Positive electrode material and preparation method thereof, and electrochemical device
A high nickel ternary positive electrode material with a hollow structure and controlled void ratio addresses stress-related breakage, enhancing cycle life and energy density by buffering volumetric strain in lithium-ion batteries.
Patent Information
- Application Number
- JP2023210456
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2023-12-13
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-12-13
AI Technical Summary
High nickel ternary positive electrode materials in lithium-ion batteries suffer from microscopic stress during charging and discharging, leading to secondary particle breakage and deterioration of cycling and gas production performance.
A high nickel ternary positive electrode material with a hollow structure formed by aggregation of primary particles, containing a cavity structure inside, where elements like sulfur are attached to the inner layer, adjusting the void ratio to buffer volumetric strain during charging and discharging.
The cavity structure effectively reduces secondary particle destruction, improving cycle life and volumetric energy density by allowing stress release, maintaining over 80% cycle capacity retention for 800 cycles with minimal gas production.
Smart Images

Figure 2024162982000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and particularly to a positive electrode material, a method for preparing the same, and an electrochemical device.
Background Art
[0002] The high-nickel ternary cathode material (LiNi x Co y Mn 1-x-y O 2 , where 0 < x < 1, 0 < y < 1) is widely used in high specific energy lithium-ion battery systems because of its higher theoretical specific capacity (about 276 mAh / g), higher voltage platform (about 3.6 V), and higher tap density. Specifically, the high-nickel ternary cathode material can obtain a ternary material with high specific energy and low cost by increasing the nickel content and decreasing the cobalt content in the material. However, considering that the ternary cathode material is secondary particles formed by the deposition of primary particles, the high-nickel ternary cathode material LiNi x Co y Mn 1-x-y O 2 (1 > x ≥ 0.8, 0 < y ≤ 0.1) generates a relatively large microscopic stress between primary particles during the charge and discharge process. This microscopic stress is gradually accumulated with the cycles and finally leads to the destruction of the secondary particles, deteriorating the cycle performance and gas generation performance of the battery.
[0003] Currently, in the prior art, the main methods for modifying the ternary cathode material are still element doping and coating optimization. Although the above methods can improve the cycle performance of the ternary material to a certain extent, they make the preparation process of the ternary material more complex and cumbersome, and do not meet the market requirements.
[0004] Therefore, it is necessary to design a cathode material, a method for preparing the same, a cathode sheet, and an electrochemical device to solve the above problems.
Summary of the Invention
Problems to be Solved by the Invention
[0005] In view of the above drawbacks of the prior art, to solve the technical problem that the positive electrode material in the prior art is easily destroyed due to microscopic stress during the charge and discharge process, and the cycle and gas generation performance deteriorate, the present invention provides a positive electrode material, a method for preparing the same, a positive electrode sheet, and an electrochemical device.
Means for Solving the Problems
[0006] To achieve the above object and other related objects, the present invention provides a positive electrode material. The positive electrode material is secondary particles formed by aggregation of primary particles, and the secondary particles contain a hollow structure inside.
[0007] In one example of the present invention, the chemical formula of the positive electrode material is Li 1+a [Ni x Co y M z O 2-b A b where 0.7 ≦ x < 1, 0 ≦ y < 0.3, 0 ≦ z < 0.3, -0.2 < a < 0.2, 0 ≦ b < 0.2, and x + y + z = 1. Here, the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W, and the A element includes one or more of F, N, Cl, S, and P.
[0008] In one example of the present invention, at least one of the A elements adheres to the inner layer of the hollow structure.
[0009] In one example of the present invention, the elements adhering to the inner layer of the hollow structure include sulfur elements, and the porosity of the positive electrode material has a positive correlation with the sulfur element content in the positive electrode material.
[0010] In one example of the present invention, when the sulfur element content in the secondary particles is 0.01 wt% to 0.35 wt%, the positive electrode material has a porosity of 0.5% to 10%, and the particle tap density of the positive electrode material is 2.38 g / cm 3~2.81g / cm 3 It is.
[0011] In one example of the present invention, the valence state of the sulfur element in the positive electrode material is at least one of −2, +4, and +6, and the sulfur element remains in the cavity structure in the form of at least one of sulfide ions, thiosulfate ions, sulfate ions, and sulfite ions.
[0012] In one embodiment of the present invention, when the sulfur element content in the secondary particles is 0.01wt%-0.1wt%, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168±2eV.When the sulfur element content in the secondary particles is 0.01wt%-0.05wt%, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168.5±1eV.
[0013] In one example of the present invention, the inner diameter of the cavity structure is from 10 nm to 1 μm.
