Method for manufacturing connection structure, and adhesive film for circuit connection

A film adhesive with specific viscosity is used for low-temperature, low-pressure bonding in COF mounting, addressing air bubble issues and enhancing alignment and productivity in circuit connections.

JP2024163714AInactive Publication Date: 2024-11-22RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023079558
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge in COF mounting is the difficulty in temporarily bonding a film adhesive to a panel at low temperature and low pressure for short time, which leads to air bubble generation around sensor marks, impairing alignment and design flexibility, and affecting productivity.

Method used

A method involving a film adhesive with a melt viscosity of 1000 to 2500 Pa·s at 70°C is used to temporarily bond circuit members, with a conductive particle-containing adhesive layer, allowing for low-temperature, low-pressure bonding to suppress air bubble generation and facilitate alignment.

Benefits of technology

The method effectively suppresses air bubble formation, enabling efficient alignment and connection of circuit members while maintaining design flexibility and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163714000005
    Figure 2024163714000005
  • Figure 2024163714000006
    Figure 2024163714000006
  • Figure 2024163714000007
    Figure 2024163714000007
Patent Text Reader

Abstract

To provide a method for manufacturing a connection structure in which generation of bubbles when a film-like adhesive is laminated on a circuit member can be sufficiently suppressed, and an adhesive film for circuit connection which can be used for the method.SOLUTION: Provided is a method for manufacturing connection structure in which a film-like adhesive is laid between a first circuit member having a first electrode and a second circuit member having a second electrode, and the first circuit member and the second circuit member are thermally compressed to electrically connect the first electrode and the second electrode with each other. The method comprises a temporary crimping step of preparing an adhesive film for circuit connection which has a first adhesive layer including conductive particles and a second adhesive layer laminated on the first adhesive layer, and includes film-like adhesive having a melt viscosity at 70°C of 1000 to 2500 Pa s, and laminating the film-like adhesive of the adhesive film for circuit connection on the first circuit member from the second adhesive layer side.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a connection structure and an adhesive film for circuit connection. [Background technology]

[0002] Driving ICs are mounted on panels of liquid crystal display devices and the like, and one of the mounting methods is COF (Chip-on-Film or Chip-on-Flexible) mounting. In COF mounting, a driving IC such as a semiconductor chip is bonded onto a film-like wiring circuit board, and these are then bonded to a glass panel. A film-like adhesive in which conductive particles are dispersed in an adhesive such as an anisotropic conductive film is used to bond the COF to the glass panel (for example, see Patent Document 1 below). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-289729 A Summary of the Invention [Problem to be solved by the invention]

[0004] In some cases, a sensor mark with a specific shape is provided near the wiring on the COF to align it with the glass panel to be joined. Position information can be obtained by detecting this sensor mark with a sensor such as a CCD camera.

[0005] Incidentally, in order to ensure workability and freedom in panel design, the COF and glass panel are generally joined by temporarily applying a film-like adhesive to the COF, and then heating and pressurizing the COF and glass panel, which are aligned so that the circuits that will become the connection parts face each other. It is difficult to temporarily apply a film-like adhesive to a panel in parts, and consolidating the connection parts in one place on the panel side reduces the freedom in designing wiring, etc. From the viewpoint of productivity, it is desirable to temporarily apply the film-like adhesive to the COF under conditions of low temperature, low pressure, and short time, but in this case, air bubbles are generated around the sensor mark part where the film-like adhesive is laminated, making the sensor mark part difficult to recognize.

[0006] Therefore, an object of the present invention is to provide a method for manufacturing a connection structure that can sufficiently suppress the generation of air bubbles when a film-like adhesive is laminated to a circuit component, and an adhesive film for circuit connection that can be used for the method. [Means for solving the problem]

[0007] The present invention provides the following inventions [1] to [3].

[0008] [1] A method for producing a connection structure, in which a film-like adhesive is interposed between a first circuit member having a first electrode and a second circuit member having a second electrode, and the first circuit member and the second circuit member are thermocompression-bonded to electrically connect the first electrode and the second electrode to each other, the method for producing a connection structure comprising: preparing an adhesive film for circuit connection, which has a first adhesive layer containing conductive particles and a second adhesive layer laminated on the first adhesive layer, and which comprises a film-like adhesive having a melt viscosity of 1000 to 2500 Pa s at 70°C; and a pre-compression bonding step of laminating the film-like adhesive of the adhesive film for circuit connection onto the first circuit member from the side of the second adhesive layer. [2] A method for manufacturing a connection structure as described in [1] above, in which the first circuit member has a flexible substrate, a first electrode and a sensor mark portion are provided on the flexible substrate, and in a pre-pressure bonding process, a film-like adhesive covers the first electrode and the sensor mark portion. [3] An adhesive film for circuit connection comprising: a peelable support film; and a film-like adhesive having a first adhesive layer containing conductive particles provided on the support film and a second adhesive layer laminated to the first adhesive layer, the film-like adhesive having a melt viscosity of 1000 to 2500 Pa s at 70°C. Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for producing a connection structure that can sufficiently suppress the generation of air bubbles when a film-like adhesive is laminated to a circuit component, and an adhesive film for circuit connection that can be used for the same.

[0010] According to the manufacturing method of the connection structure of the present invention, even when a film-like adhesive is temporarily bonded to a circuit component under conditions of low temperature, low pressure, and short time (e.g., 70°C, 1 MPa, and 1 second), the generation of air bubbles can be sufficiently suppressed, and the circuit components can be aligned and efficiently connected using the sensor mark portion. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of an adhesive film for circuit connection. [Diagram 2] 2A to 2C are schematic cross-sectional views showing steps in a method for producing a circuit connection structure using the adhesive film shown in FIG. [Diagram 3] 3 is a schematic cross-sectional view showing a process subsequent to that shown in FIG. 2. [Figure 4] 4 is a schematic cross-sectional view showing a process subsequent to that shown in FIG. 3. [Diagram 5] 5 is a schematic cross-sectional view showing a connection structure obtained through the steps of FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings as needed. In this specification, the upper limit and lower limit values ​​described individually can be arbitrarily combined. In addition, in this specification, "(meth)acrylate" means at least one of acrylate and the corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl".

[0013] [Method of manufacturing circuit connection structure] The method for manufacturing a circuit connection structure of the present embodiment is a method for manufacturing a connection structure in which a film-like adhesive is interposed between a first circuit member having a first electrode and a second circuit member having a second electrode, and the first circuit member and the second circuit member are thermocompression-bonded to electrically connect the first electrode and the second electrode to each other, and the method includes a pre-compression bonding step of preparing an adhesive film for circuit connection having a first adhesive layer containing conductive particles and a second adhesive layer laminated on the first adhesive layer, the adhesive film comprising a film-like adhesive having a melt viscosity of 1000 to 2500 Pa·s at 70°C, and laminating the film-like adhesive of the adhesive film for circuit connection from the second adhesive layer side to the first circuit member.

[0014] First, the adhesive film for circuit connection will be described.

[0015] <Adhesive film for circuit connection> Fig. 1 is a schematic cross-sectional view showing one embodiment of an adhesive film for circuit connection. As shown in Fig. 1, an adhesive film for circuit connection 11 (hereinafter also simply referred to as "adhesive film 11") includes a peelable support film 12, and a film-like adhesive 15 having a first adhesive layer 13 provided on the support film 12 and a second adhesive layer 14 laminated on the first adhesive layer 13. The first adhesive layer 13 contains conductive particles P.

[0016] In the adhesive film 11, conductive particles P are dispersed in the first adhesive layer 13. Therefore, the adhesive film 11 is an anisotropically conductive adhesive film having anisotropic conductivity. The adhesive film 11 is used to electrically connect the first electrode and the second electrode to each other by interposing a film-like adhesive 15 (first adhesive layer and second adhesive layer) between a first circuit member having a first electrode and a second circuit member having a second electrode and thermocompressing the first circuit member and the second circuit member.

[0017] Furthermore, when the circuit component to be connected has a flexible substrate, the film-like adhesive 15 of the circuit connection adhesive film 11 can be attached to the first circuit component so that the second adhesive layer is in contact with the first circuit component.

[0018] In this embodiment, the thickness of the first adhesive layer 13 may be 0.1 to 1.0 times, and more preferably 0.1 to 0.7 times, the average particle size of the conductive particles P. In the first adhesive layer 13, 90% or more of the conductive particles P may be separated from other conductive particles.

[0019] In this embodiment, the melt viscosity of the film-like adhesive 15 at 70° C. is 1000 to 2500 Pa·s. In this specification, the melt viscosity of the film-like adhesive at 70° C. is measured by the following procedure.

