All-solid-state battery

The Li-Ga alloy in the negative electrode active material layer addresses the high resistance issue in all-solid-state batteries by maintaining interface stability, resulting in reduced cell impedance and interfacial resistance.

JP2024163440AInactive Publication Date: 2024-11-22TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023079035
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face issues with high resistance, particularly at the end of discharge, due to potential peeling at the interface between the negative electrode active material layer and the solid electrolyte layer.

Method used

The use of a Li-Ga alloy as the negative electrode active material in the all-solid-state battery, which maintains the interface integrity during lithium desorption, reducing resistance by forming a stable interface with the solid electrolyte.

Benefits of technology

The Li-Ga alloy-based battery exhibits significantly reduced resistance, with a decrease of up to 99.5% in cell impedance and 44% decrease in interfacial resistance, maintaining a stable interface and lowering overall cell resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163440000001_ABST
    Figure 2024163440000001_ABST
Patent Text Reader

Abstract

To provide an all-solid-state battery with reduced resistance.SOLUTION: An all-solid-state battery that utilizes a precipitation-dissolution reaction of metallic Li as an anode reaction includes a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, the negative electrode active material layer contains a Li-Ga alloy as an anode active material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to all-solid-state batteries. [Background technology]

[0002] An all-solid-state battery is a battery having a solid electrolyte layer between a positive electrode active material layer and a negative electrode active material layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries having an electrolyte solution containing a flammable organic solvent. In addition, among all-solid-state batteries, batteries that utilize the deposition and dissolution reaction of metallic lithium as a reaction at the negative electrode are known.

[0003] For example, Patent Document 1 discloses an all-solid-state battery that utilizes a deposition-dissolution reaction of metallic lithium as a negative electrode reaction, contains a β single-phase alloy of metallic lithium and metallic magnesium as a negative electrode active material, and when the all-solid-state battery is fully charged, the element ratio of lithium element in the alloy is 81.80 atomic % or more and 99.97 atomic % or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-184513 A Summary of the Invention [Problem to be solved by the invention]

[0005] In order to improve battery performance, it is preferable that the resistance of the battery is suppressed. The present disclosure has been made in view of the above-mentioned circumstances, and has a main object to provide an all-solid-state battery having suppressed resistance. [Means for solving the problem]

[0006] [1] An all-solid-state battery utilizing a precipitation-dissolution reaction of metallic Li as an anode reaction, the all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, the negative electrode active material layer containing a Li-Ga alloy as an anode active material. Effect of the Invention

[0007] The present disclosure has an effect of providing an all-solid-state battery with reduced resistance. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an all-solid-state battery according to the present disclosure. [Diagram 2] 1 shows the results of impedance measurement in an example and a comparative example. [Diagram 3] 1 is a graph showing the results of impedance measurement and charge / discharge curves in an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The all-solid-state battery according to the present disclosure will be described in detail below.

[0010] FIG. 1 is a schematic cross-sectional view illustrating an all-solid-state battery according to the present disclosure. The all-solid-state battery 10 shown in FIG. 1 is an all-solid-state battery that utilizes a deposition-dissolution reaction of metallic Li as an anode reaction. Such an all-solid-state battery has the advantage of having a high energy density. The all-solid-state battery 10 also has a positive electrode active material layer 1, a negative electrode active material layer 2, and a solid electrolyte layer 3 disposed between the positive electrode active material layer 1 and the negative electrode active material layer 2. The all-solid-state battery 10 also has a positive electrode current collector 4 that collects electrons from the positive electrode active material layer 1 and a negative electrode current collector 5 that collects electrons from the negative electrode active material layer 2. In particular, the all-solid-state battery 10 is characterized in that the negative electrode active material layer 2 contains a Li-Ga alloy as a negative electrode active material.

[0011] According to the present disclosure, in an all-solid-state battery utilizing the precipitation-dissolution reaction of metallic Li, since the negative electrode active material layer contains a Li-Ga alloy as the negative electrode active material, the all-solid-state battery has reduced resistance.