[0014] The present invention further provides a method for preparing a positive electrode material, the method includes: mixing a nickel source, a cobalt source, an M element carrier source, a precipitating agent and a complexing agent to obtain a nickel-cobalt precursor material; mixing the nickel-cobalt precursor material with a lithium source and then sintering to obtain a positive electrode material, the M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W; and the carrier source of at least one of the nickel source, the cobalt source, and the M source is a sulfate. During the co-precipitation reaction synthesis process, the nickel-cobalt precursor forms a cavity structure in the secondary particles.
[0015] In one embodiment of the present invention, the nickel source, the cobalt source, and the M element carrier source include an A element, and the A element includes one or more of F, N, Cl, S, and P, and the A element is deposited in the cavity structure during the co-precipitation reaction synthesis process of the nickel-cobalt precursor.
[0016] In one embodiment of the present invention, the sulfur element in the A element is attached in the cavity structure, and the void ratio of the positive electrode material is 0.5% to 10%.
[0017] The present invention further provides a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active material layer, and the positive electrode active material layer adopts any one of the positive electrode materials in the above examples.
[0018] The present invention further provides an electrochemical device, comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, the positive electrode sheet comprising any one of the positive electrode materials in the above examples, or a positive electrode material prepared by any one of the preparation methods in the above examples. Effect of the Invention
[0019] In the positive electrode material and its preparation method, positive electrode sheet and electrochemical device of the present invention, based on the positive correlation characteristic between the content of A element in the positive electrode material particles and the void ratio, in order to ensure that the positive electrode material can buffer the volume distortion during the charging and discharging process through the appropriate ratio of internal void structure, and to reduce the destruction phenomenon of secondary particles during cycles, the void structure formed in the precursor has an appropriate void ratio by introducing an appropriate ratio of A element when the positive electrode material precursor is formed, thereby improving the cycle life and volumetric energy density of the positive electrode battery. Therefore, the present invention effectively overcomes some practical problems in the prior art, and thus has high application value and usage significance. [Brief description of the drawings]
[0020] In order to more clearly describe the technical problems in the embodiments of the present invention or the prior art, the following briefly introduces the figures required in the description of the embodiments or the prior art. Of course, the figures in the following description are only some examples of the present invention. Those skilled in the art can obtain other figures based on these figures without inventive efforts.
[0021] [Figure 1] FIG. 2 is a scanning electron microscope test diagram of the positive electrode material in the present invention. [Diagram 2] FIG. 1 is a flow diagram of a method for preparing a positive electrode material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The embodiments of the present invention will be described below with reference to specific examples. Those skilled in the art can easily understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied by other different specific implementation methods. The details of this specification can also be modified or changed based on different perspectives and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments may be combined with each other if not inconsistent. It should also be understood that the terms used in the embodiments of the present invention are for describing specific implementations and are not intended to limit the scope of the present invention. It should be noted that the test methods not showing specific conditions in the following embodiments are usually in accordance with conventional conditions or conditions proposed by each manufacturer.
[0023] It should be noted that terms such as "upper", "lower", "left", "right", "middle", and "one side" used in this specification are used for convenience of description only and are not used to limit the scope in which the present invention is practiced, and that changing or adjusting their relative relationships is considered to be within the scope in which the present invention can be practiced without substantially changing the technical content.
[0024] The present invention discloses a positive electrode material and its preparation method, a positive electrode sheet, and an electrochemical device. By introducing an appropriate proportion of A element when the positive electrode material precursor is formed, the cavity structure formed in the precursor has an appropriate void ratio, so as to ensure that the positive electrode material can buffer the volume distortion during the charging and discharging process through the internal void structure with an appropriate proportion, and to reduce the destruction phenomenon of secondary particles during cycling, thereby solving the technical problem that the positive electrode material in the prior art is easily destroyed by microscopic stress during charging and discharging, which deteriorates the cycle performance and gas generation performance of the battery.
[0025] Referring to FIG. 1, the positive electrode material of the present invention is a high-nickel ternary positive electrode material. The positive electrode material is spherical secondary particles 1 formed by aggregation of primary particles. The spherical secondary particles 1 include a cavity structure 2 dispersed therein. The cavity structure 2 present in the secondary particles 1 has a rich form. These cavity structures 2 facilitate the release of microscopic stress generated in the positive electrode material during the charge and discharge process, reduce the destruction of the secondary particles 1 due to the accumulation of stress between the primary particles, and thereby improve the cycle life of the positive electrode material. Note that the cavity structure is a hollow cavity structure formed inside the secondary particles of the positive electrode material due to the volatilization of internal elements and gas generation during the sintering and molding of the positive electrode material. Specifically, during the formation of the cavity structure of the positive electrode material, the A element introduced into the positive electrode material adheres to the inner wall of the cavity structure, thereby expanding the volume of the cavity structure.