[0020] The film-like adhesives are laminated together to prepare a 600 μm thick laminate for measurement. This laminate for measurement is measured using a shear viscoelasticity measuring device (manufactured by TA Instruments, product name: ARES-G2) at a heating rate of 10° C. / min, a measuring frequency of 10 Hz, and a measuring temperature of 40 to 200° C., and the melt viscosity at 70° C. is derived.

[0021] The melt viscosity of the film-like adhesive at 70° C. may be 1000 to 2000 Pa·s, 1000 to 1500 Pa·s, or 1500 to 2000 Pa·s, from the viewpoint of suppressing the generation of bubbles during temporary pressure bonding.

[0022] (Support film) The support film 12 is formed of, for example, polyethylene terephthalate (PET), polyethylene, polypropylene, or the like. The support film 12 may contain any filler. The surface of the support film 12 may be subjected to a release treatment, a plasma treatment, or the like. The support film 12 can be peeled off after the film-like adhesive 15 (the first adhesive layer and the second adhesive layer) is transferred to the circuit member.

[0023] (First adhesive layer) The first adhesive layer is, for example, made of a cured product of a first curable composition. The first curable composition may be a photocurable composition, a thermosetting composition, or a mixture of a photocurable composition and a thermosetting composition. The first curable composition contains, for example, (A) a polymerizable compound (hereinafter also referred to as "(A) component"), (B) a polymerization initiator (hereinafter also referred to as "(B) component"), and (C) conductive particles (hereinafter also referred to as "(C) component"). When the first curable composition is a photocurable composition, the first curable composition contains a photopolymerization initiator as the (B) component, and when the first curable composition is a thermosetting composition, the first curable composition contains a thermal polymerization initiator as the (B) component. Such a first adhesive layer can be obtained, for example, by irradiating a layer made of the first curable composition with light or heating to polymerize the (A) component and cure the first curable composition. That is, the first adhesive layer may be composed of conductive particles and an adhesive component obtained by photocuring the first curable composition. The first adhesive layer may be a cured product obtained by completely curing the first curable composition, or may be a cured product obtained by partially curing the first curable composition. That is, when the first curable composition contains the (A) component and the (B) component, the adhesive component may or may not contain unreacted (A) component and (B) component. The first adhesive layer may be composed of a resin composition other than the cured product of the curable composition. For example, the first adhesive layer may be composed of a resin composition containing a resin component such as a phenoxy resin such as PKHC, a polyester urethane resin, a polyurethane resin, or an acrylic rubber.

[0024] [Component (A): Polymerizable compound] The component (A) is a compound that is polymerized by, for example, radicals, cations, or anions generated by a polymerization initiator (photopolymerization initiator or thermal polymerization initiator) upon irradiation with light (e.g., ultraviolet light) or heating. The component (A) may be any of a monomer, oligomer, and polymer. As the component (A), one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0025] The (A) component has at least one or more polymerizable groups. The polymerizable group is, for example, a group containing a polymerizable unsaturated double bond (ethylenically unsaturated bond). The polymerizable group is preferably a radically polymerizable group that reacts with a radical, from the viewpoint of easily obtaining a desired melt viscosity, from the viewpoint of preventing peeling between the circuit member and the circuit connection part in a high-temperature and high-humidity environment, and from the viewpoint of further improving the effect of reducing the connection resistance and providing better connection reliability. That is, the (A) component is preferably a radically polymerizable compound. Examples of the radically polymerizable group include a vinyl group, an allyl group, a styryl group, an alkenyl group, an alkenylene group, a (meth)acryloyl group, and a maleimide group. The number of polymerizable groups in the (A) component may be 2 or more from the viewpoint of easily obtaining a desired melt viscosity after polymerization and from the viewpoint of easily controlling the physical properties of the resin after curing, and may be 10 or less from the viewpoint of suppressing curing shrinkage during polymerization. In order to balance the crosslink density and cure shrinkage, a polymerizable compound having a number of polymerizable groups within the above range may be used, and then a polymerizable compound having a number outside the above range may be additionally used.

[0026] Specific examples of the component (A) include (meth)acrylate compounds, maleimide compounds, vinyl ether compounds, allyl compounds, styrene derivatives, acrylamide derivatives, nadimide derivatives, natural rubber, isoprene rubber, butyl rubber, nitrile rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, and carboxylated nitrile rubber.

[0027] Examples of (meth)acrylate compounds include epoxy (meth)acrylate, (poly)urethane (meth)acrylate, methyl (meth)acrylate, polyether (meth)acrylate, polyester (meth)acrylate, polybutadiene (meth)acrylate, silicone acrylate, ethyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-hexyl (meth)acrylate, and 2-methylethyl (meth)acrylate. Acrylate, 2-hydroxyethyl (meth)acrylate, isopropyl (meth)acrylate, hydroxypropyl (meth)acrylate, isobutyl (meth)acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, isooctyl (meth)acrylate, n-lauryl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-(meth)acryloyloxyethyl phosphate, N,N-di Methylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, polyethylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, neo Pentyl glycol di(meth)acrylate, pentaerythritol (meth)acrylate, dipentaerythritol hexa(meth)acrylate, isocyanuric acid modified bifunctional (meth)acrylate, isocyanuric acid modified trifunctional (meth)acrylate, tricyclodecanyl acrylate, dimethylol-tricyclodecane diacrylate, 2-hydroxy-1,3-diacryloxypropane, 2,2-bis[4-(acryloxymethoxy)phenyl]propane, 2,2-bis[4-(acryloxypolyethoxy)phenyl]propane, 2,Examples include 2-di(meth)acryloyloxydiethyl phosphate and 2-(meth)acryloyloxyethyl acid phosphate.

[0028] Examples of the maleimide compound include 1-methyl-2,4-bismaleimidebenzene, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, N,N'-m-toluylene bismaleimide, N,N'-4,4-biphenylene bismaleimide, N,N'-4,4-(3,3'-dimethyl-biphenylene) bismaleimide, N,N'-4,4-(3,3'-dimethyldiphenylmethane) bismaleimide, N,N'-4,4-(3,3'-diethyldiphenylmethane) bismaleimide, N,N'-4,4-diphenylmethane bismaleimide, and N,N'-4,4-diphenylpropane. Examples of the bismaleimide include propane bismaleimide, N,N'-4,4-diphenyl ether bismaleimide, N,N'-3,3-diphenyl sulfone bismaleimide, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, 2,2-bis(3-s-butyl-4-8(4-maleimidophenoxy)phenyl)propane, 1,1-bis(4-(4-maleimidophenoxy)phenyl)decane, 4,4'-cyclohexylidene-bis(1-(4maleimidophenoxy)-2-cyclohexylbenzene, and 2,2'-bis(4-(4-maleimidophenoxy)phenyl)hexafluoropropane.

[0029] Examples of the vinyl ether compound include diethylene glycol divinyl ether, dipropylene glycol divinyl ether, cyclohexane dimethanol divinyl ether, and trimethylolpropane trivinyl ether.

[0030] Examples of the allyl compound include 1,3-diallyl phthalate, 1,2-diallyl phthalate, and triallyl isocyanurate.

[0031] The (A) component is preferably a (meth)acrylate compound from the viewpoint of easily obtaining a desired melt viscosity and from the viewpoint of being able to select from compounds with various structures and being easily available. The (A) component may be a (poly)urethane (meth)acrylate compound (urethane (meth)acrylate compound or polyurethane (meth)acrylate compound) from the viewpoint of obtaining further excellent adhesive properties. The (A) component may be a (meth)acrylate compound having a high Tg skeleton such as a dicyclopentadiene skeleton from the viewpoint of obtaining further excellent adhesive properties.

[0032] From the viewpoint of easily obtaining a desired melt viscosity, and from the viewpoint of balancing the crosslink density and the cure shrinkage, further reducing the connection resistance, and improving the connection reliability, the (A) component may be a compound (e.g., polyurethane (meth)acrylate) in which a polymerizable group such as a vinyl group, an allyl group, or a (meth)acryloyl group is introduced into the end or side chain of a thermoplastic resin such as an acrylic resin, a phenoxy resin, or a polyurethane resin. In this case, the weight average molecular weight of the (A) component may be 3000 or more, 5000 or more, or 10,000 or more, from the viewpoint of excellent balance between the crosslink density and the cure shrinkage. In addition, the weight average molecular weight of the (A) component may be 1,000,000 or less, 500,000 or less, or 250,000 or less, from the viewpoint of excellent compatibility with other components. The weight average molecular weight refers to a value measured using a calibration curve of standard polystyrene by gel permeation chromatography (GPC) according to the conditions described in the examples.

