Method for manufacturing semiconductor wafer and method for manufacturing semiconductor device

By controlling temperature deviations during RTA processing with first and second offsets and supporting the wafer on a sloping surface, the method addresses slips caused by thermal stress, producing high-quality semiconductor wafers with improved gettering properties and reduced defects.

JP2024162803APending Publication Date: 2024-11-21GLOBALWAFERS JAPAN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023078710
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing RTA processing methods for semiconductor wafers result in slips due to thermal stress, particularly at the wafer's edge, which can lead to device failures, and existing methods to control temperature distribution are insufficient in suppressing these slips.

Method used

The method involves performing RTA treatment with controlled temperature deviations across the wafer surface using first and second offsets, where the outer circumference receives a temperature correction of +0.1°C to +5.0°C more than the inner areas, and the wafer is supported on a sloping surface to minimize thermal stress during heating and cooling.

Benefits of technology

This approach effectively suppresses slips caused by thermal stress, ensuring high-quality semiconductor wafers with improved gettering properties and reduced defects, enhancing device reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162803000001_ABST
    Figure 2024162803000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a semiconductor wafer that suppresses slip caused by RTA treatment.SOLUTION: A method for manufacturing a semiconductor wafer according to the present invention includes a step of performing an RTA process on a semiconductor wafer 1, and for example, a first correction is made to eliminate temperature deviation over the entire surface of the wafer throughout the entire process from a heating process to a cooling process in the RTA process, and further, in the cooling process, a second correction of +0.1°C or more and +5.0°C or less is made to part or all of a wafer outer periphery 1d, which is the outer periphery region including the wafer edge.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor wafer, which includes a step of performing an RTA (Rapid Thermal Annealing) process. [Background technology]

[0002] Semiconductor wafers obtained by slicing semiconductor single crystal ingots grown by the CZ (Czochralski) method have numerous grown-in defects on their surfaces and surface layers. However, because semiconductor wafers are required to have surfaces and surface layers that are almost defect-free, RTA processing has been used for some time as a method for eliminating defects on the surface and surface layers.

[0003] The rapid heating and cooling heat treatment by RTA eliminates defects on the surface and surface layer of the semiconductor wafer and also forms a high density of BMD (Bulk Micro Defects) in the bulk portion. The BMD in the bulk portion acts as a gettering site for metal impurities that are diffused during the semiconductor device fabrication process and affect the device characteristics.

[0004] For example, as a method for manufacturing a semiconductor wafer having a step of performing an RTA treatment, Patent Document 1 listed below discloses a method in which an RTA treatment is performed on a silicon wafer in an oxidizing atmosphere at a temperature of 1300° C. or higher and 1400° C. or lower, and a large number of vacancies, which are point defects, are left in the bulk of the silicon wafer, thereby forming a high density of BMDs during a subsequent precipitation heat treatment.

[0005] Furthermore, as a heat treatment technique for suppressing slippage due to RTA treatment, the following Patent Document 2 discloses a technique for performing heat treatment in a semiconductor wafer manufacturing method having a step of performing heat treatment at a predetermined temperature using an RTA apparatus, in which the temperature of the contact portion with a support jig that supports the semiconductor wafer is controlled to be 3 to 20°C lower than the temperature of the center of the semiconductor wafer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-204326 A [Patent Document 2] JP 2002-164300 A Summary of the Invention [Problem to be solved by the invention]

[0007] The above-mentioned Patent Document 1 describes that RTA processing is performed in an oxidizing atmosphere at 1300°C to 1400°C, but when such RTA processing is performed, slips occur due to the temperature difference within the wafer surface and stress caused by the weight of the semiconductor wafer. In particular, in the case of an edge ring in which a wafer support member supports the semiconductor wafer from the outer periphery of the rear surface, the stress due to the wafer weight and the thermal stress due to the temperature difference between the semiconductor wafer and the wafer support member act simultaneously at the contact position between the semiconductor wafer and the wafer support member, making slips likely to occur at the wafer edge.

[0008] In addition, to eliminate defects on the surface and surface layer of a semiconductor wafer and to form BMD in the bulk, it is desirable to perform RTA treatment at 1300°C or higher, which allows for rapid heating and cooling, but when such RTA treatment is performed, the effects of slip due to thermal stress become particularly large. Specifically, in the process of rapid cooling from the maximum temperature, the edge of the wafer is more likely to dissipate heat than the center of the wafer, and the transfer of heat from the edge of the wafer to the wafer support member and the stress of the wafer's own weight combine to easily cause slip.

