All-solid-state secondary battery

By employing organic sulfur-based materials as negative electrodes in all-solid-state secondary batteries, the charge/discharge capacity and cycle characteristics are significantly enhanced, addressing the inferior performance issues of existing all-solid-state batteries.

JP2024163583AInactive Publication Date: 2024-11-22ADEKA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023079330
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

All-solid-state secondary batteries suffer from inferior charge/discharge characteristics, particularly cycle characteristics, despite their potential for high sulfur content to enhance capacity.

Method used

Utilizing an organic sulfur-based electrode active material as the negative electrode active material in an all-solid-state secondary battery, combined with specific solid electrolytes and electrode layers, to improve charge/discharge capacity and characteristics.

Benefits of technology

The use of organic sulfur-based materials as negative electrodes results in all-solid-state secondary batteries with large charge/discharge capacity and excellent cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163583000001
    Figure 2024163583000001
  • Figure 2024163583000002
    Figure 2024163583000002
  • Figure 2024163583000003
    Figure 2024163583000003
Patent Text Reader

Abstract

To provide an all-solid-state secondary battery having a large charging / discharging capacity and excellent charging / discharging characteristics such as cycle characteristics.SOLUTION: In an all-solid-state secondary battery having a positive electrode layer including a positive electrode active material, a negative electrode layer including a negative electrode active material, and a solid-state electrolyte layer between the positive electrode layer and the negative electrode layer, by using an organic sulfur-based electrode active material as the negative electrode active material, it is possible to provide an all-solid-state secondary battery in which a charging / discharging capacity is increased, charging / discharging cycle characteristics are improved, and the charging / discharging capacity is unlikely to decrease even when charging / discharging is repeated.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state secondary battery. [Background technology]

[0002] Currently, lithium ion secondary batteries, which are widely used as secondary batteries, use organic solvents as a solvent for the electrolyte, which is a medium for moving ions. For this reason, lithium ion secondary batteries have the risk of electrolyte leakage, and batteries with high safety are required. As one measure to improve the safety of secondary batteries, development of all-solid-state secondary batteries using solid electrolytes instead of liquid electrolytes as electrolytes is underway. However, all-solid-state secondary batteries are inferior in charge and discharge characteristics such as cycle characteristics compared to secondary batteries using liquid electrolytes, and are not yet satisfactory as secondary batteries.

[0003] Organic sulfur-based electrode active materials such as sulfur-modified polyacrylonitrile compounds have a large charge / discharge capacity and have been studied as positive electrode active materials (see, for example, Patent Documents 1-2) or negative electrode active materials (see, for example, Patent Documents 3-4) for lithium ion secondary batteries using liquid electrolytes. Organic sulfur-based electrode active materials have also been studied as positive electrode active materials (see, for example, Patent Documents 5-6) for all-solid-state secondary batteries, but have not been known as negative electrode active materials for all-solid-state secondary batteries.

[0004] The sulfur content of an organic sulfur-based electrode active material is preferably high from the standpoint of charge / discharge capacity (see, for example, Patent Document 2). However, when an organic sulfur-based electrode active material with a high sulfur content is used as a positive electrode active material, there is a problem that charge / discharge characteristics such as cycle characteristics are deteriorated. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2010 / 044437 [Patent Document 2] International Publication No. 2013 / 001693 [Patent Document 3] JP 2014-096326 A [Patent Document 4] International Publication No. 2019 / 225588 [Patent Document 5] International Publication No. 2015 / 030053 [Patent Document 5] International Publication No. 2021 / 075440 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide an all-solid-state secondary battery that has a large charge / discharge capacity and excellent charge / discharge characteristics such as cycle characteristics. [Means for solving the problem]

[0007] As a result of intensive research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using an organic sulfur-based electrode active material as the negative electrode active material of an all-solid-state secondary battery, and have completed the present invention. That is, the present invention is an all-solid-state secondary battery having a positive electrode layer containing a positive electrode active material, a negative electrode layer containing a negative electrode active material, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, in which the negative electrode active material is an organic sulfur-based electrode active material. Effect of the Invention

[0008] According to the present invention, by using an organic sulfur-based electrode active material as a negative electrode active material, it is possible to provide an all-solid-state secondary battery having a large charge / discharge capacity and excellent charge / discharge characteristics such as cycle characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [A. Solid electrolyte layer] The all-solid-state secondary battery of the present invention is an all-solid-state secondary battery containing a solid electrolyte selected from the group consisting of sulfide-based solid electrolytes, oxide-based solid electrolytes, polymer-based solid electrolytes, complex hydride-based solid electrolytes, phosphoric acid-based solid electrolytes, and organic molecular crystal-based solid electrolytes in the solid electrolyte layer. The solid electrolyte may be a crystalline material or a non-crystalline (amorphous) material. Since sulfide-based solid electrolytes are softer than oxide-based solid electrolytes and can reduce interface resistance, the solid electrolyte of the all-solid-state secondary battery of the present invention is preferably a sulfide-based solid electrolyte or a polymer-based solid electrolyte.

