Electrode material with core-shell structure
The core-shell electrode material with a high glass transition temperature polymer electrolyte shell addresses the issues of low conductivity and safety in conventional polymer electrolytes by ensuring high ionic conductivity and structural integrity, enhancing safety and performance in lithium secondary batteries.
Patent Information
- Application Number
- JP2024065882
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-04-16
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional polymer electrolytes used in lithium secondary batteries suffer from low ionic conductivity, poor high-temperature stability, and limited safety due to deformation or evaporation of the electrolyte at high temperatures, exposing the active material and increasing the risk of combustion or explosion.
A core-shell electrode material is developed, where a polymer electrolyte with a high glass transition temperature forms a shell around an electrode active material core, ensuring high ionic conductivity and maintaining structural integrity at high temperatures, with a coverage rate of 85% or more.
The core-shell structure enhances safety by preventing electrolyte evaporation and active material exposure, maintaining structural integrity, and reducing heat generation, thereby improving the safety and performance of lithium secondary batteries.
Smart Images

Figure 2024163028000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode material having a core-shell structure. [Background technology]
[0002] In recent years, alkaline secondary batteries, including lithium secondary batteries, have been used for a variety of purposes, such as portable devices such as smartphones and mobile phones, hybrid vehicles, electric vehicles, and home electricity storage devices, and research and development into these batteries is being actively conducted.
[0003] There is a strong demand for improved safety in lithium secondary batteries, especially for use in electric vehicles. Conventional liquid batteries using electrolytes have been known to burn or explode because of the use of flammable electrolytes. In particular, the positive electrodes of lithium-ion batteries using transition elements can release oxygen when charged or at high temperatures of 200°C or higher. The released oxygen reacts with the electrolyte, etc., leading to unsafe conditions such as heat release, which can cause combustion or explosion. Therefore, the safety of the electrodes has become an issue.
[0004] As one of the means to solve the above problems, research on solid electrolytes that can contribute to improving safety has been active. Solid electrolytes are generally divided into oxide-based solid electrolytes, sulfide-based solid electrolytes, and polymer-based solid electrolytes. On the other hand, each solid electrolyte has its own problems. For example, polymer-based solid electrolytes have relatively low ionic conductivity at room temperature, oxide-based solid electrolytes have problems with productivity and formability, and sulfide-based solid electrolytes have problems such as the release of toxic gases such as hydrogen sulfide and the fact that they can only be used under constraints. Therefore, when a solid electrolyte is used for the entire battery, while there is an effect of improving safety, the characteristics of the battery may be deteriorated compared to a liquid battery. In response to the above problems, the safety of a liquid battery can be improved while suppressing the deterioration of battery characteristics by coating the electrode part of the liquid battery with a solid electrolyte. For example, Patent Documents 1 to 5 disclose a technology for coating the surface of an active material with a solid electrolyte. Among them, polymer-based solid electrolytes have the advantages of high plasticity and high formability, and compared to oxide-based solid electrolytes and sulfide-based solid electrolytes, they can be used to uniformly and completely cover electrodes, and are compatible with electrolytes. Therefore, polymer-based solid electrolytes are also being developed for use in electrolyte batteries as electrode covering materials.
[0005] On the other hand, conventional polymer-based solid electrolytes (hereafter referred to as polymer electrolytes) that do not contain electrolyte, such as polyethylene oxide (hereafter sometimes abbreviated as PEO), have a low glass transition temperature (Tg), and the electrode active material in particular may deform or the coating film may be destroyed at high temperatures of 200°C or more, at which an exothermic reaction occurs, limiting the safety of the electrode. In addition, polymer electrolytes that contain electrolyte, such as polyvinylidene fluoride (hereafter referred to as PVDF), generally contain a large amount of electrolyte, because their ionic conductivity deteriorates unless they contain a large amount of electrolyte. Therefore, when the electrode active material is heated to high temperatures of 200°C or more, at which an exothermic reaction occurs, a large amount of the electrolyte contained in the polymer electrolyte evaporates, leaving the parts where the electrolyte has evaporated hollow, exposing the electrode active material, and the effect of the coating in improving safety is limited. In recent years, among polymer electrolytes, polymer electrolytes using polyarylene sulfide (hereinafter abbreviated as PAS), represented by polyphenylene sulfide (hereinafter abbreviated as PPS), have been attracting attention due to their excellent high temperature resistance and flame retardancy. As in Patent Document 6, it is known that PPS is a conjugated polymer and can be made electronically conductive by adding an electron-accepting dopant, but in recent years, Patent Documents 7 to 9 have disclosed polymer electrolytes in which a mixture of PPS and an alkali metal salt is doped with an electron acceptor. Furthermore, in Patent Documents 7 to 9, the PPS polymer electrolyte is produced by a method in which each raw material, such as PPS, an alkali metal salt, and an electron-accepting dopant, is mixed at high temperature and then molded. In addition, Patent Document 10 discloses a PPS polymer electrolyte containing a meta-copolymerized PPS and an ionization assistant. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2000-323121 A [Patent Document 2] JP 2013-191391 A [Patent Document 3] International Publication No. 2022 / 244445 [Patent Document 4] International Publication No. 2014 / 038535 [Patent Document 5] Patent Publication No. 2021-197306 [Patent Document 6] Japanese Patent Publication No. 59-157151 [Patent Document 7] US Patent Application Publication No. 2018 / 006308 [Patent Document 8] China Patent Application Publication No. 106450424 [Patent Document 9] US Patent Application Publication No. 2017 / 0005356 [Patent Document 10] Patent Publication No. 2022-31092 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the polymer electrolyte coated on the electrode described in Patent Document 1 contains a large amount of organic electrolyte, which evaporates at high temperatures of 200°C or higher, and the evaporated parts become voids, exposing the active material, and the safety improvement effect is insufficient. In Patent Documents 2, 4, and 5, a low melting point material is used for the coating layer, which makes it difficult to maintain the shape of the coating layer at 200°C or higher, and the coating layer may deform at 200°C or higher, exposing the active material, and the safety improvement effect cannot be expected. In addition, Patent Document 3 uses an inorganic solid electrolyte as the coating layer, but since the moldability and plasticity of the inorganic solid electrolyte are low, there is room for improvement in the coverage rate, and the safety improvement effect is limited.
[0008] In addition, the PPS polymer electrolytes described in Patent Documents 6 to 9 have excellent high-temperature resistance, but because melt molding is required, it is difficult to mold them into a coating film, and it is difficult to create a coating layer with a high coverage rate. Furthermore, molding at a high temperature of 300° C. is required, and there is a problem that coating an active material with the PPS polymer electrolyte deteriorates the active material due to the high temperature. The polymer electrolyte having meta-copolymerized PPS described in Patent Document 10 has a reduced molding temperature due to the presence of meta-copolymerization, but still requires melt molding at 200° C. or higher, and deterioration of the active material in the process of coating the active material with the polymer electrolyte in a molten state is an issue.
[0009] In view of the above circumstances, an object of the present invention is to provide an electrode material that exhibits high ionic conductivity at room temperature, has high safety, and is inhibited from deteriorating the active material. [Means for solving the problem]
[0010] As a result of extensive research aimed at solving the above problems, the present inventors discovered that the problems could be solved as follows, and arrived at the present invention.
[0011] That is, in order to solve the above problems, the present invention comprises the following configuration. (1) An electrode having a core portion containing an electrode active material and a shell portion, the shell portion covering the core portion, the shell portion containing a polymer electrolyte as a main component, the polymer electrolyte containing a polymer as a main component, and an ionic conductivity of the polymer electrolyte at 25° C. of 10 -5 3. An electrode material, comprising: a viscosity modulus of 1 S / cm or more and 1 S / cm or less; and a glass transition temperature of the polymer is 40° C. or more. (2) The electrode material according to (1), wherein the polymer electrolyte further contains an alkali metal salt and an ionization assistant. (3) The electrode material according to (1) or (2), wherein the polymer is soluble in at least one organic solvent. (4) The polymer is a polyarylene sulfide copolymer in which the polyarylene sulfide has a structural unit represented by the formula -(Ar-S)-, The electrode material according to any one of (1) to (3), wherein Ar has a structural unit represented by (A) in chemical formula (1) and at least one structural unit selected from the group consisting of (B) to (G) in chemical formula (1).
