Conductive adhesive composition

A blend of flaky and spherical silver powders with specific properties in a conductive adhesive composition maintains conductivity and reliability, addressing cost and oxidation issues, and achieving good electrical properties.

JP2024163636AActive Publication Date: 2024-11-22KYOTO ELEX
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023079414
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

Conductive adhesive compositions face challenges in achieving good electrical conductivity and reliability while reducing the cost by minimizing the use of expensive silver powder, and copper-based powders introduce oxidation concerns.

Method used

A conductive adhesive composition using a blend of flaky silver powder with specific properties and spherical silver powder, along with a resin component, to maintain conductivity and reliability even with reduced silver content, avoiding copper-based powders.

Benefits of technology

The composition achieves good electrical properties, including connection resistance and adhesive strength, while minimizing silver usage, thus reducing costs and ensuring high reliability in applications requiring it.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163636000001_ABST
    Figure 2024163636000001_ABST
Patent Text Reader

Abstract

To provide a conductive adhesive composition which can achieve good electric characteristics containing a connection resistance without impairing conductivity even if an amount of blended silver powder is relatively reduced.SOLUTION: A conductive adhesive composition contains (A) silver powder, and (B) a resin component. As (A) the silver powder, (a1) flaky silver powder and (a2) spherical silver powder are contained. (a1) The flaky silver powder has thickness of 0.3 μm or less, an average particle diameter D50 of 4 to 9 μm and a BET specific surface area of 1.5 to 2.5 m2 / g. (a2) The spherical silver powder has an average particle diameter D50 of 0.01 to 3 μm, a BET specific surface area of 0.5 to 2.5 m2 / g, and tap density of less than 2 g / cm3. Furthermore, a ratio of (A) the silver powder in a solid content is 70 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrically conductive adhesive composition, and in particular to an electrically conductive adhesive composition containing silver powder and a resin component. [Background technology]

[0002] Conventionally, in conductive adhesive compositions (or conductive paste compositions), powders of precious metals, typically silver, have been widely used as conductive powders from the viewpoint of obtaining good conductivity and good reliability. However, since precious metal powders such as silver powder are expensive, reduction of the content of the conductive powder has been considered in order to reduce costs.

[0003] If the content of the conductive powder is reduced, the resulting conductive adhesive composition will not have good electrical conductivity, leading to deterioration of electrical properties. Therefore, in order to achieve good electrical properties, for example, the use of copper powder or silver-coated copper powder instead of silver powder has been considered. However, if such copper-based powder is used as the conductive powder, there is a concern that reliability will decrease due to oxidation of copper, etc.

[0004] Therefore, for example, Patent Document 1 discloses a conductive paste composition using two types of flake silver powder (thin silver powder) in order to achieve good conductivity while reducing the silver powder content. In Patent Document 1, the average particle size, specific surface area, and apparent density of the two types of flake silver powder are optimized, and the compounding ratio and the content relative to the resin component are specified. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-111057 A Summary of the Invention [Problem to be solved by the invention]

[0006] In Patent Document 1, two different types of flaky silver powders are mixed in a predetermined ratio to reduce the silver powder content in the conductive paste composition. However, as a result of intensive research by the present inventors, it has become clear that if the conductive powder is only flaky silver powder, it may not be possible to practically achieve a satisfactory connection resistance (resistance in the thickness direction) after the conductive adhesive composition is cured.

[0007] The present invention has been made to solve such problems, and aims to provide a conductive adhesive composition that can achieve good electrical properties, including connection resistance, without impairing conductivity, even when the amount of silver powder mixed is relatively small. [Means for solving the problem]

[0008] In order to solve the above problems, the conductive adhesive composition according to the present disclosure contains (A) silver powder and (B) a resin component, and as the (A) silver powder, it contains (a1) flaky silver powder and (a2) spherical silver powder, and the (a1) flaky silver powder has a thickness of 0.3 μm or less, an average particle size D50 in the range of 4 to 9 μm, and a BET specific surface area of ​​1.5 to 2.5 m. 2 / g, and the (a2) spherical silver powder has an average particle size D50 in the range of 0.01 to 3 μm and a BET specific surface area of ​​0.5 to 2.5 m 2 / g and has a tap density of 2 g / cm 3 and further, the ratio of the (A) silver powder in the solid content is 70 mass % or less.

[0009] According to the above-mentioned configuration, since the (A) silver powder is a combination of the (a1) flake silver powder and the (a2) spherical silver powder, which satisfy the predetermined conditions, the conductive adhesive composition can achieve good electrical properties including connection resistance without impairing the conductivity even if the amount of the (A) silver powder is relatively small. In addition, since it is possible to reduce the amount of expensive (A) silver powder used (amount of the mixture), it is possible to suppress or avoid the increase in the cost of the conductive adhesive composition.

[0010] In addition, in conventional conductive adhesive compositions, copper-containing powders such as copper powder or silver-coated copper powder may be used as the conductive powder in order to suppress high costs. In such copper-containing powders, there may be concerns about the reliability of the conductive adhesive composition due to oxidation of copper, etc. Therefore, conductive adhesive compositions using copper-containing powders tend to be difficult to use in applications requiring high reliability. In contrast, according to the above configuration, it is possible to reduce the blending amount (content) of (A) silver powder without using copper-containing powder, making it possible to use the composition in applications requiring high reliability.

[0011] In the conductive adhesive composition having the above-mentioned configuration, the (a1) flaky silver powder and the (a2) spherical silver powder may be blended in a mass ratio within the range of 20 / 80 to 80 / 20.

[0012] In the conductive adhesive composition having the above-mentioned configuration, the (B) resin component may be a thermosetting resin and its curing agent or reaction initiator.

[0013] In the conductive adhesive composition having the above configuration, the thermosetting resin may be at least one resin selected from the group consisting of epoxy resin, phenol resin, acrylic resin, urethane resin, and silicone resin.

[0014] The conductive adhesive composition having the above-mentioned configuration may be used by applying it onto a substrate with a printer or a dispenser.

[0015] The conductive adhesive composition having the above configuration may be used for bonding electronic components.

[0016] In the conductive adhesive composition having the above configuration, the electronic component may be a solar cell module. Effect of the Invention

[0017] In the present invention, the above-mentioned configuration has the effect of providing a conductive adhesive composition that can achieve good electrical characteristics including connection resistance without impairing conductivity, even if the amount of silver powder mixed is relatively small. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1A is a model diagram showing the state of the solid content in a conductive adhesive composition containing only flaky silver powder, and FIG. 1B is a model diagram showing the electrical conductivity and the number of interfacial contacts of silver powder in a conductive adhesive composition containing only flaky silver powder and a conductive adhesive composition according to the present disclosure. [Diagram 2] FIG. 2 is a plan view showing a schematic configuration of an evaluation conductor pattern used to evaluate the conductivity and adhesive strength of a conductive adhesive composition after curing in the examples of the present disclosure. [Diagram 3] FIG. 2 is a model diagram showing a schematic configuration of an evaluation sample used to evaluate the connection resistance and adhesive strength after curing of a conductive adhesive composition in the examples of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Representative embodiments of the present disclosure will be described below. The conductive adhesive composition according to the present disclosure contains (A) silver powder and (B) a resin component. As the silver powder (A), the conductive adhesive composition contains (a1) flaky silver powder and (a2) spherical silver powder. The flaky silver powder (a1) has a thickness of 0.3 μm or less, an average particle size D50 in the range of 4 to 9 μm, and a BET specific surface area of ​​1.5 to 2.5 m. 2 / g, and (a2) the spherical silver powder has an average particle size D50 in the range of 0.01 to 3 μm and a BET specific surface area of ​​0.5 to 2.5 m 2 / g and has a tap density of 2 g / cm 3 and further, the ratio of the (A) silver powder in the solid content is 70 mass % or less.