[0026] Specifically, the primary particles of the positive electrode material are high-nickel ternary materials, and the chemical formula of the high-nickel ternary material is Li 1+a [Ni x Co y M z O 2-b A b where 0.7 ≦ x < 1, 0 ≦ y < 0.3, 0 ≦ z < 0.3, -0.2 < a < 0.2, 0 ≦ b < 0.2, and x + y + z = 1. In one optional embodiment, it is preferable that the high-nickel ternary material is Li 1+a [Ni x Co y M z O 2-b A b where 0.8 ≦ x < 1, 0 ≦ y < 0.1, 0 ≦ z < 0.2, -0.2 < a < 0.2, 0 ≦ b < 0.2, and x + y + z = 1.
[0027] In some embodiments, the M element in the high nickel ternary material is selected from one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W. That is, the M element can be any one of the element types listed above, such as Mn, Al, Ti, Zr, Mg, Sr, W, Mo, or B. The M element can be a combination of two or more of the elements listed above. For example, the M element can be a combination of Mn and Zr, or a combination of Al and Ti, or a combination of Al and Ce, a combination of Mn, Al, and W, Mn, Al, Nb, and Ru, or other combinations not listed here.
[0028] The A element in the high nickel ternary material is selected from one or more of F, N, Cl, S, and P. That is, the A element can be any one of the element types listed above, such as F, N, Cl, S, or P. The A element can be a combination of two or more of the elements listed above. For example, the A element is a combination of S and Cl, or a combination of F and S, or a combination of N and Cl, or a combination of S, P, and Cl, or a combination of S, N, F, and Cl, or other combinations not listed here.
[0029] In addition, when the A element and the M element are two or more combinations, there is no restriction on the ratio of each element in the combination, and they may be mixed in any ratio, etc. In other embodiments, the A element and the M element may be element types not listed above.
[0030] Specifically, the A element contained in the positive electrode material remains in the secondary particles when the nickel source, the cobalt source, and the M element carrier source are co-precipitated to synthesize the nickel-cobalt precursor. In one embodiment of the present invention, in the positive electrode material, at least one element of the A element is attached to the cavity structure in the secondary particles, and the A element remaining in the cavity is positively correlated with the void ratio in the secondary particles. Therefore, for the positive electrode material, the microstructure in the secondary particles of the positive electrode material may be judged by the cross-sectional void ratio of the positive electrode material and the A element content index. It should be noted that the "void ratio" of the positive electrode material here refers to the area ratio of the void structure in the cross section of the secondary particle. The void ratio is measured as follows. The secondary particles of the positive electrode material are cut using a focused ion beam, a cross-sectional photograph is obtained using a scanning electron microscope, and then the cross-sectional photograph is used to calculate the ratio of the total area of the void structure to the cross-sectional area of the secondary particle. The content of the A element in the positive electrode material can be obtained by EDS energy spectrum analysis of a transmission electron microscope test.
[0031] In the positive electrode material, when at least one element contained in the A element is attached to the inner wall of the cavity structure of the secondary particle, and the void ratio of the cross section of the secondary particle and the content of the A element are within a suitable range, for example, when the void ratio is 0.5%-10%, the cavity structure and morphology in the positive electrode material are abundant. These void structures facilitate the release of microscopic stress generated by the positive electrode material during the charge and discharge process, and reduce the destruction of the secondary particles caused by the stress accumulated between the primary particles, thereby improving the cycle life of the high nickel ternary positive electrode material.
[0032] When the void ratio and A element content in the positive electrode material are too low (i.e., when the void ratio of the positive electrode material is less than 0.5%), the secondary particles of the positive electrode material are denser and have a higher tap density. The stress generated by the volume phase transition of the material during the charging and discharging process has no place to be released, which easily causes the destruction of the secondary particles during the stress accumulation process, making it difficult to improve the cycle life of the positive electrode material. When the void ratio and A element content in the positive electrode material are too high (i.e., when the void ratio of the positive electrode material is more than 15%), the tap density of the positive electrode material particles is lower, the volume energy density of the battery cell is lower, and the contact area with the electrolyte increases during the charging and discharging process, which causes the side reaction with the electrolyte to intensify, resulting in the deterioration of the cycle of the positive electrode material.
[0033] It should be mentioned that tap density (TD) refers to placing a certain amount of powder in a container, periodically vibrating it under certain conditions, compressing the gap between particles as much as possible, and finally reading the volume of the powder when the gap between particles cannot be reduced, and then dividing the weight of the powder by the volume to obtain the tap density.The tap density of the positive electrode material in the present invention is obtained by testing according to national standard GB / T5162-2006.
