Inorganic coated sand and method for manufacturing the same, mold for casting, and method for improving storage stability of inorganic coated sand

By controlling cation exchange capacity and applying metasilicate hydrate coatings on recycled and refractory aggregates, the inorganic coated sand maintains dryness and stability, addressing mold formation issues and reducing energy consumption and emissions.

JP2024163866AActive Publication Date: 2024-11-22KAO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024075788
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-08
Publication Date
2024-11-22
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

Inorganic coated sand used in casting processes becomes wet during storage, leading to mold formation issues, and conventional methods for regenerating inorganic binders require high-temperature treatments that increase energy consumption and CO2 emissions.

Method used

Applying a first coating layer on recycled or refractory aggregates to control cation exchange capacity (CEC) between 3 mmol(+)/kg and 40 mmol(+)/kg, followed by a metasilicate hydrate second coating layer, to produce dry inorganic coated sand that suppresses moisture and enhances storage stability.

Benefits of technology

Improves storage stability of inorganic coated sand while reducing thermal energy consumption and environmental impact by omitting high-temperature roasting processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024163866000001
    Figure 2024163866000001
  • Figure 2024163866000002
    Figure 2024163866000002
  • Figure 2024163866000003
    Figure 2024163866000003
Patent Text Reader

Abstract

To provide inorganic coated sand which has improved storage stability while reducing environmental loads in manufacture of casting sand for inorganic coated sand.SOLUTION: Inorganic coated sand in a dried state has casting sand having one or two kinds of aggregates selected from recycled sand (A) and a fire resistant aggregate (B) and a first coating layer which coats the aggregate and is positioned on the surface, and a second coating layer containing a metasilicate on the first coating layer of the casting sand, wherein the fire resistant aggregate (B) contains SiO2, and a cation exchange capacity (CEC) of the casting sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to inorganic coated sand, a method for producing the same, a casting mold, and a method for improving the storage stability of inorganic coated sand. [Background technology]

[0002] In recent years, the importance of product design that takes people and the environment into consideration has been increasing from the perspective of the Sustainable Development Goals (SDGs), and technological development of environmentally friendly casting processes that reduce CO2 emissions and VOCs is accelerating. As an environmentally friendly casting process, for example, a wet sand inorganic binder process using refractory aggregate and an inorganic binder made of liquid water glass is known, for example, as described in Patent Document 1 (JP Patent Publication No. 2010-519042).

[0003] Patent Document 2 (JP Patent Publication No. 2021-536367) describes that by mixing recycled sand with particulate amorphous oxide containing silicon dioxide to obtain a mixture, and then heat-treating the mixture at a temperature of 400°C or higher, the pot life is improved, the surface quality of the castings is improved, and significant energy savings can be achieved.

[0004] Patent Document 3 (JP 2014-117740 A) describes a method for producing dry coated sand having fluidity at room temperature, in which a specific water glass aqueous solution is mixed with heated refractory aggregate as a binder, and the water is evaporated to form a coating layer of binder on the surface of the refractory aggregate. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2010-519042 [Patent Document 2] Special Publication No. 2021-536367 [Patent Document 3] JP 2014-117740 A Summary of the Invention [Problem to be solved by the invention]

[0006] After casting, the coated sand used for the molds is usually broken down (crushed) into single particles, which are then recycled as reclaimed sand by various methods. From the standpoint of economy and waste reduction, it has become essential for foundries to manufacture molds using reclaimed sand.

[0007] The present inventors have found that when inorganic coated sand is produced by forming a metasilicate hydrate layer on foundry sand using reclaimed sand produced by an inorganic binder process using a conventional inorganic binder as described in Patent Documents 2 and 3, the sand quickly becomes wet during storage, making it impossible to mold the desired mold. Also, when a refractory aggregate with a relatively high degree of amorphization is used and a metasilicate hydrate layer is formed to produce inorganic coated sand, the sand also tends to become wet during storage.