[0020] [(A) Silver powder] The silver powder (A) contained in the conductive adhesive composition according to the present disclosure is composed of a mixture of a flake silver powder (a1) and a spherical silver powder (a2). In other words, in the present disclosure, two types of silver powders with different shapes are used in combination as the conductive component. Both of these silver powders satisfy the specified conditions (specified physical properties).

[0021] First, (a1) the flaky silver powder has a flake shape (scale-like or thin plate-like), a thickness of 0.3 μm or less, an average particle size D50 in the range of 4 to 9 μm, and a BET specific surface area of ​​1.5 to 2.5 m. 2 The (a1) flake silver powder further has an apparent density of 1.0 g / cm. 3 The tap density may be less than 2 g / cm 3 It may be less than.

[0022] (a2) Spherical silver powder has a spherical (granular) shape, an average particle size D50 in the range of 0.01 to 3 μm, and a BET specific surface area of ​​0.5 to 2.5 m. 2 / g and has a tap density of 2 g / cm 3 The spherical silver powder (a2) has to satisfy the specified physical property of having an apparent density of less than 1.0 g / cm 3 It may be less than.

[0023] In the present disclosure, the average particle size, BET specific surface area, tap density, and apparent density of the (a1) flaky silver powder and the (a2) spherical silver powder, as well as the thickness of the (a1) flaky silver powder, are measured or calculated by the methods shown in the Examples described below.

[0024] In addition, the various conditions in the various measurement or evaluation methods for silver powder can be conditions known in the field of conductive adhesive compositions or resin-type conductive pastes (for example, the conditions described in the published patent applications of the applicant of this application).

[0025] In the conductive adhesive composition according to the present disclosure, it is important to use, as the silver powder (A), a combination of a flake silver powder (a1) and a spherical silver powder (a2) that satisfy predetermined physical properties. For example, as shown in FIG. 1(A), a configuration is assumed in which thick flake silver powder 11 or thin flake silver powder 12 is dispersed in a resin component 10 as a cured product of the conductive adhesive composition.

[0026] As shown in FIG. 1A, when the same mass of flaky silver powder 11 and flaky silver powder 12 are mixed, the density of the silver powder in the resin component 10 is relatively lower for the flaky silver powder 11. As a result, the conductor resistance of the cured product is relatively more likely to increase. In particular, when the predetermined physical properties set for the flaky silver powder (a1) according to the present disclosure are not satisfied, the conductor resistance of the cured product is more likely to increase.

[0027] 1(B), when focusing on the resistance in the thickness direction, it is considered that the thicker flaky silver powder 11 has a smaller number of interface contacts between the flaky powders than the thinner flaky silver powder 12. As a result, in the obtained cured product, it is considered that the thicker flaky silver powder 11 has a lower connection resistance in the thickness direction, contrary to FIG.

[0028] In contrast, in the conductive adhesive composition according to the present disclosure, both the (a1) flake silver powder and the (a2) spherical silver powder satisfy the above-mentioned specific physical properties, so that the spherical powder can easily come into good contact with the flake powder. As a result, it is considered that the increase in the number of interface contacts of the (A) silver powder in the cured product can be effectively suppressed. This makes it possible to effectively reduce the (lateral) conductor resistance and the connection resistance in the thickness direction in the cured product.

[0029] In the conductive adhesive composition according to the present disclosure, the blending ratio (mixing ratio) of the (a1) flaky silver powder and the (a2) spherical silver powder in the total amount of the (A) silver powder is not particularly limited. Typically, as shown in the examples described later, the blending ratio ((a1) / (a2)) of the (a1) flaky silver powder and the (a2) spherical silver powder may be within a range of 20 / 80 to 80 / 20 by mass. If the blending ratio of the (a1) flaky silver powder and the (a2) spherical silver powder is within this range, it is possible to easily achieve both good electrical properties and good adhesive strength in the cured product of the conductive adhesive composition according to the present disclosure.

[0030] In the conductive adhesive composition according to the present disclosure, the (a1) flaky silver powder among the (A) silver powders may be one type of silver powder satisfying the predetermined physical properties, or two or more types of silver powders satisfying the predetermined physical properties may be combined appropriately. Similarly, the (a2) spherical silver powder may be one type of silver powder satisfying the predetermined physical properties, or two or more types of silver powders satisfying the predetermined physical properties may be combined appropriately.

[0031] The conductive adhesive composition according to the present disclosure may contain a conductive powder (particle) made of a material other than (A) silver powder. However, the conductive adhesive composition according to the present disclosure needs to achieve good electrical properties while relatively reducing the content of (A) silver powder. Therefore, it is preferable not to contain a conductive powder made of a material with lower conductivity than silver (Ag). Examples of conductive powders that can be used in combination with (A) silver powder include gold (Au) and palladium (Pd).

[0032] In addition, the (A) silver powder does not contain any other metal components except for containing a general trace amount of impurities. In other words, the (A) silver powder in the present disclosure may be a metal powder substantially composed of only silver. The term "trace amount" as used herein means a range known in the field of silver powder manufacturing, and is not specifically limited. On the other hand, the material composition of other conductive powders that can be used in combination with the (A) silver powder is not particularly limited, and may be a powder (metal powder) substantially composed of one type of metal (or conductive material), or an alloy powder composed of multiple types of metals.

[0033] The shape of the silver powder (A) is limited to (a1) flake silver powder and (a2) spherical silver powder as described above, but other shapes of silver powder may be contained as necessary. The shape of the other conductive powder that can be used in combination with the silver powder (A) is also not particularly limited, and may be spherical, flake, or other shapes.

[0034] In addition, the (a1) flake-shaped silver powder in this disclosure may be a powder having a shape close to a flat plate or a thin rectangular parallelepiped when viewed as a whole, even if it has some unevenness and deformation. "Flake-shaped" can be rephrased as thin flake-shaped or scale-shaped. In addition, the (a2) spherical silver powder in this disclosure may be a powder having a three-dimensional shape closer to a cube than a rectangular parallelepiped when viewed as a whole, even if it has some unevenness and deformation. In addition, "spherical" can be rephrased as granular.

[0035] (A) The method of producing silver powder is not particularly limited, and known methods can be used. (a2) In the case of spherical silver powder, examples include powder produced by a wet reduction method, and powder produced by other known methods such as an electrolytic method or an atomization method, but are not particularly limited. (a1) In the case of flaky silver powder, flaky silver powder can be produced by using spherical silver powder produced by a known method as the base powder and subjecting the base powder to a known mechanical treatment.

[0036] [(B) Resin component] The conductive adhesive composition according to the present disclosure contains the above-mentioned (A) silver powder and (B) resin component. In the present disclosure, the total amount of (A) silver powder and (B) resin component constitutes the solid content of the conductive adhesive composition. However, in the present disclosure, other components may be contained as solid content.

[0037] In the conductive adhesive composition according to the present disclosure, the specific type of the resin component (B) is not particularly limited, but is typically a thermosetting resin and its curing agent, or a thermosetting resin and its reaction initiator (or polymerization initiator). In the following description, the reaction initiator (polymerization initiator) may be abbreviated to "initiator" as appropriate.

[0038] In the present disclosure, the specific type of thermosetting resin usable as the resin component (B) is not particularly limited, but a representative example is at least one resin selected from the group consisting of epoxy resins, phenolic resins, acrylic resins, urethane resins, and silicone resins. In other words, in the present disclosure, as the resin component (B), only one of these resins may be used, or two or more of them may be appropriately selected and used.

[0039] In addition, the "thermosetting resin" in this disclosure includes a curable composition (e.g., a monomer or a prepolymer) that becomes an epoxy resin, a phenolic resin, an acrylic resin, a urethane resin, a silicone resin, or another resin upon curing.