[0009] In order to suppress slips caused by thermal stress as described above, it is necessary to uniformly control the temperature distribution in the wafer surface, but the above-mentioned Patent Document 1 does not disclose a method for suppressing slips caused by RTA treatment at 1300° C. or higher, that is, a method for suppressing slips caused by thermal stress. Since the above-mentioned slips cause device defects, a heat treatment that can suppress slips is required.

[0010] Furthermore, the above-mentioned Patent Document 2 describes a method of suppressing slips by controlling the heat treatment temperature, in which the temperature is gradually lowered from the center of the wafer toward the outer periphery of the wafer, and the temperature distribution is set so that the temperature difference between the center and outer periphery of the wafer is in the range of 3° C. to 20° C. However, this method does not allow for uniform control of the temperature distribution within the wafer surface, and does not provide a sufficient slip suppression effect as a measure for suppressing slips due to thermal stress.

[0011] Furthermore, a method for suppressing slip caused by the RTA process is required not only for semiconductor wafers but also for manufacturing semiconductor devices from semiconductor wafers.

[0012] The present invention has been made in consideration of the above problems, and has an object to provide a method for manufacturing a semiconductor wafer that suppresses slip caused by thermal stress due to the implementation of an RTA process. Another object of the present invention is to provide a method for manufacturing a semiconductor device that suppresses slip due to the implementation of an RTA process. [Means for solving the problem]

[0013] The method for manufacturing a semiconductor wafer according to the present invention is a method for manufacturing a semiconductor wafer having a step of performing an RTA process, and is characterized in that a first correction is performed using a first offset, which is a temperature correction value for eliminating temperature deviation over the entire surface of the wafer, throughout the entire process from the heating step to the cooling step in the RTA process, and further, in the cooling step, a second correction is performed using a second offset, which is a temperature correction value set so that the temperature correction value for the wafer outer periphery, which is the outer periphery region including the wafer edge, is relatively set to +0.1°C or more and +5.0°C or less compared to the temperature correction value for the wafer region other than the wafer outer periphery. As an example, in the second correction, a correction of +0.1°C or more and +5.0°C or less is performed for a part or all of the wafer outer periphery.

[0014] The RTA treatment is preferably performed under conditions of holding the maximum temperature of 1250° C. or higher for 1 s to 60 s in an oxidizing atmosphere, and cooling to 1000° C. or lower at a cooling rate of 75° C. / s to 120° C. / s. The second correction is preferably performed during the cooling process, at least for a period of 5 seconds from the start of cooling.

[0015] According to the semiconductor wafer manufacturing method of the present invention, even when the RTA treatment is performed at 1300° C. or higher, which can ensure gettering properties for metal impurities that are diffused during the semiconductor device formation process and affect the device characteristics, slip generated from the outer periphery of the wafer during rapid cooling in the RTA treatment can be suppressed.

[0016] In the semiconductor wafer manufacturing method according to the present invention, the RTA treatment is performed with the semiconductor wafer placed on a wafer support member having a support surface that slopes downward inward, and the surface roughness of the semiconductor wafer around the contact position between the semiconductor wafer and the wafer support member is preferably 5.0 nm≦Ra≦30.0 nm. Furthermore, in the semiconductor wafer manufacturing method according to the present invention, the diameter of the semiconductor wafer to be subjected to the RTA treatment is preferably 300 mm or more, and the outer periphery of the wafer is preferably a region extending 10 mm or less from the edge of the semiconductor wafer toward the center.

[0017] The semiconductor device manufacturing method according to the present invention is a semiconductor device manufacturing method having a step of performing an RTA process on a semiconductor wafer, and is characterized in that a first correction is performed using a first offset, which is a temperature correction value for eliminating temperature deviation over the entire surface of the wafer, throughout the entire process from the heating process to the cooling process in the RTA process, and further, in the cooling process, a second correction is performed using a second offset, which is a temperature correction value set so that the temperature correction value for the outer periphery of the wafer, which is the outer periphery region including the wafer edge, is relatively +0.1°C or more and +5.0°C or less compared to the temperature correction value for the wafer region other than the outer periphery of the wafer. Effect of the Invention

[0018] According to the method for producing a semiconductor wafer of the present invention, slip caused by thermal stress due to the RTA treatment can be suppressed. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a cross-sectional view that typically illustrates a method for producing a semiconductor wafer according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of an RTP device. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a schematic diagram of a method for producing a semiconductor wafer according to Comparative Example 1. As shown in FIG. [Figure 4]FIG. 4 is a diagram showing the results of measurement of the distortion area ratio by SIRD for each silicon wafer that was subjected to the RTA treatment by the methods of Experimental Examples 1 to 4 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of a method for manufacturing a semiconductor wafer according to the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to this embodiment.