[0034] In some embodiments, the elements attached to the inner walls of the cavity structure include sulfur. Specifically, when the sulfur content in the positive electrode material is 0.01 wt% to 0.35 wt%, the cross section of the secondary particles of the positive electrode material has a void ratio of 0.5% to 10%. In this case, the particle tap density of the positive electrode material is 2.38 g / cm. 3 ~2.81g / cm 3 The positive electrode material can maintain a cycle capacity retention rate of 80% or more for 800 cycles, has a lower increase in gas generation, and has a longer cycle life.
[0035] When the sulfur content in the positive electrode material is 0.01 wt% to 0.05 wt%, the secondary particle cross section of the positive electrode material has a void ratio of 0.5% to 5%, and the particle tap density of the positive electrode material is 2.49 g / cm 3 ~2.81g / cm 3At this time, the positive electrode material can maintain a cycle capacity retention rate of 80% or more for 800 cycles, and the gas generation increase rate of the positive electrode material after 56 days of operation is less than 4%.
[0036] In some embodiments, the valence state of elemental sulfur in the positive electrode material is at least one of −2, +4, and +6, and in the positive electrode material, elemental sulfur is stored in the cavity structure in the form of at least one of sulfide ions, thiosulfate ions, sulfate ions, and sulfite ions.
[0037] Specifically, the content of sulfur element in the secondary particles affects the valence state of sulfur element in the positive electrode material. For example, when the content of sulfur element in the secondary particles of the positive electrode material is 0.01wt%-0.1wt%, the XPS photoelectron peak binding energy range of sulfur element in the positive electrode material is 168±2eV, the valence state of sulfur element in the positive electrode material is -2, +4, and +6, and the sulfur element is stored in the cavity structure in the form of sulfur ion, thiosulfate ion, sulfate ion, and sulfite ion. When the content of sulfur element in the secondary particles of the positive electrode material is 0.01wt%-0.05wt%, the XPS photoelectron peak binding energy range of sulfur element in the positive electrode material is 168.5±1eV, the valence state of sulfur element in the positive electrode material is +4 and +6, and the sulfur element is stored in the cavity structure in the form of sulfate ion and sulfite ion.
[0038] As shown in FIG. 1, in some embodiments, the inner diameter of the cavity structure in the secondary particles of the positive electrode material is 10 nm to 1 μm.
[0039] Referring to FIG. 2, the present invention provides a method for preparing a positive electrode material, which includes the following steps.
[0040] S1. A nickel source, a cobalt source, and an M element carrier source are mixed with a precipitating agent and a complexing agent for a coprecipitation reaction. After the coprecipitation reaction is completed, the product is washed and dried to obtain a nickel-cobalt precursor material. The nickel-cobalt precursor is Ni x Co y M z (OH)2-b A b It is.
[0041] S2. The nickel-cobalt precursor material is mixed with a lithium source, then sintered, and the sintered material is crushed and classified to obtain the finished cathode material.
[0042] Step S1 specifically includes: pouring a nickel source, a cobalt source, and an M element carrier source into a continuous stirring reactor according to the molar ratio of nickel, cobalt, and M elements being (70-100):(0-30):(0-30) to obtain a mixed solution; then mixing the mixed solution with a precipitant aqueous solution and a complexing agent aqueous solution for coprecipitation reaction and maturing to obtain a solid-liquid mixture; pressing the solid-liquid mixture to obtain a filter cake; washing and drying the filter cake to obtain the nickel-cobalt precursor Ni x Co y M z (OH) 2-b A b where 0.7≦x<1, 0≦y<0.3, 0≦z<0.3, 0≦b<0.2, x+y+z=1, and the molar ratio between each element may be selected within the above ranges according to specific requirements.
[0043] In step S1, the nickel source, the cobalt source, and the M element carrier source are soluble salts to which nickel, cobalt, and M elements are added, respectively. As an example, the nickel source, the cobalt source, and the M element carrier source may be one or more of soluble sulfates, oxalates, acetates, chlorides, nitrates, or carbonates. Specifically, the nickel source, the cobalt source, and the M element carrier source include an A element, where the A element is selected from one or more of F, N, Cl, S, and P, and the M element is selected from one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W.
[0044] In some embodiments, at least one of the nickel source, the cobalt source, and the M element carrier source used in step S1 is preferably a sulfate.
[0045] The solution is not particularly limited as long as the nickel source, the cobalt source, and the M element carrier source are dissolved in the solution. As an example, the solution may be selected from one or more of deionized water, methanol, ethanol, acetone, isopropanol, and n-hexanol.
[0046] The precipitating agent is selected from one or more of NaOH, KOH, and LiOH, and the complexing agent is selected from one or more of aqueous ammonia, ammonium bicarbonate, ammonium carbonate, citric acid, and ethylenediaminetetraacetic acid.