[0008] A conventional regeneration method for inorganic binder processes is roasting regeneration, as shown in Patent Document 1. However, it is not possible to sufficiently suppress wetting, and since high-temperature treatment is performed at 600 to 800°C, there are problems in terms of energy consumption and CO2 emissions. Patent Document 1 also relates to an inorganic binder process for wet sand that uses an inorganic binder made of liquid water glass. In other words, an object of the present invention is to prevent inorganic coated sand made from reclaimed sand or the like from becoming wet during storage, and to reduce the environmental load when using the same to produce foundry sand for use as inorganic coated sand. [Means for solving the problem]

[0009] The inventors have discovered that applying a coating layer to recycled sand or refractory aggregate containing SiO2 and setting the cation exchange capacity (CEC) of the foundry sand to a specific value is effective in solving the above problems, and have completed the present invention.

[0010] According to the present invention, A dry inorganic coated sand comprising: a molding sand in which a first coating layer is disposed on the surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate on the first coating layer of the molding sand, The refractory aggregate (B) contains SiO2, The foundry sand is provided with a dry inorganic coated sand having a cation exchange capacity (CEC) of 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.

[0011] The present invention also provides a casting mold made of the above-mentioned inorganic coated sand.

[0012] Further, according to the present invention, A step (1) of mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming a first coating layer on the surface of the aggregate to obtain molding sand; (2) mixing the obtained foundry sand with a molten liquid of metasilicate hydrate to obtain a mixture; (3) cooling the mixture to a temperature below the melting point of the metasilicate hydrate; Including, The method for producing inorganic coated sand is provided, wherein the refractory aggregate (B) contains SiO2.

[0013] Further, according to the present invention, (4) mixing one or two aggregates selected from the recycled sand (A) and the refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming a first coating layer on the surface of the aggregate to obtain molding sand; (5) mixing the obtained foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate; Including, The method for producing inorganic coated sand is provided, wherein the refractory aggregate (B) contains SiO2.

[0014] Further, according to the present invention, A foundry sand containing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate coating the foundry sand, comprising: The refractory aggregate (B) contains SiO2, The present invention provides a method for improving the storage stability of inorganic coated sand, which comprises preparing the dry inorganic coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less. Effect of the Invention

[0015] According to the present invention, it is possible to reduce the environmental load during the production of foundry sand for inorganic coated sand, while improving the storage stability of the inorganic coated sand. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, embodiments of the present invention will be described. In addition, in this specification, "A to B" indicating a numerical range means a range from A to B, unless otherwise specified. In addition, the components and elements described in each embodiment can be appropriately combined as long as the effect of the invention is not impaired.

[0017] Furthermore, the "coating" and "coating layer" are not limited to being continuous, and may have some discontinuous portions.

[0018] <Inorganic coated sand> The inorganic coated sand of this embodiment is a dry inorganic coated sand comprising foundry sand having one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), a first coating layer covering the aggregate and positioned on the surface, and a second coating layer containing metasilicate on the first coating layer of the foundry sand. The refractory aggregate (B) contains SiO2, and the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.

[0019] That is, in the inorganic coated sand of this embodiment, when the inorganic coated sand is produced using one or two types of aggregates selected from recycled sand (A) and refractory aggregate (B), a first coating layer and a second coating layer containing silicate are laminated in this order on the surface of the aggregate, and the cation exchange capacity (CEC) of the foundry sand is controlled, thereby making it possible to improve the storage stability of the inorganic coated sand produced using one or two types of aggregates selected from recycled sand (A) and refractory aggregate (B).