[0021] <Semiconductor wafer manufacturing method> Fig. 1 is a cross-sectional view that shows a schematic diagram of a method for manufacturing a semiconductor wafer (sometimes simply called a wafer) according to the present embodiment. The manufacturing method shown in Fig. 1 includes a step of performing an RTA process on a semiconductor wafer 1, and for example, the RTA process is performed in a state where the semiconductor wafer 1 is placed on a wafer support member 2 having a support surface 2a that is inclined downward toward the inside.

[0022] The method for manufacturing a semiconductor wafer according to this embodiment will be described in detail below. First, a semiconductor single crystal ingot grown by the CZ method is obtained, and then the semiconductor single crystal ingot is sliced ​​into wafers using a wire saw or the like. Then, the semiconductor wafer obtained by slicing is beveled. After that, the uneven layer formed during slicing is removed in a lapping process and a grinding process, and the flatness and surface roughness are adjusted. Then, the processing damage introduced in the lapping and grinding processes is removed in an etching process.

[0023] In this embodiment, the above-mentioned manufacturing process (Slicing → Beveling → Lapping → Grinding → Etching) is used to produce a semiconductor wafer 1 in which the angle between the wafer back surface 1a and the back surface bevel 1b is an obtuse angle, as shown in Fig. 1. Here, as an example, a semiconductor wafer 1 having a diameter of 300 mm is produced. At that time, the semiconductor wafer 1 is processed so that when the semiconductor wafer 1 is placed on the support surface 2a (support surface 2a inclined downward toward the inside) of the wafer support member 2, the boundary portion (apex 1c of the obtuse angle) between the wafer back surface 1a and the back surface bevel 1b comes into contact with the support surface 2a.

[0024] Thereafter, the semiconductor wafer 1 produced by the above-mentioned manufacturing process is subjected to the RTA process shown in Fig. 1. Here, the RTA process is performed under the conditions of holding the maximum temperature of 1250°C or higher (preferably 1300°C or higher and 1350°C or lower) for 1 s or higher and 60 s or lower in an oxidizing atmosphere, and then cooling to 1000°C or lower at a cooling rate of 75°C / s or higher and 120°C / s or lower. In this case, in the RTA process in the manufacturing method of this embodiment, for example, a first correction (a first offset is set in advance) is performed to eliminate temperature deviation over the entire wafer surface throughout the entire process from the heating process to the cooling process, and further, in the cooling process, a second correction (a second offset is set in advance) is performed using a second offset, which is a temperature correction value set so that the temperature correction value for the wafer outer periphery 1d, which is the outer periphery region including the wafer edge, is relatively set to be +0.1°C or more and +5.0°C or less, preferably +0.5°C or more and +3.0°C or less, and particularly preferably +1.0°C or more and +1.5°C or less, compared to the temperature correction value for the wafer region other than the wafer outer periphery.

[0025] In this embodiment, after the above-mentioned RTA process is performed, the surface of the semiconductor wafer obtained by the RTA process is mirror-polished.

[0026] For example, when the semiconductor wafer 1 is mirror-finished and then RTA treatment is performed, the semiconductor wafer after mirror-finishing tends to have a larger contact area with the wafer support member 2 due to the reduced roughness, and therefore slippage due to welding between the semiconductor wafer and the wafer support member 2 is likely to occur in RTA treatment at 1250°C or higher. In this embodiment, in order to further reduce slippage due to the RTA treatment, the surface roughness of the semiconductor wafer 1 around the contact position between the semiconductor wafer 1 and the wafer support member 2 is set to 5.0 nm≦Ra≦30.0 nm in the above-mentioned manufacturing process. This reduces the contact area between the semiconductor wafer 1 and the wafer support member 2, and can further suppress slippage due to welding. For example, when the surface roughness is Ra<5.0 nm, the contact area between the semiconductor wafer and the wafer support member 2 becomes large, and slippage due to welding is likely to occur, which is not preferable. Furthermore, if Ra>30.0 nm, the surface of the semiconductor wafer becomes too rough, causing variations in the wafer contact area, which is undesirable since slippage due to self-weight stress becomes more likely to occur.