[0012] [ka]
[0013] (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is an alkylene group, a substituent selected from O, CO, SO, and SO2, or a direct bond.) (5) The electrode material according to (4), wherein the polymer contains 30 mol % or more of monomer units selected from the group consisting of (B) to (G) in the chemical formula (1) based on 100 mol % of all monomer units. (6) A battery comprising the electrode material according to any one of (1) to (5). Effect of the Invention
[0014] According to the present invention, there is provided an electrode material which exhibits high ionic conductivity at room temperature, has high safety, and is inhibited from deteriorating in the active material. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view of a core-shell structure provided in an electrode material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] (core-shell structure) The electrode material of the present invention has a core portion containing an electrode active material and a shell portion, the shell portion covering the core portion, the shell portion having a polymer electrolyte as a main component, and the polymer electrolyte having a polymer as a main component. Here, a structure in which the core portion is substantially entirely covered by the shell portion is referred to as a core-shell structure. That is, the electrode material of the present invention has a core-shell structure. By providing the electrode material of the present invention with the core-shell structure, deterioration of the active material in the electrode material is suppressed, and the safety of the electrode material is also excellent.
[0017] Here, the shell portion substantially entirely covers the core portion means that the ratio of the surface of the core portion covered by the shell portion to the entire surface of the core portion (hereinafter, sometimes referred to as the coverage rate) is 85% or more. This coverage rate is preferably 90% or more, and more preferably 95% or more, because this further suppresses deterioration of the active material in the electrode material and improves the safety of the electrode material. Here, the details of the method for measuring the coverage rate of the core-shell structure are as described in the following section "Coverage rate" and the section on the measurement method in the examples.
[0018] 1 shows a schematic cross-sectional view of a core-shell structure included in an electrode material of one embodiment of the present invention. This core-shell structure 5 has a core portion 1 and a shell portion 2, and the shell portion 2 covers the core portion 1 almost entirely, and this core-shell structure 5 has a covering portion 3 and an exposed portion 4. This covering portion 3 is a part of the surface of the core portion 1 that is covered by the shell portion 2 and is not exposed. This exposed portion 4 is a part of the surface of the core portion 1 that is not covered by the shell portion 2 and is exposed.
[0019] (Coverage rate) The coverage of the surface of the core part by the shell part can be measured using a surface analysis method. For example, X-ray photoelectron spectroscopy (XPS), secondary ion mass spectrometry (TOF-SIMS), etc. can be mentioned. As a measurement method, one element X that is contained in the core part and not contained in the shell part is selected from the composition elements of the complex of the core part and the shell part (i.e., the core-shell structure). Furthermore, a surface analysis is performed using the above analysis method on the element X on the surface of the core-shell structure. The peak intensity of the obtained element X is set to P1. Similarly, a surface analysis is performed using the same method on the element X on the surface of a structure having only the core part. The peak intensity of the obtained element X is set to P0. The coverage A of the surface of the core part by the target shell part is calculated by Equation 1.
[0020]
number
[0021] In addition, when it is difficult to select one element X that is contained in the core part and not contained in the shell part from among the composition elements of the core-shell structure, or when the above surface analysis is difficult, SEM-EDS image analysis of the cross section of the electrode material may be used. First, a cross section of the electrode material containing multiple core-shell structures is extracted using an ion milling device (IM4000 manufactured by Hitachi). Furthermore, an SEM image of the cross section of the electrode material at a magnification of 2000 times is obtained using an electrode scanning electron microscope (SEM: SU8010 manufactured by Hitachi High-Tech, EDS detector: X-Max150 manufactured by Horiba Techno Service) equipped with an EDS detector. EDS measurement is performed in the same field of view as the obtained SEM image, and an image (hereinafter referred to as SEM-EDS image) in which elements derived from the shell part (e.g., sulfur element, etc.) and other elements are color-coded is obtained.
[0022] The obtained SEM-EDS images were processed using image processing software (e.g., Image-J) to detect elements (e.g., sulfur element, etc.) derived from the shell part above the core part. Ten or more independent core part cross sections were randomly selected from the detected images, and the maximum diameter R of each core part cross section was measured. i (For example, if 10 core cross sections are selected, R1 to R 10 ) and the coverage rate A of the shell part covering the above cross section i (For example, if 10 core cross sections are selected, A1 to A 10 ) is calculated from the image. Here, the coverage rate A i is the ratio of the length of the core covered by the shell to the total length of the core's circumference as viewed from the cross section. Finally, the coverage rate A of the core-shell structure is calculated using Equation 2.
[0023]
number
[0024] (Core) The core part of the electrode material of the present invention contains an electrode active material. Any conventionally known electrode active material can be used. Furthermore, any conventionally known positive electrode active material or negative electrode active material may be used.
[0025] (Cathode active material) For example, the positive electrode active material is LiFePO4, Li(Ni x Co y Al z )O2, LiMn2O4, LiCoO2, LiNiO2, Li(Ni x ,Co y ,Mn z )O2, Li2MnO3, Li2MnO3-LiMO2 (M=Co, Ni, etc.) solid solutions, and lithium-transition metal composite oxides such as those in which a part of these transition metals is replaced with other elements, lithium-transition metal phosphate compounds, and lithium-transition metal sulfate compounds may be used. In some cases, two or more kinds of positive electrode active materials may be used in combination. From the viewpoint of capacity and output characteristics, preferably, lithium-transition metal composite oxides are suitable as the positive electrode active material. Note that positive electrode active materials other than those mentioned above may also be used.
[0026] (Negative electrode active material) The negative electrode active material has a composition that can release lithium ions during discharge and absorb lithium ions during charging. The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium. Examples of the negative electrode active material include metals such as Si and Sn, metal oxides such as TiO, Ti2O3, TiO2, SiO2, SiO, and SnO2, Li 4 / 3 Ti 5 / 3Preferred examples include composite oxides of lithium and transition metals such as O4 or Li7MnN, Li-Pb alloys, Li-Al alloys, Li, and carbon materials such as natural graphite, artificial graphite, carbon black, activated carbon, carbon fiber, coke, soft carbon, and hard carbon. Among these, by using an element that alloys with lithium, it is possible to obtain a battery with a high capacity and excellent output characteristics having a high energy density compared to conventional carbon-based materials. The above-mentioned negative electrode active material may be used alone or in the form of a mixture of two or more kinds. The above-mentioned elements that alloy with lithium are not limited to the following, but specifically include Si, Ge, Sn, Pb, Al, In, Zn, H, Ca, Sr, Ba, Ru, Rh, Ir, Pd, Pt, Ag, Au, Cd, Hg, Ga, Tl, C, N, Sb, Bi, O, S, Se, Te, Cl, etc. It should be noted that negative electrode active materials other than those mentioned above may be used.
[0027] (Shell part) The shell part of the electrode material of the present invention is an ion-conductive structure that contains the above-mentioned polymer electrolyte as a main component and that substantially entirely covers the core part having the above-mentioned active material. Here, the main component means that the above-mentioned polymer electrolyte accounts for 50% or more of the mass of the entire shell part. The above-mentioned polymer electrolyte preferably further contains an alkali metal salt and an ionization assistant. By further containing the alkali metal salt and the ionization assistant, the ion conductivity of the electrode material of the present invention is improved.
[0028] The shell part may further contain a conductive assistant or additive in addition to the polymer electrolyte as the main component. The conductive assistant is a substance that promotes the electronic conduction of the electrode material, and a known one may be used. As long as the effect of the present invention is not impaired, the conductive assistant is not limited, but examples thereof include carbon black and carbon nanofiber. The additive may also contain a surfactant. Here, the surfactant refers to a molecule that has both a polar part and a non-polar part in the molecule, and the polar part acts with other polar substances and the non-polar part acts with other non-polar substances, thereby allowing the polar substance and the non-polar substance to be dispersed well. For example, carboxylates, phosphate esters, sulfonates, and sulfate esters of hydrocarbons and organic fluorine compounds are exemplified. When the shell part contains a surfactant, the dispersibility of the alkali metal salt described below is improved.
[0029] Furthermore, the shell part may be used in combination with an inorganic solid electrolyte. As long as the effect of the present invention is not impaired, the inorganic solid electrolyte is not limited, but examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.