[0010] Sulfide-based solid electrolytes include Li2S-P2S5-based compounds, Li2S-SiS2-based compounds, Li2S-GeS2-based compounds, Li2S-B2S3-based compounds, Li2S-P2S3-based compounds, LiI-Si2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li 10 GeP2S 12 The term "sulfide-based solid electrolyte" is used as a general term for solid electrolytes that mainly contain raw materials such as "Li2S" and "P2S5" as described before "sulfide-based compound". For example, Li2S-P2S5-based compounds include solid electrolytes that contain Li2S and P2S5 and also contain other raw materials. Li2S-P2S5-based compounds also include solid electrolytes with different mixture ratios of Li2S and P2S5.

[0011] Li2S-P2S5 compounds include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, and Li2S-P2S5-Z. m S n (Z is Ge, Zn or Ga, and m and n are positive numbers).

[0012] Li2S-SiS2 compounds include Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li2SO4, and Li2S-SiS2-Li x MO y (M is P, Si, Ge, B, Al, Ga or In; x and y are positive numbers), etc.

[0013] Examples of Li2S-GeS2 based compounds include Li2S-GeS2, Li2S-GeS2-P2S5, and the like.

[0014] Examples of oxide-based solid electrolytes include perovskite-type oxides, Nasicon-type oxides, Lisicon-type oxides, garnet-type oxides, boric acid-based compounds, and β-alumina.

[0015] Examples of perovskite oxides include Li a La 1-a Li-La-Ti perovskite oxides, such as TiO3, Li b La 1-b Li-La-Ta perovskite oxides, such as TaO3, Li c La 1-c Examples include Li-La-Nb perovskite oxides such as NbO3 (where 0 <a<1、0<b<1、0<c<1)。

[0016] As an example of Nasicon-type oxide, Li d+l Al d Ti 2-d Li with (PO4)3 as the main crystal e X f Y g P h O j(X is B, Al, Ga, In, C, Si, Ge, Sn, Sb, or Se; Y is Ti, Zr, Ge, In, Ga, Sn, or Al; 0≦d≦1, e, f, g, p, h, and j are positive numbers). A specific example is LiTi2(PO4)3.

[0017] Examples of the lithium-type oxide include oxides represented by Li4XO4-Li3YO4 (X is Si, Ge, or Ti, and Y is P, As, or V).

[0018] Garnet-type oxides include, for example, Li7La3Zr2O 12 Li-La-Zr oxides and their derivatives are typified by the following:

[0019] Examples of boric acid compounds include Li3BO3, Li3BO3-Li2SO4, Li3BO3-Li2SO4-Li2CO3, and the like.

[0020] Examples of polymer-based solid electrolytes include materials used as polymer electrolytes, such as fluororesins, polyethylene oxide, polyacrylonitrile, polyacrylate, polystyrene sulfonic acid, and derivatives thereof, as disclosed in JP-A-2010-262860.

[0021] Examples of fluororesins that are polymer-based solid electrolytes include polymers that contain vinylidene fluoride, hexafluoropropylene, tetrafluoroethylene, and derivatives thereof as structural units. Specific examples include homopolymers such as polyvinylidene fluoride, polyhexafluoropropylene, and polytetrafluoroethylene; copolymers of vinylidene fluoride and hexafluoropropylene, and the like.

[0022] The polymer-based solid electrolyte may contain a supporting electrolyte. Examples of the supporting electrolyte include salts containing lithium ions. Specific examples of the supporting electrolyte include those commonly used in the field of the present invention, such as LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, LiBCl4, borates, imide salts, etc.

[0023] Complex hydride solid electrolytes include Li(CB9H 10 ), Li(CB 11 H 12 ), Li2(B 12 H 12 ), Li(BH4), LiBH4-LiI, Li(NH2), Li(AlH4), Li3(AlH6), LiBH4-Li(NH2), Li(BH4)-Li(NH2), Li(CB9H 10 )-Li(CB 11 H 12 ), Li(BH4)-KI, Li(BH4)-P2I4, ​​Li(BH4)-P2S5, Li2(NH2), Li(BH4)-GdCl3, Li(BH4)-NaI, Li(BH4)-Li(NH2), etc.

[0024] Phosphate-based solid electrolytes include Li3PO4, LiPON, and Li 2.9 PO 3.3 N 0.46 Examples of organic molecular crystal solid electrolytes include Li{N(SO2F)2}-NCCH2CH2CN.

[0025] The particle diameter of the solid electrolyte is set to the average particle diameter (D 50) is preferably 0.1 μm to 50.0 μm. In the present invention, the average particle size refers to the 50% particle size measured by a laser diffraction light scattering method. The particle size is a diameter based on volume, and in the laser diffraction light scattering method, the diameter of secondary particles is measured.

[0026] The solid electrolyte layer may contain a binder to bind the solid electrolytes together and to exhibit plasticity. Examples of such binders include the binders used in the positive electrode layer and the negative electrode layer described below. However, if the binder content is too high, the charge / discharge capacity of the battery decreases, so the binder content in the solid electrolyte layer is preferably 5 mass% or less.