[0027] The semiconductor wafer manufactured by the semiconductor wafer manufacturing method of the present embodiment can suppress slippage that occurs from the outer periphery of the wafer (wafer end face) during rapid cooling in the RTA treatment, even when the RTA treatment is performed at 1300°C or higher, which is a temperature at which gettering properties against metal impurities can be ensured.

[0028] The wafer outer periphery 1d where the second correction is performed is preferably an outer periphery region including the wafer periphery, for example, a region of 10 mm or less from the periphery toward the center of the semiconductor wafer 1. If the region of the wafer outer periphery 1d exceeds 10 mm, it is not preferable because slip may occur in the wafer central region.

[0029] Furthermore, there is no particular limitation on the diameter (size) of the semiconductor wafer 1, but the method for producing a semiconductor wafer according to this embodiment is useful as a method for producing a semiconductor wafer having a diameter of 300 mm or more, for example.

[0030] <RTP Apparatus and RTA Process> Here, taking an RTP apparatus (heat treatment apparatus) 10 using a halogen lamp (for example, a high-voltage tungsten halogen lamp) as a heat source as an example, the RTA process in the manufacturing method of this embodiment will be described in more detail.

[0031] FIG. 2 is a cross-sectional view schematically showing an RTP apparatus 10 for performing an RTA process. This RTP apparatus 10 includes a chamber 20, and this chamber 20 has a chamber side wall 20a, a chamber bottom 20b coupled to the chamber side wall 20a, and a quartz window 20c disposed above the chamber side wall 20a.

[0032] The chamber side wall 20a, the chamber bottom 20b, and the quartz window 20c constituting the chamber 20 form a reaction space 25 for processing the semiconductor wafer 1 placed therein. In the RTP apparatus 10, a slit valve door (not shown) penetrating the chamber side wall 20a is provided to transfer the semiconductor wafer 1 into the reaction space 25.

[0033] Further, the RTP apparatus 10 includes a gas inlet 20d formed in the chamber side wall 20a, and this gas inlet 20d is connected to a gas supply source 30 configured to supply one or more processing gases to the reaction space 25. Also, the RTP apparatus 10 includes a gas outlet 20e formed in the chamber side wall 20a, and this gas outlet 20e is connected to a vacuum pump (P) 31 for exhausting from the reaction space 25 to the outside. Further, the RTP apparatus 10 includes a wafer support portion 40 for supporting the semiconductor wafer 1 in the reaction space 25. Also, although not shown, it includes a rotating means for rotating the semiconductor wafer 1 at a predetermined speed around its central axis.

[0034] The wafer support section 40 includes an annular wafer support member 40a (corresponding to the above-mentioned wafer support member 2) that supports the outer periphery of the semiconductor wafer 1, and a stage 40b that supports the wafer support member 40a. A plurality of radiation thermometers (pyrometers) 50 are embedded in the stage 40b. The radiation thermometers 50 are connected to a controller 60, which is a computer, and the controller 60 controls a plurality of halogen lamps 70 based on wafer temperature information acquired from the radiation thermometers 50.

[0035] The halogen lamps 70 are arranged above the quartz window 20c and configured to send thermal energy through the quartz window 20c toward the reaction space 25, and are arranged, for example, in a hexagonal pattern in a plan view. Each halogen lamp 70 is connected to a heating assembly base 90 for electrical connection to a power supply 80. A lamp voltage is applied to each halogen lamp 70 from the power supply 80, and the value of this lamp voltage is controlled by the controller 60.

[0036] When performing RTA processing on the semiconductor wafer 1 using the above-mentioned RTP apparatus 10, the semiconductor wafer 1 is introduced into the reaction space 25 through a slit valve door (not shown) provided in the chamber 20, and the semiconductor wafer 1 is placed on the wafer support member 40a. Then, gas is introduced from the gas inlet 20d, and the semiconductor wafer 1 is rotated by the rotating means while the halogen lamp 70 irradiates the wafer surface under the control of the controller 60.