[0012] As in the above-mentioned Patent Document 1, in an all-solid-state battery utilizing the deposition-dissolution reaction of metallic lithium as the reaction of the negative electrode, it is known to use an alloy of metallic lithium and metallic magnesium (Li-Mg alloy) as the negative electrode active material. On the other hand, in the all-solid-state battery of the present disclosure, since a Li-Ga alloy is used, the resistance can be suppressed. Also, when the Li element is released from the Li-Mg alloy (Li disappears from the negative electrode) during the discharge of the battery, peeling may occur at the interface between the negative electrode active material layer and the solid electrolyte layer, and the resistance may increase. In particular, the resistance may increase at the end of the discharge of the battery. On the other hand, since Ga has a melting point (29.8°C) in the expected operating temperature range of the all-solid-state battery, it is considered that the above interface is maintained and the resistance at the end of the discharge is also good.

[0013] 1.Negative electrode active material layer The negative electrode active material layer in the present disclosure contains a Li—Ga alloy as the negative electrode active material.

[0014] The atomic ratio of Li element to Ga element in the Li-Ga alloy is not particularly limited. For example, in the charged state of the all-solid-state battery, the ratio of Li element in the Li-Ga alloy is, for example, 56 at% or more, and may be 60 at% or more. On the other hand, the ratio of Li element in the Li-Ga alloy is, for example, 99 at% or less, may be 90 at% or less, may be 80 at% or less, or may be 70 at% or less. In addition, in the discharged state, the ratio of Li element in the Li-Ga alloy is, for example, 45 at% or less, and may be 40 at% or less. On the other hand, the ratio of Li element in the Li-Ga alloy is, for example, 1 at% or more, may be 10 at% or more, may be 20 at% or more, or may be 30 at% or more. The charged state can be regarded as a state in which the all-solid-state battery is charged and reaches a predetermined SOC (State of charge). In addition, the discharged state can be regarded as a state in which the all-solid-state battery is discharged and reaches a predetermined SOC. The SOC can be set appropriately.

[0015] The negative electrode active material layer may contain a metal other than the Li-Ga alloy. For example, Ga metal may be used as a single substance. The negative electrode active material layer may or may not contain a binder. The binder may be a conventionally known material for batteries. For example, as shown in the examples described later, when Ga is deposited on the negative electrode current collector by vapor deposition, there is little need to use a binder in the negative electrode layer.

[0016] 2. Positive electrode active material layer The positive electrode active material layer in the present disclosure contains at least a positive electrode active material. The positive electrode active material may also contain at least one of a conductive assistant, a binder, and a solid electrolyte.

[0017] The positive electrode active material, conductive assistant, binder, and solid electrolyte may be any of materials conventionally known in the art for batteries.

[0018] 3.Solid electrolyte layer The solid electrolyte layer in the present disclosure is a layer disposed between the positive electrode active material layer and the negative electrode active material layer.

[0019] The solid electrolyte layer contains at least a solid electrolyte, and may contain a binder as necessary. The solid electrolyte and the binder are as described above. In particular, the solid electrolyte is preferably a sulfide solid electrolyte.

[0020] 4.All-solid-state battery The all-solid-state battery of the present disclosure generally includes a positive electrode current collector that collects electrons from the positive electrode active material layer and a negative electrode current collector that collects electrons from the negative electrode active material layer. The materials for the positive electrode current collector and the negative electrode current collector may be conventionally known materials for batteries.

[0021] The all-solid-state battery in the present disclosure can be manufactured, for example, by the following method. First, Ga metal is evaporated onto the negative electrode collector to prepare a negative electrode having a negative electrode collector and a Ga metal layer. Next, a positive electrode having a positive electrode collector and a positive electrode active material layer is manufactured. Then, a solid electrolyte layer is disposed between the positive electrode and the negative electrode to prepare a precursor battery having a negative electrode collector, a Ga metal layer, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode collector in this order. By initially charging this precursor battery, a negative electrode active material layer containing a Li-Ga alloy is obtained from the Ga metal layer. In this way, the above-mentioned all-solid-state battery can be manufactured. The conditions for the initial charge are not particularly limited.