[0033] The component (A) preferably contains, as a (meth)acrylate compound, a radically polymerizable compound having a phosphate structure represented by the following general formula (1): In this case, the adhesive strength to the surface of an inorganic material (metal, etc.) is improved, making it suitable for bonding electrodes (for example, circuit electrodes), for example. [ka] [In the formula, n represents an integer of 1 to 3, and R represents a hydrogen atom or a methyl group.]

[0034] The radical polymerizable compound having the phosphoric acid ester structure can be obtained, for example, by reacting phosphoric anhydride with 2-hydroxyethyl (meth)acrylate. Specific examples of the radical polymerizable compound having the phosphoric acid ester structure include mono(2-(meth)acryloyloxyethyl)acid phosphate, di(2-(meth)acryloyloxyethyl)acid phosphate, etc.

[0035] The content of the (A) component may be 5% by mass or more, 10% by mass or more, or 20% by mass or more based on the total mass of the first curable composition from the viewpoint of easily obtaining a desired melt viscosity and a desired physical property of the cured product. The content of the (A) component may be 90% by mass or less, 80% by mass or less, or 70% by mass or less based on the total mass of the first curable composition from the viewpoint of suppressing cure shrinkage during polymerization.

[0036] [Component (B): Polymerization initiator] The (B) component may be a photopolymerization initiator (photoradical polymerization initiator, photocationic polymerization initiator, or photoanionic polymerization initiator) that generates radicals, cations, or anions by irradiation with light having a wavelength in the range of 150 to 750 nm, preferably light having a wavelength in the range of 254 to 405 nm, and more preferably light having a wavelength of 365 nm (for example, ultraviolet light), or may be a thermal polymerization initiator (thermal radical polymerization initiator, thermal cationic polymerization initiator, or thermal anionic polymerization initiator) that generates radicals, cations, or anions by heat. The (B) component is preferably a radical polymerization initiator (photoradical polymerization initiator or thermal radical polymerization initiator) from the viewpoint of easily obtaining a desired melt viscosity, further improving the effect of reducing the connection resistance and providing better connection reliability, and making it easier to cure at low temperature and in a short time. As the (B) component, one type of compound may be used alone, or multiple types of compounds may be used in combination. For example, the first curable composition may contain both a photopolymerization initiator and a thermal polymerization initiator as the (B) component.

[0037] The photoradical polymerization initiator is decomposed by light to generate free radicals. That is, the photoradical polymerization initiator is a compound that generates radicals by applying light energy from the outside. Examples of the photoradical polymerization initiator include compounds having an oxime ester structure, a bisimidazole structure, an acridine structure, an α-aminoalkylphenone structure, an aminobenzophenone structure, an N-phenylglycine structure, an acylphosphine oxide structure, a benzyl dimethyl ketal structure, an α-hydroxyalkylphenone structure, and the like. From the viewpoint of easily obtaining a desired melt viscosity and from the viewpoint of being more excellent in the effect of reducing the connection resistance, the photoradical polymerization initiator preferably has at least one structure selected from the group consisting of an oxime ester structure, an α-aminoalkylphenone structure, and an acylphosphine oxide structure.

[0038] Specific examples of compounds having an oxime ester structure include 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-o-benzoyloxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime, 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(o-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), and the like.

[0039] Specific examples of compounds having an α-aminoalkylphenone structure include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-morpholinophenyl)-butanone-1, and the like.

[0040] Specific examples of the compound having an acylphosphine oxide structure include bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.

[0041] The thermal radical polymerization initiator decomposes by heat to generate free radicals. That is, the thermal radical polymerization initiator is a compound that generates radicals by applying thermal energy from the outside. The thermal radical polymerization initiator can be arbitrarily selected from conventionally known organic peroxides and azo compounds. From the viewpoints of stability, reactivity, and compatibility, the thermal radical polymerization initiator is preferably an organic peroxide having a one-minute half-life temperature of 90 to 175°C and a weight average molecular weight of 180 to 1000. By having the one-minute half-life temperature in this range, the storage stability is further excellent, the radical polymerizability is sufficiently high, and curing in a short time is possible.

[0042] Specific examples of organic peroxides include 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, cumyl peroxyneodecanoate, dilauroyl peroxide, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, 1,1,3,3-Tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, t-amylperoxy-3,5,5-trimethylhexanoate peroxyneodecanoate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, t-amyl peroxyneodecanoate, t-amyl peroxy-2-ethylhexanoate, di(3-methylbenzoyl) peroxide, dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate peroxybenzoate, 2,5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxybenzoate, dibutyl peroxytrimethyladipate, t-amyl peroxy normal octoate, t-amyl peroxy isononanoate, and t-amyl peroxybenzoate.

[0043] Specific examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile).

[0044] The content of the (B) component may be 0.1 mass% or more, or 0.5 mass% or more, based on the total mass of the first curable composition, from the viewpoint of excellent fast curing property and excellent effect of reducing connection resistance. The content of the (B) component may be 15 mass% or less, 10 mass% or less, or 5 mass% or less, based on the total mass of the first curable composition, from the viewpoint of improving storage stability and excellent effect of reducing connection resistance.

[0045] From the viewpoint of easily obtaining the desired viscosity, the first curable composition preferably contains at least one of a photopolymerization initiator and a thermal polymerization initiator as component (B), and from the viewpoint of facilitating the production of the adhesive film for circuit connection, it is more preferable for the first curable composition to contain a photopolymerization initiator.

[0046] [(C) Component: Conductive particles] The component (C) is not particularly limited as long as it is a particle having electrical conductivity, and may be a metal particle composed of a metal such as Au, Ag, Ni, Cu, or solder, or a conductive carbon particle composed of conductive carbon. The component (C) may be a coated conductive particle having a core containing non-conductive glass, ceramic, plastic (polystyrene, etc.), and a coating layer containing the above metal or conductive carbon and coating the core. Among these, metal particles formed of a heat-fusible metal, or coated conductive particles having a core containing a plastic and a coating layer containing a metal or conductive carbon and coating the core are preferably used. In this case, since the cured product of the first curable composition can be easily deformed by heating or pressure, when the electrodes are electrically connected to each other, the contact area between the electrodes and the component (C) can be increased, and the conductivity between the electrodes can be further improved.

[0047] The (C) component may be an insulating coated conductive particle comprising the above-mentioned metal particle, conductive carbon particle, or coated conductive particle, and an insulating layer containing an insulating material such as resin and coating the surface of the particle. When the (C) component is an insulating coated conductive particle, even if the content of the (C) component is high, the particle surface is coated with resin, so that the occurrence of a short circuit due to contact between the (C) components can be suppressed, and the insulation between adjacent electrode circuits can also be improved. The (C) component is used as one type of the above-mentioned various conductive particles alone or in combination of two or more types.

[0048] The maximum particle size of the (C) component must be smaller than the minimum distance between the electrodes (the shortest distance between adjacent electrodes). From the viewpoint of excellent dispersibility and electrical conductivity, the maximum particle size of the (C) component may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and electrical conductivity, the maximum particle size of the (C) component may be 50 μm or less, 30 μm or less, or 20 μm or less. In this specification, the particle size of 300 arbitrary conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the largest value obtained is defined as the maximum particle size of the (C) component. Note that, when the (C) component has protrusions or the like and is not spherical, the particle size of the (C) component is defined as the diameter of a circle circumscribing the conductive particle in the SEM image.

[0049] From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (C) component may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (C) component may be 50 μm or less, 30 μm or less, or 20 μm or less. In this specification, the particle size of 300 arbitrary conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the average value of the particle sizes obtained is defined as the average particle size.

[0050] In the first adhesive layer, the component (C) is preferably uniformly dispersed. From the viewpoint of obtaining a stable connection resistance, the particle density of the component (C) in the first adhesive layer is preferably 100 pcs / mm 2 It may be more than 1000pcs / mm 2 More than 2000pcs / mm 2 From the viewpoint of improving the insulating properties between adjacent electrodes, the particle density of the component (C) in the first adhesive layer may be 100,000 pcs / mm 2 may be less than 50000pcs / mm 2 It may be less than 10000pcs / mm 2 It may be the following:

[0051] The content of the (C) component may be 0.1 volume % or more, 1 volume % or more, or 5 volume % or more based on the total volume in the first adhesive layer from the viewpoint of further improving the electrical conductivity. The content of the (C) component may be 50 volume % or less, 30 volume % or less, or 20 volume % or less based on the total volume in the first adhesive layer from the viewpoint of easily suppressing short circuits. The content of the (C) component in the first curable composition (based on the total volume of the first curable composition) may be the same as the above range.

[0052] [Other ingredients] The first curable composition may further contain other components in addition to the components (A), (B) and (C). Examples of the other components include a thermoplastic resin, a coupling agent and a filler. These components may be contained in the first adhesive layer.