[0037] The temperature control in the reaction space 25 of this RTP apparatus 10 is performed by measuring the temperature of the semiconductor wafer 1 during the RTA process using a plurality of radiation thermometers 50 embedded in the stage 40b, and controlling a plurality of halogen lamps 70 based on the measured temperature. Specifically, the controller 60 measures the average temperature at multiple points within the wafer surface in the wafer radial direction below the semiconductor wafer 1 using the radiation thermometer 50, and based on this measured temperature, performs automatic control of the halogen lamps 70 (such as individual ON-OFF control of each lamp, control of the increase and decrease of the supplied power, control of the emission intensity of the emitted light, etc.) so that the in-plane temperature becomes substantially uniform throughout the entire process from the heating step to the cooling step in the RTA process.

[0038] <Details of the RTA process> In this embodiment, using the above-described RTP apparatus 10, for example, in an oxidizing atmosphere, it is held at a maximum temperature of 1250°C or higher (preferably 1300°C or higher and 1350°C or lower) for a time of 1 s or longer and 60 s or shorter, and cooled at a cooling rate of 75°C / s or higher and 120°C / s or lower until it reaches 1000°C or lower, and the RTA process is carried out. Thereby, a semiconductor wafer having sufficient gettering characteristics with respect to metal impurities is manufactured.

[0039] Also, in this embodiment, in the RTA process under the above conditions, the above-described first correction and second correction with respect to the above automatic control are carried out. Specifically, in order to achieve higher wafer quality, while performing the above-described automatic control throughout the entire process from the heating step to the cooling step in the RTA process, a first correction for eliminating the temperature deviation across the entire surface of the semiconductor wafer 1 is carried out (see Fig. 1(a)). Further, as a measure for suppressing slip (slip due to thermal stress) caused by the RTA process at 1250°C or higher, in the cooling step, a second correction is carried out on the outer peripheral portion 1d of the wafer (see Fig. 1(b)).

[0040] In detail, under the control of the controller 60, a first offset, which is a temperature correction value for eliminating temperature deviation across the entire surface of the wafer, is set in advance with reference to the thickness of an oxide film formed on the wafer after RTA processing in an oxidizing atmosphere and the distortion area ratio of the wafer measured by SIRD (Scanning Infrared Depolarization), and a correction (first correction) is made to the wafer temperature calculated from each pyrometer 50 throughout the entire process from the heating step to the cooling step of the RTA processing. This reduces the temperature difference occurring within the wafer surface throughout the RTA processing, suppressing variations in thermal stress and BMD density.

[0041] A known method can be adopted as a method for determining the first offset, and specifically, the technique described in Japanese Patent Application Laid-Open No. 2002-043227 or Japanese Patent Application Laid-Open No. 2002-522912 can be adopted. In the present embodiment, as an example, the first offset is determined by adopting one or more of the techniques described in these documents.

[0042] In the cooling process, while performing the above-mentioned automatic control and first correction, for example, a correction (second correction) of +0.1°C to +5.0°C, preferably +0.5°C to +3.0°C, particularly preferably +1.0°C to +1.5°C is performed on the wafer outer periphery 1d, which is a region of 10 mm from the edge toward the center of the semiconductor wafer 1 (a region of 140 mm to 150 mm from the wafer center in the case of a diameter of 300 mm). That is, a second offset, which is a temperature correction value of +0.1°C to +5.0°C, is set in advance under the control of the controller 60. In the process of rapidly cooling from the highest temperature reached (cooling process), the wafer outer periphery 1d, which is the end face of the wafer, is more likely to dissipate heat than the wafer center, so that the thermal stress generated in the cooling process can be minimized by applying a temperature correction to the wafer temperature calculated by the pyrometer 50 at the position of the wafer outer periphery 1d. This also minimizes slip due to thermal stress (see FIG. 1(c)). For example, if the second offset is less than +0.1° C., the thermal stress caused by heat dissipation at the wafer outer periphery 1d cannot be sufficiently suppressed, which is undesirable. Also, if the second offset exceeds +5.0° C., heat greater than the amount of heat dissipated is introduced into the wafer outer periphery 1d, which is undesirable because it results in slippage caused by thermal stress.