[0022] Examples of applications of the all-solid-state battery in the present disclosure include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicle (BEVs), gasoline-powered automobiles, diesel-powered automobiles, etc. The all-solid-state battery in the present disclosure may also be used as a power source for moving objects other than vehicles (e.g., railways, ships, and aircraft), and may also be used as a power source for electrical products such as information processing devices.

[0023] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0024] [Example] <Preparation of positive electrode> The positive electrode active material, solid electrolyte, binder, and conductive additive were added to butyl butyrate and stirred to prepare a positive electrode slurry. The positive electrode active material was nickel cobalt lithium aluminum oxide (NCA)-based positive electrode active material, the solid electrolyte was a sulfide solid electrolyte (10LiI·15LiBr·75 (0.75Li2S·0.25P2S5)), the binder was polyvinylidene fluoride, and the conductive additive was acetylene black. The weight ratio of each material in the positive electrode slurry was 84.7:13.4:0.6:1.27 (positive electrode active material: solid electrolyte: binder: conductive additive). The obtained positive electrode slurry was applied to a positive electrode current collector (Al foil) with a coating gap of 225 μm. It was then pre-dried at 60°C and further dried at 165°C for 1 hour. As a result, a positive electrode having a positive electrode current collector and a positive electrode active material layer was obtained. 2 The capacity is 3.0mAh / cm 2 It was made so that

[0025] <Preparation of solid electrolyte layer> The sulfide solid electrolyte and the polyvinylidene fluoride were added to butyl butyrate and stirred to prepare a slurry for a solid electrolyte layer. The ratio of each material in the slurry was sulfide solid electrolyte:binder=92.6:7.4 by weight. The slurry was applied to a release film (Al foil) with a coating gap of 325 μm. Then, it was pre-dried at room temperature for 3 hours, and further dried at 165° C. for 1 hour. Then, two release films were punched out with a diameter of 14.5 mm, and the slurry-coated surfaces were overlapped and pressed at 7 t. After pressing, the release film was peeled off to prepare a self-supporting solid electrolyte layer (sulfide solid electrolyte layer).

[0026] <Preparation of evaluation cell> The positive electrode was punched out to a diameter of φ11.28 mm. A Ga-deposited foil prepared by evaporating Ga element on Ni foil was punched out to a diameter of φ14.5 mm. The thickness of the Ga layer on the Ni foil was 0.84 μm. The solid electrolyte layer was placed between the punched positive electrode and the Ga-deposited foil. Then, a positive electrode tab (Al) and a negative electrode tab (Ni) were attached to obtain a laminate. The obtained laminate was vacuum sealed using a laminate film. After that, the laminate was pressed at 392 MPa by cold isostatic pressing (CIP) to prepare an evaluation cell (an all-solid-state battery before the first charge: a precursor battery). The evaluation cell was restrained at 1 MPa by a constant pressure jig with a spring inserted so that the restraining pressure was constant.

[0027] [Comparative Example] An evaluation cell was prepared in the same manner as in the example, except that an Mg-deposited foil prepared by depositing Mg element on Ni foil was used instead of the Ga-deposited foil. The thickness of the Mg layer on the Ni foil was set to 1.0 μm.

[0028] [evaluation] The resistance of each evaluation cell was measured before the first charge and discharge by the AC impedance method. The cell 1s resistance and the interface resistance were measured. The measurement conditions were an amplitude of 10 mV, a frequency of 1 MHz to 10 mHz, and a temperature of 60°C or 25°C. The results are shown in Figure 2 and Table 1. Note that the interface resistance in the comparative example was too large to be measured.

