Negative electrode for lithium secondary battery, and lithium secondary battery

The use of a copolymer binder and oriented Si-C composite in the negative electrode of lithium secondary batteries addresses the challenge of high energy density and expansion issues, ensuring effective adhesion and stability during charging and discharging.

JP2024163013AInactive Publication Date: 2024-11-21SAMSUNG SDI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024038064
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-10
Filing Date
2024-03-12
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face challenges in achieving high energy density and effective expansion properties, particularly with silicon-based negative electrodes that suffer from excessive volume changes during charging and discharging.

Method used

A negative electrode for lithium secondary batteries is designed with a copolymer binder containing a (meth)acrylic acid and (meth)acrylonitrile monomer units, along with a Si-C composite and crystalline carbon second negative active material, oriented at an angle to the current collector using a magnetic field, enhancing adhesion and suppressing volumetric expansion.

Benefits of technology

The solution results in improved energy density and reduced expansion characteristics, preventing the negative electrode active material from detaching from the current collector, thereby maintaining battery performance and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163013000001_ABST
    Figure 2024163013000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode for a lithium secondary battery, and a lithium secondary battery including the same.SOLUTION: A negative electrode includes a current collector, and a negative electrode active material layer existing in the current collector and including a copolymer binder, a Si-C composite body first negative electrode active material, and a crystalline carbon second negative electrode active material. The copolymer binder includes a first repeating unit derived from (meth)acrylic acid monomer and a second repeating unit derived from (meth)acrylonitrile monomer. The DD value defined in Formula 1 below is 30 or more: DD(Degree of Divergence)=(Ia / Itotal)*100 (Formula 1). In Formula 1, when XRD is measured using the CuKα beam, Ia represents the total of the peak intensity values of four peaks in the definition, and when XRD is measured using the CuKα beam, Itotal represents the total of the peak intensity values of six peaks in the definition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode for a lithium secondary battery and a lithium secondary battery including the same. [Background technology]

[0002] Lithium secondary batteries, which have been attracting attention in recent years as a power source for small portable electronic devices, use an organic electrolyte and therefore exhibit a discharge voltage more than twice as high as that of existing batteries that use alkaline aqueous solutions, and as a result, exhibit a high energy density.

[0003] As an anode active material for lithium secondary batteries, silicon anode active material has a high discharge specific capacity of 3400mAh / g and is capable of rapid bonding with lithium ions, allowing for rapid charging and discharging. Research on this material is currently being actively conducted. Summary of the Invention [Problem to be solved by the invention]

[0004] An object of one embodiment is to provide a negative electrode for a lithium secondary battery having high energy density and improved expansion characteristics.

[0005] Another embodiment provides a lithium secondary battery including the negative electrode.

[0006] According to an embodiment, there is provided a negative electrode for a lithium secondary battery, the negative electrode active material layer being located on the current collector and including a copolymer binder, a Si-C composite first negative electrode active material, and a crystalline carbon second negative electrode active material, the copolymer binder including a first repeating unit derived from a (meth)acrylic acid-based monomer and a second repeating unit derived from a (meth)acrylonitrile monomer, and having a Degree of Divergence (DD) value of 30 or more as defined by the following Formula 1:

[0007] DD(Degree of Divergence)=(I a / I total )*100 (formula 1) In Equation 1, I a is the sum of the peak intensities at 2θ = 42.4 ± 0.2°, 43.4 ± 0.2°, 44.6 ± 0.2°, and 77.5 ± 0.2° when measuring with CuKα radiation. I total is the sum of the peak intensity values ​​appearing at 2θ = 26.5 ± 0.2°, 42.4 ± 0.2°, 43.4 ± 0.2°, 44.6 ± 0.2°, 54.7 ± 0.2°, and 77.5 ± 0.2° when XRD measurement was performed using CuKα radiation. According to another embodiment, a lithium secondary battery is provided that includes a negative electrode; a positive electrode including a positive electrode active material; and a non-aqueous electrolyte.

[0008] Other specific details of the embodiment are included in the following detailed description.

[0009] The negative electrode for a lithium secondary battery according to an embodiment may exhibit improved expansion characteristics. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram illustrating an orientation according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing the orientation of a negative electrode according to an embodiment. [Diagram 3] 1 is a schematic diagram illustrating a method of providing orientation in a process for manufacturing a negative electrode according to an embodiment; FIG. [Figure 4] 1 is a schematic diagram of a lithium secondary battery according to an embodiment; [Diagram 5] 1 is a photograph of the lithium secondary battery produced in Example 6, disassembled after chemical charge / discharge. [Figure 6] 1 is a photograph of the lithium secondary battery produced in Reference Example 1, disassembled after chemical charge / discharge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail, but they are presented as examples and are not to be construed as limiting the present invention, which is defined only by the scope of the claims that follow.

[0012] The terms used herein are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise.

[0013] As used herein, "combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like of compositions.

[0014] As used herein, terms such as "comprise," "comprise," or "have" are intended to specify the presence of embodied features, numerals, steps, components, or combinations thereof, and are to be understood as not precluding the presence or addition of one or more other features, numerals, steps, components, or combinations thereof.

[0015] In this specification, unless otherwise specified, when a part such as a layer, film, region, plate, etc. is "on" another part, this includes not only when it is "directly on" the other part, but also when there is another part in between.

[0016] In this specification, the phrase "A and / or B" means "A or B or all of these."

[0017] When a layer, film, region, plate, or other part is described as being "on" or "on top of" another part, this includes not only when it is "directly on" the other part, but also when there is another part between them. Conversely, when a part is "directly on" another part, it means that there is no other part between them.

[0018] In the present invention, the "particle size" and "particle diameter" may refer to the average particle diameter. If the particle is spherical, the size refers to the diameter, and if the particle is non-spherical, the size may refer to the major axis.