[0043] In addition, if the above-mentioned second correction is performed during the cooling process at least from the cooling start time (immediately after the end of the heating process including the maximum temperature holding time) until 5 seconds have elapsed, that is, if it is performed for 5 seconds from the start of cooling, a sufficient slip suppression effect can be obtained. For example, if the second correction is not performed during this period, it is not preferable because the thermal stress due to heat dissipation from the wafer outer periphery 1d cannot be sufficiently suppressed. On the other hand, the second correction only needs to be performed for at least 5 seconds from the start of cooling, and for example, it can be performed continuously even after 5 seconds have elapsed from the start of cooling within the cooling process.

[0044] In the RTA process of this embodiment, the cooling step includes the automatic control and the first correction, and further includes the second correction of +0.1° C. to +5.0° C. for the outer periphery 1d of the wafer, but is not limited thereto. For example, the second correction may be performed such that the temperature correction value for the outer periphery 1d of the wafer is relatively +0.1° C. to +5.0° C. compared with the temperature correction value for the other wafer regions (wafer regions ranging from the wafer center to the inner circumference of the outer periphery 1d of the wafer), and the second offset may be preset by the control of the controller 60 so as to satisfy this condition.

[0045] As an example, in the cooling process, while performing the above-mentioned automatic control and first correction, a correction (second correction) of -5.0°C to -0.1°C (preferably -3.0°C to -0.5°C, particularly preferably -1.5°C to -1.0°C) may be performed on the region other than the wafer outer periphery 1d of the semiconductor wafer 1 (region 140 mm from the wafer center in the case of a diameter of 300 mm). This minimizes the thermal stress generated in the cooling process as described above, and therefore minimizes slip due to thermal stress.

[0046] In the RTA process of this embodiment, it is preferable to perform the second correction of +0.1°C to +5.0°C on the entire outer peripheral portion 1d of the wafer while performing the above-mentioned automatic control and first correction in the cooling step, but other forms may be applied depending on the required performance of the semiconductor wafer 1, for example. Specifically, in the cooling step, the second correction of +0.1°C to +5.0°C (preferably +0.5°C to +3.0°C, particularly preferably +1.0°C to +1.5°C) may be performed on a part of the outer peripheral portion 1d of the wafer, such as only the wafer periphery or the outer peripheral portion excluding the wafer periphery, while performing the above-mentioned automatic control and first correction. Such a second correction can also suppress the thermal stress generated in the cooling step, thereby obtaining a slip suppression effect.

[0047] In addition, in the method for manufacturing a semiconductor device according to the present embodiment, a step of performing an RTA process on a semiconductor wafer is included, and as the manufacturing process of the semiconductor device, for example, a conventionally known method can be adopted. In the step of performing the RTA process on the semiconductor wafer described above, in the entire process from the heating step to the cooling step, first correction is performed by a first offset which is a temperature correction value for eliminating the temperature deviation across the entire wafer. Further, in the cooling step, the temperature correction value for the outer peripheral portion of the wafer, which is an outer peripheral region including the wafer periphery, is compared with the temperature correction value for the wafer region other than the outer peripheral portion of the wafer, and a second correction is performed by a second offset which is a temperature correction value set so as to be relatively +0.1 °C or more and +5.0 °C or less (preferably +0.5 °C or more and +3.0 °C or less, particularly preferably +1.0 °C or more and +1.5 °C or less). By applying such temperature correction, the thermal stress generated in the cooling step can be minimized, and the slip due to the thermal stress can also be minimized.

[0048] Also, in the method for manufacturing a semiconductor device according to the present embodiment, in the cooling step, while performing the above-described automatic control and first correction, a second correction of +0.1 °C or more and +5.0 °C or less (preferably +0.5 °C or more and +3.0 °C or less, particularly preferably +1.0 °C or more and +1.5 °C or less) may be performed on a part or all of the outer peripheral portion 1d of the wafer, such as only the wafer periphery or the outer peripheral portion excluding the wafer periphery. Even by such a second correction, the thermal stress generated in the cooling step can be suppressed, and thus a slip suppressing effect can be obtained.

Example

[0049] Next, the method for manufacturing a semiconductor wafer according to the present invention will be further described based on examples. Note that the present invention is not limited by the following examples.