[0027] The thickness of the solid electrolyte layer is preferably 1 μm to 500 μm in terms of cycle characteristics and rate characteristics. Methods for forming the solid electrolyte layer include a pressure molding method in which a powder of a solid electrolyte material containing a solid electrolyte is pressure molded, and a solvent casting method in which a composition in which a solid electrolyte material containing a solid electrolyte is dispersed or dissolved in a medium is applied and dried. The pressing pressure when the powder of the solid electrolyte material is pressure molded is usually about 1 MPa to 1,000 MPa. When the solid electrolyte layer is formed by the solvent casting method, the composition containing the solid electrolyte material may be directly applied to the positive electrode layer or the negative electrode layer and dried, or may be applied to a support and dried to prepare a film-like solid electrolyte layer. Examples of supports used in the solvent casting method include a glass plate and a polyethylene terephthalate film.

[0028] [B. Positive electrode layer] The positive electrode layer is a layer containing a positive electrode active material. Examples of the positive electrode active material include lithium transition metal composite oxides, lithium-containing transition metal phosphate compounds, lithium-containing silicate compounds, and lithium-containing transition metal sulfate compounds. The transition metal of the lithium transition metal composite oxide is preferably vanadium, titanium, chromium, manganese, iron, cobalt, nickel, copper, or the like.

[0029] Examples of lithium transition metal composite oxides include lithium cobalt composite oxides such as LiCoO2, lithium nickel composite oxides such as LiNiO2, lithium manganese composite oxides such as LiMnO2, LiMn2O4, and Li2MnO3, and lithium transition metal composite oxides in which a part of the transition metal atoms that are the main components of these lithium transition metal composite oxides has been replaced with other metals such as aluminum, titanium, vanadium, chromium, manganese, iron, cobalt, lithium, nickel, copper, zinc, magnesium, gallium, and zirconium. Examples of lithium transition metal composite oxides in which a part of the main transition metal atoms has been replaced with other metals include Li 1.1 Mn 1.8 Mg 0.1 O4, Li 1.1 Mn 1.85 Al 0.05 O4, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.5 Mn 0.5 O2, LiNi 0.80 Co 0.17 Al 0.03 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiMn 1.8 Al 0.2 O4, LiNi 0.5 Mn 1.5 O4, Li2MnO3-LiMO2 (M = Co, Ni, Mn), etc.

[0030] The transition metal of the lithium-containing transition metal phosphate compound is preferably vanadium, titanium, manganese, iron, cobalt, nickel, etc. Examples of the lithium-containing transition metal phosphate compound include LiFePO4, LiMxFe 1-xExamples include iron phosphate compounds such as PO4 (M = Co, Ni, Mn), cobalt phosphate compounds such as LiCoPO4, lithium transition metal phosphate compounds in which some of the transition metal atoms that make up the main part of the lithium transition metal phosphate compounds have been replaced with other metals such as aluminum, titanium, vanadium, chromium, manganese, iron, cobalt, lithium, nickel, copper, zinc, magnesium, gallium, zirconium, and niobium, and vanadium phosphate compounds such as Li3V2(PO4)3.

[0031] Examples of the lithium-containing silicate compound include Li2FeSiO4, etc. Examples of the lithium-containing transition metal sulfate compound include LiFeSO4, LiFeSO4F, etc.

[0032] The positive electrode layer preferably further contains a solid electrolyte because the ion conductivity is improved. The solid electrolyte of the positive electrode layer can be the solid electrolyte exemplified in [A. Solid electrolyte layer]. The solid electrolyte of the positive electrode layer may be the same as or different from the solid electrolyte of the solid electrolyte layer. The ratio of the positive electrode active material and the solid electrolyte in the positive electrode layer is preferably higher, so long as the shape of the positive electrode layer can be maintained and the required ion conductivity can be ensured. For example, the weight ratio of the positive electrode active material:solid electrolyte is preferably within the range of 9:1 to 2:8, and more preferably 8:2 to 4:6.

[0033] The positive electrode layer may contain, as necessary, a conductive assistant such as carbon black, acetylene black, ketjen black, carbon fiber, carbon nanotube, or graphene; or a binder such as polyalkylene glycol, polyvinylidene fluoride, polytetrafluoroethylene, an ethylene-vinyl alcohol copolymer, or styrene-butadiene rubber.

[0034] The thickness of the positive electrode layer is not particularly limited as long as it functions as a positive electrode layer, but is preferably 1 μm to 1,000 μm, and more preferably 10 μm to 200 μm.

[0035] The positive electrode layer may have a current collector for collecting the current of the positive electrode layer. The current collector is not particularly limited as long as it is a conductive material having a current collecting function, and examples thereof include stainless steel, aluminum, nickel, iron, titanium, conductive resin, and carbon. The current collector may be a dense current collector or a porous current collector. The current collector may be surface-treated to improve adhesion and electrical properties.

[0036] The method for forming the positive electrode layer includes a pressure molding method in which a powder of a positive electrode layer material containing a positive electrode active material is pressure molded, and a collector coating method in which a slurry in which a powder of the positive electrode layer material is dispersed in a medium is applied to a current collector and dried. The pressing pressure when the powder of the positive electrode layer material is pressure molded is usually about 1 MPa to 500 MPa. In addition, when forming the positive electrode layer by the collector coating method, the application and drying of the slurry containing the positive electrode layer material may be performed multiple times, or the slurry containing the positive electrode layer material may be applied and dried, and then the solid electrolyte solution may be impregnated and dried.