[0020] Although the details of the reason for this are not clear, it is speculated as follows. (i) The surface of the reclaimed sand (A) may have residues of an inorganic binder that has been used once for casting. If the surface of the reclaimed sand (A) that has residues of an inorganic binder is coated with metasilicate hydrate to produce inorganic coated sand, the components in the residues will react with the metasilicate hydrate, causing the metasilicate hydrate crystals to melt and the inorganic coated sand to become wet. (ii) On the other hand, when inorganic coated sand is produced by coating the surface of refractory aggregate (B) containing SiO2 with silicate hydrate, the SiO2 component of the refractory aggregate (B) may react with the silicate hydrate, causing the silicate hydrate crystals to melt and the inorganic coated sand to become wet, as in (i). (iii) Therefore, by forming the first coating layer to cover the surface of the recycled sand (A) or the fire-resistant aggregate (B) and using foundry sand with a specific CEC, it is possible to suppress the reaction with the residues. Even if a second coating layer containing metasilicate is then laminated, the melting of the metasilicate hydrate in the second coating layer can be suppressed. As a result, it is presumed that the wetting of the inorganic coated sand can be suppressed and the storage stability can be improved.

[0021] In addition, when the first coating layer that coats the surface of the recycled sand (A) or the refractory aggregate (B) is formed from an aluminosilicate-containing material, it can be formed at a relatively low temperature. Therefore, the roasting process at 600 to 800°C that was required in the conventional inorganic binder regeneration process can be omitted, and the consumption of thermal energy and CO2 emissions can be reduced, reducing the environmental burden.

[0022] The inorganic coated sand of this embodiment will be described in more detail below.

[0023] The inorganic coated sand is in a dry state. Dry coated sand means coated sand that can obtain a measured value when the dynamic angle of repose is measured regardless of the moisture content. The dynamic angle of repose is preferably 80° or less, more preferably 45° or less, and even more preferably 30° or less. The dynamic angle of repose can be measured by the following method. (Method of measuring dynamic angle of repose) Put half the volume of coated sand into a cylindrical transparent plastic bottle, hold it so that its axis is horizontal, and rotate it around the horizontal axis at a rotation speed of 60 rpm. The inclined surface of the coated sand layer flowing inside the cylinder becomes flat. Measure the angle formed between this inclined surface and the horizontal plane. If the coated sand does not flow inside the cylinder, or if it does flow but the inclined surface of the coated sand layer does not form a flat surface, and as a result the dynamic angle of repose cannot be measured, it is in a wet state.

[0024] Specifically, the inorganic coated sand is composed of a group of inorganic coated sand particles.

[0025] From the viewpoint of improving the fluidity and further improving the filling property into the molding die, the inorganic coated sand is preferably spherical. Here, the inorganic coated sand being spherical means that it has a round shape like a ball. More specifically, from the viewpoint of improving the fluidity, mold quality, and mold strength, and from the viewpoint of ease of molding the mold, the sphericity of the inorganic coated sand is preferably 0.75 or more, more preferably 0.80 or more, and even more preferably 0.82 or more. The upper limit of the sphericity is specifically 1. In this embodiment, the sphericity of the inorganic coated sand specifically coincides with the sphericity of the refractory aggregate described below.

[0026] The sphericity of the inorganic coated sand was determined by analyzing the image (photograph) of the particle taken with an optical microscope or a digital scope (e.g., Keyence VH-8000) to determine the area of ​​the projected cross section of the particle and the perimeter of the cross section, and then calculating the sphericity = [area of ​​the projected cross section of the particle (mm 2 The particle diameter can be calculated by dividing the circumference (mm) of a perfect circle with the same area as the particle diameter by the circumference (mm) of the projected cross section of the particle, and then averaging the values ​​obtained for any 50 particles.

[0027] The average particle size of the inorganic coated sand is preferably 0.05 mm or more, more preferably 0.1 mm or more, from the viewpoints of improving mold quality and mold strength, ease of mold making, and storage stability. In addition, if the average particle size of the inorganic coated sand is equal to or more than the above lower limit, the amount of the second coating layer, etc. used during mold production can be reduced, which is also preferable in that the inorganic coated sand can be easily regenerated. From the viewpoints of improving mold quality and strength, and of ease of mold making, the average particle size of the inorganic coated sand is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. In addition, when the average particle size of the inorganic coated sand is equal to or less than the above upper limit, it is also preferable in that the porosity is reduced during mold production, and the mold strength can be increased.