[0019] Unless otherwise defined in this specification, the particle size refers to the average particle size (D50), which means the diameter of particles with a cumulative volume of 50% by volume in the particle size distribution. The diameter and average particle size (D50) can be measured by a method widely known to those skilled in the art, for example, by using a particle size analyzer, a transmission electron microscope, a scanning electron microscope, or a field emission scanning electron microscopy (FE-SEM). As another method, the average particle size (D50) value can be obtained by calculating the number of particles counted for each particle size range after measuring using a measuring device using dynamic light-scattering, or by using a laser diffraction method. More specifically, when measuring by the laser diffraction method, the particles to be measured are dispersed in a dispersion medium, then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000) and irradiated with ultrasonic waves of about 28 kHz at an output of 60 W, after which the average particle size (D50) based on the 50% standard of the particle size distribution in the measuring device can be calculated.

[0020] According to an embodiment, a negative electrode for a lithium secondary battery includes a current collector; a negative electrode active material layer located on the current collector, the negative electrode active material layer including a copolymer binder, a Si-C composite first negative electrode active material, and a crystalline carbon second negative electrode active material.

[0021] The copolymer binder may include a first repeat unit derived from a (meth)acrylic acid monomer and a second repeat unit derived from a (meth)acrylonitrile monomer. In one embodiment, the copolymer binder may further include a third repeat unit derived from an additional monomer copolymerizable with the (meth)acrylic acid monomer and / or the (meth)acrylonitrile monomer.

[0022] In one embodiment, "(meth)" means that the methyl group may or may not be present. For example, (meth)acrylic acid means methacrylic acid or acrylic acid.

[0023] The content of the first repeating unit derived from the (meth)acrylic acid monomer may be 35% by weight to 65% by weight, or 40% by weight to 65% by weight, based on 100% by weight of the copolymer binder. When the content of the first repeating unit derived from the (meth)acrylic acid monomer in the copolymer binder is within the range, the dispersion of the negative electrode active material can be further improved, and the storage stability of the negative electrode active material composition used in manufacturing the negative electrode can be further improved.

[0024] In addition, the content of the second repeating unit derived from the (meth)acrylonitrile monomer may be 35% by weight to 65% by weight, or 35% by weight to 60% by weight, based on 100% by weight of the copolymer binder. When the content of the second repeating unit derived from the (meth)acrylonitrile monomer in the copolymer binder is within the range, the negative electrode can be manufactured more easily, the negative electrode active material layer can be more easily adhered to the current collector, and the storage stability of the negative electrode active material composition used in manufacturing the negative electrode can be further improved.

[0025] In one embodiment, the (meth)acrylic acid monomer may be (meth)acrylic acid, an alkali metal salt of (meth)acrylic acid, an ammonium salt of (meth)acrylic acid, or a combination thereof. The alkali metal salt of (meth)acrylic acid may be sodium acrylate, lithium acrylate, potassium acrylate, calcium acrylate, magnesium acrylate, sodium (meth)acrylate, lithium (meth)acrylate, potassium (meth)acrylate, calcium (meth)acrylate, or a combination thereof. The ammonium salt of (meth)acrylic acid may be an ammonia-neutralized product of (meth)acrylic acid, a monoethanolamine-neutralized product, a diethanolamine-neutralized product, a hydroxylamine-neutralized product, or a combination thereof.

[0026] In an embodiment, the copolymer binder may further include a third repeat unit derived from an additional monomer copolymerizable with the (meth)acrylic acid-based monomer and / or the (meth)acrylonitrile monomer.

[0027] The additional monomer copolymerizable with the (meth)acrylic acid monomer and / or the (meth)acrylonitrile monomer can include a hydroxyl group-containing monomer or an amide group-containing monomer. The hydroxyl group-containing monomer can include, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyhexyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, 4-hydroxymethylcyclohexyl (methyl)acrylate, N-methylol (meth)acrylamide, N-hydroxy (meth)acrylamide, vinyl alcohol, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, or a combination thereof. Examples of the amide group-containing monomer include acrylamide, methacrylamide, diethyl(meth)acrylamide, N-vinylpyrrolidone, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N'-methylenebisacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, or combinations thereof.

[0028] When the copolymer binder further includes a third repeat unit derived from a monomer copolymerizable with a (meth)acrylic acid monomer and / or a (meth)acrylonitrile monomer, the content of the third repeat unit may be more than 0 wt% and 20 wt% or less, based on 100 wt% of the copolymer binder.

[0029] In this case, the content of the first repeating unit or the second repeating unit can be appropriately adjusted. For example, the content of the first repeating unit or the second repeating unit can be 35% by weight or more and less than 65% by weight.

[0030] When the copolymer binder further contains a third repeating unit, the electrode expansion of the negative electrode can be more effectively suppressed.

[0031] The copolymer binder may be a water-soluble copolymer for stabilizing the dispersion of the polymer. The copolymer binder may have a viscosity of 500 mPa·s to 3000 mPa·s, 750 mPa·s to 2500 mPa·s, 750 mPa·s to 2000 mPa·s, 750 mPa·s to 1500 mPa·s, or 1000 mPa·s to 1500 mPa in an aqueous solution having a solid content of 7% by weight. When the viscosity of the aqueous solution having a solid content of 7% by weight of the copolymer binder is within the range, the adhesion of the negative electrode active material layer to the current collector can be further improved, and the cycle life characteristics can be further improved. The above viscosity can be measured, for example, at 30 rpm and room temperature (25 degrees) using a Brookfield viscometer with an LV4 spindle, but is not limited thereto.

[0032] In one embodiment, the copolymer binder may be a copolymer of acrylic acid and acrylonitrile.

[0033] The weight average molecular weight (Mw) of the copolymer binder may be 100,000 g / mol to 1500,000 g / mol, and may be 500,000 g / mol to 1,000,000 g / mol. In one embodiment, the weight average molecular weight (Mw) may be measured by GPC (gel permeation chromatography).

[0034] In an embodiment, the negative electrode may have a degree of divergence (DD) value defined by the following Formula 1 of 30 or more, 30 to 60, 30 to 55, 35 to 55, or 40 to 55.