[0037] [C. Negative electrode layer] The all-solid-state secondary battery of the present invention is characterized in that an organic sulfur-based electrode active material is used as the negative electrode active material of the negative electrode layer. In the present invention, the organic sulfur-based electrode active material refers to a compound that can absorb and release alkali metal ions and can be used as an electrode active material of a secondary battery, and that has carbon atoms and sulfur atoms. The organic sulfur-based active material is represented by the general formula (CS x ) m (x is 0.5 to 2, and m is a number of 4 or more), polycarbon sulfide represented by the general formula (C2S y ) n (y is 2.5 to 50, and n is a number of 2 or more), and thermally modified organic sulfur compounds. Thermally modified organic sulfur compounds are compounds obtained by heat treating a mixture of an organic compound and elemental sulfur in a non-oxidizing atmosphere, and examples of such compounds include sulfur-modified polyacrylonitrile, sulfur-modified elastomer, sulfur-modified polynuclear aromatic ring compound, sulfur-modified pitch, polythienoacene compound, sulfur-modified polyether, sulfur-modified polyamide solvent, and sulfur-modified aliphatic hydrocarbon oxide.

[0038] The sulfur-modified polyacrylonitrile compound is a compound obtained by heat-treating a polyacrylonitrile compound and elemental sulfur in a non-oxidizing atmosphere. The polyacrylonitrile compound is a homopolymer of acrylonitrile or a copolymer of acrylonitrile and another monomer. When the content of acrylonitrile in the polyacrylonitrile compound is low, the battery performance is low. Furthermore, carbonization is relatively easy and the carbonized material exhibits relatively high conductivity, so that the utilization rate of the active material is improved and a high capacity can be achieved. From this viewpoint, the content of acrylonitrile in the copolymer of acrylonitrile and another monomer is preferably at least 90% by mass, and polyacrylonitrile homopolymer is more preferable. Examples of other monomers include acrylic acid, vinyl acetate, N-vinylformamide, and N,N'-methylenebis(acrylamide). The heat treatment temperature is preferably 250°C to 550°C, and the sulfur content of the sulfur-modified polyacrylonitrile is preferably 25 parts by mass to 60 parts by mass, and more preferably 30 parts by mass to 55 parts by mass, per 100 parts by mass of the sulfur-modified polyacrylonitrile, since a large charge / discharge capacity can be obtained. The sulfur content of the organic sulfur-based electrode active material can be calculated from the analysis results using a CHN analyzer capable of analyzing sulfur and oxygen.

[0039] The sulfur-modified elastomer compound is a compound obtained by heat-treating a mixture of rubber and elemental sulfur in an inert gas atmosphere. Examples of rubber include natural rubber, isoprene rubber, butadiene rubber, styrene butadiene rubber, and acrylonitrile butadiene rubber. These rubbers can be used alone or in combination of two or more. The raw rubber may be vulcanized rubber or rubber before vulcanization. The heat treatment temperature is preferably 250°C to 550°C, and the sulfur content of the sulfur-modified elastomer compound is preferably 40 parts by mass to 70 parts by mass relative to 100 parts by mass of the sulfur-modified elastomer compound, since a large charge / discharge capacity can be obtained. More preferably, the sulfur content is 45 parts by mass to 60 parts by mass.

[0040] The sulfur-modified pitch compound is a compound obtained by heating a mixture of pitches and elemental sulfur in an inert gas atmosphere. Examples of pitches include petroleum pitch, coal pitch, mesophase pitch, asphalt, coal tar, coal tar pitch, organic synthetic pitch obtained by polycondensation of condensed polycyclic aromatic hydrocarbon compounds, and organic synthetic pitch obtained by polycondensation of heteroatom-containing condensed polycyclic aromatic hydrocarbon compounds. Pitches are a mixture of various compounds and contain condensed polycyclic aromatics. The condensed polycyclic aromatics contained in pitches may be one type or may be multiple types. The condensed polycyclic aromatics may contain nitrogen and sulfur in the ring in addition to carbon and hydrogen. The heat treatment temperature is preferably 300°C to 500°C, and the sulfur content of the sulfur-modified pitch compound is preferably 25 parts by mass to 70 parts by mass, more preferably 30 parts by mass to 60 parts by mass, based on 100 parts by mass of the sulfur-modified pitch compound, because a large charge / discharge capacity can be obtained.

[0041] The sulfur-modified polynuclear aromatic ring compound is a compound obtained by heating a mixture of a benzene-based aromatic ring compound such as naphthalene, anthracene, tetracene, pentacene, phenanthrene, chrysene, picene, pyrene, benzopyrene, perylene, coronene, and other benzene-based aromatic ring compounds and elemental sulfur in an inert gas atmosphere. In addition, examples of the sulfur-modified polynuclear aromatic ring compound include aromatic ring compounds in which a part of the benzene-based aromatic ring compound is a 5-membered ring, and heteroatom-containing heteroaromatic ring compounds in which a part of the carbon atoms of these compounds is replaced by sulfur, oxygen, nitrogen, and the like. Furthermore, these polynuclear aromatic ring compounds may have a substituent such as a linear or branched alkyl group having 1 to 12 carbon atoms, an alkoxyl group, a hydroxyl group, a carboxyl group, an amino group, an aminocarbonyl group, an aminothio group, a mercaptothiocarbonylamino group, or a carboxyalkylcarbonyl group. The heat treatment temperature is preferably 250°C to 550°C, and the sulfur content of the sulfur-modified pitch compound is preferably 40 parts by mass to 70 parts by mass, and more preferably 45 parts by mass to 60 parts by mass, per 100 parts by mass of the sulfur-modified polynuclear aromatic ring compound, because a large charge / discharge capacity can be obtained.