[0028] In this embodiment, the average particle size of the inorganic coated sand and the refractory aggregate described later can be specifically measured by the following method.

[0029] (Method of measuring average particle size) If the sphericity of the particle from the projected cross section is 1, the diameter (mm) is measured, whereas if the sphericity is <1, the long axis diameter (mm) and short axis diameter (mm) of the randomly oriented particles are measured to calculate (long axis diameter + short axis diameter) / 2, and the average of the values ​​obtained for any 100 particles is used as the average particle diameter (mm). The long axis diameter and short axis diameter are defined as follows: A particle is stabilized on a flat surface, and when the projected image of the particle on the flat surface is sandwiched between two parallel lines, the width of the particle at which the distance between the parallel lines is the smallest is called the short axis diameter, whereas the distance when the particle is sandwiched between two parallel lines perpendicular to the parallel lines is called the long axis diameter. The major axis diameter and minor axis diameter of a particle can be determined by taking an image (photograph) of the particle using an optical microscope or a digital scope (for example, VH-8000 model, manufactured by Keyence Corporation) and subjecting the obtained image to image analysis.

[0030] Each component of the inorganic coated sand will be described below.

[0031] [Recycled sand (A)] The reclaimed sand (A) is an aggregate, and is a refractory material that is recycled from used casting molds or cores formed from a refractory aggregate and a binder. Preferably, the reclaimed sand (A) has a refractory aggregate and an inorganic binder layer formed on the surface of the refractory aggregate and containing one or more selected from silicates and reaction products of silicates. The reclaimed sand (A) is obtained, for example, by the manufacturing method described below.

[0032] (Fireproof aggregate) The material of the refractory aggregate constituting the reclaimed sand (A) may be one or more selected from the group consisting of natural sand and artificial sand. The refractory aggregate is specifically composed of a group of refractory aggregate particles.

[0033] Examples of natural sand include one or more types selected from the group consisting of silica sand, which is mainly composed of quartz, chromite sand, zircon sand, olivine sand, and alumina sand.

[0034] Examples of artificial sand include one or more types selected from the group consisting of synthetic mullite sand, SiO2-based foundry sand mainly composed of SiO2, Al2O3-based foundry sand mainly composed of Al2O3, SiO2 / Al2O3-based foundry sand, SiO2 / MgO-based foundry sand, SiO2 / Al2O3 / ZrO2-based foundry sand, SiO2 / Al2O3 / Fe2O3-based foundry sand, and slag-derived foundry sand. Here, the term "major component" refers to the component contained in the sand in the greatest amount. Artificial sand is not found in nature, but is found in sand that has been artificially prepared from metal oxide components and melted or sintered. In addition, recycled sand made from recycled refractory aggregate and recycled sand that has been regenerated can also be used.

[0035] The content of each component such as SiO2, Al2O3, and Fe2O3 in the refractory aggregate can be measured using the following X-ray fluorescence method. The refractory aggregate is adjusted to a size of approximately 0.1 μm or less using a vibration mill and heated at 1050°C for 1 hour. Then, 5 g of lithium tetraborate and 0.5 g of refractory aggregate are mixed and heated at 1200°C for 10 minutes to melt, and then cooled to prepare a glassy sample (glass bead method). The sample is subjected to X-ray fluorescence analysis using the Fundamental Parameter (FP) method using an X-ray fluorescence analyzer ZSX Primus II (manufactured by Rigaku Corporation).

[0036] In this embodiment, the sphericity of the refractory aggregate is the same as that of the inorganic coated sand, and therefore the preferred conditions are the same. The average particle size of the refractory aggregate is preferably 0.05 mm or more, more preferably 0.1 mm or more, from the viewpoints of improving mold quality and mold strength, and of ease of mold making. When the average particle size of the refractory aggregate is equal to or more than the above lower limit, the amount of inorganic binder layer used as the second coating layer during mold production can be reduced, which is also preferable in that it makes it easier to regenerate the inorganic coated sand. The average particle size of the refractory aggregate is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less, from the viewpoints of improving the mold quality and strength, and of ease of mold making. In addition, if the average particle size of the refractory aggregate is equal to or less than the above upper limit, it is also preferable in that the porosity is reduced during mold production, and the mold strength can be increased.