[0029] After the impedance measurement, the temperature was set to 60°C, and the cutoff voltage was set to 4.2 V-3.0 V. The constant current (current density: 0.15 mA / cm 2 , equivalent to 0.05C) - Low voltage (cutoff current density: 0.03mA / cm 2 The initial charge and discharge was performed at a current of 100 V (equivalent to 0.01 C). After the initial charge and discharge, the battery was left to stand in an open circuit for 1 hour, and then the resistance (resistance after the initial charge and discharge) was measured using the AC impedance method. The measurement conditions were an amplitude of 10 mV, a frequency of 1 MHz-10 mHz, and 60°C. The cell impedance results are shown in Figure 3(a) and Table 2. The charge and discharge curves are shown in Figure 3(b).

[0030] [Table 1]

[0031] As shown in Table 1 and FIG. 2, in the examples, the cell impedance was reduced in all frequency ranges compared to the comparative examples. In particular, at 60°C, the cell impedance was reduced by about 99.5% compared to the comparative examples. This is believed to be because the contact area was increased by using Ga alone, a good negative electrode / solid electrolyte interface was formed, and the cell resistance was reduced. In addition, when the resistance was measured at 60°C, which is higher than the melting point of Ga (29.8°C), Ga was in a molten state, and the cell 1s resistance was reduced by about 73% compared to below the melting point (25°C), and the interface resistance in the high frequency range was reduced by about 62%. This suggests that at an operating temperature exceeding the melting point of Ga, molten Ga impregnated the negative electrode side solid electrolyte layer in the cell to form a Ga-solid electrolyte complex, which contributed to the generation of a good interface and the reduction of cell resistance.

[0032] [Table 2]

[0033] As shown in FIG. 3(a), in the comparative example (Mg), no tail due to diffusion was observed on the low frequency side, and the semicircle due to the interface resistance was observed halfway. On the other hand, in the example (Ga), a clear tail due to diffusion was observed after the semicircle due to the interface resistance (total of ~300Ω) on the low frequency side, and a significant decrease in the interface resistance in the cell was observed. This difference on the low frequency side suggests whether the interface in the cell, especially the interface between the negative electrode and solid electrolyte, is maintained well at the end of the discharge because the entire semicircle is visible. In addition, since the interface resistance in Mg cannot be determined, a comparison was made instead by comparing the cell impedance at 1 Hz, which includes the interface resistance in Ga, and a 44% decrease was observed in Ga compared to Mg (Table 1). This is presumably because the Li desorption reaction from the Li-Ga alloy at the end of the discharge produced a low-melting point alloy close to Ga alone, which maintained the interface between the negative electrode and solid electrolyte.

[0034] In this manner, it was confirmed that the resistance was suppressed in the all-solid-state battery according to the present disclosure.

[0035] The results of the charge and discharge curves will be considered. As shown in Fig. 3(b), the charge capacity was 213mAh / g for both the Example and the Comparative Example, and the discharge capacity was 179mAh / g for the Example and 186mAh / g for the Comparative Example, based on the positive electrode active material. Thus, the Example and the Comparative Example showed similar charge and discharge capacities.

[0036] In the examples, the cell voltage is lower than that of the comparative examples in the 3.2V-3.5V region at the beginning of charging, indicating that Li insertion and alloying into Ga occurs before the deposition of metallic Li occurs at a negative electrode potential of 0V vs Li. Also, in the examples, a drop in cell voltage was observed in the 3.2V-3.5V region even at the end of discharge. This is thought to be due to the disappearance of metallic Li followed by Li desorption from the Li-Ga alloy, resulting in partial reduction to an alloy composition close to Ga alone. It is also presumed that Li desorption from the Li-Ga alloy progresses more rapidly as it approaches the negative electrode / solid electrolyte interface in the negative electrode. [Explanation of symbols]

[0037] 1...Cathode active material layer 2 ...Negative active material layer 3 …Solid electrolyte layer 4 ...Positive electrode collector 5 ...Negative electrode current collector 10 …All-solid-state batteries

Claims

[Claim 1] An all-solid-state battery that utilizes a deposition-dissolution reaction of metallic Li as a negative electrode reaction, the all-solid-state battery has a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, The negative electrode active material layer contains a Li-Ga alloy as a negative electrode active material.

Citation Information

Patent Citations

  • All-solid battery and method for manufacturing the same

    JP2020184513A