[0053] Examples of the thermoplastic resin include phenoxy resin, polyester resin, polyamide resin, polyurethane resin, polyester urethane resin, and acrylic rubber. When the first curable composition contains a thermoplastic resin, the first adhesive layer can be easily formed. When the first curable composition contains a thermoplastic resin, the stress of the first adhesive layer generated during curing of the first curable composition can be alleviated. When the thermoplastic resin has a functional group such as a hydroxyl group, the adhesion of the first adhesive layer is likely to be improved. The content of the thermoplastic resin may be, for example, 5% by mass or more and 80% by mass or less based on the total mass of the first curable composition.

[0054] Examples of the coupling agent include silane coupling agents having organic functional groups such as (meth)acryloyl groups, mercapto groups, amino groups, imidazole groups, and epoxy groups, silane compounds such as tetraalkoxysilanes, tetraalkoxytitanate derivatives, and polydialkyltitanate derivatives. When the first curable composition contains a coupling agent, the adhesiveness can be further improved. The content of the coupling agent may be, for example, 0.1% by mass or more and 20% by mass or less based on the total mass of the first curable composition.

[0055] Examples of the filler include non-conductive fillers (e.g., non-conductive particles). When the first curable composition contains a filler, further improvement in connection reliability can be expected. The filler may be either an inorganic filler or an organic filler. Examples of the inorganic filler include inorganic fine particles such as metal oxide fine particles such as silica fine particles, alumina fine particles, silica-alumina fine particles, titania fine particles, and zirconia fine particles; and nitride fine particles. Examples of the organic filler include organic fine particles such as silicone fine particles, methacrylate-butadiene-styrene fine particles, acrylic-silicone fine particles, polyamide fine particles, and polyimide fine particles. These fine particles may have a uniform structure or a core-shell structure. The maximum diameter of the filler is preferably less than the minimum particle diameter of the conductive particles. The content of the filler may be, for example, 0.1% by volume or more and 50% by volume or less based on the total volume of the first curable composition.

[0056] The first curable composition may contain other additives such as a softener, an accelerator, an anti-degradant, a colorant, a flame retardant, a thixotropic agent, etc. The content of these additives may be, for example, 0.1 to 10 mass% based on the total mass of the first curable composition. These additives may be contained in the first adhesive layer.

[0057] The first curable composition may contain a thermosetting resin instead of the (A) and (B) components, or in addition to the (A) and (B) components. The thermosetting resin is a resin that is cured by heat and has at least one thermosetting group. The thermosetting resin is, for example, a compound that crosslinks by reacting with a curing agent by heat. As the thermosetting resin, one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0058] The thermosetting group may be, for example, an epoxy group, an oxetane group, an isocyanate group, or the like, from the viewpoint of easily obtaining a desired melt viscosity and further improving the effect of reducing connection resistance and providing more excellent connection reliability.

[0059] Specific examples of thermosetting resins include epoxy resins such as bisphenol-type epoxy resins which are reaction products of epichlorohydrin with bisphenol A, F, AD, or the like; epoxy novolac resins which are reaction products of epichlorohydrin with phenol novolac, cresol novolac, or the like; naphthalene-based epoxy resins having a skeleton containing a naphthalene ring; and various epoxy compounds having two or more glycidyl groups in one molecule, such as glycidyl amine and glycidyl ether.

[0060] When a thermosetting resin is used instead of the components (A) and (B), the content of the thermosetting resin in the first curable composition may be, for example, 20 mass% or more and 80 mass% or less based on the total mass of the first curable composition. When a thermosetting resin is used in addition to the components (A) and (B), the content of the thermosetting resin in the first curable composition may be, for example, 30 mass% or more and 70 mass% or less based on the total mass of the first curable composition.

[0061] When the first curable composition contains a thermosetting resin, the first curable composition may contain the above-mentioned curing agent for the thermosetting resin. Examples of the curing agent for the thermosetting resin include a thermal radical generator, a thermal cation generator, and a thermal anion generator. The content of the curing agent may be, for example, 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the thermosetting resin.

[0062] The first adhesive layer may contain components derived from the first curable composition, such as unreacted (A) component and (B) component. The content of the (B) component in the first adhesive layer may be 15% by mass or less, 10% by mass or less, or 5% by mass or less, based on the total mass of the first adhesive layer. The content of the (B) component in the first adhesive layer may be 0.1% by mass or more, based on the total mass of the first adhesive layer.

[0063] The thickness of the first adhesive layer may be 0.1 times or more, 0.2 times or more, or 0.3 times or more of the average particle size of the conductive particles, from the viewpoint of making the conductive particles more easily trapped between the electrodes and further reducing the connection resistance. The thickness of the first adhesive layer may be 1.0 times or less, 0.8 times or less, or 0.7 times or less of the average particle size of the conductive particles, from the viewpoint of making the conductive particles more easily crushed when sandwiched between the opposing electrodes during thermocompression bonding and further reducing the connection resistance. From these viewpoints, the thickness of the first adhesive layer may be 0.1 to 0.7 times, 0.2 to 0.8 times, or 0.3 to 0.7 times the average particle size of the conductive particles. The thickness of the adhesive layer refers to the thickness of the adhesive layer located in the space between adjacent conductive particles. When the thickness of the first adhesive layer and the average particle size of the conductive particles satisfy the above-mentioned relationship, for example, as shown in Fig. 1, some of the conductive particles P in the first adhesive layer 13 may protrude from the first adhesive layer 13 toward the second adhesive layer 14. In this case, the boundary S between the first adhesive layer 13 and the second adhesive layer 14 is located in the space between adjacent conductive particles P. The conductive particles P are not exposed on the surface of the first adhesive layer 13 opposite the second adhesive layer 14, and the opposite surface may be a flat surface.

[0064] The thickness of the first adhesive layer may be appropriately set according to the height of the electrodes of the circuit members to be bonded. The thickness of the first adhesive layer may be, for example, 0.5 μm or more and 20 μm or less. In addition, when a part of the conductive particles is exposed from the surface of the first adhesive layer (for example, protruding to the second adhesive layer side), the distance from the surface of the first adhesive layer opposite to the second adhesive layer side to the boundary S between the first adhesive layer and the second adhesive layer located in the spaced portion between the adjacent conductive particles is the thickness of the first adhesive layer, and the exposed portion of the conductive particles is not included in the thickness of the first adhesive layer. The length of the exposed portion of the conductive particles may be, for example, 0.1 μm or more and 20 μm or less. The thickness of the adhesive layer can be measured by the following method. The adhesive film was sandwiched between two pieces of glass (thickness: approximately 1 mm) and a resin composition consisting of 100 g of bisphenol A type epoxy resin (product name: JER811, manufactured by Mitsubishi Chemical Corporation) and 10 g of a hardener (product name: Epomount Hardener, manufactured by Refine Tech Co., Ltd.) was poured into the mold. The cross section was then polished using a polishing machine, and the thickness of each adhesive layer was measured using a scanning electron microscope (SEM, product name: SE-8020, manufactured by Hitachi High-Tech Science Corporation).

[0065] (Second adhesive layer) The second adhesive layer is, for example, made of a second curable composition. The second curable composition contains, for example, (a) a polymerizable compound (hereinafter also referred to as (a) component) and (b) a polymerization initiator (hereinafter also referred to as (b) component). The second curable composition may be a thermosetting composition containing a thermal polymerization initiator as the (b) component, a photocurable composition containing a photopolymerization initiator as the (b) component, or a mixture of a thermosetting composition and a photocurable composition. The second curable composition constituting the second adhesive layer is an uncured curable composition that can flow when a circuit is connected, for example, an uncured curable composition.

[0066] [Component (a): Polymerizable compound] The component (a) is a compound that polymerizes, for example, by radicals, cations, or anions generated by a polymerization initiator (photopolymerization initiator or thermal polymerization initiator) upon irradiation with light (e.g., ultraviolet light) or heating. As the component (a), the compounds exemplified as the component (A) can be used. From the viewpoints of facilitating connection at low temperature in a short time and making it easier to obtain a desired melt viscosity, and of further improving the effect of reducing connection resistance and providing superior connection reliability, the component (a) is preferably a radically polymerizable compound having a radically polymerizable group that reacts with a radical. Examples of preferred radically polymerizable compounds and preferred combinations of radically polymerizable compounds in the component (a) are the same as those for the component (A).

[0067] Component (a) may be any of a monomer, oligomer, or polymer. As component (a), one type of compound may be used alone, or multiple types of compounds may be used in combination. Component (a) may be the same as or different from component (A).