[0037] The degree of amorphization of the refractory aggregate is preferably 20% or more, more preferably 30% or more, and even more preferably 40% or more, from the viewpoint of obtaining a smoother surface of the aggregate and thus improving mold strength, and from the viewpoint of obtaining low thermal expansion. The upper limit of the degree of amorphization of the refractory aggregate is not limited, but may be, for example, 100% or less, and may be 99% or less.

[0038] The degree of amorphization of the refractory aggregate can be measured by the following X-ray diffraction method. (X-ray diffraction method) The refractory aggregate is crushed in a mortar and pressed against an X-ray glass holder of a powder X-ray diffractometer for measurement. The powder X-ray diffractometer is a Rigaku MultiFlex (CuKα light source, tube voltage 40 kV, tube current 40 mA), and the measurement is performed in the range of 2θ = 5 to 90° with a scan interval of 0.01°, a scan speed of 2° / min, and slits DS1, SS1, and RS0.3 mm. In the range of 2θ = 10° to 50°, the X-ray intensities on the low angle side and the high angle side are connected with a straight line, the area under the straight line is taken as the background, the crystallinity is calculated using the software attached to the device, and the degree of amorphousness is calculated by subtracting it from 100. Specifically, for the area above the background, the amorphous peak (halo) and each crystalline component are separated by curve fitting, the area of ​​each is calculated, and the degree of amorphousness (%) is calculated using the following formula. Amorphous content (%) = halo area / (crystalline component area + halo area) x 100

[0039] There are various methods for controlling the degree of amorphization of refractory aggregate, but it is generally preferable to use a manufacturing method that rapidly cools the molten material. For example, there is a method in which the raw material is melted and rapidly cooled by crushing it with air, or a method in which it is treated in a flame and rapidly cooled. In either case, the cooling method may be appropriately selected at various speeds depending on the material and particle size. Another possible method is to amorphize a material that has once been crystallized by heat treatment and cooling treatment. Among these, the use of a flame fusion method, in which heating and cooling can be easily controlled, is preferable.

[0040] (Inorganic binder layer) The reclaimed sand (A) preferably has an inorganic binder layer. Specifically, the inorganic binder layer contains one or more selected from silicates and reaction products of silicates, and covers the surface of the refractory aggregate. The coating is not limited to a continuous coating, and may have discontinuous portions.

[0041] The inorganic binder layer is intended to be one in which, when inorganic coated sand having a refractory aggregate and an inorganic binder formed on the surface of the refractory aggregate is molded into a casting mold, used as a mold, and then regenerated to produce regenerated sand, the inorganic binder is present on the surface of the refractory aggregate as a residual inorganic binder. That is, the silicate and the reaction product of the silicate contained in the inorganic binder layer intend that the residual inorganic binder is present on the surface of the refractory aggregate. The above-mentioned silicate and reaction product of silicate are specifically, for example, silicate and metasilicate, and the reaction product can be, for example, a reaction product of silicate and amorphous silica, or a reaction product of silicate and amorphous silica, and one or more types are mixed.The cations constituting the salt can be, for example, monovalent cations such as sodium, potassium, lithium, and ammonium, and divalent cations such as magnesium, calcium, and zinc.

[0042] Methods for confirming that the inorganic binder layer contains silicates or reactants of silicates include, for example, a method in which the recycled sand is stirred in a hydrochloric acid solution, the components eluted are analyzed with an ICP emission spectrometer, and the concentrations of silicate ions, sodium ions, etc. are determined, a method in which the surface of the recycled sand is subjected to elemental analysis with a scanning electron microscope - energy dispersive X-ray spectroscopy (SEM-EDX) to confirm the presence of silicon, sodium, etc., or 23 Na, 29 One method is to confirm the silicate-derived structure using Si solid-state NMR.