[0035] DD(Degree of Divergence)=(I a / I total )*100 (formula 1) In Equation 1, I a is the sum of the peak intensities that appear at non-planar angles when measuring XRD using CuKα radiation, and I total is the sum of the peak intensity values ​​appearing at all angles when XRD measurement is performed using CuKα radiation.

[0036] The non-planar angles are 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, and 77.5±0.2° when measured by XRD using CuKα radiation, i.e., (100) plane, (101)R plane, (101)H plane, and (110) plane. Generally, graphite is classified into a hexagonal structure and a rhombohedral structure having an ABAB stacking sequence according to the stacking order of the graphene layers, with the R plane representing the rhombohedral structure and the H plane representing the hexagonal structure.

[0037] Therefore, I a can be the sum of peak intensity values ​​shown at θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, and 77.5±0.2° when XRD measurement is performed using CuKα radiation.

[0038] The "all angles" are 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2°, and 77.5±0.2° when measured by XRD using CuKα radiation, i.e., these represent the (002) plane, (100) plane, (101)R plane, (101)H plane, (004) plane, and (110) plane. The peak appearing at 2θ=43.4±0.2° can be seen as an overlap of the peaks corresponding to the (101)R plane of the carbon-based material and the (111) plane of the current collector, e.g., Cu.

[0039] Therefore, I total can be the sum of the peak intensity values ​​appearing at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2°, and 77.5±0.2° when XRD measurement is performed using CuKα radiation.

[0040] In general, the peak intensity value refers to the height value of a peak or the integrated area value of a peak, and according to an embodiment, the peak intensity value refers to the integrated area value of a peak.

[0041] In one embodiment, the XRD measurement was performed using CuKα radiation as a target radiation, and the monochromator device was removed to improve peak intensity resolution. The measurement conditions were 2θ=10°~80°, scan speed (° / S) of 0.044~0.089, and step size (° / step) of 0.013~0.039.

[0042] The DD value is a value indicating that the negative active material contained in the negative active material layer is oriented at a certain angle, and the larger this value is, the better the orientation of the negative active material is. That is, as shown simply in FIG 1, when the negative active material 3 is oriented at an angle (a) with respect to one surface of the substrate 1, the larger the DD value is, the greater the angle (a) is. In addition, such a DD value is maintained even when charging and discharging are performed.

[0043] In an embodiment, the DD value of the negative electrode may be 30 or more, 30 to 60, or 30 to 50. The DD value of the negative electrode being 30 or more means that the negative electrode active material layer of the negative electrode is an oriented layer since it means that the negative electrode active material stands substantially perpendicular to the current collector at a certain angle. For example, the substantially perpendicular state does not only mean that the negative electrode stands at an angle of 90° to the current collector, but also means that the negative electrode active material stands at an angle close to 90°.

[0044] If the DD value of the negative electrode is less than 30, the negative electrode active material layer contained therein corresponds to a non-oriented layer, or even if the negative electrode active material layer is an oriented layer, the expansion effect is small, which is not appropriate.

[0045] In this way, since the negative electrode active material 3a is positioned in a vertical direction relative to the current collector 1, volume expansion can occur in a horizontal direction during charging and discharging of a battery including this negative electrode (see FIG. 2). Therefore, excessive vertical volume expansion that can occur when using a negative electrode active material containing Si can be effectively suppressed, the battery thickness increase rate can be significantly reduced, and the active material layer can be prevented from being detached from the current collector. Therefore, a negative electrode active material containing Si that can improve energy density can be easily applied to a battery.

[0046] In particular, the negative electrode according to an embodiment includes a copolymer binder in the binder, which can more effectively suppress volume expansion of the negative electrode, ensure flexibility and adhesive strength during the manufacture of the negative electrode, and prevent the negative electrode active material layer from falling off the current collector even after charging and discharging a battery including the negative electrode.

[0047] In an embodiment, the content of the copolymer binder may be 0.5 wt% to 5 wt%, 0.8 wt% to 5 wt%, 1.0 wt% to 5 wt%, or 1.2 wt% to 4.0 wt%, based on 100 wt% of the total negative electrode active material layer. When the content of the copolymer binder is within the range, the volume expansion of the negative electrode during charging and discharging of the battery can be further reduced.

[0048] In one embodiment, the negative electrode active material includes a Si-C composite first negative electrode active material and a crystalline carbon second negative electrode active material, and the Si content may be 1 wt% to 20 wt% or 3 wt% to 20 wt% based on 100 wt% of the total of the first negative electrode active material and the second negative electrode active material. When the negative electrode active material includes Si in the range, the energy density can be further improved and a high capacity can be obtained.

[0049] In an embodiment, the crystalline carbon-based active material may be amorphous, plate-like, flake-like, spherical or fibrous artificial graphite, natural graphite, or a combination thereof.

[0050] The Si-C composite may include Si and a carbon-based material. The carbon-based material may be amorphous carbon or crystalline carbon. An example of the composite may include a core including Si particles and a carbon-based material surrounding the core. The core may further include a carbon-based material. For example, the Si-C composite may include a core in which Si particles and a first carbon-based material are mixed, and a second carbon-based material surrounding the core. The first carbon-based material and the second carbon-based material may be the same or different, and may be amorphous carbon or crystalline carbon. A specific example of the composite may include at least one secondary particle in which Si nanoparticle primary particles and crystalline carbon are assembled, i.e., an assembly, and may include an amorphous carbon coating layer surrounding the assembly, and may include amorphous carbon filled between the assemblies and surrounding the surface of the primary particles.

[0051] In the Si-C composite, the Si content can be adjusted to fall within the range of 1 wt % to 20 wt %, or 3 wt % to 20 wt %, relative to 100 wt % of the total first and second negative electrode active materials.

[0052] The particle size of the Si may be 10 nm to 30 μm, and in one embodiment, 10 nm to 1000 nm, and in another embodiment, 20 nm to 150 nm. When the average particle size of the Si is within this range, volume expansion that occurs during charging and discharging can be suppressed, and the conductive path can be prevented from being broken due to particle crushing during charging and discharging.

