing a balloon catheter 10.

[0047] The method for manufacturing a parison for a balloon catheter according to this embodiment can also process a plurality of tubes 30 at once to manufacture a plurality of parisons 20. As shown in Fig. 13, a plurality of tubes 30 can be arranged along the long wall 72a of the wall surface 72 in the space 73 of the thermal molds 70, 70 of the heating mechanism unit 52. The plurality of tubes 30 arranged in the space 73 are heated by the thermal molds 70, 70 at once.

[0048] When one or more tubes 30 are arranged in the space 73 of the thermal mold 70, 70, the ratio of the cross-sectional area of ​​the space 73 cut by a plane perpendicular to the long axis direction of the tube 30 to the total cross-sectional area of ​​the tube 30 cut by a plane perpendicular to the long axis direction of the tube 30 is 2 times or more and less than 10 times, preferably 4 times or more and less than 8 times.

[0049] 14, a plurality of tubes 30 can be arranged along the long wall 102a of the wall surface 102 in the space 103 of the cooling molds 100, 100 of the cooling mechanism section 55. The plurality of tubes 30 arranged in the space 103 are heated by the cooling molds 100, 100 at once.

[0050] Next, a description will be given of a hot mold 110 and a cold mold 120 according to a modified example. As shown in Fig. 15, the hot mold 110 has a heating section 111, and the surfaces facing each other are planar wall surfaces 112. The hot mold 110 is made of an elastic material.

[0051] 16, when the thermal mold 110 is closed, the wall surface 112 is deformed by the tube 30. Therefore, in the heating process, the thermal mold 110, which is a heat source, can be brought into contact with the entire circumference of the surface of the tube 30. By heating the thermal mold 110 in contact with the surface of the tube 30, heat is transferred from the thermal mold 110 to the tube 30 by thermal conduction, and the tube 30 can be heated efficiently even if the heating temperature of the thermal mold 110 is kept low.

[0052] 17 and 18, the cooling molds 120, 120 may also be formed of an elastically deformable material and may come into contact with the surface of the tube 30. The cooling mold 120 having a cooling portion 121 has a wall surface 122 on the surface facing the opposing cooling mold 120, and is elastically deformed by the surface of the tube 30, so that when the cooling molds 120, 120 are closed, the wall surface 122 of the cooling mold 120 comes into contact with the surface of the tube 30, so that heat is transferred between the cooling mold 120 and the tube 30 by thermal conduction, and the tube 30 can be cooled efficiently.

[0053] After the heating and cooling steps are performed with the hot mold 110 and the cooling mold 120 closed, the hot mold 110 and the cooling mold 120 are opened and separated from the surface of the tube 30, and then the stretching step is performed.

[0054] As shown in Fig. 19, a plurality of tubes 30 can be heated at once by a heating mold 110 that contacts the surface of the tube 30. Also, as shown in Fig. 20, a plurality of tubes 30 can be heated at once by a cooling mold 100 that contacts the surface of the tube 30.

[0055] As shown in Fig. 21, the thermal mold 110 may have a recess 113 on a wall surface 112, and the thermal mold 110 may be in contact with a circumferential portion of the surface of the tube 30. In this case, it is preferable that the area where the thermal mold 110 contacts the surface of the tube 30 is larger than the area where the thermal mold 110 does not contact. As shown in Fig. 22, the cooling molds 120, 120 may have a recess 123 on a wall surface 122, and the cooling molds 120, 120 may be in contact with a circumferential portion of the surface of the tube 30. In this case, it is preferable that the area where the cooling mold 120 contacts the surface of the tube 30 is larger than the area where the cooling mold 120 does not contact.