[0068] The content of the (a) component may be 10 mass % or more, 20 mass % or more, or 30 mass % or more based on the total mass of the second curable composition, from the viewpoint of easily obtaining a crosslink density required for reducing connection resistance and improving connection reliability. The content of the (a) component may be 90 mass % or less, 80 mass % or less, or 70 mass % or less based on the total mass of the second curable composition, from the viewpoint of suppressing cure shrinkage during polymerization and obtaining good reliability.

[0069] [Component (b): Polymerization initiator] As the component (b), a polymerization initiator similar to the polymerization initiator exemplified as the component (B) can be used. The component (b) is preferably a radical polymerization initiator. Examples of preferred radical polymerization initiators for the component (b) are the same as those for the component (B). As the component (b), one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0070] The content of the (b) component may be 0.1 mass % or more, 0.5 mass % or more, or 1 mass % or more, based on the total mass of the second curable composition, from the viewpoint of facilitating connection at low temperature in a short time and from the viewpoint of more excellent connection reliability. The content of the (b) component may be 30 mass % or less, 20 mass % or less, or 10 mass % or less, based on the total mass of the second curable composition, from the viewpoint of pot life.

[0071] [Other ingredients] The second curable composition may further contain other components in addition to the components (a) and (b). Examples of the other components include a thermoplastic resin, a coupling agent, a filler, a softener, an accelerator, an anti-degradant, a colorant, a flame retardant, a thixotropic agent, etc. Details of the other components are the same as those of the other components in the first adhesive layer.

[0072] The second curable composition may contain a thiol compound from the viewpoint of promoting curing. The thiol compound may be a thiol compound having one thiol group (monofunctional thiol compound) or a thiol compound having multiple thiol groups (polyfunctional thiol compound). The thiol group of the thiol compound may be a primary thiol group, a secondary thiol group, or a tertiary thiol group.

[0073] Examples of monofunctional thiol compounds include 2-mercaptobenzothiazole, 2-methyl-4,5-dihydrofuran-3-thiol, 3-mercapto-1-hexanol, mercaptomethylbutanol, 3-mercapto-2-methylpentanol, 3-mercapto-3-methylbutanol, 4-ethoxy-2-methyl-2-butanethiol, hexanethiol, isobutylthiol, 1,1-dimethylheptanethiol, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3-mercaptopropionate, and stearyl-3-mercaptopropionate.

[0074] Examples of polyfunctional thiol compounds include dipentaerythritol hexakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), ethanedithiol, 1,3-propanethiol, 1,4-butanethiol, trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, and tetraethylene glycol bis(3-mercaptopropionate).

[0075] The second curable composition may contain a thermosetting resin instead of the (a) component and the (b) component, or in addition to the (a) component and the (b) component. When the second curable composition contains a thermosetting resin, the second curable composition may contain a curing agent used to cure the thermosetting resin. As the thermosetting resin and the curing agent, the same thermosetting resin and curing agent as the thermosetting resin and the curing agent exemplified as the other components in the first curable composition can be used. When a thermosetting resin is used instead of the (a) component and the (b) component, the content of the thermosetting resin in the second curable composition may be, for example, 20% by mass or more and 80% by mass or less based on the total mass of the second curable composition. When a thermosetting resin is used in addition to the (a) component and the (b) component, the content of the thermosetting resin in the second curable composition may be, for example, 20% by mass or more and 80% by mass or less based on the total mass of the second curable composition. The content of the curing agent may be in the same range as that described above for the content of the curing agent in the first curable composition.

[0076] The content of the conductive particles in the second adhesive layer may be, for example, 1 mass % or less, or may be 0 mass %, based on the total mass of the second adhesive layer. It is preferable that the second adhesive layer does not contain conductive particles.

[0077] From the viewpoint of lamination with the first adhesive layer, the melt viscosity of the second adhesive layer at 70°C may be 1000 to 3000 Pa s, 1000 to 1500 Pa s, or 1500 to 3000 Pa s. The melt viscosity of the second adhesive layer at 70°C refers to a value measured in the same manner as the melt viscosity of the above-mentioned film-like adhesive at 70°C.

[0078] The melt viscosity of the second adhesive layer at 70° C. can be adjusted by changing the composition of the second curable composition, etc. For example, the (a) component such as a (poly)urethane (meth)acrylate compound, a thermoplastic resin, and a filler may be blended, and the blending amounts thereof may be adjusted.

[0079] The thickness of the second adhesive layer may be appropriately set according to the height of the electrodes of the circuit member to be bonded. The thickness of the second adhesive layer may be 5 μm or more and 200 μm or less from the viewpoint of being able to sufficiently fill the space between the electrodes to seal the electrodes and obtain better reliability. In addition, when a part of the conductive particles is exposed from the surface of the first adhesive layer (for example, protruding toward the second adhesive layer), the thickness of the second adhesive layer is the distance from the surface of the second adhesive layer opposite to the first adhesive layer side to the boundary S between the first adhesive layer and the second adhesive layer located in the space between the adjacent conductive particles.

[0080] The ratio of the thickness of the first adhesive layer to the thickness of the second adhesive layer (thickness of the first adhesive layer / thickness of the second adhesive layer) may be 1 or more and 1000 or less, from the viewpoint of being able to sufficiently fill the space between the electrodes to seal the electrodes and obtain better reliability. Furthermore, from the viewpoint of making it easier to adjust the melt viscosity of the film-like adhesive at 70°C to within the above range, the thickness of the first adhesive layer / the thickness of the second adhesive layer may be 0.05 to 1.0, 0.05 to 0.5, or 0.1 to 1.0.

[0081] The thickness of the film-like adhesive (the total thickness of all layers constituting the film-like adhesive) may be, for example, 5 μm or more and 200 μm or less.

[0082] The above-mentioned adhesive film for circuit connection comprises a peelable support film and an adhesive layer provided on the support film, the adhesive layer containing an adhesive component and conductive particles, the conductive particles being unevenly distributed on the support film side and dispersed in a direction perpendicular to the thickness direction of the adhesive layer, and the adhesive layer may have, in the thickness direction of the adhesive layer from the support film side, a first region containing the cured product of the above-mentioned first curable composition and a second region containing the above-mentioned second curable composition. The ranges of the first region and the second region in the thickness direction of the adhesive layer can be set in the same manner as the thicknesses of the above-mentioned first adhesive layer and second adhesive layer, respectively. The conductive particles can also be set in the same manner as the above-mentioned conditions.

[0083] The method of this embodiment may include, as a pre-pressure bonding process, a preparation process for preparing the above-mentioned adhesive film for circuit connection of this embodiment, and a lamination process for laminating the film-like adhesive of the adhesive film for circuit connection from the second adhesive layer side to the first circuit component.

[0084] (preparation process) In this step, a pre-manufactured adhesive film for circuit connection of this embodiment may be prepared, or the adhesive film for circuit connection of this embodiment may be manufactured.

[0085] The method for producing the adhesive film for circuit connection of this embodiment may, for example, include a preparation step (first preparation step) of the above-mentioned first adhesive layer, and a lamination step of laminating the above-mentioned second adhesive layer on the first adhesive layer. The method for producing the adhesive film for circuit connection may further include a preparation step (second preparation step) of preparing the second adhesive layer.

[0086] In the first preparation step, for example, the first adhesive layer is formed on a support film to obtain a first adhesive film, thereby preparing the first adhesive layer. Specifically, first, the (A) component, the (B) component, and the (C) component, as well as other components added as necessary, are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc., to prepare a varnish composition. Thereafter, the varnish composition is applied to a substrate that has been subjected to a release treatment using a knife coater, roll coater, applicator, comma coater, die coater, etc., and the organic solvent is volatilized by heating to form a layer made of the first curable composition on the substrate. Next, the layer made of the first curable composition is irradiated with light or heated to cure the first curable composition, thereby forming a first adhesive layer on the substrate (curing step). This results in a first adhesive film.

[0087] The organic solvent used in the preparation of the varnish composition is preferably one that has the property of dissolving or dispersing each component uniformly, and examples thereof include toluene, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, propyl acetate, butyl acetate, etc. These organic solvents can be used alone or in combination of two or more. The stirring and mixing and kneading in the preparation of the varnish composition can be performed using, for example, a stirrer, a grinding machine, a three-roll mill, a ball mill, a bead mill, or a homodisper.

[0088] The support film is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent when the first curable composition is cured by light, and is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent and the heating conditions when curing the first curable composition when the first curable composition is cured by heating. As the support film, for example, a substrate (for example, a film) made of oriented polypropylene (OPP), polyethylene terephthalate (PET), polyethylene naphthalate, polyethylene isophthalate, polybutylene terephthalate, polyolefin, polyacetate, polycarbonate, polyphenylene sulfide, polyamide, polyimide, cellulose, ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, synthetic rubber, liquid crystal polymer, etc. can be used. From the viewpoint of high versatility, polyethylene terephthalate can be preferably used.