[0030] (Polymer electrolyte) The polymer electrolyte is a substance that has a polymer matrix and easily migrates ions when an electric field is applied from the outside. The polymer electrolyte has a polymer as a main component, and the glass transition temperature of the polymer is 40° C. or higher. Here, the main component means that the polymer accounts for 50% or more of the mass of the solid polymer electrolyte and 35% or more of the mass of the entire polymer electrolyte. In addition, the polymer electrolyte preferably contains an alkali metal salt and an ionization assistant, which will be described later.
[0031] The polymer that is the main component of the polymer electrolyte has a glass transition temperature of 40° C. or higher, and from this viewpoint, polyamide 6, polyamide 66, polyethersulfone, polyphenylene oxide, polyamideimide, polyvinyl chloride, polyethylene terephthalate, polyarylene sulfide, etc. are suitable. Among them, polyarylene sulfide is preferable from the viewpoint of excellent ion conductivity. Details of this polyarylene sulfide will be described later.
[0032] The mobility of the alkali metal ions in the above polymer electrolyte can be determined by the ion diffusion coefficient at 25°C. The ion diffusion coefficient (m 2 / s) can be determined by measuring PFG-NMR (Pulsed Field Gradient Nuclear Magnetic Resonance Spectroscopy).
[0033] In addition, since the ion diffusion coefficient measured by PFG-NMR may take multiple values even under the same temperature conditions, the ion diffusion coefficient in the present invention refers to the maximum ion diffusion coefficient of the ion at 25°C. From the viewpoint of ion conductivity, the ion diffusion coefficient of the above polymer electrolyte at 25°C is 10 -13 m 2 / s or more is preferable, and 10 -12 m 2 / s or more is more preferable, and 10 -11 m 2 It is even more preferable that the ratio is 1 / s or more.
[0034] The polymer electrolyte of the present invention may further contain additives. For example, from the viewpoint of improving ion conductivity, inorganic oxide particles may be contained. As long as the effect of the present invention is not impaired, the additives are not limited, and examples thereof include Al2O3, CuO, Fe2O3, Fe3O4, SiO2, TiO2, Y2O3, and ZrO2. From the same viewpoint, cellulose, metal-organic frameworks (MOFs), and the like may further be contained.
[0035] (Ionic Conductivity) From the viewpoint of ionic conductivity as an electrolyte for battery applications and charge / discharge performance of a battery, the higher the ionic conductivity of the polymer electrolyte, the more preferable it is. In particular, when the polymer electrolyte is contained in a shell portion that covers a core portion having an electrode active material, the ionic conductivity of the polymer electrolyte directly affects the efficiency of release and absorption of alkali metal ions, and is therefore important in the present invention. From the above viewpoint, the ionic conductivity of the polymer electrolyte of the present invention at 25° C. is 10 -5 From the same viewpoint, 10 -4 S / cm or more is preferable, and 5×10 -4 It is more preferable that the conductivity of the polymer electrolyte is 1 S / cm or more. On the other hand, the conductivity of the polymer electrolyte is 1 S / cm or less.
[0036] Ion conductivity can be measured by the following method. A circular sample of 10 mm in diameter is taken from the polymer electrolyte and used as the measurement sample. The thickness of this sample is measured with a micrometer, and then the sample is placed on a sample holder. An AC voltage of 100 Hz to 100 MHz is applied using a high-frequency impedance measurement system (4990EDMS-120K, manufactured by Toyo Corporation) to measure the ion conductivity by the complex impedance method.
[0037] (glass transition temperature) As described above, the glass transition temperature (Tg) of the polymer contained as the main component in the polymer electrolyte is 40°C or higher. Here, the glass transition temperature (Tg) generally refers to the temperature at which a polymer transitions from a glassy state to a rubbery state. It is known that in a polymer electrolyte, the lower the glass transition temperature, the higher the ionic conductivity. On the other hand, Tg is a parameter indicating the ease of deformation of a polymer at high temperatures, and it is known that the higher the glass transition temperature, the lower the fluidity of the polymer at high temperatures and the less likely it is to deform. Conventional polyethylene oxide (PEO)-based polymer electrolytes have a Tg of -60°C or lower, and from the viewpoint of improving safety as a shell part, deformation at high temperatures occurs easily, and the active material is exposed at high temperatures, which may reduce the barrier properties between oxygen and the electrolyte and the active material. In response to the above problem, the present invention provides a highly safe electrode material by using a polymer having a high glass transition temperature and coating an electrode active material with a polymer electrolyte having high ionic conductivity.
[0038] Specifically, in the present invention, the shell part covers the core part almost entirely, and thus the effect of blocking the release of decomposition products of the core part is realized, and the effect of improving the safety of the battery is found. Furthermore, the shell part has a polymer electrolyte mainly composed of a polymer having a high glass transition temperature, and thus the thermal stability of the shell part at high temperatures is improved, deformation is less likely to occur, and the structure of covering the core part almost entirely even at high temperatures can be maintained. As a result, the effect of blocking the release of decomposition products of the core part at high temperatures is realized. The above-mentioned blocking effect makes it possible to suppress the progress of the reaction of the electrode active material of the core part at high temperatures, and furthermore, the effect of suppressing the reaction of the product with the electrolyte at high temperatures is found.
[0039] Although the specific mechanism is not clear, it is presumed to be as follows. For example, when LiCoO2 is used as the core part, it is known that oxygen is released from a state of 200°C or higher, and the crystal lattice of LiCoO2 changes, and Co3O4 is generated. The released oxygen may further react with the electrolyte, leading to heat generation and ignition. In the electrode material of the present invention, the core part is almost entirely covered with the shell part, which has the effect of suppressing the release of oxygen and reducing the amount of heat generation. This effect makes the electrode material of the present invention excellent in safety. On the other hand, polymers that are the main components of conventional polymer electrolytes, such as polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), and poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), which have low glass transition temperatures, are easily deformed at high temperatures and cannot maintain the shell structure at high temperatures, and the release of oxygen from the core part cannot be sufficiently suppressed. As a result, the released oxygen may further react with the electrolyte, leading to heat generation, etc.
[0040] In addition, it is known that LiCoO2, which is given as an example, undergoes an oxygen release reaction under high temperature conditions, and undergoes a structural change from LiCoO2, which has a rock-salt structure, to Co3O4, which has a spinel structure. The core part is covered almost entirely by the shell part, and the almost entirely covered state can be maintained even under high temperature conditions, which has the effect of suppressing the above structural change. As a result, the effect of suppressing the amount of heat generated by the electrode material under high temperatures is exerted, and the safety of the electrode material is improved.
[0041] From the above viewpoints, the glass transition temperature of the polymer contained as the main component in the polymer electrolyte is 40° C. or higher, and preferably 50° C. or higher.
[0042] The glass transition temperature of the polymer contained as the main component in the polymer electrolyte can be measured by differential scanning calorimetry (DSC). Specifically, the polymer is first held in a nitrogen atmosphere at a temperature about 50°C lower than the transition temperature until the apparatus stabilizes, and then the temperature is raised at a heating rate of 20°C / min to a temperature about 30°C higher than the end of the transition, and a DSC curve with a stepwise change near the glass transition temperature is drawn. In addition, baselines are drawn in the temperature range before and after the occurrence of the glass transition. The glass transition temperature (Tg) is the temperature at the point where a line equidistant in the vertical direction from the extended straight lines of each baseline intersects with the curve of the stepwise change portion of the glass transition.
[0043] (alkali metal salts) From the viewpoint of ionic conductivity, the polymer electrolyte preferably contains an alkali metal salt. The alkali metal salt refers to a salt containing an alkali metal ion and an anion as constituent ions.
[0044] Examples of the alkali metal salt include metal salts containing alkali metal ions such as lithium metal ions, sodium metal ions, and potassium metal ions. In general, metal ions with small ion diameters are preferred from the viewpoint of ion diffusibility. In addition, from the viewpoint of compatibility with the electrode active material, when the electrode active material has an alkali metal ion, an alkali metal salt having the same type of alkali metal ion as the electrode active material is preferred.
[0045] The anion is preferably a soft base based on the HSAB rule because of its high dissociation property into ions, and is preferably a bis(trifluoromethanesulfonyl)imide anion or a bis(fluorosulfonyl)imide anion. That is, the alkali metal salt preferably contains at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethane)sulfonimide.