[0042] The sulfur-modified aliphatic hydrocarbon oxide is a compound obtained by heat-treating an aliphatic hydrocarbon oxide such as an aliphatic alcohol, an aliphatic aldehyde, an aliphatic ketone, an aliphatic epoxide, or a fatty acid with elemental sulfur in an inert gas atmosphere. The heat-treating temperature is preferably 300°C to 500°C. The sulfur content of the sulfur-modified aliphatic hydrocarbon oxide is preferably 45 parts by mass to 75 parts by mass relative to 100 parts by mass of the sulfur-modified aliphatic hydrocarbon oxide, since a large charge / discharge capacity can be obtained. It is more preferably 50 parts by mass to 70 parts by mass.

[0043] The sulfur-modified polyether compound is a compound obtained by heat-treating a polyether compound and elemental sulfur in an inert gas atmosphere. Examples of the polyether compound include polyethylene glycol, polypropylene glycol, ethylene oxide / propylene oxide copolymer, and polytetramethylene glycol. The polyether compound may have an alkyl ether group, an alkylphenyl ether group, or an acyl group at its terminal, or may be an ethylene oxide adduct of a polyol such as glycerin or sorbitol. The heat treatment temperature is preferably 250°C to 500°C. The sulfur content of the sulfur-modified polyether compound is preferably 30 parts by mass to 75 parts by mass relative to 100 parts by mass of the sulfur-modified polyether compound, since a large charge / discharge capacity can be obtained. More preferably, the sulfur content is 40 parts by mass to 70 parts by mass.

[0044] The polythienoacene compound is a compound having a sulfur-containing polythienoacene structure represented by the following general formula (1).

[0045] [ka]

[0046] (In the formula, * represents a bond.)

[0047] The polythienoacene compound is a compound obtained by heat-treating an aliphatic polymer having a linear structure such as polyethylene or a polymer having a thiophene structure such as polythiophene with elemental sulfur in an inert gas atmosphere. The heat treatment temperature is preferably 300°C to 600°C. The sulfur content of the polythienoacene compound is preferably 30 parts by mass to 80 parts by mass relative to 100 parts by mass of the polythienoacene compound, since a large charge / discharge capacity can be obtained. More preferably, the sulfur content is 40 parts by mass to 70 parts by mass.

[0048] The sulfur-modified polyamide compound is an organic sulfur-based electrode active material having a carbon skeleton derived from a polymer having an amide bond, specifically, a compound obtained by heat-treating an aminocarboxylic acid compound and elemental sulfur, or a polyamine compound, a polycarboxylic acid compound and elemental sulfur in an inert gas atmosphere. The heat-treating temperature is preferably 250°C to 600°C. The sulfur content of the sulfur-modified polyamide compound is preferably 40 parts by mass to 70 parts by mass relative to 100 parts by mass of the sulfur-modified polyamide compound, since a large charge / discharge capacity can be obtained. More preferably, the sulfur content is 45 parts by mass to 60 parts by mass.

[0049] In addition to the above-mentioned materials, the thermally modified organic sulfur compound that can be used during the heat treatment includes graphite-based carbon materials such as natural graphite, artificial graphite, and expanded graphite, carbon materials such as carbon black, nanocarbon, activated carbon, carbon fiber, coke, soft carbon, and hard carbon, and vulcanization accelerators such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.

[0050] The particle size of the organic sulfur-based electrode active material is the average particle size (D 50 ) is preferably from 0.5 μm to 100 μm, more preferably from 1 μm to 50 μm, and even more preferably from 1 μm to 20 μm.

[0051] The organic sulfur-based electrode active material is preferably a sulfur-modified polyacrylonitrile compound because of its excellent cycle characteristics and rate characteristics. The organic sulfur-based electrode active material may be used alone or in combination of two or more organic sulfur-based electrode active materials. The organic sulfur-based electrode active material may also be used in combination with other sulfur-based electrode active materials, such as elemental sulfur, sulfur-carbon composite materials, etc.

[0052] The negative electrode layer preferably further contains a solid electrolyte because the ion conductivity is improved. Examples of the solid electrolyte of the negative electrode layer include the solid electrolytes exemplified in [A. Solid Electrolyte Layer]. The solid electrolyte of the negative electrode layer may be the same as or different from the solid electrolyte layer and the solid electrolyte of the positive electrode layer. The ratio of the negative electrode active material to the solid electrolyte in the negative electrode layer is preferably higher as long as the shape of the negative electrode can be maintained and the required ion conductivity can be ensured. For example, the weight ratio of the negative electrode active material:solid electrolyte is preferably within a range of 9:1 to 2:8, and more preferably 8:2 to 4:6.

[0053] The negative electrode layer may contain, as necessary, a conductive assistant such as carbon black, acetylene black, ketjen black, carbon fiber, carbon nanotube, or graphene; or a binder such as polyalkylene glycol, polyvinylidene fluoride, polytetrafluoroethylene, an ethylene-vinyl alcohol copolymer, or styrene-butadiene rubber.