[0040] Furthermore, in the present disclosure, even when only one type of resin constituting these groups is used, two or more different types of resins classified into the resins may be appropriately combined and used. Of course, the same applies when two or more types of resins constituting these groups are used. For convenience, resins such as epoxy resins, phenolic resins, acrylic resins, urethane resins, and silicone resins are considered to be "higher classifications" and specific resins corresponding to epoxy resins are considered to be "lower classifications." One or more types of resins in the higher classifications may be used, or one or more types of resins in the lower classifications may be used.

[0041] For example, in Examples 1 to 7 described later, a combination of an epoxy resin, which is a higher-level classification, and a phenolic resin, which is a higher-level classification, is used as the (B) resin component, but two types of epoxy resins, which are lower-level classifications, are used in combination as the epoxy resin (there is only one type of phenolic resin, which is a lower-level classification). Also, in Examples 8 to 14, only an acrylic resin, which is a higher-level classification, is used as the (B) resin component, but a total of four types of acrylic resins, which are lower-level classifications, are used in combination.

[0042] In the present disclosure, the resin component (B) may be a combination of thermosetting resins (curable compositions that become resins by curing) other than epoxy resins, phenolic resins, acrylic resins, urethane resins, and silicone resins. In addition, when epoxy resins, phenolic resins, acrylic resins, urethane resins, silicone resins, or other thermosetting resins are used in combination, the compounding ratio (mixing ratio) is not particularly limited. Not only is the compounding ratio in the combination of resins in higher classification not limited, but the compounding ratio in the combination of multiple resins in lower classification is also not particularly limited.

[0043] Next, each of the resins corresponding to the higher classification constituting the group used in the present disclosure will be specifically described, focusing on the lower classification.

[0044] First, the specific structure of the epoxy resin used as the resin component (B) in the present disclosure is not particularly limited. A representative example is a polyfunctional epoxy resin having two or more oxirane rings (epoxy groups) in one molecule.

[0045] Examples of such polyhydric epoxy resins include glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type. The glycidyl ether type is obtained by reacting epichlorohydrin with novolac, polyhydric phenol, polyhydric alcohol, etc. Examples of novolac include phenol novolac and cresol novolac, examples of polyhydric phenol include bisphenol A, hydrogenated bisphenol A, bisphenol F, bisphenol AD, and resorcin, and examples of polyhydric alcohol include ethylene glycol, neopentyl glycol, glycerin, trimethylolpropane, pentaerythritol, triethylene glycol, and polypropylene glycol. Examples of monofunctional glycidyl ether type epoxy resins include phenyl glycidyl ether. The glycidyl amine type is obtained by reacting epichlorohydrin with a polyamino compound such as ethylenediamine, triethylenetetramine, and aniline. The glycidyl ester type is obtained by reacting epichlorohydrin with a polyvalent carboxyl compound such as adipic acid, phthalic acid, isophthalic acid, etc. The alicyclic type is synthesized by oxidation of olefin, etc. These epoxy resins may be used alone or in combination of two or more.

[0046] In addition, when an epoxy resin is used as the resin component (B) in the present disclosure, a blocked polyisocyanate compound may be used in combination. The epoxy equivalent of the epoxy resin used in the present disclosure is not particularly limited, but is typically within the range of 100 to 1000, and may be within the range of 100 to 400. If the epoxy equivalent is less than 100, there is a risk that some effect will be caused on the physical properties of the cured product formed from the obtained conductive adhesive composition. On the other hand, if the epoxy equivalent exceeds 1000, the thixotropy of the obtained conductive adhesive composition tends to decrease.

[0047] In the examples 1 to 7 and comparative examples 1 to 7 described later, a commercially available phenol novolac glycidyl ether type epoxy resin and a commercially available monofunctional glycidyl ether type epoxy resin monomer, phenyl glycidyl ether, are used as one of the resin components (B).

[0048] Next, the specific structure of the phenolic resin used as the resin component (B) in the present disclosure is not particularly limited. Typically, known phenolic resins obtained by reacting phenols with aldehydes can be suitably used. Specifically, for example, novolac-type phenolic resins, resol-type phenolic resins, trisphenylmethane-type phenolic resins, naphthalene-type phenolic resins, cyclopentadiene-type phenolic resins, aryl alkylene-type phenolic resins, etc. can be mentioned. Among these, novolac-type phenolic resins or resol-type phenolic resins can be mentioned, but are not particularly limited.

[0049] The novolak-type phenolic resin is not particularly limited as long as it is obtained by reacting a known phenol with a known aldehyde in the presence of an acid catalyst.

[0050] The phenols used in the novolac phenolic resin are not particularly limited, and examples thereof include phenol, cresol, xylenol, ethylphenol, p-phenylphenol, p-tert-butylphenol, p-tert-amylphenol, p-octylphenol, p-nonylphenol, p-cumylphenol, bisphenol A, bisphenol F, resorcinol, etc. These phenols may be used alone or in appropriate combination of two or more.

[0051] The aldehydes used in the novolac phenolic resin are not particularly limited, and examples thereof include alkyl aldehydes such as formaldehyde, acetaldehyde, propylaldehyde, and butylaldehyde; aromatic aldehydes such as benzaldehyde and salicylaldehyde; etc. These aldehydes may be used alone or in appropriate combination of two or more.

[0052] In producing a novolac phenolic resin, the acid catalyst for reacting a phenol with an aldehyde is not particularly limited, and known organic sulfonic acids, inorganic acids, etc. can be suitably used. In addition, the molar ratio in reacting a phenol with an aldehyde is not particularly limited, and a known molar ratio can be selected.

[0053] The resol type phenolic resin is not particularly limited as long as it is obtained by reacting a known phenol with a known aldehyde in the presence of a catalyst such as an alkali metal, an amine, or a divalent metal salt.

[0054] The phenols used in the resol-type phenolic resin are not particularly limited, and examples thereof include cresols such as phenol, o-cresol, m-cresol, and p-cresol; xylenols such as 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, and 3,5-xylenol; ethylphenols such as o-ethylphenol, m-ethylphenol, and p-ethylphenol; butylphenols such as isopropylphenol, butylphenol, and p-tert-butylphenol; p-tert-amylphenol, p-octylphenol, p-nonylphenol, p-cumiphenol, and the like. Examples of the phenols include alkylphenols such as phenylphenol, halogenated phenols such as fluorophenol, chlorophenol, bromophenol, and iodophenol, substituted monohydric phenols such as p-phenylphenol, aminophenol, nitrophenol, dinitrophenol, and trinitrophenol, monohydric phenols such as 1-naphthol and 2-naphthol, and polyhydric phenols such as resorcin, alkylresorcin, pyrogallol, catechol, alkylcatechol, hydroquinone, alkylhydroquinone, phloroglucin, bisphenol A, bisphenol F, bisphenol S, and dihydroxynaphthalene. Only one of these phenols may be used, or two or more of them may be used in appropriate combination.

[0055] The aldehydes used in the resol type phenolic resin are not particularly limited, but examples thereof include formaldehyde, paraformaldehyde, trioxane, acetaldehyde, propionaldehyde, polyoxymethylene, chloral, hexamethylenetetramine, furfural, glyoxal, n-butylaldehyde, caproaldehyde, allylaldehyde, benzaldehyde, crotonaldehyde, acrolein, tetraoxymethylene, phenylacetaldehyde, o-tolualdehyde, salicylaldehyde, etc. These aldehydes may be used alone or in appropriate combination of two or more.

[0056] In producing the resol type phenolic resin, various catalysts for reacting phenols with aldehydes are not particularly limited. Specific examples include hydroxides, oxides, carbonates of metal elements of Group 1 or Group 2 of the periodic table, known low molecular weight organic amines, divalent metal acetates, etc. In addition, the molar ratio when reacting phenols with aldehydes is not particularly limited, and a known molar ratio can be selected.