[0046] The HSAB rule (Principle of Hard and Soft Acids and Bases) is a classification of acids and bases proposed by R.G. Pearson in terms of their strength. Hard acids have a high affinity for hard bases, and soft acids have a high affinity for soft bases. A hard acid is an acid whose electron acceptor atom is small, has no valence electrons in an orbit that can be easily deformed, and has a large positive charge. A soft acid is an acid whose electron acceptor atom is large, has valence electrons in an orbit that can be easily deformed, and has no or only a small charge. A hard base is a base whose valence electrons are strongly bonded to the atom, and a soft base is a base whose valence electrons are easily polarized. The HSAB rule and the classification of acids and bases according to the HSAB rule are described in Chapter 9, Section 15 on Acids and Bases in "Inorganic Chemistry - A Guide to Advanced Study" by R.B. Heslop and K. Jones.
[0047] Specifically, the alkali metal salt preferably contains lithium salts and sodium salts, and more preferably contains one or more selected from lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalate)borate (LiBOB), sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium bis(fluorosulfonyl)imide (NaFSI), and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI). From the viewpoint of high ion dissociability, it is even more preferable to contain LiTFSI and one or more obtained from LiFSI.
[0048] In addition, the alkali metal salt may be used by mixing a plurality of types of salts in an appropriate ratio. From the viewpoint of mechanical properties and thermal stability of the polymer electrolyte, the mass of the alkali metal salt is preferably 50% or less, more preferably 40% or less, of the total mass of the polymer electrolyte.
[0049] From the viewpoint of ion conductivity, the mass of the alkali metal salt is preferably 1% or more, and more preferably 5% or more, based on the mass of the entire polymer electrolyte.
[0050] (Ionization agent) The polymer electrolyte preferably contains an ionization assistant. The ionization assistant contained in the polymer electrolyte more preferably contains a solvent. From the viewpoint of dissociation of the alkali metal salt and ionic conductivity, the solvent is preferably as follows. That is, the solvent preferably has an ionic dissociation degree (1-ξ) at 25°C obtained by formula 3 of 0.1 or more, and a solvent diffusion coefficient (Dsolvent) obtained by formula 4 of 15 or less.
[0051]
number
[0052]
number
[0053] The degree of ionic dissociation (1-ξ) obtained from formula 3 may vary depending on the ionization assistant, temperature, ion concentration, and ion type. Here, the degree of ionic dissociation is calculated for a temperature of 25°C, an ion concentration of 0.2 mol / L, a cation of lithium ion, and an anion of N(SO2CF3)2 - This refers to the degree of ionic dissociation when
[0054] The notations in Equation 3 and Equation 4 represent the following values. σ imp : ionic conductivity, e0: electron charge, N: Avogadro constant, k: Boltzmann constant, T: temperature, D Lithium: Diffusion coefficient of lithium ions, D Anion :N(SO2CF3)2 - Diffusion coefficient of , (1-ξ): degree of ion dissociation, D solvent : Solvent diffusion coefficient, c: Boundary condition constant, η: Viscosity, r a : Spread radius.
[0055] The ionization assistant described above can bond with lithium ions at the interface or amorphous portion of the polymer electrolyte to form a third phase having better ion conductivity than the polymer matrix. The third phase forms an ion conduction path, thereby improving the ion conductivity of the polymer electrolyte.
[0056] The degree of ionic dissociation (1-ξ) obtained from formula 3 indicates the rate of ionic dissociation. From the viewpoint of promoting dissociation of the alkali metal salt, the degree of ionic dissociation (1-ξ) of the above solvent obtained from formula 4 is preferably 0.1 or more.
[0057] In addition, the solvent diffusion coefficient (Dsolvent) obtained by formula 4 indicates the viscosity of the solvent, and the lower this value, the higher the conductivity of the alkali metal ion tends to be. From the above viewpoint, the solvent diffusion coefficient (Dsolvent) obtained by formula 4 of the above solvent is preferably 15 or less.
[0058] From the above viewpoint, it is preferable that the ionization assistant contains one or more solvents in which the degree of ion dissociation (1-ξ) obtained by the formula 3 is 0.1 or more and the solvent diffusion coefficient (Dsolvent) obtained by the formula 4 is 15 or less.
[0059] From the same viewpoint, the ionization assistant may contain one or more selected from the group consisting of water, gamma-butyrolactone (GBL), N-methylpyrrolidone (NMP), butylene carbonate (BC), ethylene carbonate (EC), propylene carbonate (PC), methyl-gamma-butyrolactone (GVL), triglyme (TG), diglyme (DG), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Among them, from the viewpoint of the potential window of the electrolyte, it is more preferable that the ionization assistant contains at least one of gamma-butyrolactone (GBL) and N-methylpyrrolidone (NMP), and from the viewpoint of affinity with the above-mentioned polymer, it is most preferable that the ionization assistant contains gamma-butyrolactone (GBL).
[0060] From the viewpoint of safety, the mass of the ionization assistant is preferably 65% or less, and more preferably 50% or less, of the mass of the polymer electrolyte.
[0061] (electrolyte) The electrolyte used in the present invention is composed of an ionization assistant and an alkali metal salt, and is not particularly limited, and the ionization assistant and the alkali metal salt used in conventional lithium ion batteries can be used. As the ionization assistant contained in the electrolyte, a compound similar to the ionization assistant used in the polymer electrolyte is exemplified as a preferred example. The ionization assistant may be used by mixing a plurality of types in any ratio.
[0062] The alkali metal salt contained in the electrolytic solution is preferably a compound similar to the alkali metal salt used in the polymer electrolyte. The alkali metal salt contained in the electrolytic solution more preferably contains at least one of lithium tetrafluoroborate and lithium hexafluorophosphate. The alkali metal salt may be a mixture of a plurality of types in any ratio.
[0063] (Method of forming a core-shell structure) In the present invention, it is important that the shell part covers the core part almost entirely from the viewpoint of suppressing the heat generation amount of the electrode material. Furthermore, the method for forming the core-shell structure is not particularly limited, and any known method may be used. For example, a solid-phase mixing method or a solution method may be used.
[0064] As the solid-phase mixing method, a method of physically mixing the core part and the shell part to obtain a core-shell structure can be mentioned, that is, for example, a method of mixing the material constituting the core part and the material constituting the shell part using a ball mill or an air flow dispersion mixer, so that the shell part covers the core part almost entirely, and obtaining a core-shell structure can be mentioned. On the other hand, from the viewpoint of the shell part covering the core part almost entirely, it is preferable to form the core-shell structure by a solution method. Although there is no limitation within a range that does not impair the effects of the present invention, as an example of the solution method, first, a polymer and an alkali metal salt are dissolved in a solvent. Furthermore, an electrode active material is added little by little while stirring to the solution of the polymer and the alkali metal salt to obtain a suspension. Then, the suspension is heated and the solvent is volatilized in a vacuum environment to obtain a core-shell structure. Here, in order for the shell part to cover the core part almost entirely, it is preferable that the electrolyte polymer that is the main component of the shell part is soluble in the solvent.
[0065] In the solution method, it is possible to control the coverage of the core part by the shell part. For example, by increasing the concentration and viscosity of the solution, it is possible to increase the coverage of the core part by the shell part. Specific examples of the solution method include the sol-gel method and the spray coating method.
[0066] (Organic solvent) Although the details will be described later, it is preferable that the polymer contained as a main component in the polymer electrolyte is soluble in at least one kind of organic solvent. The organic solvent is generally a solvent used to dissolve a polymer. Although there is no limitation as long as the effect of the present invention is not impaired, from the viewpoint of productivity and storage, it is preferable that the organic solvent is liquid at room temperature and normal pressure. From the above viewpoint, it is preferable that the melting point of the organic solvent is 10°C or less and the boiling point is 50°C or more. In addition, in order to dissolve the polymer, it may be necessary to heat the organic solvent, and from this viewpoint, the boiling point of the organic solvent is preferably 100°C or more, and more preferably 150°C or more. From the viewpoint of dissolving the polymer, it is preferable that the organic solvent has a high polarity. In addition, from the viewpoint of forming the core-shell structure, a solvent having high volatility at a temperature above the boiling point is preferable. Known examples include acetonitrile, acetone, carbon tetrachloride, chloroform, cyclohexane, ethylene dichloride, toluene, N-methylpyrrolidone (NMP), etc. From the viewpoint of high boiling point, toluene and NMP are preferable.