[0043] [Fire-resistant aggregate (B)] The refractory aggregate (B) has an amorphous degree of at least 20% or more, preferably 30% or more, from the viewpoint of improving mold strength by making the surface of the aggregate smoother, and from the viewpoint of obtaining low thermal expansion, and from the viewpoint of improving storage stability, the amorphous degree is preferably 99% or less, more preferably 80% or less, even more preferably 70% or less, and even more preferably 60% or less.

[0044] From the viewpoint of storage stability, the SiO2 content of the refractory aggregate (B) is preferably 10% or more, more preferably 20% or more, and even more preferably 30% or more, and from the viewpoint of further improving mold strength, it is preferably 99% or less, more preferably 80% or less, and even more preferably 70% or less. From the viewpoint of improving storage stability, the SiO2 content of the refractory aggregate (B) is preferably 50% or less, and more preferably 40% or less.

[0045] The degree of amorphization of the refractory aggregate (B) is determined by the X-ray diffraction method in the same manner as for the refractory aggregate of the recycled sand (A). In addition, the SiO2 content in the refractory aggregate (B) can be measured using the same X-ray fluorescence method as for the refractory aggregate in the recycled sand (A).

[0046] [Casting sand] The molding sand has a first coating layer formed on the surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B) as its outermost layer. The molding sand can function as inorganic coated sand by further forming a second coating layer on the first coating layer. The cation exchange capacity (CEC) of the foundry sand needs to be controlled to a specific value in order to prevent the inorganic coated sand from becoming wet. The cation exchange capacity (CEC) can be controlled by combining known methods, for example, by selecting the material of the coating layer, adjusting the content, and adjusting the firing temperature and time. Specifically, molding sand is composed of a group of molding sand particles.

[0047] The CEC of foundry sand is determined by the ammonium acetate method shown below (Fertilizer Analysis Method (Ministry of Agriculture, Forestry and Fisheries National Institute for Agro-Environmental Sciences Method) 5.31.1). First, a small piece of absorbent cotton is placed at the bottom of the permeation tube as a support layer, and filter paper pulp made by cutting filter paper into small pieces and stirring it in hot water is packed on top of it to a thickness of about 5 mm to create a flat filtration surface. Next, a plug is placed at the bottom end of the permeation tube and several mL of 1M ammonium acetate solution is added, and 2-4 g of the analytical sample (casting sand) is weighed out and allowed to fall and settle in small amounts until the sample is filled. The plug is then removed, the device is assembled, and washing with ammonium acetate solution begins. 100 mL of 1M ammonium acetate solution is used, and the dripping speed is adjusted so that permeation is complete in 4-20 hours. After permeation is complete, the upper inside of the permeation tube is washed off with a small amount of alcohol, and the sample layer is washed with 50 mL of 80% alcohol to remove excess ammonium acetate solution. The NH4 + The analytical sample saturated with NH4 was washed with 100 mL of 10% sodium chloride solution. + The amount of ammonia nitrogen in the leachate is determined by steam distillation and alkali titration, and expressed as millimole equivalents per kg of analytical sample, which is the cation exchange capacity.

[0048] The cation exchange capacity (CEC) is 3 mmol(+) / kg or more, and preferably 6 mmol(+) / kg or more, from the viewpoint of enhancing storage stability. On the other hand, from the viewpoint of enhancing storage stability, the cation exchange capacity (CEC) is 40 mmol(+) / kg or less, preferably 20 mmol(+) / kg or less, and more preferably 10 mmol(+) / kg or less.

[0049] (1st coating layer) The first coating layer constituting the molding sand is a layer for coating the surface of one or two types of aggregate selected from the recycled sand (A) and the refractory aggregate (B). The first coating layer constitutes the outermost layer of the molding sand, and in the case of inorganic coated sand, it is located between the second coating layer (described below) and the surface of the aggregate.