[0054] The thickness of the negative electrode layer is not particularly limited as long as it functions as a negative electrode layer, but is preferably 1 μm to 1000 μm, and more preferably 10 μm to 200 μm.

[0055] The negative electrode layer may have a negative electrode current collector for collecting the current of the negative electrode layer. The negative electrode current collector is not particularly limited as long as it is a conductive material having a current collecting function, and examples thereof include stainless steel, copper, aluminum, nickel, iron, conductive resin, and carbon. The negative electrode current collector may be a dense current collector or a porous current collector. The negative electrode current collector may be surface-treated to improve adhesion and electrical properties.

[0056] The method for forming the negative electrode layer includes a pressure molding method in which a powder of a negative electrode layer material containing an organic sulfur-based electrode active material is pressure molded, and a current collector coating method in which a slurry in which the powder of the negative electrode layer material is dispersed in a medium is applied to a current collector and dried. The pressing pressure when the powder of the negative electrode layer material is pressure molded is usually about 1 MPa to 500 MPa. In addition, when forming the negative electrode layer by the current collector coating method, the application and drying of the slurry containing the negative electrode layer material may be performed multiple times, or the slurry containing the negative electrode layer material may be applied and dried, and then the solid electrolyte solution may be impregnated and dried.

[0057] 〔shape〕 The shape of the all-solid-state secondary battery of the present invention may be a coin type, a laminate type, a cylindrical type, a square type, or the like, among which the square type and the laminate type are preferred, and the laminate type is particularly preferred.

[0058] 〔others〕 The present disclosure includes the following aspects. [1] An all-solid-state secondary battery having a positive electrode layer containing a positive electrode active material, a negative electrode layer containing a negative electrode active material, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, wherein the negative electrode active material is an organic sulfur-based electrode active material. [2] The all-solid-state secondary battery according to [1], wherein the organic sulfur-based electrode active material is a sulfur-modified polyacrylonitrile compound. [3] The all-solid-state secondary battery according to [1] or [2], wherein the positive electrode active material is a lithium transition metal oxide or a lithium-containing transition metal phosphate compound. [4] The all-solid-state secondary battery according to any one of [1] to [3], wherein the solid electrolyte of the solid electrolyte layer is a sulfide-based solid electrolyte or a polymer-based solid electrolyte. EXAMPLES

[0059] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited by the following examples. The sulfur content in the organic sulfur-based electrode active material was calculated from the analysis results using a CHN analyzer capable of analyzing sulfur and oxygen.

[0060] [Production Example 1: Sulfur-modified polyacrylonitrile compound SPAN1] Sulfur-modified polyacrylonitrile was produced by a method according to the production example of JP 2013-054957 A. That is, 10 parts by mass of polyacrylonitrile powder (Sigma-Aldrich, average particle size 200 μm) and 30 parts by mass of sulfur powder (Sigma-Aldrich, average particle size 200 μm) were mixed using a mortar. 20 g of this mixture was placed in a bottomed cylindrical glass tube with an outer diameter of 45 mm and a length of 120 mm, and then a silicone plug having a gas inlet tube and a gas outlet tube was attached to the opening of the glass tube. After replacing the air inside the glass tube with nitrogen, the lower part of the glass tube was placed in a crucible-type electric furnace, and heated at 400 ° C. for 1 hour while introducing nitrogen from the gas inlet tube to remove the generated hydrogen sulfide. The sulfur vapor was condensed at the top or lid of the glass tube and refluxed. The obtained intermediate product was placed in a glass tube oven at 260 ° C., reduced pressure and heated at 20 hPa for 3 hours to remove sulfur. The obtained sulfur-modified product was pulverized using a ball mill and then classified with a sieve to obtain a sulfur-modified polyacrylonitrile compound SPAN1 having an average particle size of 10 μm. SPAN1 is an organic sulfur-based electrode active material, and the sulfur content per 100 parts by mass of SPAN1 was 42.3 parts by mass.

[0061] [Production Example 2: Sulfur-modified polyacrylonitrile compound SPAN2] The same operation as in Production Example 1 was carried out except that the conditions for removing sulfur from the intermediate product were changed from 3 hours at 260°C and reduced pressure of 20 hPa to 24 hours at 260°C and normal pressure under a nitrogen stream, to obtain a sulfur-modified polyacrylonitrile compound SPAN2. SPAN2 is an organic sulfur-based electrode active material, and the sulfur content per 100 parts by mass of SPAN2 was 50.0 parts by mass.