[0053] In an embodiment, the mixing ratio of the Si-C composite first negative electrode active material and the crystalline carbon second negative electrode active material may be 3:97 to 10:90 by weight, 3:97 to 15:85 by weight, or 7:93 to 10:90 by weight. When the mixing ratio of the Si-C composite first negative electrode active material and the crystalline carbon second negative electrode active material is within the range, a higher capacity or a high energy density effect can be obtained.

[0054] The amorphous carbon can be pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a combination thereof, and the crystalline carbon can be amorphous, plate-like, flake-like, spherical, or fibrous natural graphite, artificial graphite, or a combination thereof.

[0055] In one embodiment, the DD value is a value obtained by measuring the XRD of the negative electrode obtained by dismantling a fully discharged lithium secondary battery including the negative electrode after charging and discharging the battery. At this time, the charging and discharging conditions are 0.1C to 0.2C, and the charging and discharging is performed once or twice. At this time, the DD value of the active material layer is a value obtained by peeling off the active material layer using tape after charging and discharging, and then measuring the XRD of the active material layer along the current collector side.

[0056] In one embodiment, the thickness of the negative electrode active material layer may be 10 μm to 100 μm. When the thickness of the negative electrode active material layer is within the range, there may be an advantage in adhesive strength. In one embodiment, the negative electrode active material layer may be formed on one or both sides of the current collector, and the thickness may be the thickness of one side of the negative electrode active material layer. For example, it may be the thickness of the negative electrode active material layer formed on one side of the current collector, and when the negative electrode active material layer is formed on both sides of the current collector, the total thickness of the negative electrode active material layer included in the negative electrode may be 20 μm to 200 μm.

[0057] The thickness of the negative electrode active material layer means the thickness after rolling and vacuum drying in the negative electrode manufacturing process. The vacuum drying process may be performed under conditions of 0.03 atm to 0.06 atm pressure and 100°C to 160°C. When the negative electrode active material layer includes only the negative electrode active material and the copolymer binder, the content of the negative electrode active material may be 96 wt% to 99.2 wt% based on the total weight of the negative electrode active material layer.

[0058] The negative electrode active material layer may further include an aqueous binder. In this case, the content of the copolymer binder in the negative electrode active material layer may be 0.8 wt% to 5 wt%, the content of the negative electrode active material may be 90 wt% to 98.2 wt%, and the content of the aqueous binder may be 1 wt% to 5 wt%, based on the total weight of the negative electrode active material layer.

[0059] The negative electrode active material layer may further include a conductive material, and the content of the copolymer binder in the negative electrode active material layer may be 0.8 wt% to 5 wt%, the negative electrode active material may be 85 wt% to 97.2 wt%, the conductive material may be 1 wt% to 5 wt%, and the aqueous binder may be 1 wt% to 5 wt%, based on the total weight of the negative electrode active material layer.

[0060] The water-based binder may be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polyvinylpyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.

[0061] The aqueous binder may contain a cellulose-based compound. The cellulose-based compound may be a mixture of one or more of carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or an alkali metal salt thereof. The alkali metal may be Na, K, or Li.

[0062] The conductive material is used to impart electrical conductivity to the electrode, and any electronically conductive material that does not cause a chemical change in the battery that is constructed can be used. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber; metal-based materials such as metal powder or metal fiber of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials including mixtures thereof.

[0063] The current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, conductive metal coated polymer substrate, and combinations thereof.

[0064] The negative electrode according to the embodiment may be formed by applying a magnetic field to a current collector while applying a negative electrode active material composition to the current collector. A process for manufacturing the negative electrode according to the embodiment will be described in detail below with reference to FIG.

[0065] As shown in FIG. 3, a magnet 7 is placed under a current collector 1, and then a negative active material layer composition containing a negative active material 3a is applied and dried to form a negative active material layer (U1). The negative active material layer composition application process is performed by moving the current collector 1 in the coating direction with a magnet placed under it. Therefore, a magnetic field (magnetic flux) from the magnet 7 is formed perpendicular to the current collector 1, but the direction in which the magnetic field is formed is formed at a certain angle as a vector function depending on the coating speed (current collector movement speed). Thus, the carbon-based negative active material contained in the negative active material layer composition can stand at a certain angle with respect to the current collector, i.e., be oriented, and thus the negative active material layer is formed as an orientation layer.

[0066] The strength of the magnetic field generated by the magnet may be 1000 Gauss to 10000 Gauss, for example, 4000 Gauss to 8000 Gauss, or 5000 Gauss to 7000 Gauss. In addition, the negative electrode active material composition may be maintained for 3 to 15 seconds after being applied to the current collector, that is, exposed to the magnetic field for 3 to 15 seconds. In one embodiment, the magnetic field exposure time may be 3 to 12 seconds. The DD value obtained may be changed depending on the magnetic field exposure time.

[0067] The DD value can also be obtained by adjusting the viscosity of the negative electrode active material layer composition.

[0068] The viscosity of the negative electrode active material layer composition at room temperature (about 20° C. to about 25° C.) may be 2000 cps to 4000 cps, may be 2000 cps to 3500 cps, or may be 2500 cps to 3500 cps.

[0069] The viscosity of the negative electrode active material layer composition may be adjusted within a range. If the viscosity of the negative electrode active material layer composition is lower than the range, the degree of standing of the crystalline carbon-based negative electrode active material contained in the negative electrode active material layer is too high, which may cause poor contact of the negative electrode active material particles and increase the electron transfer resistance of the active material layer. If the viscosity is higher than the range, the orientation effect may be reduced, which may cause poor electrolyte impregnation.

[0070] The negative electrode active material layer composition can be prepared by mixing the negative electrode active material and the copolymer binder in a solvent. An aqueous binder can be further added to the negative electrode active material layer composition, or an aqueous binder and a conductive material can be further added.