[0050] <Manufacture of RTA-Processing Semiconductor Wafer> Oxygen concentration: 1.0×10 18 / cm 3The above-mentioned manufacturing process (Beveling → Lapping → Grinding → Etching) was carried out on the wafer obtained by slicing the silicon single crystal ingot, and 50 silicon wafers with a diameter of 300 mm were manufactured. The silicon wafer manufactured by this manufacturing process was processed so that the angle between the back surface of the wafer and the back surface bevel was formed as an obtuse angle, and when the silicon wafer was placed on the wafer support member prepared inside the RTP device, the apex of this obtuse angle was made to contact the support surface that sloped downward toward the inside (corresponding to semiconductor wafer 1 in Figure 1(a)). At this time, the surface roughness of the silicon wafer around the contact position between the silicon wafer and the wafer support member was set to Ra = 20 nm.

[0051] <Experimental Example 1> Ten of the 50 silicon wafers manufactured as described above were used, and in a state in which the silicon wafers were placed on a wafer support member prepared inside the RTP equipment, the RTA treatment was carried out one by one by the method of Experimental Example 1 (see Fig. 1). The RTP equipment used was an RTP equipment as shown in Fig. 2.

[0052] Specifically, in the method of Experimental Example 1, a first offset, which is a temperature correction value for eliminating temperature deviations on the entire surface of the wafer, was set in advance with reference to the thickness of the oxide film formed on the wafer after RTA processing in an oxidizing atmosphere and the area ratio of the wafer in distortion due to SIRD. Then, in this state, RTA processing was performed on each silicon wafer under the condition that the maximum temperature reached was 1350°C in an oxidizing atmosphere and held for 30 s, and cooled to 1000°C or less at a cooling rate of 120°C / s. At this time, correction was performed on the wafer temperature calculated from a pyrometer at a position 140 mm to 150 mm from the center of the wafer during the period from the start of cooling (immediately after the end of the heating process) to 5 seconds (a second offset was set in the RTP device in advance). The second offset was set to +0.5°C based on the first offset.

[0053] <Experimental Example 2> Ten of the remaining 40 silicon wafers were used, and with the silicon wafers placed on a wafer support member prepared inside the RTP device, RTA processing was carried out one by one by the method of Experimental Example 2 (see Figure 1). The method of Experimental Example 2 was the same as that of Experimental Example 1, except for the value of the second offset. The second offset in the method of Experimental Example 2 was set to +1.0°C based on the first offset.

[0054] <Experimental Example 3> Ten of the remaining 30 silicon wafers were used, and with the silicon wafers placed on a wafer support member prepared inside the RTP device, RTA processing was carried out one by one by the method of Experimental Example 3. The method of Experimental Example 3 was the same as that of Experimental Example 1, except for the value of the second offset. The second offset in the method of Experimental Example 3 was set to +1.5°C based on the first offset.

[0055] <Experimental Example 4> Ten of the remaining 20 silicon wafers were used, and with the silicon wafers placed on a wafer support member prepared inside the RTP device, RTA processing was carried out one by one by the method of Experimental Example 4. The method of Experimental Example 4 was the same as that of Experimental Example 1 except for the value of the second offset. The second offset in the method of Experimental Example 4 was set to +2.0°C based on the first offset.

[0056] <Comparative Example 1> The remaining 10 silicon wafers were placed on a wafer support member prepared inside the RTP device and subjected to RTA processing one by one by the method of Comparative Example 1 (see FIG. 3). The method of Comparative Example 1 is the same as that of Experimental Example 1 except that the second offset is not performed. That is, the cooling step of FIG. 3(b) is different from that of FIG. 1.

[0057] <Evaluation method> After RTA, each silicon wafer was measured by SIRD to evaluate the slip and the strain area ratio. In other words, the ratio of the area where the strain stress increased due to slip to the total area of ​​the silicon wafer (strain area ratio) was calculated and evaluated. For example, the larger the strain area ratio, the worse the slip quality, and the smaller the strain area ratio, the better the slip quality.

[0058] <Evaluation Results> 4 is a diagram showing the results of measurement of the distortion area ratio by SIRD for each silicon wafer subjected to RTA processing by the methods of Experimental Examples 1 to 4 and Comparative Example 1. The silicon wafer subjected to RTA processing by the method of Comparative Example 1 (without second offset) had an average distortion area ratio of 1.2×10 -3 In the cooling process of Comparative Example 1, the edge of the wafer was more susceptible to heat dissipation than the center of the wafer, and the transfer of heat from the edge of the wafer to the wafer support member and the stress of the wafer's own weight combine to cause slippage (see Figure 3).