[0056] As described above, the method for manufacturing a parison 20 for a balloon catheter according to this embodiment (1) is a method for manufacturing a parison 20 for a balloon catheter, and includes a fixing step of fixing a thermoplastic tube 30 extending along the longitudinal direction at a pair of fixing regions 31, 31 spaced apart in the longitudinal direction, a heating step of heating a pair of heated regions 32, 32 spaced apart in the longitudinal direction between the pair of fixing regions 31, 31 of the tube 30, a cooling step of cooling at least a part of the region between the pair of heated regions 32, 32 of the tube 30 during the heating step, and a stretching step of pulling the tube 30 in the direction in which the pair of fixing regions 31, 31 are separated, and stretching the pair of heated regions 32, 32 heated in the heating step of the tube 30, thereby forming a thick diameter portion 21 having an outer diameter larger than the portion stretched between the pair of heated regions 32, 32 stretched in the stretching step. In the method for manufacturing the parison 20 for a balloon catheter configured as described above, when the tube 30 is heated, a clear temperature difference can be created between the region between the pair of heating regions 32, 32 of the tube 30 and the heating region. Therefore, the shape of the parison 20 can be stably formed in the stretching process.

[0057] (2) In the above-mentioned (1) method for producing the parison 20 for a balloon catheter, in the cooling step, at least a part of the cooling means may be in contact with the surface of the tube 30. This allows the tube 30 to be stably cooled by thermal conduction.

[0058] (3) In the method for producing the parison 20 for a balloon catheter described above in (1), in the cooling step, the space 103 surrounded by the wall surface 102 having a rectangular cross section cut along a plane perpendicular to the longitudinal axis may be cooled by a cooling means. This allows the tube 30 to be stably cooled by a combination of radiant heat and convective heat transfer.

[0059] (4) In any of the above (1) to (3) methods for producing a parison 20 for a balloon catheter, the surface of the region between the pair of heated regions 32, 32 may be maintained at a temperature lower than the glass transition temperature of the tube 30 in the cooling step. This makes it possible to suppress a rise in temperature in the portion that will become the large-diameter portion 21 of the tube 30, and to clearly form the shape of the shoulder of the parison 20 to be produced.

[0060] (5) In any of the above (1) to (4) methods for producing the parison 20 for a balloon catheter, in the heating step, the surface of the heated region may be maintained at a temperature higher than the glass transition temperature of the tube 30. This allows the heated region of the tube 30 to be reliably stretched in the stretching step, thereby increasing its strength.

[0061] (6) In any one of the above methods for producing a parison 20 for a balloon catheter (1) to (5), the difference between the surface temperature of the tube 30 in the heating step and the surface temperature of the tube 30 in the cooling step can be 50° C. or more and 140° C. or less. This allows a sufficient temperature difference to be created between the heating region and the cooling region of the tube 30, and the shape of the large diameter portion 21 of the tube 30 can be stably formed.

[0062] (7) In any one of the above methods for producing a parison 20 for a balloon catheter (1) to (6), the time from the start of cooling the tube 30 to the state where the tube 30 is maintained at a temperature lower than the glass transition temperature in the cooling step may be 5 seconds or more and 45 seconds or less. This allows the unheated portion of the tube 30 to be reliably cooled in accordance with the heating time of the tube 30.

[0063] (8) In the method for producing a balloon catheter 10 according to this embodiment, a balloon catheter parison 20 produced by any one of the production methods (1) to (7) above is biaxially stretched to form a balloon 12, and a shaft 11 is placed on the formed balloon 12. Because the shape of the balloon catheter parison 20 is stably formed by any one of the production methods (1) to (7) above, a balloon catheter 10 having a balloon 12 with a stable shape can be produced.

[0064] The manufacturing device 50 for a balloon catheter parison 20 according to the present embodiment (9) is a manufacturing device 50 for a balloon catheter parison 20, and includes a fixing mechanism 51 for fixing a thermoplastic tube 30 extending along the longitudinal direction at a pair of fixing regions 31, 31 spaced apart in the longitudinal direction, a heating mechanism 52 for heating a pair of heating regions 32, 32 spaced apart in the longitudinal direction between the pair of fixing regions 31, 31 of the tube 30, a cooling mechanism 55 for cooling a region between the pair of heating regions 32, 32 of the tube 30, and a pulling mechanism 53 for moving the fixing mechanism 51 in a direction in which the distance between the pair of fixing regions 31, 31 of the tube 30 increases. The manufacturing device for a balloon catheter parison 20 configured in this manner can clearly provide a temperature difference between the region between the pair of heating regions 32, 32 of the tube 30 and the heating region when heating the tube 30, and can stably form the shape of the parison 20.