[0089] The heating conditions for volatilizing the organic solvent from the varnish composition applied to the support film are preferably conditions that allow the organic solvent to volatilize sufficiently, for example, at 40° C. or higher and 120° C. or lower for 0.1 minutes or longer and 10 minutes or shorter.

[0090] For the light irradiation in the curing step, irradiation light having a wavelength in the range of 150 to 750 nm (e.g., ultraviolet light) can be used. The light irradiation can be carried out using, for example, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a metal halide lamp, or the like. The amount of light irradiation can be, for example, 100 mJ / cm2 in terms of the integrated light amount of light with a wavelength of 365 nm. 2 or more, and 2 or more, and 2 The amount of light irradiation may be, for example, 10,000 mJ / cm2 in terms of the integrated light amount of light with a wavelength of 365 nm. 2 may be less than 5000 mJ / cm 2 or less than 3000 mJ / cm 2 It may be the following:

[0091] The heating conditions in the curing step may be, for example, 30° C. to 300° C. for 0.1 to 5000 minutes, or 50° C. to 150° C. for 0.1 to 3000 minutes.

[0092] In the second preparation step, the second adhesive layer is prepared by forming a second adhesive layer on a substrate to obtain a second adhesive film in the same manner as in the first preparation step, except that the (a) component, the (b) component, and other components added as necessary are used, and the curing step is not performed (light irradiation and heating are not performed). The substrate may be the same as the support film described above.

[0093] In the lamination process, the second adhesive layer may be laminated onto the first adhesive layer by bonding the first adhesive film and the second adhesive film together, or the second adhesive layer may be laminated onto the first adhesive layer by applying a varnish composition obtained using components (a) and (b) and other components added as necessary onto the first adhesive layer and volatilizing the organic solvent.

[0094] Examples of the method for bonding the first adhesive film and the second adhesive film include hot pressing, roll lamination, vacuum lamination, etc. Lamination may be performed under heating conditions of, for example, 0 to 80°C.

[0095] In addition, in this embodiment, when using an adhesive film for circuit connection in which 90% or more of the conductive particles P are separated from other conductive particles in the first adhesive layer, such a dispersed state can be formed by a magnetic field application step described later. In this case, as the conductive particles P, particles containing nickel are preferably used from the viewpoint of performing dispersion by the magnetic field application step. In general, iron, cobalt, and nickel are ferromagnetic materials and are known to be magnetized by an external magnetic field, but among these, the use of nickel is significant in that it can achieve both electrical conductivity and dispersibility by applying a magnetic field. In addition, in order to obtain storage stability of the conductive particles P, the surface layer of the conductive particles P may be made of platinum group precious metals such as gold and silver instead of nickel. In addition, the surface of nickel may be coated with precious metals such as Au. Furthermore, non-conductive glass, ceramic, plastic, etc. coated with a conductive material such as the above metal may be used, and in this case, a nickel layer may also be provided to form a multilayer structure.

[0096] In addition, since the magnetism of nickel is affected by the phosphorus concentration contained in the nickel plating, the magnetism required for dispersing the conductive particles P by the magnetic field can be adjusted as needed. The magnetism of the conductive particles P can be measured by, for example, saturation magnetization using a vibrating sample magnetometer (VSM). In order to disperse the conductive particles P by an external magnetic field, the saturation magnetization may be in the range of 5.0 emu / g to 50 emu / g in the VSM measurement. If it is 5.0 emu / g or more, it becomes easy to sufficiently disperse the conductive particles P. On the other hand, if it is 50 emu / g or less, the magnetization of the conductive particles P does not become too large, and the conductive particles P are prevented from bonding in the thickness direction of the first adhesive layer 13, and the dispersibility of the conductive particles P tends to be high.

[0097] The average particle size of the conductive particles P may be 1.0 μm or more and 10.0 μm or less. When the average particle size of the conductive particles P is 1.0 μm or more, the coating accuracy on the support film is high, and it is easy to disperse the conductive particles P well in the first adhesive layer. When the average particle size of the conductive particles P is 10.0 μm or less, there is a tendency that good insulation between adjacent circuit electrodes of the connection structure is obtained. In order to obtain good dispersibility of the conductive particles P, the average particle size of the conductive particles P may be 2.0 μm or more, or may be 2.5 μm or more. On the other hand, from the viewpoint of ensuring insulation between adjacent circuit electrodes of the connection structure, the average particle size of the conductive particles P may be 8.5 μm or less, may be 7 μm or less, or may be 6.0 μm or less.

[0098] The amount of conductive particles P is preferably 1 to 100 parts by volume per 100 parts by volume of the components other than the conductive particles P in the first adhesive layer. From the viewpoint of preventing short-circuiting between adjacent circuit electrodes due to the presence of an excessive amount of conductive particles P, the amount of conductive particles P is more preferably 10 to 50 parts by volume. Furthermore, when the average particle size of the conductive particles is in the range of 1.0 μm or more and 10.0 μm or less, the particle density of the conductive particles is more preferably 1000 particles / mm 2 More than 50000 pieces / mm 2 In this case, it is possible to more suitably achieve both the dispersibility of the conductive particles P and the insulation between adjacent circuit electrodes.

[0099] (Lamination process) 2 is a schematic cross-sectional view showing a lamination step in the manufacturing method of the connection structure of this embodiment. In this step, as shown in the figure, the circuit connection adhesive film 11 is laminated onto the first circuit member 2 so that the second adhesive layer 14 side of the circuit connection adhesive film 11 faces the surface of the first circuit member 2 on which the first circuit electrode 6 is provided. If the circuit connection adhesive film 11 has a release film provided on the second adhesive layer 14, the second adhesive layer 14 can be laminated onto the first circuit member 2 after or while peeling off the release film so that the second adhesive layer 14 is in close contact with the first circuit member 2.

[0100] The first circuit member 2 has a circuit electrode 6 on the mounting surface 5a side of the main body 5. Examples of the first circuit member 2 include members having a flexible substrate such as COP, FCP, and polyimide. Examples of the circuit electrode 6 include copper plated with a metal such as tin. Note that an insulating layer may be formed on the mounting surface 5a in a portion where the circuit electrode 6 is not formed.

[0101] In this embodiment, the first circuit member 2 may have a flexible substrate, and the first electrode and the sensor mark portion may be provided on the flexible substrate. In this case, the adhesive film for circuit connection may be laminated onto the first circuit member so that the film-like adhesive covers the first electrode and the sensor mark portion, and the second adhesive layer of the film-like adhesive may cover the first electrode and the sensor mark portion.

[0102] The material of the sensor mark may be the same as that of the circuit wiring, and examples of the material of the circuit wiring include copper and copper plated with nickel and gold. The height of the sensor mark may be 1 to 35 μm, 1 to 18 μm, or 18 to 35 μm.

[0103] A known laminator can be used as a means for lamination. The lamination conditions can be appropriately set, but from the viewpoint of productivity, they may be 50 to 90°C, 0.5 to 2 MPa, and 0.5 to 3 seconds, or 50 to 70°C, 0.5 to 1.0 MPa, and 0.5 to 1.0 seconds, or 70 to 90°C, 1 to 2 MPa, and 1 to 3 seconds. Even under such conditions, the adhesive film for circuit connection of this embodiment can suppress the generation of air bubbles around the sensor mark portion even under the above lamination conditions.

[0104] 3 is a schematic cross-sectional view showing a laminate obtained through a lamination process, in which a film-like adhesive is temporarily pressure-bonded onto a first circuit member, and support film 12 has been removed.

[0105] The method for producing a circuit connection structure of the present embodiment includes, after a temporary pressure-bonding step, a heating and pressurizing step of placing a second circuit member on the first circuit member laminated with the film-like adhesive so that the first circuit electrode and the second circuit electrode face each other, and, while heating the film-like adhesive, pressurizing the first circuit member and the second circuit member in a direction in which the first circuit electrode and the second circuit electrode face each other; It can be provided with:

[0106] (Heat and pressure process) 4 is a schematic cross-sectional view showing a heating and pressurizing step in the manufacturing method of the connection structure of this embodiment. In this step, as shown in the figure, the second circuit member 3 is placed on the first circuit member 2 on which the film-like adhesive (second adhesive layer 14 and first adhesive layer 13) is laminated so that the first circuit electrode 6 and the second circuit electrode 8 face each other, and while heating the film-like adhesive (second adhesive layer 14 and first adhesive layer 13), the first circuit member 2 and the second circuit member 3 are pressed in a direction in which the first circuit electrode 6 and the second circuit electrode 8 face each other.