[0067] (Polymer Solvent Solubility) In the present invention, the polymer contained as a main component in the polymer electrolyte is preferably soluble in at least one organic solvent. The polymer is soluble in at least one organic solvent, so that the shell part can be covered with the core part almost entirely to obtain a core-shell structure. In addition to the above, the organic solvent is preferably one that is easily volatilized, and the organic solvent preferably has a saturation solubility of 5% or more at a temperature lower than the boiling point of the organic solvent at normal pressure or 150°C, more preferably 10% or more. The above solubility means that the saturation solubility is 5% or more at a temperature lower than the boiling point of the solvent at normal pressure or 150°C.
[0068] (Polyarylene sulfide) As described above, the polymer contained as the main component of the polymer electrolyte is preferably polyarylene sulfide (hereinafter, sometimes referred to as PAS). PAS (arylene group is abbreviated as "Ar") is a polymer having a structural unit of the formula -(Ar-S)-. In addition, Ar in the structural unit -(Ar-S)- has a structural unit (A) in chemical formula (1) and at least one structural unit selected from the group consisting of (B) to (G) in chemical formula (1). From the viewpoint of controlling the melting point and molecular weight, it is particularly preferable that Ar has a structural unit (B) in chemical formula (1) or a structural unit (C) in chemical formula (1).
[0069] [ka]
[0070] (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is an alkylene group, a substituent selected from O, CO, SO, and SO2, or a direct bond.) In addition, in the PAS having the above formula -(Ar-S)- as a structural unit, it is preferable that the monomer unit selected from the group consisting of (B) to (G) in the above chemical formula (1) is contained at 30 mol % or more in 100 mol % of all monomer units. On the other hand, as an upper limit, in the PAS having the above formula -(Ar-S)- as a structural unit, it is preferable that the monomer unit selected from the group consisting of (B) to (G) in the above chemical formula (1) is contained at 70 mol % or less in 100 mol % of all monomer units. It is more preferable that the content of the above monomer unit is 35 mol % or more and 50 mol % or less. When the content of the above monomer unit is 30 mol % or more, the flexibility of the main chain is increased, the solvent solubility of the PAS is greatly increased, and the formation of a core-shell structure that is covered almost entirely becomes easy. On the other hand, when the content of the above monomer unit is 70 mol % or less, when the PAS copolymer is recovered from the reaction solution after the polymerization reaction of the PAS copolymer is completed, the recovery tends to be performed efficiently. The content ratio of the copolymerization units in the PAS copolymer is the same as the ratio of the amounts of the compounds (B') to (G') added as copolymerization components to the total amount of the dihalogenated aromatic compounds represented by the formulas (A') to (G') added during polymerization.
[0071] As long as the unit represented by -(Ar-S)- is the main structural unit, it may contain branch units or crosslinking units represented by the following formulae (H) to (J). The copolymerization amount of these branch units or crosslinking units is preferably in the range of 0 to 1 mol % per 1 mol of the structural unit represented by -(Ar-S)-.
[0072] [ka]
[0073] The PAS copolymer in the present invention may be any one of a random copolymer, a block copolymer, and a mixture thereof.
[0074] The method for synthesizing the PAS copolymer for polymer electrolytes of the present invention is not particularly limited, and examples thereof include a method in which a sulfidizing agent is reacted with a dihalogenated aromatic compound in an organic polar solvent, and a method in which a diiodo aromatic compound is melt-reacted with sulfur in the absence of a solvent. From the viewpoint of versatility, however, it is preferable to adopt the former polymerization method, which is industrially produced.
[0075] (Crystallization degree) Here, the crystallinity of the polymer electrolyte refers to the crystallinity in a state in which no ionization aid is contained. From the viewpoints of melting point, processability, and impregnation of the ionization aid, the polymer electrolyte of the present invention preferably has a crystallinity of 10% or less, and more preferably is completely amorphous, i.e., has a crystallinity of 0%.
[0076] The degree of crystallinity generally refers to the proportion of crystalline regions in the entire polymer, but here, the value obtained by dividing the heat of crystalline fusion of the polymer electrolyte before impregnation with the ionization assistant by the heat of fusion of perfectly crystalline paraphenylene sulfide (146.2 J / g) is regarded as the degree of crystallinity of the polymer.
[0077] It is known from Patent Document 6 and the like that a high degree of crystallinity of a polymer electrolyte is important for ionic conductivity, but by lowering the degree of crystallinity, the melting point of the polymer tends to be lower, the affinity with the ionization assistant increases, and ionic conduction paths are easily formed, so that high ionic conductivity can be achieved even with a low degree of crystallinity. In addition, when the degree of crystallinity is low, it becomes possible to dissolve in a solvent, and it becomes possible to form a core-shell structure that covers almost the entire surface.
[0078] (electrode) The electrode refers to a positive electrode or a negative electrode. The positive electrode or the negative electrode generally has an electrode material and a current collector foil. From the viewpoint of safety, at least one of the positive electrode or the negative electrode may contain an electrode material having a core-shell structure of the present invention, and both the positive electrode and the negative electrode may have a core-shell structure. The current collector foil may be selected according to the positive electrode active material and the negative electrode active material by a known method, for example, aluminum foil, copper foil, etc. are exemplified.
[0079] The above-mentioned electrode is not limited as long as it does not impair the effects of the invention, and can be produced by a known method. For example, the above-mentioned electrode material having a core-shell structure, a binder, and a conductive assistant are mixed, applied to a current collector foil, and the resulting coating is dried to obtain an electrode.
[0080] (battery) The battery preferably includes an electrode having the electrode material of the present invention. A liquid battery using an electrolyte generally has a positive electrode, a negative electrode, and a separator, and the positive electrode, the negative electrode, and the separator are further impregnated with the electrolyte. The electrolyte is obtained by dissolving a supporting salt in an organic solvent. The organic solvent is not particularly limited as long as it is an organic solvent that is usually used in electrolytes of alkali metal secondary batteries, and for example, carbonates, halogenated hydrocarbons, ethers, ketones, nitriles, lactones, oxolane compounds, etc. can be used.
[0081] The above-mentioned supporting salt is not particularly limited in type, but is preferably at least one of inorganic salts selected from LiPF6, LiBF4, LiClO4, and LiAsF6, derivatives of the inorganic salts, organic salts selected from LiSO3CF3, LiC(SO3CF3)2, LiN(SO3CF3)2, LiN(SO2C2F5)2, and LiN(SO2CF3)(SO2C4F9), and derivatives of the organic salts.
[0082] The separator serves to electrically insulate the positive and negative electrodes and to retain the electrolyte, and may be, for example, a porous synthetic resin film, particularly a porous film of a polyolefin polymer (polyethylene, polypropylene).
[0083] The battery can be manufactured by any known method as long as the effect is not impaired. The above-mentioned known manufacturing method can also be used for batteries using an electrolyte or a solid electrolyte. For example, first, a positive electrode material, a separator, and a negative electrode material are punched out to the size of a coin cell, and are laminated in order. Then, the positive electrode material and the negative electrode material are placed in the exterior of the coin cell, and the electrolyte is added and the material is crimped to obtain a coin cell. As another method, the separator, the positive electrode material, and the negative electrode material are wound by a winding machine to obtain a wound body. Then, the obtained wound body is sealed with an exterior material, and an electrolyte is injected to obtain a battery. Alternatively, the solid electrolyte layer, the positive electrode material, and the negative electrode material are wound by a winding machine to obtain a wound body. Then, the obtained wound body is sealed with an exterior material to obtain a solid battery.
[0084] (Safety of electrode materials) The electrode material of the present invention has a core-shell structure in which the core part is covered almost entirely by the shell part, thereby improving safety. The improvement in safety here means that the electrode material has a core-shell structure, and thus the amount of self-heating at high temperatures of the electrode material of the present invention alone or a battery using the electrode material of the present invention is reduced. In addition, the core-shell structure in which the core part is covered almost entirely by the shell part can suppress contact between the electrode active material and the electrolyte, and can suppress the reaction between the electrode active material and the electrolyte. Furthermore, the core part is covered almost entirely by the shell part, which has the effect of suppressing mechanical deformation of the electrode active material contained in the core part or alleviating internal stress. From the above viewpoint, the electrode material of the present invention has a core-shell structure in which the core part is covered almost entirely by the shell part, thereby suppressing decomposition of the electrode active material itself at high temperatures. That is, in order to achieve this effect, it is important that the electrode material has a core-shell structure in which the core part is covered almost entirely by the shell part even at high temperatures, and the glass transition temperature of the polymer contained as a main component in the polymer electrolyte is 40° C. or higher, and the ionic conductivity of the polymer electrolyte is 10 -5 It is important that the resistance is between 1S / cm and 1S / cm. EXAMPLES
[0085] The present invention will be described below with reference to examples, but the present invention is not necessarily limited to these.