[0047] Specifically, during the synthesis process of the coprecipitation reaction, the nickel-cobalt precursor forms a cavity structure inside the secondary particles aggregated by the primary particles. The A element contained in the nickel source, the cobalt source, and the M element carrier source remains and adheres to the inside of the cavity structure as the cavity structure is formed. The A element remaining in the cavity can effectively adjust the cavity structure formed in the secondary particles so as to enrich the morphology of the cavity structure in the positive electrode material. Furthermore, there is a positive correlation between the A element remaining in the cavity and the void ratio in the secondary particles.
[0048] In some embodiments, the A element attached inside the cavity structure includes at least sulfur element, and the content of sulfur element in the positive electrode material is directly proportional to the void ratio of the particle cross section. In step S1, the void ratio in the nickel-cobalt precursor is adjusted by adjusting the sulfur element content of the nickel source, the cobalt source, and the M element carrier source in the coprecipitation reaction, so that the void ratio and sulfur content of the secondary particle cross section of the obtained positive electrode material are within a suitable range. In this way, the void structure morphology inside the positive electrode material is enriched, and the cycle life performance of the positive electrode material is improved at the same time. For example, in one example, when the content of sulfur element in the positive electrode material is 0.01wt%-0.35wt%, the positive electrode material has a void ratio of 0.5%-10%.
[0049] In some embodiments, the lithium source in step S2 may be selected from one or more of lithium carbonate, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium oxide, and lithium nitrate. Further, the lithium source may be selected from one or more of lithium carbonate, lithium hydroxide, and lithium nitrate. Further, the lithium source is lithium carbonate.
[0050] There is no particular limitation on the grinding method in step S2, and any grinding and classification method in the prior art may be used, for example, a jet mill may be used. The specific parameters for grinding the sinter may be selected according to actual requirements.
[0051] The present invention further provides a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector, the positive electrode active material layer including the positive electrode material of the present invention.
[0052] The process for preparing the positive electrode sheet is as follows. The positive electrode material prepared above, the conductive agent, and the binder are mixed in a mass ratio of (90-99):1.5:1.5, with a preferred mass ratio of 97:1.5:1.5. The mixture is added to a solvent N-methylpyrrolidone (NMP) and thoroughly stirred and mixed to obtain a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil positive electrode current collector, and a positive electrode sheet is prepared through processes such as drying, cold pressing, and slitting. Specifically, the conductive agent may be selected from at least one of conductive materials such as Super P (carbon black), acetylene black, carbon nanotubes (CNT), graphene, and carbon nanofibers (VGCF). For example, the conductive agent is SP and CNT, and the mass ratio of SP and CNT is 1:0.5. The binder may be selected from at least one of PVDF, PTEE, and the like.
[0053] The present invention provides an electrochemical device. The electrochemical device includes the positive electrode material or the positive electrode sheet of the present invention. The electrochemical device is, for example, a lithium ion battery. Specifically, the lithium ion battery includes a positive electrode sheet, a negative electrode sheet, a separator provided between the positive electrode sheet and the negative electrode sheet, and an electrolyte.
[0054] Specifically, the positive electrode sheet is produced by the production method described above in the present invention.
[0055] Negative electrode sheet preparation: Negative electrode materials such as graphite, conductive agent acetylene black, thickener CMC (sodium carboxymethyl cellulose), and binder SBR (styrene butadiene rubber) are mixed in a mass ratio of 96.4:1:1.2:1.4, deionized water is added, and the mixture is thoroughly stirred to obtain negative electrode slurry. The negative electrode slurry is uniformly coated on the negative electrode current collector copper foil, and the negative electrode sheet is prepared through processes such as drying, cold pressing, and slitting.
[0056] Separator: Materials PE and PP porous membrane are used as separators, and the thickness of the PP / PE / PP porous membrane is preferably 9μm to 18μm, such as 9μm, 12μm, 16μm, or 18μm. The air permeability is 180s / 100mL to 380s / 100mL, such as 180s / 100mL, 280s / 100mL, or 380s / 100mL. The porosity is 30% to 50%, for example 30%, 40%, or 50%.
[0057] Preparation of electrolyte: EC (ethylene carbonate), DMC (dimethyl carbonate), and EMC (ethyl methyl carbonate) were mixed in a mass ratio of 1:1:1 to obtain an organic solvent, which was then completely dried and mixed with lithium salt LiPF 6 is dissolved in the mixed organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L.
[0058] Battery assembly: The obtained positive electrode sheet, separator, and negative electrode sheet are laminated in order so that the separator is between the positive electrode sheet and the negative electrode sheet to function as an insulator. Then, this is covered with an aluminum-plastic film, and after drying, the electrolyte prepared above is injected. After processes such as packaging, leaving, and chemical formation, a soft-pack battery (i.e., a lithium-ion battery) with a capacity of 1 Ah is finally completed.