[0057] In the examples described later, Examples 1 to 7 and Comparative Examples 1 to 7, a commercially available novolac type phenolic resin is used as one of the resin components (B).

[0058] Next, the specific structure of the acrylic resin used as the resin component (B) in the present disclosure is not particularly limited. In general, polymers of acrylic compounds having polymerizability, such as acrylic acid (acrylate) or methacrylic acid (methacrylate), or esters thereof, can be mentioned. The acrylic resin in the present disclosure may be used in combination with other monomers or prepolymers that are polymerizable with the acrylic compound.

[0059] Representative acrylic compounds include, for example, (meth)acrylate (acrylate or methacrylate), ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isoamyl (meth)acrylate (isopentyl (meth)acrylate), isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, and deci. chain alkyl (meth)acrylates such as butyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), stearyl (meth)acrylate (octadecyl (meth)acrylate); cyclic alkyl (meth)acrylates such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate; alkoxy group-containing (meth)acrylates such as 1-methoxyethyl (meth)acrylate, ethoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate; Phosphate (meth)acrylate, 2-(meth)acryloyloxyethyl acid phosphate, di-(2-methacryloyloxyethyl)-phosphate, 2-(meth)acryloyloxypropyl acid phosphate, 2-(meth)acryloyloxybutyl acid phosphate, acid phosphooxy polyoxypropylene glycol mono(meth)acrylate, acid phosphooxy polyoxyethylene glycol mono(meth)acrylate, butyrolactone-modified phosphate (meth)acrylate, valerolactone-modified phosphate (meth)acryloyloxy acrylate, propiolactone-modified phosphate (meth)acrylate, caprolactone-modified phosphate (meth)acrylate and other phosphoric acid-containing (meth)acrylates; aryl (meth)acrylates such as benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxytetraethylene glycol (meth)acrylate, nonylphenoxyethyl (meth)acrylate, nonylphenoxytetraethylene glycol (meth)acrylate and other aryl (meth)acrylates;(Meth)acrylate-based urethane prepolymers such as phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer; bisphenol A diglycidyl ether (meth)acrylic acid adduct, 2-hydroxy-3-phenoxypropyl (meth)acrylate, etc. Meth)acrylate epoxy esters; amino (meth)acrylates such as dimethylaminoethyl (meth)acrylate and dimethylaminopropyl (meth)acrylate; polyfunctional (meth)acrylates such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethylene glycol di(meth)acrylate, and diethylene glycol di(meth)acrylate; and the like. These acrylic compounds may be used alone or in appropriate combination of two or more.

[0060] In the examples described later, in Examples 8 to 14 and Comparative Examples 8 to 13, an acrylic resin having commercially available isoamyl acrylate, phenoxyethyl acrylate, 2-methacryloyloxyethyl acid phosphate, and phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer as monomers is used as the resin component (B).

[0061] Next, the specific structure of the urethane resin used as the resin component (B) in the present disclosure is not particularly limited. A representative example is a compound in which the isocyanate group of a known polyisocyanate compound is blocked (blocked polyisocyanate compound).

[0062] Specific examples of the polyisocyanate compound that can be used include aromatic isocyanate compounds such as phenylene diisocyanate, tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymethylene polyphenyl polyisocyanate, polyaryl polyisocyanate, tolidine diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate; ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, and dicyclohexyl isocyanate. Examples of the polyisocyanate compound include, but are not limited to, aliphatic polyisocyanate compounds such as silmethane diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, octamethylene diisocyanate, and trimethylhexamethylene diisocyanate; modified products of these polyisocyanate compounds containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, a uretdione group, a uretoimine group, an isocyanurate group, or an oxazolidone group; isocyanurate compounds (which may be classified as isocyanurate modified products) that are cyclized trimers of these polyisocyanate compounds; and the like.

[0063] Among these polyisocyanate compounds, for example, those containing a trinuclear or higher polymethylene polyphenyl polyisocyanate in its components can be used. In addition, a terminal isocyanate group-containing compound synthesized by reacting a polyisocyanate with a polyol by a known method can also be used as the urethane resin in the present disclosure. In this case, the polyol is not particularly limited, but general polyether polyols, polyester polyols, polycarbonate polyols, etc. can be suitably used.

[0064] Among these polyols, examples of polyether polyols (or polyalkylene polyols) include those obtained by adding ethylene dioxide, propylene oxide or butylene oxide to a polyhydric alcohol or a phenol compound such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, bisphenol A, hydrogenated bisphenol A, glycerin, trimethylolpropane, or pentaerythritol.

[0065] Examples of polyester polyols include those obtained by condensing polyhydric alcohols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanediol, and trimethylolpropane with polybasic acids such as malonic acid, succinic acid, adipic acid, phthalic acid, and terephthalic acid.

[0066] Examples of polycarbonate polyols include those obtained by reacting polyhydric alcohols or phenolic compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and bisphenol A with dimethyl carbonate, diphenyl carbonate, or phosgene.

[0067] In addition, the blocking agent for the polyisocyanate compound is not particularly limited, and specific examples thereof include imidazoles such as imidazole, 2-methylimidazole, pyrazole, 3-methylpyrazole, 3,5-dimethylpyrazole, and 1,2,4-triazole; phenols such as phenol, cresol, ethylphenol, n-propylphenol, isopropylphenol, n-butylphenol, octylphenol, nonylphenol, xylenol, diisopropylphenol, di-t-butylphenol, xylenol, chlorophenol, and ethylphenol; and oximes such as formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketone oxime (MEK oxime), methyl isobutyl ketone oxime (MIBK oxime), diacetyl monooxime, and cyclohexanone oxime.

[0068] In the present disclosure, each of the above-mentioned compounds used as the urethane resin may be used alone or in combination of two or more kinds.

[0069] Next, the specific structure of the silicone resin used as the resin component (B) in the present disclosure is not particularly limited, but a representative example is a known thermosetting silicone resin.

[0070] Specifically, for example, the skeletal structure may be a structure having one or more reactive functional groups, such as a silane, a silicone oligomer, a silicone resin, an organosiloxane, a diorganosiloxane, an organopolysiloxane, a diorganopolysiloxane, etc. The skeletal structure may be a linear structure or may have a branched chain.

[0071] Examples of the reactive functional group bonded to a silicon atom contained in the skeletal structure include, but are not limited to, a hydroxy group, an alkenyl group, a hydrogensilyl group, a (meth)acryloyl group, an epoxy group, an amino group, a carbinol group, a mercapto group, a carboxy group, a phenol group, etc. In addition, the skeletal structure may have a functional group such as an alkyl group, an alkenyl group, an aromatic group, etc. in addition to the reactive functional group.

[0072] The thermosetting silicone resin used as the resin component (B) in the present disclosure may have a single type of skeletal structure and a single type of reactive functional group, or may have multiple types of skeletal structures and multiple types of reactive functional groups. As described above, one or more reactive functional groups may be contained in one skeletal structure, in other words, one molecule of silicone resin (having any skeletal structure) may have at least one reactive functional group. The reactive functional group may be at the end of the skeletal structure, may be in the side chain, or may be at either the end or the side chain.

[0073] [Other ingredients] The conductive adhesive composition according to the present disclosure may contain components other than the (A) silver powder and the (B) resin component. As described above, typical examples of the components include a curing catalyst or a reaction initiator (polymerization initiator).

[0074] In the present disclosure, when an epoxy resin is used as the resin component (B), a curing agent is used for curing. The curing agent used in the present disclosure is not particularly limited as long as it can cure the above-mentioned epoxy resin.