[0065] The present invention is not limited to the above-described embodiment, and various modifications can be made by those skilled in the art within the technical concept of the present invention. [Explanation of symbols]

[0066] 10 Balloon Catheter 11 Shaft 12. Balloon 13. Hub 20 Parison 21 Large diameter part 21a Same diameter part 21b Shoulder 22 Thin section 30 Tubes 31 Fixed area 32 Heating area 50 Manufacturing equipment 51 Fixing mechanism section 52 Heating mechanism section 53 Pulling mechanism 54 Moving mechanism section 55 Cooling mechanism section 60 Fixed part 70 Heat type 71 Heating section 72 Wall 72a long wall 72b short wall 73 Space 100 cooling type 101 Cooling section 102 Wall 102a long wall 102b short wall 103 Space section

Claims

1. 1. A method for producing a parison for a balloon catheter, comprising: A fixing step of fixing a thermoplastic tube extending along a longitudinal direction at a pair of fixing regions spaced apart in the longitudinal direction; a heating step of heating a pair of heating regions spaced apart from each other in the longitudinal direction between the pair of fixing regions of the tube; a cooling step of cooling at least a portion of the region of the tube between the pair of heated regions during the heating step; a stretching step of pulling the tube in a direction in which the pair of fixed regions are separated from each other to stretch the pair of heated regions of the tube heated in the heating step; Equipped with a thickened portion having an outer diameter larger than that of the stretched portion is formed between the pair of heated regions stretched by the stretching step.

2. 2. The method for producing a parison for a balloon catheter according to claim 1, wherein in the cooling step, at least a part of a cooling means is in contact with a surface of the tube.

3. 2. The method for producing a parison for a balloon catheter according to claim 1, wherein in the cooling step, a cooling means cools a space surrounded by walls having a rectangular cross-sectional shape cut along a plane perpendicular to the longitudinal axis direction.

4. 2. The method for producing a parison for a balloon catheter according to claim 1, wherein in the cooling step, the surface of the region between the pair of heated regions is maintained at a temperature lower than the glass transition temperature of the tube.

5. 5. The method for producing a parison for a balloon catheter according to claim 4, wherein in the heating step, the surface of the heating region is maintained at a temperature higher than the glass transition temperature of the tube.

6. 2. The method for producing a parison for a balloon catheter according to claim 1, wherein a difference between a surface temperature of the tube in the heating step and a surface temperature of the tube in the cooling step is 50° C. or more and 140° C. or less.

7. 5. The method for producing a parison for a balloon catheter according to claim 4, wherein in the cooling step, a time from a temperature at which the tube starts to be cooled to a state where the temperature is maintained below the glass transition temperature of the tube is 5 seconds or more and 45 seconds or less.

8. A method for producing a balloon catheter, comprising biaxially stretching the parison for a balloon catheter produced by the method according to any one of claims 1 to 7 to form a balloon, and installing a shaft in the formed balloon.

9. An apparatus for manufacturing a parison for a balloon catheter, comprising: a fixing mechanism that fixes a thermoplastic tube extending along a longitudinal direction at a pair of fixing regions that are spaced apart in the longitudinal direction; a heating mechanism configured to heat a pair of heating regions spaced apart from each other in the longitudinal direction between the pair of fixing regions of the tube; a cooling mechanism for cooling a region of the tube between the pair of heating regions; a tension mechanism that moves the fixing mechanism in a direction that increases the distance between the pair of fixing regions of the tube; An apparatus for manufacturing a parison for a balloon catheter, comprising:

Citation Information

Patent Citations

  • Balloon and production method for same

    WO2014141382A1