[0071] The solvent may be water.

[0072] According to another embodiment, a lithium secondary battery includes a negative electrode, a positive electrode, and an electrolyte.

[0073] The positive electrode includes a current collector and a positive electrode active material layer formed on the current collector and including a positive electrode active material.

[0074] As the positive electrode active material, a compound capable of reversible intercalation and deintercalation of lithium (lithiated intercalation compound) can be used. Specifically, one or more of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used. More specifically, a compound represented by any one of the following chemical formulas can be used. Li a A 1-b X b D 1 2(0.90≦a≦1.8, 0≦b≦0.5);Li a A 1-b X b O 2-c1 D 1 c1 (0.90≦a≦1.8, 0≦b≦0.5, 0≦c1≦0.05);Li a E 1-b X b O2-c1 D 1 c1 (0.90≦a≦1.8、0≦b≦0.5、0≦c1≦0.05);Li a HAVE BEEN 2-b X b O 4-c1 D 1 c1 (0.90≦a≦1.8、0≦b≦0.5、0≦c1≦0.05);Li a Ni 1-b-c Co b X c D 1 α (0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α≦2);Li a Ni 1-b-c Co b X c O 2-α T α (0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α<2);Li a Ni 1-b-c Co b X c O 2-α T2(0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α<);Li a Ni 1-b-c Mr b X c D 1 α (0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α≦2);Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T2(0.90≦a≦1.8、0≦b≦0.5、0≦c≦0.5、0<α<2);Li a Ni b HAVE BEEN c G d O2(0.90≦a≦1.8、0≦b≦0.9、0≦c≦0.5、0.001≦d≦0.1);Lia Ni b Co c L 1 d G e O2(0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0≦e≦0.1);Li a NiG b O2(0.90≦a≦1.8, 0.001≦b≦0.1)Li a CoG b O2(0.90≦a≦1.8, 0.001≦b≦0.1);Li a Mn 1-b G b O(0.90≦a≦1.8, 0.001≦b≦0.1);Li a Mn2G b O4(0.90≦a≦1.8, 0.001≦b≦0.1);Li a Mn 1-g G g PO4(0.90≦a≦1.8, 0≦g≦0.5);QO2;QS2;LiQS2;V2O5;LiV2O5;LiZO2;LiNiVO4;Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) Fe2(PO4)3(0≦f≦2;Li a FePO4(0.90≦a≦1.8) In the chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; T is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; Z is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof; L 1 is Mn, Al or a combination thereof.

[0075] Of course, the compound may have a coating layer on its surface, or may be used in combination with a compound having a coating layer. The coating layer may contain at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds constituting the coating layer may be amorphous or crystalline. The coating elements contained in the coating layer may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating layer forming process may use any coating method as long as the compound can be coated with such elements by a method (e.g., spray coating, immersion method, etc.) that does not adversely affect the physical properties of the positive electrode active material, and this is well understood by those working in the field, so a detailed explanation will be omitted.

[0076] In the positive electrode, the content of the positive electrode active material may be 90 wt % to 98 wt % based on the total weight of the positive electrode active material layer.

[0077] In an embodiment, the positive electrode active material layer may further include a binder and a conductive material, each of which may be in a range of 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.

[0078] The binder serves to adhere the positive electrode active material particles to each other well and to the current collector well. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.

[0079] The conductive material is used to give the electrode electrical conductivity, and any material that does not undergo chemical change and is electronically conductive in the battery that is constructed can be used. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber; metal-based materials such as metal powders or metal fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures thereof.

[0080] The current collector may be, but is not limited to, aluminum foil, nickel foil, or a combination thereof.

[0081] The positive electrode active material layer is formed by mixing an active material, a binder, and an optional conductive material in a solvent to prepare an active material composition, and then coating the active material composition on a current collector. Since such a method for forming an active material layer is well known in the art, a detailed description thereof will be omitted in this specification. The solvent may be, but is not limited to, N-methylpyrrolidone, water, etc. In one embodiment, the solvent for the negative electrode active material layer composition may be water.

[0082] The electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0083] The non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can migrate.

[0084] As the non-aqueous organic solvent, a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent can be used.

[0085] Examples of the carbonate solvent include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropylene carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of the ester solvent include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanolide, mevalonolactone, and caprolactone. Examples of the ether solvent include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran. Examples of the ketone solvent include cyclohexanone. Examples of the alcohol solvent that can be used include ethyl alcohol and isopropyl alcohol. Examples of the aprotic solvent that can be used include nitriles such as R-CN (R is a hydrocarbon group having a linear, branched, or cyclic structure with 2 to 20 carbon atoms and can contain a double bond oriented ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane and 1,4-dioxolane, and sulfolanes.

[0086] The non-aqueous organic solvent may be used alone or in combination of two or more. When two or more organic solvents are used in combination, the mixing ratio may be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.

[0087] In addition, in the case of carbonate-based solvents, it is preferable to mix cyclic carbonate and chain carbonate. In this case, the cyclic carbonate and chain carbonate should be mixed in a volume ratio of 1:1 to 1:9, which is appropriate in terms of electrolyte performance.

[0088] When a mixture of non-aqueous organic solvents is used, a mixed solvent of a cyclic carbonate and a chain carbonate, a mixed solvent of a cyclic carbonate and a propionate-based solvent, or a mixed solvent of a cyclic carbonate, a chain carbonate, and a propionate-based solvent can be used. As the propionate-based solvent, methyl propionate, ethyl propionate, propyl propionate, or a combination thereof can be used.

[0089] In this case, when a cyclic carbonate and a chain carbonate or a cyclic carbonate and a propionate-based solvent are mixed and used, it is appropriate from the viewpoint of the performance of the electrolyte to mix them in a volume ratio of 1:1 to 1:9. In addition, when a cyclic carbonate, a chain carbonate and a propionate-based solvent are mixed and used, they can be mixed and used in a volume ratio of 1:1:1 to 3:3:4. Of course, the mixing ratio of the solvents can be appropriately adjusted according to the desired physical properties.