[0059] The technical solutions of the present invention are described in detail below through some specific examples and comparative examples. Unless otherwise specified, all raw materials and reagents used in the following examples are commercially available or can be prepared by conventional methods in the art.
[0060] Example 1
[0061] Step 1: Nickel sulfate, cobalt sulfate and manganese sulfate solutions were mixed with a Ni:Co:Mn molar ratio of 90:5:5, and ammonia water and sodium hydroxide solution were added to the mixed salt solution for coprecipitation reaction, and the product was washed and dried after the coprecipitation reaction was completed. Here, the sulfur content of the obtained nickel-cobalt precursor was detected to be 523 ppm after washing and drying.
[0062] Step 2: Add nickel-cobalt precursor and lithium hydroxide to ZrO 2 The mixture was fired in an oxygen atmosphere at a temperature of 760° C. for 12 hours to obtain a polycrystalline positive electrode material substrate.
[0063] Step 3: The polycrystalline positive electrode material substrate is mixed with 0.1 wt% Al 2 O 3 and then sintered at a temperature of 400° C. for 8 hours in an oxygen atmosphere, and the finished positive electrode material was obtained after crushing and classification.
[0064] Example 2
[0065] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction was adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 was 1345 ppm.
[0066] Example 3
[0067] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction was adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 was 2732 ppm.
[0068] Example 4
[0069] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction was adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 was 3209 ppm.
[0070] Example 5
[0071] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 is 5378 ppm.
[0072] Example 6
[0073] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 is 8427 ppm.
[0074] Example 7
[0075] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction was adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 was 2937 ppm.
[0076] Example 8
[0077] The difference between this embodiment and Example 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction is adjusted to make the sulfur element content of the nickel-cobalt precursor prepared in step 1 2863 ppm; in step 2, the nickel-cobalt precursor is mixed with lithium hydroxide, ZrO 2 , and Al with a content ratio of 0.2 wt% 2 O 3 The mixture is sintered in an oxygen atmosphere at a temperature of 760° C. for 12 hours. In step 3, the polycrystalline positive electrode material substrate obtained in step 2 is mixed with 0.1 wt% Al 2 O 3 , and TiO with a content ratio of 0.1 wt% 2 Then the mixture was sintered at 350°C for 8 hours in an oxygen atmosphere, and the finished positive electrode material was obtained after grinding and classification.
[0078] Example 9
[0079] The difference between this embodiment and embodiment 1 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction is adjusted to make the sulfur element content of the nickel-cobalt precursor prepared in step 1 2749 ppm; in step 2, the nickel-cobalt precursor is mixed with lithium hydroxide, ZrO 2 , Al content ratio 0.2wt% 2 O 3 and 0.1 wt% MgO, and the mixture is fired at 760°C for 12 hours in an oxygen atmosphere. In step 3, the polycrystalline positive electrode material substrate obtained in step 2 is mixed with 0.1 wt% Al 2 O 3 , and B with a content ratio of 0.1 wt% 2 O 3 Then the mixture was sintered at 350°C for 8 hours in an oxygen atmosphere, and the finished positive electrode material was obtained after grinding and classification.
[0080] Example 10
[0081] The difference between this embodiment and Example 5 is that in step 1, the solutions of nickel sulfate, cobalt sulfate, and manganese sulfate involved in the coprecipitation reaction were mixed in a Ni:Co:Mn molar ratio of 70:15:15.
[0082] Example 11
[0083] The difference between this embodiment and Example 5 is that in step 1, the solutions of nickel sulfate, cobalt sulfate, and manganese sulfate involved in the coprecipitation reaction were mixed in a Ni:Co:Mn molar ratio of 80:10:10.
[0084] Comparative Example 1
[0085] The difference between this comparative example and Example 8 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction was adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 was 230 ppm.
[0086] Comparative Example 2
[0087] The difference between this comparative example and Example 9 is that in step 1, the sulfur element concentration in the reactor during the coprecipitation reaction is adjusted so that the sulfur element content of the nickel-cobalt precursor prepared in step 1 is 12027 ppm.
[0088] The nickel-cobalt precursor prepared in step 1 in Examples 1-11 and Comparative Examples 1-2 was tested for sulfur element content, and the sulfur content test method of the precursor included dissolving the nickel-cobalt precursor sample obtained in step 1 in hydrochloric acid, diluting it to a certain amount with water, and testing the sulfur element content by inductively coupled plasma mass spectrometry (ICP-MS).