[0107] The second circuit member 3 is, for example, a glass substrate or plastic substrate on which a circuit is formed using ITO, IZO, or a metal used in liquid crystal displays, a ceramic wiring board, etc. The second circuit member 3 has second circuit electrodes 8 corresponding to the first circuit electrodes 6 on the mounting surface 7a side of the main body 7, as shown in Fig. 4.

[0108] The circuit electrodes 8 are, for example, rectangular in plan view and have a thickness of, for example, about 100 nm to 1000 nm. The surfaces of the circuit electrodes 8 are made of one or more materials selected from, for example, gold, silver, copper, tin, ruthenium, rhodium, palladium, osmium, iridium, platinum, indium tin oxide (ITO), and indium zinc oxide (IZO). An insulating layer may also be formed on the mounting surface 7a in the areas where the circuit electrodes 8 are not formed.

[0109] In this embodiment, the first circuit electrodes 6 and the second circuit electrodes 8 can be aligned by detecting a sensor mark portion provided on the first circuit member with a CCD camera.

[0110] A known thermocompression bonding device can be used as the heating means. The heating temperature of the film-like adhesive (the second adhesive layer 14 and the first adhesive layer 13) can be set to a temperature at which active polymerization species are generated in the curing agent and polymerization of the polymerization monomer is initiated or higher. The heating temperature may be, for example, 80°C to 200°C, or 100°C to 180°C. The heating time may be, for example, 0.1 seconds to 30 seconds, or 1 second to 20 seconds. If the heating temperature is 80°C or higher, a sufficient curing speed is easily obtained, and if it is 200°C or lower, undesired side reactions are less likely to proceed. If the heating time is 0.1 seconds or higher, the curing reaction is easily allowed to proceed sufficiently, and if it is 30 seconds or shorter, the productivity of the cured product is easily maintained, and undesired side reactions are also less likely to proceed.

[0111] As the pressing means, a known thermocompression device can be used. The pressure and time of pressing can be appropriately set.

[0112] 5 is a schematic cross-sectional view showing a circuit connection structure obtained through a heating and pressurizing process. In the heating and pressurizing process, the adhesive component of the film-like adhesive (the second adhesive layer 14 and the first adhesive layer 13) flows, and the distance between the first circuit electrode 6 and the second circuit electrode 8 is shortened and the conductive particles P are interlocked, and the second adhesive layer and the first adhesive layer are cured. By curing the second adhesive layer and the first adhesive layer, the first circuit electrode 6 and the second circuit electrode 8 are electrically connected, and adjacent circuit electrodes 6, 6 and adjacent circuit electrodes 8, 8 are electrically insulated from each other, and a cured product 4 of the film-like adhesive (the second adhesive layer 14 and the first adhesive layer 13) is formed, and the circuit connection structure 1 shown in FIG. 5 is obtained. In the obtained circuit connection structure 1, the cured product 4 of the film-like adhesive (second adhesive layer 14 and first adhesive layer 13) sufficiently prevents the distance between the first circuit electrode 6 and the second circuit electrode 8 from changing over time, while also ensuring the long-term reliability of the electrical characteristics.

[0113] The cured product 4 of the film-like adhesive (second adhesive layer 14 and first adhesive layer 13) has a first region 9 formed by curing the first adhesive layer 13, and a second region 10 formed by curing the second adhesive layer 14. In this embodiment, the first region 9 is located on the second circuit member 3 side, and the second region 10 is located on the first circuit member 2 side.

[0114] The conductive particles P are interposed between the first circuit electrode 6 and the second circuit electrode 8 in a state where they are slightly deformed into a flat shape by compression bonding. This realizes an electrical connection between the first circuit electrode 6 and the second circuit electrode 8. Furthermore, the conductive particles P are spaced apart between adjacent first circuit electrodes 6, 6 and between adjacent second circuit electrodes 8, 8, realizing electrical insulation between adjacent first circuit electrodes 6, 6 and adjacent second circuit electrodes 8, 8. EXAMPLES

[0115] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0116] <Synthesis of polyurethane acrylate (UA1)> Into a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser having a calcium chloride drying tube, and a nitrogen gas inlet tube, 2500 parts by mass (2.50 mol) of poly(1,6-hexanediol carbonate) (trade name: Duranol T5652, manufactured by Asahi Kasei Chemicals Corporation, number average molecular weight 1000) and 666 parts by mass (3.00 mol) of isophorone diisocyanate (manufactured by Sigma-Aldrich Co.) were uniformly dropped over 3 hours. Next, after sufficient nitrogen gas was introduced into the reaction vessel, the inside of the reaction vessel was heated to 70 to 75°C to cause a reaction. Next, 0.53 parts by mass (4.3 mmol) of hydroquinone monomethyl ether (Sigma-Aldrich) and 5.53 parts by mass (8.8 mmol) of dibutyltin dilaurate (Sigma-Aldrich) were added to the reaction vessel, and then 238 parts by mass (2.05 mol) of 2-hydroxyethyl acrylate (Sigma-Aldrich) were added and reacted at 70°C for 6 hours under air atmosphere. This resulted in polyurethane acrylate (UA1). The weight-average molecular weight of polyurethane acrylate (UA1) was 15,000. The weight-average molecular weight was measured by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene under the following conditions. (Measurement conditions) Equipment: Tosoh Corporation GPC-8020 Detector: Tosoh RI-8020 Column: Gelpack GLA160S+GLA150S manufactured by Hitachi Chemical Co., Ltd. Sample concentration: 120mg / 3mL Solvent: Tetrahydrofuran Injection volume: 60μL Pressure: 2.94×10 6 Pa(30kgf / cm 2 ) Flow rate: 1.00mL / min

[0117] <Preparation of conductive particles> A layer of nickel was formed on the surface of the polystyrene particles to a thickness of 0.2 μm, thus obtaining conductive particles with an average particle size of 4 μm, a maximum particle size of 4.5 μm, and a specific gravity of 2.5.

[0118] <Method for preparing polyester urethane resin> 48 parts by mass of isophthalic acid and 37 parts by mass of neopentyl glycol were put into a stainless steel autoclave equipped with a stirrer, a thermometer, a condenser, a vacuum generator, and a nitrogen gas inlet tube, and 0.02 parts by mass of tetrabutoxy titanate as a catalyst was further put in. Then, the temperature was raised to 220°C under a nitrogen stream, and the mixture was stirred for 8 hours. Then, the pressure was reduced to atmospheric pressure (760 mmHg), and the mixture was cooled to room temperature. This caused a white precipitate to precipitate. Next, the white precipitate was taken out, washed with water, and then vacuum dried to obtain a polyester polyol. The obtained polyester polyol was thoroughly dried, and then dissolved in MEK (methyl ethyl ketone), and put into a four-neck flask equipped with a stirrer, a dropping funnel, a reflux condenser, and a nitrogen gas inlet tube. In addition, dibutyltin dilaurate was added as a catalyst in an amount of 0.05 parts by mass relative to 100 parts by mass of polyester polyol, and 4,4'-diphenylmethane diisocyanate was dissolved in MEK in an amount of 50 parts by mass relative to 100 parts by mass of polyester polyol and added using a dropping funnel, and the mixture was stirred at 80°C for 4 hours to obtain the desired polyester urethane resin. The weight average molecular weight of the polyester urethane resin was 15,000. The weight average molecular weight was measured in the same manner as above.

[0119] <Preparation of first varnish composition> The components shown below were mixed in the amounts (parts by mass) shown in Table 1 to prepare a first varnish composition 1-1.