[0090] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent in addition to the carbonate-based solvent, and the carbonate-based solvent and the aromatic hydrocarbon-based organic solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0091] As the aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound represented by the following chemical formula 1 can be used. [ka] (In Chemical Formula 1, R1 to R6 are the same or different and are selected from the group consisting of hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group, and combinations thereof.)

[0092] Specific examples of aromatic hydrocarbon organic solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, It is selected from the group consisting of fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.

[0093] The electrolyte may further contain vinylene carbonate or an ethylene carbonate-based compound of the following formula 2 as a life-improving additive in order to improve the battery life. [ka] (In Chemical Formula 2, R7 and R8 are the same or different and are selected from the group consisting of hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, and at least one of R7 and R8 is selected from the group consisting of a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, with the proviso that R7 and R8 are not all hydrogen.)

[0094] Representative examples of ethylene carbonate-based compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, etc. When such life-improving additives are used, the amount used can be appropriately adjusted.

[0095] The electrolyte may further include vinyl ethylene carbonate, propane sultone, succinonitrile, or a combination thereof, in which case the amount used may be appropriately adjusted.

[0096] Lithium salts are substances that dissolve in organic solvents and act as a source of lithium ions in batteries, enabling basic lithium secondary battery operation and facilitating the movement of lithium ions between the positive and negative electrodes. Representative examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+1 SO2)(C y F 2y+1The electrolyte contains one or more selected from the group consisting of lithium difluoro(bisoxolato)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB) and lithium difluoro(oxalato)borate (LiDFOB) as a supporting electrolyte salt. The concentration of the lithium salt is preferably within a range of 0.1M to 2.0M. When the concentration of the lithium salt is within the range, the electrolyte has appropriate conductivity and viscosity, and therefore excellent electrolyte performance can be exhibited and lithium ions can be effectively transferred.

[0097] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multi-layer film of two or more layers of these may be used, and it is of course possible to use a mixed multi-layer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator.

[0098] An exploded perspective view of a lithium secondary battery according to an embodiment of the present invention is shown in Fig. 4. Although the lithium secondary battery according to the embodiment is described as being prismatic, the present invention is not limited thereto and may be applied to batteries of various shapes such as cylindrical and pouch types.

[0099] 4, a lithium secondary battery 100 according to an embodiment may include an electrode assembly 40 formed by winding a positive electrode 10 and a negative electrode 20 with a separator 30 interposed therebetween, and a case 50 in which the electrode assembly 40 is housed. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte (not shown).

[0100] Examples and comparative examples of the present invention are described below. However, the following examples are merely examples of the present invention and are not intended to limit the present invention.

[0101] Example 1 5 wt% Si-C composite, 91 wt% artificial graphite, 2 wt% acrylic acid-acrylonitrile copolymer binder, and 2 wt% styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry with a viscosity of 3000 cps (at 25°C). The viscosity was measured at 30 rpm and room temperature (25°C) using a Brookfield viscometer with an LV4 spindle.

[0102] The acrylic acid-acrylonitrile copolymer contained 44% by weight of acrylic acid and 56% by weight of acrylonitrile, and the viscosity of an aqueous solution of this copolymer with a solid content of 7% by weight in water (at 25°C) was 1200 mPa·s.

[0103] The Si-C composite had a silicon core and a soft carbon amorphous carbon layer on the core surface, with the silicon core content being 60% by weight and the soft carbon amorphous carbon content being 40% by weight, based on a 100% composite. The silicon core was a silicon nanoparticle with an average particle size (D50) of 20 nm, and the soft carbon amorphous carbon layer had an average thickness of 100 nm.

[0104] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector and exposed to a magnetic field for 8 seconds. The slurry was then pressurized and dried at a high temperature of 100° C. or higher, and rolled to form a negative electrode active material layer with a thickness of 80 μm, thereby producing a negative electrode.

[0105] 96 wt% of LiCoO2 positive active material, 2 wt% of carbon black conductive material, and 2 wt% of polyvinylidene fluoride binder were mixed in N-methylpyrrolidone solvent to prepare a positive active material slurry. The prepared slurry was applied to an Al current collector, dried, and rolled to prepare a positive electrode.

[0106] A lithium secondary battery (full cell) was manufactured using the negative electrode, positive electrode and electrolyte. The electrolyte was 1.5MLiPF6 dissolved in ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate (volume ratio 20:10:70).

[0107] Example 2 A negative electrode active material layer slurry having a viscosity of 3200 cps (at 25° C.) was produced in the same manner as in Example 1, except that 5% by weight of Si-C composite, 91% by weight of artificial graphite, 2% by weight of acrylic acid-acrylonitrile copolymer binder, and 2% by weight of styrene-butadiene rubber were mixed in a water solvent.

[0108] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 9 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0109] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0110] Example 3 The procedure of Example 1 was repeated, except that 5% by weight of Si-C composite, 91% by weight of artificial graphite, 2% by weight of acrylic acid-acrylonitrile copolymer, and 2% by weight of styrene-butadiene rubber were mixed in a water solvent, to produce a negative electrode active material layer slurry having a viscosity of 3400 cps (at 25° C.).

[0111] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 10 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0112] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0113] Example 4 The procedure of Example 1 was repeated, except that 5% by weight of Si-C composite, 91% by weight of artificial graphite, 2% by weight of acrylic acid-acrylonitrile copolymer, and 2% by weight of styrene-butadiene rubber were mixed in a water solvent, to produce a negative electrode active material layer slurry having a viscosity of 3,300 cps (at 25° C.).

[0114] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 11 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0115] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0116] Example 5 The procedure of Example 1 was repeated, except that 5% by weight of Si-C composite, 91% by weight of artificial graphite, 2% by weight of acrylic acid-acrylonitrile copolymer, and 2% by weight of styrene-butadiene rubber were mixed in a water solvent, to produce a negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.).