[0059] On the other hand, the silicon wafers subjected to RTA treatment using the method of Experimental Example 1 (second offset: +0.5°C) had an average area distortion ratio of 2.6 × 10 -4 The silicon wafers subjected to RTA treatment by the method of Experimental Example 4 (second offset: +2.0°C) had an average area distortion ratio of 1.9 × 10 -4 These were able to suppress slip more than the silicon wafers that had been subjected to RTA treatment by the method of Comparative Example 1.

[0060] In addition, the silicon wafers subjected to RTA treatment by the method of Experimental Example 2 (second offset: +1.0°C) and the method of Experimental Example 3 (second offset: +1.5°C) had an average area distortion ratio of 4.1 × 10 -5 , 5.7×10 -5It was found that the average distortion area ratio was very small and slip was suppressed. Furthermore, compared with the silicon wafer that had been subjected to RTA processing by the method of Comparative Example 1 (without the second offset), it was confirmed that the distortion area ratio of the wafer edge surface was reduced by about 96%. [Explanation of symbols]

[0061] 1. Semiconductor wafer 1a Wafer backside 1b Back side bevel 1c top 1d Wafer outer periphery 2 Wafer support member 2a Support surface 10 RTP device 20 Chamber 20a Chamber side wall 20b Chamber bottom 20c Quartz window 20d Gas inlet 20e Gas outlet 25 Reaction Space 30 Gas supply source 31 Vacuum Pump 40 Wafer support 40a Wafer support member 40b Stage 50 Radiation thermometer (pyrometer) 60 Controller 70 Halogen lamp 80 power supply 90 Heating Assembly Base

Claims

1. A method for manufacturing a semiconductor wafer, comprising a step of performing an RTA process, performing a first correction using a first offset, which is a temperature correction value for eliminating a temperature deviation on the entire surface of the wafer, throughout the entire process from the heating process to the cooling process in the RTA treatment; Furthermore, in the cooling step, a second correction is performed using a second offset, which is a temperature correction value set so that a temperature correction value for a wafer outer periphery, which is an outer periphery region including the wafer edge, is relatively set to be +0.1° C. or more and +5.0° C. or less compared to a temperature correction value for a wafer region other than the wafer outer periphery. A method for manufacturing a semiconductor wafer comprising the steps of:

2. In the second correction, a correction of +0.1° C. or more and +5.0° C. or less is performed on a part or the whole of the outer periphery of the wafer.

2. The method for producing a semiconductor wafer according to claim 1.

3. RTA treatment is performed under the conditions of holding the maximum temperature of 1250°C or more for 1 s to 60 s in an oxidizing atmosphere, and then cooling to 1000°C or less at a cooling rate of 75°C / s to 120°C / s.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

4. The second correction is performed during the cooling process, at least during a period from the start of cooling to 5 seconds after the start of cooling.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

5. The RTA process is performed in a state where the semiconductor wafer is placed on a wafer support member having a support surface that is inclined downward toward the inside, The surface roughness of the semiconductor wafer around the contact position between the semiconductor wafer and the wafer support member is set to 5.0 nm≦Ra≦30.0 nm.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

6. The diameter of the semiconductor wafer to be subjected to the RTA treatment is 300 mm or more.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

7. The outer periphery of the wafer is a region extending from the periphery of the semiconductor wafer toward the center of the wafer by 10 mm or less.

3. The method for producing a semiconductor wafer according to claim 1 or 2.

8. A method for manufacturing a semiconductor device, comprising a step of performing an RTA treatment on a semiconductor wafer, performing a first correction using a first offset, which is a temperature correction value for eliminating a temperature deviation on the entire surface of the wafer, throughout the entire process from the heating process to the cooling process in the RTA treatment; Furthermore, in the cooling step, a second correction is performed using a second offset, which is a temperature correction value set so that a temperature correction value for a wafer outer periphery, which is an outer periphery region including the wafer edge, is relatively set to be +0.1° C. or more and +5.0° C. or less compared to a temperature correction value for a wafer region other than the wafer outer periphery.

1. A method for manufacturing a semiconductor device comprising the steps of:

9. In the second correction, a correction of +0.1° C. or more and +5.0° C. or less is performed on a part or the whole of the outer periphery of the wafer.

9. The method for manufacturing a semiconductor device according to claim 8.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor wafer

    JP2002164300A

  • Heat treatment method of silicon wafer and silicon wafer

    JP2015204326A