[0062] In the following evaluations, the following abbreviations were used: [Cathode active material] NCM: LiNi coated with LiNbO3 1 / 3 Co 1 / 3 Mn 1 / 3 O2 LFP: LifePO4 [Negative electrode active material (negative electrode layer)] InLi: Indium-lithium alloy foil LiM: Lithium metal foil [Solid electrolyte] LPS:Li3PS4 (manufactured by NEI Corporation) LGPS:Li 10 GeP2S 12 (Manufactured by Piotrek Co., Ltd.) PEO: Polyethylene oxide solid electrolyte (manufactured by NEI Corporation, product name: NANOMYTE H-Polymer) [Conductive assistant] AB: Acetylene black (manufactured by Denka Co., Ltd.) [Binding Agent] PVDF: Polyvinylidene fluoride (Kureha Corporation, product name: KF Polymer) CMC: Sodium carboxymethylcellulose (manufactured by Daicel Miraize Co., Ltd.) SBR: Styrene-butadiene rubber (40% by mass aqueous dispersion, manufactured by Zeon Corporation) [Current collector] SUS: Stainless steel foil (thickness 10 μm) CAL: Carbon-coated aluminum foil

[0063] [All-solid-state secondary battery: sulfide-based solid electrolyte] [Positive electrode layer MA1] The positive electrode layer MA1 was produced by using NCM, a lithium transition metal oxide, as the positive electrode active material, AB as the conductive additive, and LPS, a sulfide-based solid electrolyte, as the solid electrolyte. The materials were weighed out to have a mass ratio of positive electrode active material:conductive additive:solid electrolyte = 50:5:45, and then mixed in a ball mill under an argon atmosphere and molded by pressing to produce the positive electrode layer MA1.

[0064] [Positive electrode layer MA2] A positive electrode layer MA2 was produced in the same manner as the positive electrode layer MA1, except that the solid electrolyte in the positive electrode layer MA1 was changed from LPS to LGPS, which is a sulfide-based solid electrolyte.

[0065] [Negative electrode layer MB1] SPAN1, an organic sulfur-based electrode active material, was used as the negative electrode active material, AB was used as the conductive additive, and LPS, a sulfide-based solid electrolyte, was used as the solid electrolyte. These were weighed out so that the mass ratio of negative electrode active material:conductive additive:solid electrolyte was 50:5:45. Then, the materials were mixed in a ball mill under an argon atmosphere and molded using a press process to produce the negative electrode layer MB1.

[0066] [Negative electrode layer MB2] A negative electrode layer MB2 was produced in the same manner as in the negative electrode layer MB1, except that the negative electrode active material was changed from SPAN1 to SPAN2.

[0067] [Negative electrode layer MB3] A negative electrode layer MB3 was produced in the same manner as the negative electrode layer MB1, except that the solid electrolyte in the negative electrode layer MB1 was changed from LPS to LGPS, which is a sulfide-based solid electrolyte.

[0068] [Negative electrode layer MB4] A negative electrode layer MB4 was produced in the same manner as the negative electrode layer MB2, except that the solid electrolyte in the negative electrode layer MB2 was changed from LPS to LGPS, which is a sulfide-based solid electrolyte.

[0069] [Solid electrolyte layer MC1] LPS was used as the solid electrolyte, and the LPS was molded by pressing to produce a circular solid electrolyte layer MC1 with a diameter of 10 mm.

[0070] [Solid electrolyte layer MC2] A solid electrolyte layer MC2 was produced in the same manner as in the solid electrolyte layer MC1, except that the solid electrolyte was changed from LPS to LGPS.

[0071] Example 1 The all-solid-state secondary battery of Example 1 was produced by laminating a current collector SUS / positive electrode layer MA1 / solid electrolyte layer MC1 / negative electrode layer MB1 / current collector SUS in this order, pressing them under a pressure of 255 MPa, and sealing them in an all-solid-state battery evaluation cell (manufactured by Hosen Co., Ltd., model KP-SolidCell).

[0072] Example 2 An all-solid-state secondary battery of Example 2 was produced in the same manner as in Example 1, except that the negative electrode layer in Example 1 was changed from MB1 to MB2.

[0073] Example 3 The all-solid-state secondary battery of Example 3 was produced by stacking a current collector SUS / positive electrode layer MA2 / solid electrolyte layer MC2 / negative electrode layer MB3 / current collector SUS in this order, press-molding the stack at a pressure of 255 MPa, and sealing the stack in an all-solid-state battery evaluation cell (manufactured by Hosen Co., Ltd., model KP-SolidCell).

[0074] Example 4 An all-solid-state secondary battery of Example 4 was produced in the same manner as in Example 3, except that the negative electrode layer in Example 3 was changed from MB3 to MB4.

[0075] Comparative Example 1 The all-solid-state secondary battery of Comparative Example 1 was produced by stacking a current collector SUS / positive electrode layer MA1 / solid electrolyte layer MC1 / negative electrode InLi / current collector SUS in that order, press-molding the stack at a pressure of 255 MPa, and sealing the stack in an all-solid-state battery evaluation cell (manufactured by Hosen Co., Ltd., model KP-SolidCell).

[0076] Comparative Example 2 The all-solid-state secondary battery of Comparative Example 2 was produced by stacking a current collector SUS / positive electrode layer MA2 / solid electrolyte layer MC2 / negative electrode InLi / current collector SUS in that order, pressing them under a pressure of 255 MPa, and sealing them in an all-solid-state battery evaluation cell (manufactured by Hosen Co., Ltd., model KP-SolidCell).