[0117] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 12 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0118] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0119] Example 6 The procedure of Example 1 was repeated, except that 5 wt % of the Si-C composite, 91.6 wt % of artificial graphite, 1.4 wt % of an acrylic acid-acrylonitrile copolymer, and 2.0 wt % of a styrene-butadiene rubber were mixed in a water solvent, to produce a negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.).

[0120] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 12 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0121] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0122] Comparative Example 1 The procedure of Example 1 was repeated, except that 5% by weight of Si-C composite, 91% by weight of artificial graphite, 2% by weight of acrylic acid-acrylonitrile copolymer, and 2% by weight of styrene-butadiene rubber were mixed in a water solvent, to produce a negative electrode active material layer slurry having a viscosity of 3000 cps (at 25° C.).

[0123] The negative electrode active material layer slurry was applied to a copper foil current collector and dried to form a negative electrode active material layer with a thickness of 80 μm, thereby producing a negative electrode.

[0124] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0125] Comparative Example 2 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.).

[0126] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 5 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0127] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0128] Comparative Example 3 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.).

[0129] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 8 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0130] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0131] Comparative Example 4 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3,300 cps (at 25° C.).

[0132] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 9 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0133] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0134] Comparative Example 5 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3250 cps (at 25° C.).

[0135] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 10 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0136] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0137] Comparative Example 6 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid binder, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3,300 cps (at 25° C.).

[0138] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 11 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0139] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0140] Comparative Example 7 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3250 cps (at 25° C.).

[0141] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 12 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0142] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0143] Comparative Example 8 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in an aqueous solvent to prepare a negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.).

[0144] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 5 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0145] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0146] Comparative Example 9 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3300 cps (at 25° C.).

[0147] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 8 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0148] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0149] Comparative Example 10 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3150 cps (at 25° C.).

[0150] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 9 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0151] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0152] Comparative Example 11 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3100 cps (at 25° C.).

[0153] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 10 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0154] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0155] Comparative Example 12 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3120 cps (at 25° C.).

[0156] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 11 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0157] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0158] Comparative Example 13 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative electrode active material layer slurry having a viscosity of 3050 cps (at 25° C.).

[0159] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 12 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0160] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0161] (Comparative Example 14) A negative electrode active material layer slurry having a viscosity of 3250 cps (at 25° C.) was prepared in the same manner as in Example 1, except that 5 wt % of Si-C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent.

[0162] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 5 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0163] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0164] (Reference example 1) A negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.) was prepared in the same manner as in Example 1, except that 5 wt % of Si-C composite, 92.3 wt % of artificial graphite, 0.7 wt % of acrylic acid-acrylonitrile copolymer, and 2.0 wt % of styrene-butadiene rubber were mixed in a water solvent.

[0165] A copper foil current collector was placed on top of a magnet with a magnetic field strength of 6000 Gauss, and the negative electrode active material layer slurry was applied while moving the copper foil current collector, exposed to a magnetic field for 12 seconds, and then dried to form a negative electrode active material layer with a thickness of 80 μm, thereby manufacturing a negative electrode.

[0166] A lithium secondary battery was produced in the same manner as in Example 1 using the negative electrode, the positive electrode and the electrolyte used in Example 1.

[0167] Experimental example 1) X-ray diffraction characteristic measurement The lithium secondary batteries manufactured in Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 were charged and discharged twice at 0.1C, and then fully discharged to 2.75V at 0.1C. The fully discharged batteries were disassembled to obtain a negative electrode. XRD was measured on the negative electrode using X'Pert (PANalytical) XRD equipment with CuKα radiation as the target radiation, and the monochromator equipment was removed to improve peak intensity resolution. The measurement conditions were 2θ=10° to 80°, scan speed (° / S)=0.06436, and step size was 0.026° / step.

[0168] The DD values ​​were calculated from the measured XRD results, and the results are shown in Table 1 below.

[0169] The DD value was calculated by measuring the integrated areas of the peaks appearing at 2θ = 26.5 ± 0.2° ((002) plane), 42.4 ± 0.2° ((100) plane), 43.4 ± 0.2° ((101)R plane), 44.6 ± 0.2° ((101)H plane), 54.7 ± 0.2° ((004 plane), and 77.5 ± 0.2° ((110) plane) in the measured XRD results, and summing the integrated areas of the peaks appearing at 2θ = 42.4 ± 0.2° ((100) plane), 43.4 ± 0.2° ((101)R plane), 44.6 ± 0.2° ((101)H plane), and 77.5 ± 0.2° ((110) plane). a The integrated areas of the peaks appearing at 2θ = 26.5 ± 0.2° ((002) plane), 42.4 ± 0.2° ((100) plane), 43.4 ± 0.2° ((101)R plane), 44.6 ± 0.2° ((101)H plane), 54.7 ± 0.2° ((004) plane), and 77.5 ± 0.2° ((110) plane) were added together to obtain I total From this value, DD(I total / I a ) values ​​were calculated.

[0170] The binders, slurry viscosities, and magnetic field application conditions in Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 are also shown in Table 1 below. In Table 1 below, P(AA-AN) is acrylic acid-acrylonitrile copolymer, SBR is styrene-butadiene rubber, PPA is acrylic acid, and CMS is carboxymethyl cellulose.

[0171] [Table 1]

[0172] Experimental example 2) Evaluation of negative electrode thickness The initial thicknesses of the negative electrodes produced in Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 were measured. In addition, the lithium secondary batteries produced in Examples 1 to 5 and Comparative Examples 1 to 14 were charged to SOC100 (fully charged, charged to a 100% charge capacity when the total battery charge capacity is taken as 100%), and then the negative electrodes were separated from the batteries to measure the thicknesses of the negative electrodes.

[0173] The negative electrode thickness expansion rate was calculated according to the following formula 2, and the results are shown in Table 2 below as a thickness increase rate.

[0174] Thickness expansion rate (%) = {(thickness after charging / discharging - initial thickness) / initial thickness}*100 (Equation 2)

[0175] [Table 2]

[0176] As shown in Table 2, when comparing the Examples and Comparative Examples having the same DD, it can be seen that the thickness increase rate of the Examples is low.