[0075] Specific examples of the curing agent include acid anhydrides such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, and succinic anhydride; imidazoles such as imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-aminoethyl-2-methylimidazole, 1-methylimidazole, and 2-ethylimidazole; dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dimethylbehenylamine, dilaurylmonoethylamine, methyl Tertiary amines such as didecylamine, methyldioleylamine, triallylamine, triisopropanolamine, triethylamine, 3-(dibutylamino)propylamine, tri-n-octylamine, 2,4,6-trisdimethylaminomethylphenol, triethanolamine, methyldiethanolamine, and diazabicycloundecene; Lewis acids or compounds thereof containing boron fluoride such as boron trifluoride ethyl ether, boron trifluoride phenol, boron trifluoride piperidine, boron trifluoride acetate, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride monoethanolamine; amine adducts such as Amicure Series PN-23 or MY-24 available from Ajinomoto Fine-Techno Co., Ltd. and Fujicure Series FXR-1020 or FXR-1030 available from Fuji Chemical Industry Co., Ltd.; dicyandiamide; and the like.

[0076] These curing agents may be used alone or in combination of two or more. The amount or conditions of use of the curing agent are not particularly limited, and the curing agent may be used in a known amount or under known conditions.

[0077] In the examples described later, Examples 1 to 7 and Comparative Examples 1 to 7, 2-ethyl-4-methylimidazole was used as the curing catalyst (C).

[0078] In the present disclosure, when the curable composition that becomes the resin (B) is radically polymerized, such as an acrylic resin or a silicone resin, a radical reaction initiator (polymerization initiator) is used. The specific initiator is not particularly limited, but representative examples include organic peroxides and azo-based initiators.

[0079] Representative organic peroxides include peroxy esters such as t-butyl peroxy-2-ethylhexanoate, t-hexyl peroxy isopropyl monocarbonate, t-butyl peroxybenzoate, t-butyl peroxy neodecanoate, t-butyl peroxy laurate, t-butyl cumyl peroxide, t-butyl peroxy acetate, and 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate; ketone peroxides such as methyl ethyl ketone peroxide; hydroperoxides such as 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and p-menthane hydroperoxide; and dialkyl peroxides such as di-t-butyl peroxide.

[0080] Representative azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 1,1'-azobis-1-cyclohexanecarbonitrile, dimethyl-2,2'-azobisisobutyrate, 2-(carbamoylazo)isobutyronitrile, 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, azodi-t-octane, azodi-t-butane, and the like.

[0081] These initiators may be used alone or in combination of two or more. The amount or conditions of use of the initiator are not particularly limited, and the initiator may be used in a known amount or conditions. In the present disclosure, organic peroxides are more preferred initiators.

[0082] In the examples described later, Examples 8 to 14 and Comparative Examples 8 to 13, t-butylperoxy-2-ethylhexanoate was used as an initiator for the acrylic resin.

[0083] In addition, the conductive adhesive composition according to the present disclosure may contain, as necessary, various additives known in the field of conductive adhesive compositions in addition to the above-mentioned components ((A) silver powder and (B) resin component, as well as the curing catalyst or initiator. The additives are not particularly limited, but specific examples include solvents, leveling agents, antioxidants, ultraviolet absorbers, silane coupling agents, defoamers, viscosity adjusters, etc. These additives can be added within a range that does not interfere with the effects of the present disclosure.

[0084] [Production and Use of Conductive Adhesive Composition] The method for producing the conductive adhesive composition according to the present disclosure is not particularly limited, and a method known in the field of conductive adhesive compositions can be suitably used. A representative example is a method in which the above-mentioned components are mixed in a predetermined mixing ratio (based on mass) and made into a paste using a known kneading device. For example, a three-roll mill can be used as the kneading device.

[0085] In the conductive adhesive composition according to the present disclosure, as described above, it is preferable that the blending amount (content) of the (A) silver powder is relatively small. Specifically, the conductive adhesive composition according to the present disclosure has the (A) silver powder and the (B) resin component as basic components (solid contents). When the total amount of these basic components (solid contents) is taken as 100 mass%, the ratio of the (A) silver powder can be 70 mass% or less of the solid contents. The fact that the ratio of the (A) silver powder can be 70 mass% or less of the solid contents means that the content of the (A) silver powder in the conductive adhesive composition can be relatively small.

[0086] In addition, the method of forming a pattern that becomes a cured adhesive layer by the conductive adhesive composition according to the present disclosure is not particularly limited, and various known forming methods can be suitably used. Representative examples include printing methods such as screen printing, gravure printing, offset printing, inkjet printing, dispenser method, and dip method. Therefore, the conductive adhesive composition according to the present disclosure may be used by applying it to a substrate by a printer or dispenser.

[0087] The method of curing the conductive adhesive composition according to the present disclosure is not particularly limited, and a known heating method can be suitably used according to the type of (B) resin component (if necessary, the type of curing catalyst or initiator). In the examples described below, when preparing an evaluation sample, the conductive adhesive composition is applied to a substrate and heated at 200°C for 60 minutes using a hot air dryer, or heated at 150°C for 30 seconds using a hot plate. However, conditions such as the type of heater, heating temperature, or heating time can be appropriately selected according to various conditions associated with the use of the conductive adhesive composition. Therefore, it goes without saying that the present disclosure is not limited to the heating method of these examples. In addition, in the present disclosure, the method of measuring or evaluating various physical properties of the cured product of the conductive adhesive composition is not particularly limited, and the methods exemplified in the examples described below can be suitably used.

[0088] The conductive adhesive composition according to the present disclosure can be widely used for forming high-definition electrodes, wiring, etc., or bonding electronic components, etc. Specifically, the conductive adhesive composition can be suitably used for applications such as bonding solar cell modules, internal or external electrodes or bonding of chip-type electronic components, electrodes, wiring, or bonding of components used in RFID (Radio Frequency IDentification), electromagnetic shielding, vibrator bonding, membrane switches, touch panels, electroluminescence, etc.

[0089] The conductive adhesive composition according to the present disclosure can be particularly suitably applied to the field of solar cells among the above-mentioned applications. Specifically, the conductive adhesive composition according to the present disclosure can be suitably used, for example, for bonding solar cell modules.

[0090] Thus, the conductive adhesive composition according to the present disclosure contains (A) silver powder and (B) a resin component, and contains, as the silver powder (A), (a1) flaky silver powder and (a2) spherical silver powder, and the (a1) flaky silver powder has a thickness of 0.3 μm or less, an average particle size D50 in the range of 4 to 9 μm, and a BET specific surface area of ​​1.5 to 2.5 m. 2 / g, and (a2) the spherical silver powder has an average particle size D50 in the range of 0.01 to 3 μm and a BET specific surface area of ​​0.5 to 2.5 m 2 / g and has a tap density of 2 g / cm 3 Furthermore, the ratio of the (A) silver powder in the solid content is 70 mass % or less.

[0091] According to this configuration, since the (A) silver powder is a combination of the (a1) flake silver powder and the (a2) spherical silver powder, which satisfy the specified conditions, the conductive adhesive composition can achieve good electrical properties including connection resistance without impairing the conductivity even if the conductive adhesive composition contains a relatively small amount of the (A) silver powder. In addition, since it is possible to reduce the amount of expensive (A) silver powder used (mixture amount), it is possible to suppress or avoid high costs of the conductive adhesive composition.

[0092] In addition, in conventional conductive adhesive compositions, copper-containing powders such as copper powder or silver-coated copper powder may be used as the conductive powder in order to suppress high costs. In such copper-containing powders, there may be concerns about the reliability of the conductive adhesive composition due to oxidation of copper, etc. Therefore, conductive adhesive compositions using copper-containing powders tend to be difficult to use in applications requiring high reliability. In contrast, according to the above configuration, it is possible to reduce the blending amount (content) of (A) silver powder without using copper-containing powder, making it possible to use the composition in applications requiring high reliability. EXAMPLES

[0093] The present disclosure will be described more specifically based on examples and comparative examples, but the present invention is not limited thereto. Those skilled in the art can make various changes, modifications, and alterations without departing from the scope of the present invention. In addition, the evaluation method of (A) silver powder and the evaluation method of the cured product in the following examples were performed as follows.