[0089] For the positive electrode sheets prepared in Examples 1 to 11 and Comparative Examples 1 and 2, the sulfur content in the cross section of the electrode particles and the void ratio in the cross section of the electrode particles were tested.
[0090] Specifically, sulfur content testing of cross sections of electrode particles involved using an ion beam to cut the electrode sheet to obtain cross-sectional samples of the electrode material, and using high-resolution EDS testing in a transmission electron microscope (TEM) to obtain the sulfur content of the cross-sectional samples.
[0091] The void ratio test of the cross section of the electrode particle included obtaining an SEM of the cross section of the positive electrode by cutting the positive electrode sheet using an ion beam and then imaging the SEM. On the SEM image, the cavities usually show a different contrast than other physical areas. Graphics software can be used to identify the cross-sectional area of the cavity area and calculate the void ratio. The present invention provides an example of calculating the void ratio of the particle cross section using the open source graphics software Image J.
[0092] Step a. First, obtain a cross section of the positive electrode sheet by ion beam cutting or the like, select a particle cross section cut from the center of the secondary particle, and image it with a high-resolution SEM. The imaged SEM must satisfy the uniform contrast of the cavity area and the uniform contrast distribution of other physical areas.
[0093] Step b. The pictures were opened using Image.J and the RGB channels were split using the “split channels” function to obtain single channel pictures.
[0094] Step c. The measurement scale was set to match the scale of the electron microscope, a circular (or elliptical or irregularly shaped) selected area was defined, the entire cross section of the secondary particle was selected, and the total area S1 of the selected area was measured.
[0095] Step d. The threshold of the photo was adjusted until all the hollow regions of the particle cross-section in the defined area were marked, and the total area S2 of the marked hollow regions was obtained using the “analyze particle” function.
[0096] Step e. The void ratio was calculated as H=S2 / S1.
[0097] For battery performance testing, the positive electrode materials prepared in Examples 1-11 and the positive electrode materials prepared in Comparative Examples 1-2 were assembled into soft-pack batteries according to the assembly method of the present invention. The battery performance testing included a cycle capacity retention test and a gas generation performance test.
[0098] Specifically, the battery cycle capacity retention test included cycling using a 2.8-4.5 V charge-discharge system at 0.21 A / g (calculated based on the mass of the positive electrode material) under conditions of 25° C. After 800 cycles, the discharge capacity of the battery at this point was divided by the discharge capacity of the first cycle, and this was defined as the 800 cycle capacity retention rate of the battery.
[0099] The battery gas generation performance test included testing the initial volume V1 of the battery after fully charging the battery, and then storing the battery in a high temperature cabinet at 60°C. Every 7 days, the battery was recharged and the volume was tested. After 56 days, the volume of the battery was V2, and (V2-V1) / V1 was the gas generation increase rate.
[0100] See Table 1 for the test results of Examples 1 to 11 and Comparative Examples 1 and 2.
[0101] Table 1: Structure and battery performance of the positive electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 2
[0102] [Table 1]
[0103] Comparing Example 3, Example 8, and Comparative Example 1, it can be seen that when the sulfur content in the positive electrode cross section is too low (<0.01 wt%), the void ratio of the positive electrode cross section is lower (<0.5%), the positive electrode material has a lower cycle capacity retention rate at 800, and the increase in gas generation is greater. This is because when the inside of the positive electrode material is dense overall, there are no cavities in the secondary particles to buffer the stress generated by the volume expansion / contraction of the material during the charge / discharge process. As a result, the secondary particles are destroyed during cycling, and side reactions are intensified at the interface between the positive electrode and the electrolyte, which deteriorates the cycle performance and gas generation performance of the battery.
[0104] Comparing Example 4, Example 9, and Comparative Example 2, it can be seen that when the sulfur content in the cross section of the positive electrode is too high (≧0.5wt%), there are too many internal cavities in the secondary particles (positive electrode cross section void ratio ≧15%), the tap density of the positive electrode material is lower, the particles are easily broken during rolling, and the side reaction at the interface between the positive electrode and the electrolyte increases, which deteriorates the cycle performance and gas generation performance of the battery.
[0105] Comparing Example 5, Example 10, and Example 11, when the sulfur content in the positive electrode cross section is the same, adjusting the composition ratio of Ni, Co, and Mn elements in the positive electrode material does not affect the tap density of the positive electrode material and the cycle performance and gas generation performance of the secondary battery assembled using the positive electrode material.