[0086] [Measurement and evaluation methods] (Measurement of glass transition temperature) The glass transition temperature of the polymer in the present invention was measured by differential scanning calorimetry (DSC). First, the polymer was pulverized in a cryomill so that the average particle size of the polymer was 0.5 mm or less. 2.5 mg of the polymer electrolyte was filled into an aluminum sample holder and placed on the sample stage. The polymer was held in a nitrogen atmosphere at a temperature about 50°C lower than the glass transition temperature until the device stabilized, and then heated at a heating rate of 20°C / min to a temperature about 30°C higher than the end of the transition, and a DSC curve with a stepwise change was drawn near the glass transition temperature. Furthermore, a baseline was drawn in each temperature range before and after the glass transition occurred. The glass transition temperature (Tg) was defined as the temperature at the point where a straight line equidistant in the vertical axis direction from the extended straight line of each baseline intersects with the curve of the stepwise change part of the glass transition.
[0087] (Measurement of crystallinity) The crystallinity of the polymer electrolyte referred to here refers to the crystallinity of a film that does not contain an ionization assistant. The crystallinity of the polymer electrolyte in the present invention was measured by a differential scanning calorimeter (DSC). First, the polymer electrolyte was pulverized in a cryomill so that the average particle size of the polymer electrolyte was 0.5 mm or less. 2.5 mg of the polymer electrolyte was filled into an aluminum sample holder and placed on the sample stage. The polymer electrolyte was heated from 25°C to 120°C at a rate of 10°C / min under a nitrogen atmosphere and held at 120°C for 2 hours. Thereafter, the temperature was raised to 400°C at a rate of 10°C / min, and the peak with the widest area among the obtained endothermic peaks was regarded as the melting peak, and the heat of fusion (J / g) calculated from the melting peak area was divided by 146.2 (J / g) to obtain the crystallinity (%).
[0088] (Measurement of ionic conductivity) The ionic conductivity in the present invention was measured by the following method. After measuring the thickness of the polymer electrolyte film, a sample was taken to have a diameter of 10 mm and an area (S) of 78.5 mm2.2 The polymer electrolyte film was placed in a sample holder with a diameter of 10 mm (KP-SolidCell manufactured by Hosen Co., Ltd.). Then, an AC voltage of 100 Hz to 100 MHz was applied using a high-frequency impedance measurement system (4990EDMS-120K manufactured by Toyo Corporation), and the impedance was measured by the complex impedance method. The resistance value (R) was calculated from the obtained impedance, and the ionic conductivity (σ) was calculated using the following formula 5 together with the measured thickness (D) and area (S).
[0089]
number
[0090] (Measurement of coverage) The coverage rate of the core-shell structure was measured by SEM-EDS image analysis of the cross section of the electrode material. First, a cross section of the electrode material including the core-shell structure was taken out using an ion milling device (HITACH IM4000). Furthermore, an SEM image of the electrode cross section magnified 2000 times was obtained using an electrode scanning electron microscope equipped with an EDS detector (scanning electron microscope: HITACH SU8010, EDS detector: HORIBA X-max). EDS measurement was performed in the same field of view as the obtained SEM image, and an image was obtained in which elements derived from the shell part (e.g., sulfur element, etc.) and other elements were color-coded (hereinafter referred to as SEM-EDS image).
[0091] The obtained SEM-EDS images were processed using image processing software (e.g., Image-J) to detect elements (e.g., sulfur element, etc.) derived from the shell part above the core part. Ten or more independent core part cross sections were randomly selected from the detected images, and the maximum diameter R of each core part cross section was measured. i (For example, if 10 core cross sections are selected, R1 to R 10 ) and the coverage rate A of the shell part covering the above cross section i (For example, if 10 core cross sections are selected, A1 to A 10 ) was calculated from the image. The coverage A of the core-shell structure was calculated using Equation 2.
[0092]
number
[0093] (Measurement of Solubility of Polymers in Organic Solvents) The solubility of the polymer in the organic solvent in the present invention was measured by the following method. The polymer was added so that the mass of NMP was 95 parts and the mass of the polymer was 5 parts per 100 parts of the total mass of NMP and the polymer at 25°C and normal pressure. The obtained mixture was thoroughly stirred, and it was visually confirmed whether the polymer was completely dissolved. If it was not completely dissolved, it was heated to the lower temperature of the boiling point of the organic solvent or 150°C in a sealed state. It was thoroughly stirred in the above state, and it was visually confirmed whether the polymer was completely dissolved. If it was completely dissolved, it was determined that the above polymer was soluble in NMP.
[0094] (Measurement of the safety of electrode materials) The measurement of the safety of the electrode material in the present invention was carried out by the following method. First, a coin cell was produced using an electrode material having a core-shell structure by the above-mentioned battery production method. In addition, for reference, a coin cell was produced using an electrode material having the same configuration as the above-mentioned electrode material except that it does not have a core-shell structure. Next, the obtained coin cell was initially charged and discharged, and then charged to a fully charged state. Furthermore, the fully charged coin cell was disassembled while maintaining an insulating state under a dew point of -40°C, and the calorific value of the electrode material was measured using a Calvet calorimeter (Calvet Calorimeter C80 manufactured by Setaram Instrumentation). The calorific value W1 (J / g) of the electrode material having the above-mentioned core-shell structure and the calorific value W2 (J / g) of the electrode material not having the core-shell structure were obtained. The safety W was calculated by Equation 6.
[0095]
number
[0096] The larger the value of safety W, the more excellent the safety of the electrode material.
[0097] (Polymer 1) A copolymer consisting of 65 mol % of paraphenylene sulfide structural units in which Ar is represented by (A) and 35 mol % of metaphenylene sulfide structural units in which Ar is represented by (C) and R1 and R2 are both hydrogen, relative to 100 mol % of all -(Ar-S)- repeating units.
[0098] (Polymer 2) A copolymer consisting of 90 mol % of paraphenylene sulfide structural units in which Ar is represented by (A) and 10 mol % of metaphenylene sulfide structural units in which Ar is represented by (C) and R1 and R2 are both hydrogen, relative to 100 mol % of all -(Ar-S)- repeating units.
[0099] (Polymer 3) A polymer composed of paraphenylene sulfide structural units in which Ar is represented by (A) relative to 100 mol % of all -(Ar-S)- repeating units (polyphenylene sulfide "TORELINA" (registered trademark) E2080 manufactured by Toray Industries, Inc.).
[0100] (Polymer 4) Polyvinylidene Fluoride (Polymer 5) Polyethylene glycol (molecular weight: 500000) (Alkali metal salt 1) Lithium bis(trifluoromethanesulfonyl)imide (Solvent 1) N-Methylpyrrolidone (Cathode active material 1) Li(Ni) 0.5 ,Co 0.2 ,Mn 0.3 )O2 (Cathode active material 2) LiCoO2 (Negative electrode active material 1) Artificial graphite (Ionization agent 1) Gamma-butyrolactone (electrolyte 1) LiPF6 (1mol / L), EC:DMC:EMC (3:3:4 volume ratio), VC (1wt%) (Conductive additive 1) Acetylene Black (Binder 1) Polyvinylidene Fluoride (Binder 2) Carboxymethylcellulose Example 1 The raw materials shown in Table 1, that is, polymer 1, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 2 relative to 1000 parts by mass of solvent 1, and completely dissolved while stirring at 140 ° C. and 400 rpm. Furthermore, positive electrode active material 1 was added to the obtained solution in the ratio shown in Table 2 relative to 1000 parts by mass of solvent 1 to obtain a mixed solution of positive electrode active material. The obtained mixed solution was stirred at 200 rpm and completely dried at 180 ° C. to obtain an electrode material having a core-shell structure. The obtained electrode material was pulverized to an average particle size of 200 micrometers or less to obtain a powder of an electrode material having a core-shell structure. The obtained electrode material powder was calculated by the above-mentioned method for measuring the coverage of the core-shell structure. The results are shown in Table 3.