[0094] [(A) Evaluation method of silver powder] (1) Average particle size D50 The average particle size D50 of (a1) flake silver powder and (a2) spherical silver powder shown in Table 1 was evaluated by laser diffraction. 0.3 g of the sample of (a1) flake silver powder or (a2) spherical silver powder was weighed into a 50 ml beaker, 30 ml of isopropyl alcohol was added, and the powder was dispersed by treating with an ultrasonic cleaner (manufactured by AS ONE Corporation, product name: USM-1) for 5 minutes, and the average particle size D50 was measured and evaluated using a Microtrack particle size distribution analyzer (manufactured by Nikkiso Co., Ltd., product name: Microtrack particle size distribution analyzer 9320-HRA X-100).

[0095] (2) Evaluation of BET specific surface area The BET specific surface area of ​​the (a1) flake silver powder or (a2) spherical silver powder shown in Table 1 was evaluated using a surface area analyzer (manufactured by Quanta Chrome, product name: Monosorb). 1 g of the (a1) flake silver powder or (a2) spherical silver powder sample was subjected to the surface area analyzer, and the specific surface area was measured and evaluated by the BET single-point method using nitrogen adsorption. In the BET specific surface area measurement, the degassing conditions before the measurement were 60°C for 10 minutes.

[0096] (3) Evaluation of apparent density The apparent density of (a1) flake silver powder or (a2) spherical silver powder shown in Table 1 was evaluated by the following calculation formula (1). (a1) flake silver powder or (a2) spherical silver powder was filled into a funnel, and dropped into a cup below while being lightly poked with a wire, and the cup was filled until the powder piled up. The piled up (a1) flake silver powder or (a2) spherical silver powder was scraped down flat along the top edge of the cup with a spatula, and the apparent density was calculated and evaluated by the following calculation formula (1). Apparent density = (cup mass + sample mass) - cup mass / cup volume (1)

[0097] (4) Evaluation of tap density The tap density of (a1) flake silver powder or (a2) spherical silver powder shown in Table 1 was evaluated using a tap density measuring device (manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd., product name: bulk specific gravity measuring device SS-DA-2) according to the following calculation formula (2). A 15 g sample of (a1) flake silver powder or (a2) spherical silver powder was weighed and placed in a 20 ml test tube, tapped 1,000 times with a drop of 20 mm, and the sample volume after tapping (cm) was measured using the tap density measuring device. 3 ) was measured, and the tap density was calculated and evaluated according to the following calculation formula (2). Tap density = sample mass / sample volume after tapping (2)

[0098] (5) Thickness evaluation The thickness of the (a1) flake silver powder shown in Table 1 was evaluated using a scanning electron microscope (manufactured by JEOL Ltd., product name: JSM-5500). A sample of the (a1) flake silver powder was observed with a scanning electron microscope, and 100 silver particles ((a1) flake silver powder) were randomly selected from an image magnified 20,000 times, and their thickness (minor diameter on the image) was measured. The thickness of the (a1) flake silver powder was evaluated by averaging the thicknesses of these 100 silver particles by number.

[0099] [Evaluation method of the cured product] (1) Conductor resistance evaluation The conductive adhesive composition of the example or comparative example was printed on an alumina substrate 12 using a printer as shown in Fig. 1 to form a print pattern 21. This print pattern 21 is composed of one wiring pattern 21a and five pad patterns 21d. The wiring pattern 21a has rectangular terminals 21b at both ends, and the wiring portion 21c is zigzag, with the aspect ratio of the wiring portion 21c being 75. The five pad patterns 21d are arranged in a row adjacent to the wiring pattern 21a, and each is a square of 2 mm x 2 mm.

[0100] Next, an aluminum rivet having a circular fixing surface with a diameter of 4 mm was placed on the pad pattern 21d (2 mm x 2 mm) on the alumina substrate 12. The alumina substrate 12 on which the rivet was placed was heated at 200°C for 60 minutes using a hot air dryer in Examples 1 to 7 and Comparative Examples 1 to 7, and at 150°C for 30 seconds using a hot plate in Examples 8 to 14 and Comparative Examples 8 to 13, to cure the conductive adhesive composition (printed pattern 21) (formation of a cured adhesive layer), and a test piece for evaluating conductivity and adhesive strength was obtained.

[0101] The conductivity of the cured adhesive layer was evaluated by the volume resistivity of the wiring pattern 21a of the test piece. Specifically, the film thickness of the wiring pattern 21a was measured with a surface roughness meter (Surfcom 480A, manufactured by Tokyo Seimitsu Co., Ltd.) and the electrical resistance was measured with a digital multimeter (R6551, manufactured by Advantest Corporation). The volume resistivity (Ω·cm) of the wiring pattern 21a was calculated based on the film thickness, electrical resistance, and aspect ratio of the wiring portion 21c, and this volume resistivity was evaluated as the resistance value (conductor resistance) of the cured adhesive layer.

[0102] (2) Evaluation method for connection resistance As shown in FIG. 3, the conductive adhesive composition of the example or comparative example was applied to a tin (Sn) plated substrate 31 using a dispenser to a diameter of 2.5 mm to form an adhesive layer 32. Then, a gold plated rivet 33 having a circular fixing surface with a diameter of 5 mm was laminated on the adhesive layer 32. At this time, a polyimide film having a thickness of 200 μm was used as a spacer to set the thickness of the adhesive layer to 200 μm. Next, in Examples 1 to 7 and Comparative Examples 1 to 7, the tin plated substrate 31 was heated at 200° C. for 60 minutes using a hot air dryer, and in Examples 8 to 14 and Comparative Examples 8 to 13, the adhesive layer 32 was cured to form a cured layer. In this way, a sample 30 for evaluating connection resistance was produced.

[0103] The electrical resistance between the tin-plated substrate 31 and the gold-plated rivet 33 in the evaluation sample 30 was measured with an electrical resistance meter 34 (digital multimeter, manufactured by Advantest Corporation, product name: R6551) and was taken as the connection resistance of the cured layer. If the measured connection resistance was less than 0.03 Ω, it was rated as "A", if it was 0.03 Ω or more and less than 0.05 Ω, it was rated as "B", and if it was 0.05 Ω or more, it was rated as "C".

[0104] (3) Evaluation of adhesive strength The adhesive strength of the cured adhesive layer was evaluated based on the adhesion of the rivet to the pad pattern 21d of the test piece described in (1) Evaluation of conductor resistance. Specifically, a horizontal shear force was applied to the rivet mounted on the pad pattern 21d, and the strength was measured when the rivet detached from the pad pattern 21d. The adhesive strength of the cured adhesive layer was evaluated as follows: "A" for a strength of 10 MPa, "B" for a strength of 5 MPa or more but less than 10 MPa, and "C" for a strength of less than 5 MPa.

[0105] [(A) Silver powder] In the conductive adhesive compositions according to the Examples and Comparative Examples, the (A) silver powder was used in appropriate combination with five types of (a1) flaky silver powder and four types of (a2) spherical silver powder shown in Table 1. In each Example or Comparative Example, the (A) silver powder is represented by the abbreviations shown in Table 1.

[0106] [Table 1]

[0107] [(B) resin component, (C) curing catalyst, (D) initiator] In the conductive adhesive compositions according to the examples and comparative examples, an appropriate combination of seven types of resins shown in Table 2 was used as the (B) resin component. To cure these resins, the (C) curing catalyst or (D) initiator shown in Table 2 was used. In each example or comparative example, the resins, curing catalysts, and initiators are represented by the abbreviations shown in Table 2, just like the (A) silver powder.