[0106] Based on the above, it can be found that when the sulfur content and void ratio of the positive electrode cross section in the positive electrode material are within a certain range, the cycle performance of the material is better, because a certain ratio of internal voids can buffer the volume distortion of the positive electrode during the charging and discharging process, and alleviate the destruction phenomenon of secondary particles during the cycling process.On the contrary, when the sulfur content is too high or low, the internal void ratio of the positive electrode particles is too high or low, which affects the stress release of the material during the charging and discharging process, and the side reaction at the interface between the electrode and the electrolyte is deteriorated, leading to the deterioration of cycle performance and gas generation performance. [Industrial Applicability]
[0107] In the positive electrode material and its preparation method, positive electrode sheet and electrochemical device of the present invention, based on the positive correlation characteristic between the content of A element in the positive electrode material particles and the void ratio, in order to ensure that the positive electrode material can buffer the volume distortion during the charging and discharging process through the appropriate ratio of internal void structure, and to reduce the destruction phenomenon of secondary particles during cycles, the void structure formed in the precursor has an appropriate void ratio by introducing an appropriate ratio of A element when the positive electrode material precursor is formed, thereby improving the cycle life and volumetric energy density of the positive electrode battery. Therefore, the present invention effectively overcomes some practical problems in the prior art, and thus has high application value and usage significance.
[0108] The above-mentioned embodiment is illustrative of the principle and effect of the present invention, and is not intended to limit the present invention. Those skilled in the art may modify or change the above-mentioned embodiment without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical idea disclosed in the present invention are also encompassed by the claims of the present invention. [Explanation of symbols]
[0109] 1: Secondary particles 2: Cavity structure
Claims
1. These are secondary particles formed by agglomeration of primary particles, The secondary particles include a hollow structure therein. Positive electrode material.
2. The chemical formula of the positive electrode material is Li 1+a [Ni x Co y M z ]O 2-b A b and where 0.7≦x<1, 0≦y<0.3, 0≦z<0.3, −0.2<a<0.2, 0≦b<0.2, and x+y+z=1; The M element includes one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W, and the A element includes one or more of F, N, Cl, S, and P; The positive electrode material according to claim 1 .
3. At least one element among the A elements is attached to an inner layer of the cavity structure. The positive electrode material according to claim 2 .
4. The elements attached to the inner layer of the hollow structure include a sulfur element, and the void ratio of the positive electrode material is positively correlated with the content of the sulfur element in the positive electrode material. The positive electrode material according to claim 3 .
5. When the sulfur content in the secondary particles is 0.01 wt % to 0.35 wt %, the positive electrode material has a void ratio of 0.5% to 10%, and the particle tap density of the positive electrode material is 2.38 g / cm 3 ~2.81g / cm 3 That is, The positive electrode material according to claim 2 .
6. The valence state of the sulfur element in the positive electrode material is at least one of −2, +4, and +6, and the sulfur element remains in the cavity structure in the form of at least one of a sulfide ion, a thiosulfate ion, a sulfate ion, and a sulfite ion. The positive electrode material according to claim 2 .
7. When the content of the sulfur element in the secondary particles is 0.01 wt % to 0.1 wt %, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168±2 eV; When the content of the sulfur element in the secondary particles is 0.01 wt % to 0.05 wt %, the XPS photoelectron peak binding energy range of the sulfur element in the positive electrode material is 168.5±1 eV; The positive electrode material according to claim 6.
8. The inner diameter of the hollow structure is 10 nm to 1 μm; The positive electrode material according to claim 1 .
9. Mixing a nickel source, a cobalt source, and an M element carrier source for a coprecipitation reaction to obtain a nickel-cobalt precursor material, wherein the M element comprises one or more of Mn, Al, Ti, Zr, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Y, and W, and at least one carrier source in the nickel source, the cobalt source, and the M source is a sulfate; mixing the nickel-cobalt precursor material with a lithium source and then sintering to obtain a positive electrode material; Including, During the co-precipitation synthesis process, the nickel-cobalt precursor forms a cavity structure within the secondary particles; Method for preparing the positive electrode material.
10. The nickel source, the cobalt source, and the M element carrier source include an A element, the A element including one or more of F, N, Cl, S, and P, and the A element is deposited in the cavity structure during the co-precipitation reaction synthesis process of the nickel-cobalt precursor; A method for preparing the positive electrode material according to claim 9.
11. The sulfur element in the A element is attached to the inside of the hollow structure, and the void ratio of the positive electrode material is 0.5% to 10%. A method for preparing the positive electrode material according to claim 10.
12. The battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte solution, The positive electrode sheet comprises the positive electrode material of claim 1. Electrochemical devices.
13. The battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte solution, The positive electrode sheet comprises the positive electrode material prepared by the method for preparing a positive electrode material according to claim 9. Electrochemical devices.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery
JP2017084628A
Positive active material for lithium secondary battery, method of preparing the same, positive electrode for lithium secondary battery including the same, and lithium secondary battery
JP2023008932A