[0101] Furthermore, as shown in Table 1, a conductive assistant and a binder were added to the powder of the electrode material at room temperature in the ratios shown in Table 2 per 1,000 parts by mass of the solvent 1, and dispersed in the solvent 1 to obtain an electrode material slurry. The obtained slurry was applied to an aluminum foil with an applicator, and vacuum dried at 180°C for 24 hours to obtain an electrode 1. Furthermore, the obtained electrode 1 was punched out to a size of 14 mmΦ, the mass was measured, and the mass of the contained polymer 1 was calculated. An ionization assistant 1 was added so that the mass ratio with the polymer 1 was 100:97, and impregnation was performed at 80°C for 10 minutes.
[0102] Furthermore, a separator manufactured by Toray (F12CD1) was punched out to 19 mmΦ, and Li metal foil (manufactured by Honjo Metal) was punched out to 16 mmΦ. Electrode 1, separator, and Li metal foil were laminated in this order, placed in a coin cell case (20 mmΦ, 3.2 mm high coin cell type 2032), and 60 microliters of electrolyte 1 was added. Finally, the cell was crimped using a coin cell crimping machine manufactured by Hosen.
[0103] The obtained coin cell was placed in a charge / discharge device manufactured by Toyo System, and initially charged and discharged to a charge voltage of 4.2 V, a discharge voltage of 3.0 V, and a charge rate of 0.05 C, and then charged to a charge voltage of 4.3 V and a charge rate of 0.05 C. The charged coin cell was disassembled using a coin cell dismantling machine (manufactured by Hosen) while maintaining insulation, and the charging electrode 1 in a charged state was taken out.
[0104] The temperature of the charged electrode 1 was raised from 30° C. to 300° C. at a rate of 1 K / min using a Calbe calorimeter, and the amount of heat generated W1 was measured.
[0105] In addition, a comparative electrode 1 not having a core-shell structure was prepared by the method described in Reference Example 2-1 below, and the heat generation amount W2 of the comparative charging electrode 1 was measured. Next, the safety W of the electrode 1 was calculated by the measurement method described in the section on the measurement of the safety of the electrode material above, and the results are shown in Table 3.
[0106] Furthermore, the room temperature ionic conductivity of electrolyte 1 contained in electrode 1 was measured by the method described in Reference Example 3-1 below. The results are shown in Table 3.
[0107] The glass transition temperature of Polymer 1 was measured by the above-mentioned method for measuring crystallinity. The solubility in Solvent 1 was measured by the above-mentioned method for measuring solubility in organic solvents. The measurement results are shown in Table 3.
[0108] (Examples 2 to 3, Comparative Examples 1 to 4) The polymer type, alkali metal salt type, electrode active material, conductive assistant, and polymer and alkali metal salt types were as shown in Table 1, and the mixing ratio of each raw material was as shown in Table 2. Except for this, samples were prepared in the same manner as in Example 1, and the measurement of the coverage and heat generation amount W1 was carried out. In addition, the comparative electrodes were used as shown in Table 1. Comparative electrodes 1 and 2 shown in Table 1 were prepared by the method described in Reference Example 2-1 or Reference Example 2-2 below, the heat generation amount W2 of these comparative charging electrodes was measured, and the safety W of each electrode was calculated by the measurement method described in the section on the measurement of the safety of the electrode material above. The polymer electrolytes contained in each electrode are as shown in Table 1. In addition, the ionic conductivity of these electrolytes was measured by the method described in any one of Reference Examples 3-1 to 3-5 below. Furthermore, the glass transition temperature and solvent solubility of the polymers shown in Table 1 were measured by the same method as in Example 1. The evaluation results are shown in Table 3.
[0109] In Example 2, the electrode material was prepared in the same manner as in Example 1, except that the positive electrode active material was changed to LiCoO2. 0.5 ,Co 0.2 ,Mn 0.3 Although the heat generation amount of LiCoO2 itself is high relative to that of LiCoO2, due to the core-shell structure, the heat generation amount of the charging electrode 2 was significantly lower than that of the comparative charging electrode 2, and the safety W value was increased to 23.5%, indicating that the electrode material of Example 2 had high safety.
[0110] In Example 3, electrode materials and the like were prepared in the same manner as in Example 1, except for the amount of polymer electrolyte. Due to the reduction in the amount of polymer electrolyte, the coverage rate was reduced compared to Example 1, but still maintained a coverage rate of 85% or more. Therefore, the heat generation amount of the charging electrode 3 was significantly lower than that of the comparative charging electrode 1, and the safety W value was large at 17.9%, and the electrode material of Example 3 demonstrated a relatively high safety.
[0111] The polymer that is the main component of the polymer electrolyte of the electrode material of Comparative Example 1 is a copolymer consisting of 90 mol% of paraphenylene sulfide constituent units in which Ar is represented by (A) and 10 mol% of metaphenylene sulfide constituent units in which Ar is represented by (C) and R1 and R2 are both hydrogen, relative to 100 mol% of all -(Ar-S)- repeating units, and is insoluble in a solvent. Therefore, the coverage is low at 30%, the core part is not covered by the shell part, and the electrode material of Comparative Example 1 does not have a core-shell structure. Therefore, in the electrode material of Comparative Example 1, the ratio of the exposed part of the active material is higher than that of the electrode material of the Example, the heat generation amount of the charging electrode 4 is not significantly different from that of the comparative charging electrode 1, and the value of safety W is small at 5.8%, which is inferior to the electrode material of the Example.
[0112] The polymer that is the main component of the polymer electrolyte of Comparative Example 2 is a polymer consisting of paraphenylene sulfide structural units in which Ar is represented by (A) relative to 100 mol% of all -(Ar-S)- repeating units, and is insoluble in a solvent. Therefore, the coverage is low at 10%, the core part is not covered by the shell part, and the electrode material of Comparative Example 2 does not have a core-shell structure. Therefore, in the electrode material of Comparative Example 2, the ratio of the exposed part of the active material is higher than that of the electrode material of the Example, the heat generation amount of the charging electrode 5 is not significantly different from that of the comparative charging electrode 1, and the value of safety W is small at 1.2%, which is inferior to the electrode material of the Example.
[0113] Comparative Example 3 uses a solvent-soluble polymer, and can form a core-shell structure with a high coverage at room temperature, but contains a large amount of ionization assistant and has a low glass transition temperature of -30 ° C., so the shell part deforms at high temperatures and the exposed core part increases. In other words, the coverage rate decreases at high temperatures, and the core-shell structure cannot be maintained. Therefore, the heat generation amount of the charging electrode 6 is almost the same as that of the comparative charging electrode 1, and the value of safety W is very small at 1.0%, indicating low safety.
[0114] Comparative Example 4 is a solvent-soluble core-shell structure having a high coverage at room temperature, but uses a polymer having a low glass transition temperature of -65°C, and the shell part deforms at high temperatures and the exposed core part increases. That is, the coverage rate decreases at high temperatures, and the core-shell structure cannot be maintained. Therefore, the heat generation amount of the charging electrode 7 is not significantly different from that of the comparative charging electrode 1, and the safety W value is small at 2.3%, indicating low safety.
[0115] Example 4 In Example 4, electrode materials, coin cells, etc. were produced using the materials shown in Table 1 and the mixing ratios shown in Table 2 in the same manner as in Example 1, except that copper foil was used instead of aluminum foil.
[0116] The obtained coin cell was placed in a charge / discharge device manufactured by Toyo System, and initially charged and discharged to a charge voltage of 0.05 V, a discharge voltage of 1.5 V, and a charge rate of 0.05 C, and then charged to a charge voltage of 0.05 V and a charge rate of 0.05 C. The charged coin cell was disassembled using a coin cell dismantling machine (manufactured by Hosen) while maintaining insulation, and the charging electrode 8 in a charged state was removed.
[0117] The temperature of the charging electrode 8 was raised from 30° C. to 300° C. at a rate of 1 K / min using a Calbe calorimeter, and the amount of heat generated W1 was measured.
[0118] In addition, a comparative electrode 3 was prepared by the method described in Reference Example 2-3 below, and the heat generation amount W2 of the comparative charging electrode 3 was measured. Next, the safety W of the electrode 8 was calculated by the measurement method described in the section on the measurement of the safety of the electrode material above, and the results are shown in Table 3.
[0119] The amount of heat generated by charging electrode 8 was lower than that of comparative electrode 3, and the value of safety W was large at 35.1%, indicating that the electrode material of Example 4 had high safety.