[0120] (polymerizable compound) A1: Diacrylate having a tricyclodecane skeleton (product name: DCP-A, manufactured by Kyoeisha Chemical Co., Ltd.) A2: Polyurethane acrylate (UA1) synthesized as described above A3: 2-Methacryloyloxyethyl acid phosphate (product name: Light Ester P-2M, manufactured by Kyoeisha Chemical Co., Ltd.) (Photopolymerization initiator) B1: 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (trade name: Irgacure (registered trademark) OXE01, manufactured by BASF) (Thermal polymerization initiator) C1: Benzoyl peroxide (product name: Niper BMT-K40, manufactured by NOF Corporation) (Conductive particles) D1: Conductive particles prepared as described above (thermoplastic resin) E1: Polyester urethane resin synthesized as described above (Coupling Agent) F1: 3-methacryloxypropyltrimethoxysilane (product name: KBM503, manufactured by Shin-Etsu Chemical Co., Ltd.) (filling material) G1: Silica fine particles (product name: R104, manufactured by Nippon Aerosil Co., Ltd., average particle size (primary particle size): 12 nm) (solvent) H1: Methyl ethyl ketone

[0121] [Table 1]

[0122] <Preparation of second varnish composition> The polymerizable compounds a1 to a3, thermal polymerization initiator c1, coupling agent f1, filler f1 and solvent h1 used were the same as the polymerizable compounds A1 to A3, thermal polymerization initiator C1, coupling agent F1, filler G1 and solvent H1 in the first varnish composition, and the thiol compound I1 used the components shown below. These components were mixed in the amounts (parts by mass) shown in Table 2 to prepare second varnish compositions 2-1 to 2-5, respectively. (Thiol compounds) I1: Dipentaerythritol hexakis(3-mercaptopropionate) (product name: DPMP, manufactured by SC Organic Chemicals)

[0123] [Table 2]

[0124] Example 1 [Preparation of the first adhesive film] The first varnish composition 1-1 was applied onto a PET film having a thickness of 50 μm using a coating device. Then, hot air drying was performed at 70° C. for 3 minutes, and a magnetic field was simultaneously applied to form a layer having a thickness (thickness after drying) of 4 μm on the PET film. The thickness here was measured using a contact thickness meter. Next, a metal halide lamp was used to apply an integrated light amount of 1500 mJ / cm 2 to this layer. 2 The polymerizable compound was polymerized by irradiating with light so that the thickness of the first adhesive layer was 4 μm (the thickness of the area where the conductive particles are present) on the PET film. The conductive particle density at this time was about 7000 pcs / mm 2 The thickness of the first adhesive layer was measured by laminating the second adhesive layer to produce a two-layered adhesive film for circuit connection, and then measuring the thickness of the first adhesive layer located in the space between adjacent conductive particles using the method described below.

[0125] [Evaluation of monodispersity of conductive particles] The monodispersity of the conductive particles (the ratio of conductive particles present in a state where they are separated from adjacent conductive particles (monodispersed state)) of the first adhesive film was evaluated, and the monodispersity was 70% or more. The monodispersity ratio is expressed as follows: Monodispersity ratio (%) = (2500 μm 2 Number of monodispersed conductive particles in / 2500μm 2 The number of conductive particles was calculated by multiplying the number of conductive particles by 100. The number of conductive particles was measured by observing with a metal microscope at a magnification of 200 times.

[0126] [Preparation of the second adhesive film] The second varnish composition 2-1 was applied onto a PET film having a thickness of 50 μm using a coating device. Then, hot air drying was performed at 70° C. for 3 minutes to form a second adhesive layer having a thickness of 8 μm on the PET film. Through the above operations, a second adhesive film having a second adhesive layer on the PET film was obtained.

[0127] [Preparation of adhesive film for circuit connection] The first adhesive film and the second adhesive film were laminated together with the PET film substrate at 40°C using a roll laminator. At this time, the PET film on the second adhesive film side was peeled off. This produced an adhesive film for circuit connection having a laminated structure in which the PET film, the first adhesive layer, and the second adhesive layer were laminated in this order.

[0128] [Measurement of the thickness of the first adhesive layer] The thickness of the first adhesive layer in the produced adhesive film for circuit connection was measured by the following method. The adhesive film for circuit connection was sandwiched between two pieces of glass (thickness: approximately 1 mm) and a resin composition consisting of 100 g of bisphenol A type epoxy resin (product name: JER811, manufactured by Mitsubishi Chemical Corporation) and 10 g of a hardener (product name: Epomount hardener, manufactured by Refine Tech Co., Ltd.) was poured into the mold. The cross section was then polished using a polishing machine, and the thickness of the first adhesive layer located in the space between adjacent conductive particles was measured using a scanning electron microscope (SEM, product name: SE-8020, manufactured by Hitachi High-Tech Science Corporation).

[0129] [Melt viscosity measurement at 70℃] The melt viscosity at 70° C. of the film-like adhesive and the second adhesive layer were each measured by the following procedure.

[0130] The film-like adhesive or the second adhesive layer is laminated together to prepare a 600 μm thick laminate for measurement. This laminate for measurement is measured using a shear viscoelasticity measuring device (manufactured by TA Instruments, product name: ARES-G2) at a heating rate of 10° C. / min, a measuring frequency of 10 Hz, and a measuring temperature of 40 to 200° C., and the melt viscosity at 70° C. is derived.

[0131] [Pre-compression test] A test COF board was prepared by providing line-shaped wiring with a height of 8 μm at a pitch of 300 μm (line width 150 μm and line interval 150 μm) on a polyimide substrate. A circuit connection adhesive film with a width of 1.5 mm was attached to the test COF board from the second adhesive layer side, and a cushioning material (100 μm) made of PTFE was attached to the test COF board. 2 ) was used for lamination under conditions of 70°C, 1 MPa, and 1 second. The obtained laminate was observed under a microscope to check for the presence or absence of air bubbles between the lines, and the temporary pressure bonding property was evaluated according to the following criteria. [Judgment criteria] A: No air bubbles are visible B: There are air bubbles between the lines that are not filled properly. C: Most of the spaces between the lines show unfilled air bubbles.

[0132] Comparative Example 1 A first adhesive film was prepared in the same manner as in Example 1. On the other hand, a second adhesive film having a second adhesive layer having a thickness of 8 μm was prepared in the same manner as in Example 1, except that the second varnish composition 2-1 was used instead of the second varnish composition 2-1.

[0133] Evaluation was performed in the same manner as in Example 1, except that an adhesive film for circuit connection having a laminated configuration in which the first adhesive layer, the second adhesive layer, and the PET film were laminated in this order was produced by laminating the first adhesive layer and the second adhesive layer and then peeling off the PET film on the first adhesive layer side. During the temporary pressure bonding test, the adhesive film for circuit connection was laminated onto the test COF board from the first adhesive layer side.

[0134] Comparative Example 2 A first adhesive film was prepared in the same manner as in Example 1. On the other hand, a second adhesive film having a second adhesive layer having a thickness of 8 μm was prepared in the same manner as in Example 1, except that the second varnish composition 2-3 was used instead of the second varnish composition 2-1.

[0135] The evaluation was carried out in the same manner as in Example 1, except that the above-mentioned second adhesive film was used.

[0136] Comparative Example 3 A first adhesive film was prepared in the same manner as in Example 1. On the other hand, a second adhesive film having a second adhesive layer having a thickness of 8 μm was prepared in the same manner as in Example 1, except that the second varnish composition 2-4 was used instead of the second varnish composition 2-1.

[0137] Evaluation was performed in the same manner as in Example 1, except that an adhesive film for circuit connection having a laminated configuration in which the first adhesive layer, the second adhesive layer, and the PET film were laminated in this order was produced by laminating the first adhesive layer and the second adhesive layer and then peeling off the PET film on the first adhesive layer side. During the temporary pressure bonding test, the adhesive film for circuit connection was laminated onto the test COF board from the first adhesive layer side.

[0138] Comparative Example 4 A first adhesive film was prepared in the same manner as in Example 1. On the other hand, a second adhesive film having a second adhesive layer having a thickness of 8 μm was prepared in the same manner as in Example 1, except that the second varnish composition 2-5 was used instead of the second varnish composition 2-1.

[0139] The evaluation was carried out in the same manner as in Example 1, except that the above-mentioned second adhesive film was used.

[0140] [Table 3] [Explanation of symbols]

[0141] 1...circuit connection structure, 2...first circuit member, 3...second circuit member, 6...first circuit electrode, 8...second circuit electrode, 11...circuit connection adhesive film, 12...support film (peeling film), 13...first adhesive layer, 14...second adhesive layer, 15...film-like adhesive, P...conductive particles.

Claims

1. A method for manufacturing a connection structure, comprising: interposing a film-like adhesive between a first circuit member having a first electrode and a second circuit member having a second electrode; and thermocompression bonding the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other, a temporary pressure-bonding step of preparing an adhesive film for circuit connection, the adhesive film having a first adhesive layer containing conductive particles and a second adhesive layer laminated on the first adhesive layer, the film-like adhesive having a melt viscosity of 1000 to 2500 Pa·s at 70°C, and laminating the film-like adhesive of the adhesive film for circuit connection from the side of the second adhesive layer onto the first circuit member; A method for manufacturing a connection structure comprising:

2. the first circuit member has a flexible substrate, and the first electrode and a sensor mark portion are provided on the flexible substrate; The method for manufacturing a connection structure according to claim 1 , wherein the film-like adhesive covers the first electrode and the sensor mark portion in the temporary pressure-bonding step.

3. A film-like adhesive including a peelable support film, a first adhesive layer including conductive particles provided on the support film, and a second adhesive layer laminated on the first adhesive layer, The film-like adhesive has a melt viscosity at 70° C. of 1000 to 2500 Pa·s.

Citation Information

Patent Citations

  • Anisotropic conductive film

    JP2009289729A