[0108] [Table 2]

[0109] Example 1 As the (A) silver powder, (a1) flaky silver powder with the abbreviation A-01 in Table 1 and (a2) spherical silver powder with the abbreviation A-11 were selected. As the (B) resin component, an epoxy resin with the abbreviation B-01, an epoxy resin with the abbreviation B-02, and a phenolic resin with the abbreviation B-03 in Table 2 were selected. Also, a (C) curing catalyst with the abbreviation C-01 shown in Table 2 was selected. These components were blended in the composition (blending ratio) shown in Table 3.

[0110] In Table 3 (and Tables 4 to 6 described below), the blending ratio of the two types of (A) silver powders is 100 mass% in total. In Example 1, the mass ratio ((a1) / (a2)) of the (a1) flaky silver powder to the (a2) spherical silver powder is 50 / 50.

[0111] In Table 3 (and Tables 4 to 6 described below), the composition of the (B) resin component is 100 mass% in total of the blending ratio of three types of resin. In Example 1, the mass ratio (B-01 / B-02 / B-03) of the epoxy resin with the abbreviation B-01, the epoxy resin with the abbreviation B-02, and the phenolic resin with the abbreviation B-03 is 50 / 20 / 25. In Table 3 (and Table 4 described below), the blending amount of the (C) curing catalyst is 1 part by mass for a total of 100 parts by mass of the (B) resin component.

[0112] Furthermore, in Table 3 (and Tables 4 to 6 described below), the blending ratio of (A) silver powder to (B) resin component is shown as a mass ratio. In Example 1, the mass ratio of the total amount of (A) silver powder to the total amount of (B) resin component (solid mass ratio (A) / (B)) is 70 / 30. The same applies to each of the following Examples and Comparative Examples.

[0113] The conductive adhesive composition of Example 1 was prepared (manufactured) by kneading the components (A) to (C) blended according to the composition shown in Table 3 using a three-roll mill.

[0114] Using the obtained conductive adhesive composition according to Example 1, as described above, samples for evaluating conductor resistance and connection resistance (and adhesive strength) were prepared (manufactured). Using these evaluation samples, the properties (conductor resistance, connection resistance, and adhesive strength) of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 3.

[0115] (Examples 2 to 4) The conductive adhesive compositions of Examples 2 to 4 were prepared (manufactured) in the same manner as Example 1, except that (a1) flake silver powder having the abbreviation A-02 was used with a solid content mass ratio (A) / (B) of 65 / 35 (Example 2), (a2) spherical silver powder having the abbreviation A-12 was used with a solid content mass ratio (A) / (B) of 65 / 35 (Example 3), or (a2) spherical silver powder having the abbreviation A-12 was used with a solid content mass ratio (A) / (B) of 65 / 35 (Example 4).

[0116] As described above, evaluation samples were prepared (manufactured) using the obtained conductive adhesive compositions according to Examples 2 to 4. Using these evaluation samples, the properties of the cured products of the conductive adhesive compositions were evaluated according to the evaluation methods described above. The results are shown in Table 3.

[0117] Example 5 The conductive adhesive composition of Example 5 was prepared (manufactured) in the same manner as in Example 1, except that the blending ratio of the silver powder (A) was (a1) / (a2) = 60 / 40 and the solid content mass ratio (A) / (B) was 60 / 40.

[0118] Using the obtained conductive adhesive composition according to Example 5, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 3.

[0119] Example 6 The conductive adhesive composition of Example 6 was prepared (manufactured) in the same manner as in Example 4, except that the blending ratio of the silver powder (A) was (a1) / (a2) = 60 / 40 and the solid content mass ratio (A) / (B) was 50 / 50.

[0120] Using the obtained conductive adhesive composition according to Example 6, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 3.

[0121] Example 7 The conductive adhesive composition of Example 7 was prepared (manufactured) in the same manner as in Example 1, except that the solid content mass ratio (A) / (B) was set to 40 / 60.

[0122] Using the obtained conductive adhesive composition according to Example 7, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 3.

[0123] [Table 3]

[0124] (Comparative Examples 1 and 2) The conductive adhesive compositions of Comparative Examples 1 and 2 were prepared (manufactured) in the same manner as in Example 1, except that either the (a2) spherical silver powder designated by the abbreviation A-13 (Comparative Example 1) or the (a2) spherical silver powder designated by the abbreviation A-14 (Comparative Example 2) was used.

[0125] As described above, evaluation samples were prepared (manufactured) using the obtained conductive adhesive composition according to Comparative Example 1 or 2. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 4.

[0126] Comparative Example 3 The conductive adhesive composition of Comparative Example 3 was prepared (manufactured) in the same manner as in Example 2, except that the solid mass ratio (A) / (B) was set to 70 / 30 and the spherical silver powder (a2) designated A-13 was used.

[0127] As described above, evaluation samples were prepared (manufactured) using the obtained conductive adhesive composition according to Comparative Example 3. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 4.

[0128] (Comparative Examples 4 and 5) The conductive adhesive compositions of Comparative Examples 4 and 5 were prepared (manufactured) in the same manner as in Example 1, except that either the (a1) flake silver powder designated A-03 (Comparative Example 4) or the (a1) flake silver powder designated A-04 (Comparative Example 5) was used.

[0129] As described above, evaluation samples were prepared (manufactured) using the obtained conductive adhesive composition according to Comparative Example 4 or 5. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 4.

[0130] Comparative Example 6 The conductive adhesive composition of Comparative Example 6 was prepared (manufactured) in the same manner as in Example 1, except that (a2) spherical silver powder was not used and two types of (a1) flaky silver powder, designated A-01 and A-05, were used instead.

[0131] Using the obtained conductive adhesive composition according to Comparative Example 6, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 4.

[0132] Comparative Example 7 The conductive adhesive composition of Comparative Example 7 was prepared (manufactured) in the same manner as in Comparative Example 5, except that the solid content mass ratio (A) / (B) was set to 90 / 10.

[0133] Using the obtained conductive adhesive composition according to Comparative Example 7, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 4.

[0134] [Table 4]

[0135] (Examples 8 to 11) As the (B) resin component, the acrylic resins designated by the abbreviations B-11, B-12, B-13, and B-14 in Table 2 were selected, and the (D) initiator designated by the abbreviation D-01 in Table 2 was selected, and these components were mixed in the composition (mixing ratio) shown in Table 5. A conductive adhesive composition according to Example 8 was prepared (manufactured) in the same manner as in Example 1, except for these compositions.

[0136] In Example 8, the mass ratio (B-11 / B-12 / B-13 / B-14) of the acrylic resins designated by the abbreviations B-11, B-12, B-13, and B-14 is 15 / 28 / 2 / 55 as shown in Table 5. In addition, in Table 5 (and Table 6 described later), the blending amount of the (D) initiator is 1 part by mass per 100 parts by mass of the (B) resin component in total.

[0137] Using the obtained conductive adhesive composition according to Example 8, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 5.

[0138] (Examples 9 to 11) The conductive adhesive compositions of Examples 9 to 11 were prepared (manufactured) in the same manner as in Example 8, except that the solid mass ratio (A) / (B) was set to 65 / 35, and either (a2) spherical silver powder with the abbreviation A-12 was used (Example 9), (a1) flaky silver powder with the abbreviation A-02 was used (Example 10), or (a1) flaky silver powder with the abbreviation A-02 and (a2) spherical silver powder with the abbreviation A-12 were used (Example 11).

[0139] Using the obtained conductive adhesive compositions according to Examples 9 to 11, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured products of the conductive adhesive compositions were evaluated according to the evaluation methods described above. The results are shown in Table 5.

[0140] Example 12 The conductive adhesive composition of Example 12 was prepared (manufactured) in the same manner as in Example 8, except that the mixing ratio of the silver powder (A) was (a1) / (a2) = 60 / 40 and the solid content mass ratio (A) / (B) was 50 / 50.

[0141] Using the obtained conductive adhesive composition according to Example 12, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 5.