[0120] [Table 1]
[0121] [Table 2]
[0122] [Table 3]
[0123] (Polymer manufacturing method) [Reference example 1-1] An autoclave equipped with a stirrer was charged with 6.005 kg (25 mol) of sodium sulfide nonahydrate, 0.787 kg (9.6 mol) of sodium acetate, and 5 kg of NMP (N-methylpyrrolidone), and the temperature was gradually raised to 205°C while nitrogen was passed through, and 3.6 liters of water was distilled off. Next, the reaction vessel was cooled to 180°C, and then 3.712 kg (25.25 mol) of 1,4-dichlorobenzene and 2.4 kg of NMP were added, sealed under nitrogen, and heated to 270°C, and reacted at 270°C for 2.5 hours. Next, the mixture was poured into 10 kg of NMP heated to 100°C, and stirred for about 1 hour, and then filtered, and washed with hot water at 80°C for 30 minutes three times. This was filtered, added to 25 L of an aqueous solution containing 10.4 g of calcium acetate, and stirred at 192°C for about 1 hour in a sealed autoclave. Then, it was filtered, washed with ion-exchanged water at about 90°C until the pH of the filtrate reached 7, and then dried under reduced pressure at 80°C for 24 hours to obtain Polymer 3.
[0124] [Reference example 1-2] With reference to Reference Example 1-1, 3.341 kg (22.72 mol) of 1,4-dichlorobenzene and 0.371 kg (2.53 mol) of 1,3-dichlorobenzene were also added at the same time, to obtain Polymer 2.
[0125] [Reference example 1-3] With reference to Reference Example 1-1, 2.413 kg (16.41 mol) of 1,4-dichlorobenzene and 1.299 kg (8.84 mol) of 1,3-dichlorobenzene were also added at the same time, thereby obtaining Polymer 1.
[0126] (Manufacturing method of the comparative electrode and measuring method of heat generation) [Reference example 2-1] At room temperature, positive electrode active material 1, conductive assistant 1, and binder 1 were added to 1,000 parts by mass of solvent 1 in the ratios shown in Table 4, and dispersed in solvent 1 to obtain an electrode material slurry. The obtained slurry was applied to aluminum foil with an applicator and vacuum dried at 180°C for 24 hours to obtain comparative electrode 1. Furthermore, the obtained comparative electrode 1 was punched out to 14 mmΦ.
[0127] Furthermore, a separator manufactured by Toray (F12CD1) was punched out to 19 mm diameter, and a Li metal foil (manufactured by Honjo Metal) was punched out to 16 mm diameter as a negative electrode. Comparative electrode 1, separator, and Li metal foil were laminated in this order, placed in a coin cell case, and 60 microliters of electrolyte 1 was added. Finally, it was crimped using a coin cell crimping machine manufactured by Hosen.
[0128] The obtained coin cell was placed in a charge / discharge device manufactured by Toyo System, and initially charged and discharged to a charge voltage of 4.2 V, a discharge voltage of 3.0 V, and a charge rate of 0.05 C, and then charged to a charge voltage of 4.3 V and a charge rate of 0.05 C. The coin cell in the charged state was disassembled using a coin cell dismantling machine (manufactured by Hosen Co., Ltd.) while maintaining insulation, and a charging electrode 1 for comparison in the charged state was taken out.
[0129] The comparative charging electrode 1 was heated from 30° C. to 300° C. at a rate of 1 K / min using a Kalbe calorimeter, and the amount of heat generated W2 was measured.
[0130] [Reference example 2-2] With reference to Reference Example 2-1, a comparative charging electrode 2 was prepared by adding a positive electrode active material 2 as shown in Table 4, and the calorific value W2 was measured.
[0131] [Reference example 2-3] Comparative electrode 3 was produced in the same manner as in Reference Example 2-1, except that the materials and ratios shown in Table 4 were used and copper foil was used instead of aluminum foil. Comparative charging electrode 3 was obtained in the same manner, except that the charging voltage was changed to 0.05 V and the discharging voltage was changed to 1.5 V, and the heat generation amount W2 was measured.
[0132] [Table 4]
[0133] (Method for measuring ionic conductivity of electrolyte) [Reference example 3-1] Polymer 1, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and completely dissolved while stirring at 140°C and 400 rpm. The obtained solution was applied by spin coating at 400 rpm, and dried at 180°C for 24 hours to obtain a film with a thickness of 20 micrometers. Ionization assistant 1 was added to the obtained film in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and the film was placed in a container and impregnated at 80°C for 1 hour to obtain electrolyte 1. The ionic conductivity of electrolyte 1 was measured at 25°C.
[0134] [Reference example 3-2] With reference to Reference Example 3-1, polymer 2, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, as shown in Table 5, and completely dissolved while stirring at 140 ° C and 400 rpm. The obtained solution was applied by spin coating at 400 rpm, and dried at 180 ° C for 24 hours to obtain a film with a thickness of 20 micrometers. Ionization assistant 1 was added to the obtained film in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and the mixture was placed in a container and impregnated at 80 ° C for 1 hour to obtain electrolyte 2. The ionic conductivity of electrolyte 2 was measured at 25 ° C.
[0135] [Reference example 3-3] With reference to Reference Example 3-1, polymer 3, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, as shown in Table 5, and completely dissolved while stirring at 140 ° C. and 400 rpm. The obtained solution was applied by spin coating at 400 rpm, and dried at 180 ° C. for 24 hours to obtain a film with a thickness of 20 micrometers. Ionization assistant 1 was added to the obtained film in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and the film was placed in a container and impregnated at 80 ° C. for 1 hour to obtain electrolyte 3. The ionic conductivity of electrolyte 3 at 25 ° C. was measured.
[0136] [Reference example 3-4] With reference to Reference Example 3-1, polymer 4, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, as shown in Table 5, and completely dissolved while stirring at 140 ° C. and 400 rpm. The obtained solution was applied by spin coating at 400 rpm, and dried at 180 ° C. for 24 hours to obtain a film with a thickness of 20 micrometers. Ionization assistant 1 was added to the obtained film in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and the film was placed in a container and impregnated at 80 ° C. for 1 hour to obtain electrolyte 4. The ionic conductivity of electrolyte 4 at 25 ° C. was measured.
[0137] [Reference example 3-5] Referring to Reference Example 3-1, polymer 5, alkali metal salt 1, and solvent 1 were mixed in the ratio shown in Table 5 relative to 100 parts by mass of polymer 1, and completely dissolved while stirring at 140° C. and 400 rpm. The resulting solution was applied by spin coating at 400 rpm and dried at 180° C. for 24 hours to obtain a film of electrolyte 5 having a thickness of 20 micrometers. The ionic conductivity of electrolyte 5 at 25° C. was measured.
[0138] [Table 5] [Explanation of symbols]
[0139] 1: Core section 2: Shell part 3: Covering part 4:Exposed part 5: Core-shell complex
Claims
1. The core portion includes an electrode active material, and the shell portion includes an electrode active material. The shell portion covers the core portion, The shell portion has a polymer electrolyte as a main component, The ionic conductivity of the polymer electrolyte at 25° C. is 10 -5 S / cm or more and 1 S / cm or less, The electrode material, wherein the glass transition temperature of the polymer containing the polymer electrolyte as a main component is 40° C. or higher.
2. The electrode material according to claim 1 , wherein the polymer electrolyte further contains an alkali metal salt and an ionization assistant.
3. 3. The electrode material according to claim 1 or 2, wherein the polymer is soluble in at least one organic solvent.
4. The polymer is a polyarylene sulfide copolymer having a structural unit of the formula -(Ar-S)-, Ar has a constitutional unit represented by (A) in chemical formula (1) and at least one constitutional unit selected from the group consisting of (B) to (G) in chemical formula (1). The electrode material according to any one of claims 1 to 3. 【Chemistry 1】 (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is an alkylene group, O, CO, SO, SO 2 or a direct bond.
5. 5. The electrode material according to claim 4, wherein the polymer contains 30 mol % or more of monomer units selected from the group consisting of (B) to (G) of the chemical formula (1) based on 100 mol % of all monomer units.
6. A battery comprising the electrode material according to any one of claims 1 to 5.
Citation Information
Patent Citations
Polymer composite solid electrolyte and preparation method and application thereof
CN106450424A
Electrically-conductive organic thermoplastic composition
JP1984157151A
Nonaqueous electrolyte secondary battery and its manufacture
JP2000323121A
Secondary battery
JP2013191391A
Electrode and method for manufacturing electrode, power storage element, capacitor, and battery