[0077] [All-solid-state secondary battery: polymer-based solid electrolyte] [Positive electrode layer PA1] LFP was used as the positive electrode active material, AB as the conductive additive, and PVDF as the binder, and the mass ratio of the positive electrode active material:conductive additive:binder was weighed out to be 90:5:5, and then N-methylpyrrolidone was added as a solvent and mixed using a rotation-revolution mixer to prepare a positive electrode forming composition. This positive electrode forming composition was applied to a current collector CAL and dried, and then the current collector was impregnated with an acetonitrile solution of solid electrolyte PEO and dried to produce a positive electrode layer PA1.

[0078] [Negative electrode layer PB1] The organic sulfur-based electrode active material SPAN1 was used as the negative electrode active material, the conductive additive AB, and SBR and CMC as binders, and the mass ratio of the positive electrode active material:conductive additive:binder SBR:binder CMC = 90:5:3:2 was measured in terms of solid content, and water was added as a solvent and mixed using a rotation / revolution mixer to prepare a slurry for forming the negative electrode. This slurry was applied to a current collector CAL and dried, and then the current collector was impregnated with an acetonitrile solution of solid electrolyte PEO and dried to produce the negative electrode layer PB1.

[0079] [Negative electrode layer PB2] A negative electrode layer PB2 was produced in the same manner as in the negative electrode layer PB1, except that SPAN2, which is an organic sulfur-based electrode active material, was used as the negative electrode active material instead of SPAN1 in the negative electrode layer PB1.

[0080] [Solid electrolyte layer PC1] A solution of the solid electrolyte PEO in acetonitrile was applied onto a support made of polyethylene terephthalate, and a film-like solid electrolyte layer PC1 was produced by a solvent casting method.

[0081] Example 5 After laminating the positive electrode layer PA1 / solid electrolyte layer PC1 / negative electrode layer PB1 in this order, the resultant was housed in a battery case and sealed using a crimping machine to produce a coin-shaped all-solid-state secondary battery of Example 5 having a diameter of 20 mm and a thickness of 3.2 mm.

[0082] Example 6 An all-solid-state secondary battery of Example 6 was produced in the same manner as in Example 5, except that the negative electrode layer PB2 was used instead of the negative electrode layer PB1 in Example 5.

[0083] Comparative Example 3 An all-solid-state secondary battery of Comparative Example 3 was assembled in the same manner as in Example 5, except that lithium metal was used as the negative electrode instead of the negative electrode layer PB1 in Example 5.

[0084] Table 1 shows the positive electrode active material and solid electrolyte of the positive electrode layer, the solid electrolyte of the solid electrolyte layer, and the negative electrode active material and solid electrolyte of the negative electrode layer for the all-solid-state secondary batteries of Examples 1 to 6 and Comparative Examples 1 to 3. [Table 1]

[0085] [Evaluation of cycle characteristics] A charge / discharge test was carried out by the following method for the all-solid-state secondary batteries of Examples 1 to 6 and Comparative Examples 1 to 3, and the capacity retention rate was calculated. The results are shown in Table 2. Note that a higher capacity retention rate indicates better cycle characteristics.

[0086] [Charge / Discharge Test Method] The all-solid-state secondary battery was placed in a thermostatic chamber at 60°C, and a charge / discharge test was performed for 50 cycles at a charge rate of 0.1C and a discharge rate of 0.1C. The ratio (%) of the discharge capacity at the 50th cycle to the discharge capacity at the 5th cycle was defined as the capacity retention rate. Note that since the positive and negative active materials used in the secondary batteries were not the same, the charge cut-off voltage and discharge cut-off voltage of each all-solid-state secondary battery were as shown in Table 2.

[0087] [Table 2]

[0088] The capacity retention rates of the all-solid-state secondary batteries of Examples 1 to 6, which used sulfur-modified polyacrylonitrile, an organic sulfur-based electrode active material, as the negative electrode active material, were nearly 100%, which was higher than the capacity retention rates of the all-solid-state secondary batteries of Comparative Examples 1 to 3, which used an indium-lithium alloy foil or a lithium metal foil. This shows that excellent cycle characteristics can be obtained by using an organic sulfur-based electrode active material as the negative electrode active material of the all-solid-state secondary battery.

Claims

1. An all-solid-state secondary battery having a positive electrode layer including a positive electrode active material, a negative electrode layer including a negative electrode active material, and a solid electrolyte layer between the positive electrode layer and the negative electrode layer, wherein the negative electrode active material is an organic sulfur-based electrode active material.

2. The all-solid-state secondary battery according to claim 1 , wherein the organic sulfur-based electrode active material is a sulfur-modified polyacrylonitrile compound.

3. 3. The all-solid-state secondary battery according to claim 1, wherein the positive electrode active material is a lithium transition metal oxide or a lithium-containing transition metal phosphate compound.

4. 3. The all-solid-state secondary battery according to claim 1, wherein the solid electrolyte of the solid electrolyte layer is a sulfide-based solid electrolyte or a polymer-based solid electrolyte.

Citation Information

Patent Citations

  • Negative electrode active material for secondary cell, and negative electrode and secondary cell using the same

    JP2014096326A

  • Sulfur-modified polyacrylonitrile, manufacturing method therefor, and application thereof

    WO2010044437A1

  • Sulfur-containing positive electrode active material and method for producing same, and positive electrode for lithium ion secondary battery

    WO2013001693A1

  • Solid-state battery and method for manufacturing electrode active material

    WO2015030053A1

  • Lithium ion secondary battery

    WO2019225588A1