[0142] Example 13 The conductive adhesive composition of Example 13 was prepared (manufactured) in the same manner as in Example 11, except that the blending ratio of the silver powder (A) was (a1) / (a2) = 55 / 45 and the solid content mass ratio (A) / (B) was 40 / 60.

[0143] Using the obtained conductive adhesive composition according to Example 13, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 5.

[0144] Example 14 The conductive adhesive composition of Example 14 was prepared (manufactured) in the same manner as in Example 8, except that the blending ratio of the silver powder (A) was (a1) / (a2) = 60 / 40 and the solid content mass ratio (A) / (B) was 30 / 70.

[0145] Using the obtained conductive adhesive composition according to Example 14, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 5.

[0146] [Table 5]

[0147] (Comparative Examples 8 and 9) The conductive adhesive composition of Comparative Example 8 or 8 was prepared (manufactured) in the same manner as in Example 8, except that the spherical silver powder designated by the abbreviation A-14 (a2) was used (Comparative Example 8) or the spherical silver powder designated by the abbreviation A-15 (a2) was used (Comparative Example 9).

[0148] Using the obtained conductive adhesive composition according to Comparative Example 8 or 9, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 6.

[0149] Comparative Example 10 The conductive adhesive composition of Comparative Example 10 was prepared (manufactured) in the same manner as in Example 10, except that the solid content mass ratio (A) / (B) was set to 70 / 30 and the spherical silver powder (a2) designated A-14 was used.

[0150] Using the obtained conductive adhesive composition according to Comparative Example 10, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured product of the conductive adhesive composition were evaluated by the evaluation method described above. The results are shown in Table 6.

[0151] (Comparative Examples 11 to 13) The conductive adhesive compositions of Comparative Examples 11 to 13 were prepared (manufactured) in the same manner as in Example 8, except that either (a1) flake silver powder having the abbreviation A-03 (Comparative Example 11), (a1) flake silver powder having the abbreviation A-04 (Comparative Example 12), or (a1) flake silver powder having the abbreviation A-04 with a solid content mass ratio (A) / (B) of 90 / 10 was used (Comparative Example 13).

[0152] As described above, evaluation samples were prepared (manufactured) using the obtained conductive adhesive compositions according to Comparative Examples 11 to 13. Using these evaluation samples, the properties of the cured products of the conductive adhesive compositions were evaluated by the evaluation methods described above. The results are shown in Table 6.

[0153] [Table 6]

[0154] (Comparison between Examples and Comparative Examples) As is clear from the results of Examples 1 to 7 and Examples 8 to 14, by using, as the silver powder (A), a combination of (a1) flaky silver powder and (a2) spherical silver powder that satisfy predetermined physical properties, the resulting cured product can achieve good conductor resistance, connection resistance, and adhesive strength.

[0155] In particular, as is clear from a comparison of the results of Examples 1 to 7 with the results of Examples 8 to 14, it is found that the obtained cured product can achieve good electrical properties and adhesive strength even when the type of the (B) resin component is an epoxy resin and a phenol resin, or when the (B) resin component is multiple types of acrylic resin.

[0156] In contrast, as is clear from a comparison of the results of Examples 1 to 4 with the results of Comparative Examples 1 to 3, or a comparison of the results of Examples 8 to 11 with the results of Comparative Examples 8 to 10, even if the (a1) flaky silver powder satisfies the specified physical properties, when the (a2) spherical silver powder does not satisfy the specified physical properties, the electrical characteristics (conductor resistance and connection resistance) in particular will be insufficient.

[0157] Furthermore, as is clear from a comparison of the results of Examples 1 to 4 with the results of Comparative Examples 4 and 5, or a comparison of the results of Examples 8 to 11 with the results of Comparative Examples 11 and 12, even if the (a2) spherical silver powder satisfies the specified physical properties, when the (a1) flaky silver powder does not satisfy the specified physical properties, the conductor resistance is particularly likely to be insufficient, and the connection resistance may also be insufficient.

[0158] In addition, from the results of Comparative Example 7 or Comparative Example 13, it can be seen that even if the (a1) flaky silver powder does not satisfy the specified physical properties, it is possible to realize good electrical properties by increasing the content of the (A) silver powder. However, from the results of Comparative Example 7 or Comparative Example 13, it can be seen that even if the electrical properties are good, it is difficult to improve the adhesive strength. This point is also considered to be the same when the (a2) spherical silver powder does not satisfy the specified physical properties.

[0159] In addition, as is clear from the comparison of the results of Examples 1 to 4 with the results of Examples 5 and 6, or the comparison of the results of Examples 8 to 11 with the results of Examples 12 to 14, it is found that the blending ratio (mixing ratio) of the (a1) flaky silver powder and the (a2) spherical silver powder that satisfies the specified physical properties is not limited to a narrow range. From these results, it is found that good electrical properties and good adhesive strength can be easily achieved as long as the blending ratio of the (a1) flaky silver powder and the (a2) spherical silver powder is within the range of 20 / 80 to 80 / 20, with the center being around (a1) / (a2)=1 / 1.

[0160] Furthermore, as is clear from a comparison of the results of Examples 1 to 7, or a comparison of the results of Examples 8 to 14, it can be seen that good electrical properties and good adhesive properties can be achieved within a wide range of the solid content mass ratio (A) / (B) of 70 / 30 to 30 / 70. These results show that when the solid content of the conductive adhesive composition, i.e., the sum of the total amount of the (A) silver powder and the (B) resin component, is taken as 100 mass%, it is possible to reduce the ratio of the (A) silver powder to 70 mass% or less.

[0161] The present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in different embodiments or multiple modified examples. [Industrial Applicability]

[0162] The present invention can be suitably used in a wide range of fields in which an adherend is bonded in a conductive manner in the fields of electric equipment and electronic equipment, and is particularly suitable for use in the field of manufacturing solar cell modules. [Explanation of symbols]

[0163] 10: Resin component 11: Flake silver powder 12: Flake silver powder 13: Spherical silver powder 20: Evaluation sample 21: Tin-plated substrate 22: Adhesive layer (or cured layer) 23: Gold-plated rivets 24: Electrical resistance meter

Claims

1. (A) silver powder and (B) a resin component; The (A) silver powder contains (a1) flake silver powder and (a2) spherical silver powder, The (a1) flake silver powder has a thickness of 0.3 μm or less, an average particle size D50 in the range of 4 to 9 μm, and a BET specific surface area of ​​1.5 to 2.5 m. 2 / g, The spherical silver powder (a2) has an average particle size D50 in the range of 0.01 to 3 μm and a BET specific surface area of ​​0.5 to 2.5 m. 2 / g and a tap density of 2 g / cm 3 is less than Further, the ratio of the (A) silver powder in the solid content is 70% by mass or less. An electrically conductive adhesive composition.

2. The (a1) flake silver powder and the (a2) spherical silver powder are blended in a mass ratio within the range of 20 / 80 to 80 / 20. The conductive adhesive composition of claim 1 .

3. The (B) resin component is a thermosetting resin and its curing agent or reaction initiator, The conductive adhesive composition of claim 1 .

4. The thermosetting resin is at least one resin selected from the group consisting of an epoxy resin, a phenolic resin, an acrylic resin, a urethane resin, and a silicone resin. The conductive adhesive composition according to claim 3 .

5. It is used by applying it to a substrate with a printer or dispenser. The conductive adhesive composition according to claim 1 .

6. Used for bonding electronic components, The conductive adhesive composition according to claim 1 .

7. The electronic component is a solar cell module. The conductive adhesive composition according to claim 6.

Citation Information

Patent Citations

  • Photocurable composition, conductive structure, and electronic component

    JP2017002267A

  • Conductive adhesive composition

    JP2022155933A

  • Conductive composition and solar cell

    WO2014013872A1

  • Conductive paste composition

    JP2004111057A