[0177] Also, it can be seen that in Examples 1 to 6 in which a P(AA-AN) copolymer binder is used and the DD value is 30 or more, the thickness increase rate is low.

[0178] On the other hand, in Comparative Example 1, where a P(AA-AN) copolymer binder was used but no magnetic field was applied, the thickness increase rate was high, while in Comparative Example 2, where a PAA binder was used but a magnetic field was applied, the thickness increase rate was high with a DD value of less than 30.

[0179] Even when the DD value was 30 or more, the thickness increase rate was somewhat high in Comparative Examples 3 and 4, in which the PAA binder was used.

[0180] At the same time, it can be seen that the thickness increase rate was high in Comparative Examples 8 and 14, in which the DD value was less than 30 even though the CMC binder or the P(AA-AN) binder was used.

[0181] At the same time, in the case of Reference Example 1, although the DD value was 51, the amount of P(AA-AN) binder used was too small at 0.7 wt%, resulting in low adhesive strength and detachment during charging and discharging, and the thickness increase rate could not be measured.

[0182] Experimental example 3) Evaluation of desorption state The lithium secondary batteries produced in Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 were subjected to a chemical charge / discharge once at 0.1 C, and then disassembled. Among the results, a photograph of the battery in Example 6 is shown in FIG. 5, and a photograph of the battery in Reference Example 1 is shown in FIG.

[0183] As shown in FIGS. 5 and 6, in the case of Example 6, the negative electrode active material layer was well attached to the current collector even after charging and discharging, whereas in the case of Reference Example 1, the negative electrode active material layer was almost entirely detached from the current collector.

[0184] The present invention is not limited to the embodiments, but may be manufactured in various different forms, and those skilled in the art to which the present invention pertains will understand that the present invention may be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the embodiment described above is illustrative in all respects and is not limiting. [Explanation of symbols]

[0185] 1 Base material 3 Negative electrode active material 3a Anode active material 10 positive electrode 20 negative electrode 30 Separator 40 Electrode assembly 50 cases 100 Lithium secondary battery U1 negative electrode active material layer

Claims

1. Current collector; a negative electrode active material layer located on the current collector, the negative electrode active material layer including a copolymer binder, a Si-C composite first negative electrode active material, and a crystalline carbon second negative electrode active material; The copolymer binder comprises a first repeat unit derived from a (meth)acrylic acid monomer and a second repeat unit derived from a (meth)acrylonitrile monomer, A negative electrode for a lithium secondary battery, having a degree of divergence (DD) value of 30 or more as defined by the following formula 1: DD (Degree of Divergence) = (I a / I total ) * 100 (Equation 1) (In the above formula 1, I a is the sum of peak intensity values ​​appearing at 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, and 77.5±0.2° when XRD measurement is performed using CuKα radiation, I total is the sum of the peak intensity values ​​appearing at 2θ = 26.5 ± 0.2°, 42.4 ± 0.2°, 43.4 ± 0.2°, 44.6 ± 0.2°, 54.7 ± 0.2°, and 77.5 ± 0.2° when XRD measurement is performed using CuKα radiation.

2. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the negative electrode has a DD value of 30 to 60.

3. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein a content of the first repeating unit derived from the (meth)acrylic acid monomer is 35% by weight to 65% by weight based on 100% by weight of the copolymer binder.

4. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein a content of the second repeating unit derived from the (meth)acrylonitrile monomer is 35 to 65% by weight, based on 100% by weight of the copolymer binder.

5. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the copolymer binder further comprises a third repeating unit derived from an additional monomer copolymerizable with the (meth)acrylic acid-based monomer and / or the (meth)acrylonitrile monomer.

6. 6. The negative electrode for a lithium secondary battery according to claim 5, wherein a content of the third repeat unit is more than 0 wt% and 20 wt% or less, based on 100 wt% of the copolymer binder.

7. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the copolymer binder is a copolymer of acrylic acid and acrylonitrile.

8. 2. The negative electrode of claim 1, wherein the content of the copolymer binder is 0.5 to 5 wt %, based on 100 wt % of the total weight of the negative electrode active material layer.

9. 2. The negative electrode of claim 1, wherein the Si content is 1 wt % to 20 wt % based on 100 wt % of the total weight of the first and second negative active materials.

10. 2. The negative electrode of claim 1, wherein the Si content is 3 wt % to 20 wt % based on 100 wt % of the total weight of the first and second negative active materials.

11. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein a mixing ratio of the first negative electrode active material and the second negative electrode active material is 3:97 to 10:90 by weight.

12. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the negative electrode active material layer has a thickness of 10 μm to 100 μm.

13. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the peak intensity value is a peak integrated area value.

14. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the copolymer binder has a viscosity of 500 mPa·s to 3000 mPa·s in an aqueous solution having a solid content of 7% by weight.

15. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the crystalline carbon is amorphous, plate-like, flake-like, spherical, or fibrous artificial graphite, natural graphite, or a combination thereof.

16. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the Si-C composite contains Si and a carbon-based material.

17. The negative electrode is manufactured by a process of placing a magnet under the current collector, coating a negative electrode active material layer composition including the first negative electrode active material and the second negative electrode active material, and drying the coating.

2. The negative electrode for a lithium secondary battery according to claim 1, wherein the strength of the magnetic field generated by the magnet is 1,000 Gauss to 10,000 Gauss.

18. 2. The negative electrode for a lithium secondary battery according to claim 1, wherein the viscosity of the negative electrode active material layer composition is 2000 cps to 4000 cps at room temperature (about 20° C. to about 25° C.).

19. The negative electrode according to any one of claims 1 to 18; a positive electrode comprising a positive electrode active material; and A lithium secondary battery comprising a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Negative electrode slurry, negative electrode, and secondary battery

    JP2022064465A

  • Building reinforcement method

    KR102390897B1