[0050] The first coating layer is made of a different material from the second coating layer, and preferably does not contain at least metasilicate, and more preferably is a layer formed from an aluminosilicate, which can efficiently prevent the silicate in the second coating layer from acting on the aggregate and promoting the wetting of the inorganic coated sand.

[0051] Examples of the aluminosilicate include a reaction product of one or more selected from silicates and reaction products of silicates with an aluminate or aluminum hydroxide. Here, silicate refers to a substance that contains an anion group with one or several silicon atoms at the center and electronegative ligands surrounding it in its composition. Specifically, it refers to either the residual inorganic binder present on the surface of the refractory aggregate or the refractory aggregate (B), or both. In order to facilitate improving storage stability, it is preferable that the aluminosilicate contains at least one selected from among silicates and reaction products of silicates, and a reaction product of sodium aluminate or aluminum hydroxide. The form of sodium aluminate is not particularly limited, and it may be either a powder or an aqueous solution.

[0052] The content of aluminum in the first coating layer, calculated as Al2O3, is preferably 0.1 part by mass or more, and more preferably 0.4 part by mass or more, per 100 parts by mass of the aggregate, in terms of enhancing storage stability. On the other hand, the aluminum content in the first coating layer, calculated as Al2O3, is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of aggregate, in order to increase the mold strength while obtaining good storage stability.

[0053] The aluminum content in the first coating layer is determined by the following method. The coefficient of elasticity can be calculated from the following formula using the analytical values ​​of the aggregates obtained by the fluorescent X-ray method and the analytical values ​​of the molding sand containing the first coating layer using these aggregates. Al2O3 of the first coating layer [parts by mass] = {Al2O3 of the molding sand [parts by mass]} - {Al2O3 of the aggregate [parts by mass]}

[0054] From the viewpoint of improving storage stability and obtaining a high-strength casting mold, the content of the first coating layer is preferably 0.02 parts by mass or more per 100 parts by mass of aggregate, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and especially preferably 2 parts by mass or more. From the viewpoint of achieving both storage stability and strength, the content of the first coating layer is preferably 10 parts by mass or less, and more preferably 9.5 parts by mass or less, relative to 100 parts by mass of the aggregate.

[0055] [Second coating layer] The second coating layer is a layer formed on the first coating layer, and is the outermost layer of the inorganic coated sand.

[0056] The second coating layer contains metasilicate and is used to impart a binder function to the aggregate. This is preferable because it can improve the crystallinity of the second coating layer, and the inorganic coated sand becomes dry and has excellent fluidity at room temperature.

[0057] Examples of metasilicates include one or more selected from sodium metasilicate, potassium metasilicate, lithium metasilicate, ammonium metasilicate, and the like, and hydrates thereof. Among them, sodium metasilicate and potassium metasilicate are preferred. The amount of water of hydration of the metasilicate hydrate is not particularly limited, but is preferably 5 to 9. Specifically, at least one selected from sodium metasilicate pentahydrate and sodium metasilicate nonahydrate is preferred, and sodium metasilicate nonahydrate is more preferred.

[0058] From the viewpoint of improving storage stability and obtaining a high-strength casting mold, the content of the second coating layer is preferably 0.05 parts by mass or more per 100 parts by mass of aggregate, more preferably 0.1 parts by mass or more, even more preferably 0.5 parts by mass or more, particularly preferably 1 part by mass or more, and even more preferably 2 parts by mass or more. On the other hand, from the standpoint of achieving both storage stability and strength, the content of the second coating layer is preferably 10 parts by mass or less per 100 parts by mass of aggregate, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less.

[0059] From the viewpoints of improving mold strength, excellent productivity, and ease of availability, the content of metasilicate in the second coating layer is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, still more preferably 98 mass% or more, and even more preferably substantially 100 mass%. Here, the term "substantially" means that it may contain components that are unintentionally contained, for example, components other than metasilicate that are contained in the metasilicate raw material. The total content of metasilicate in the second coating layer refers to the total content of metasilicate relative to all components other than water in the second coating layer.

[0060] The content of metasilicate in the second coating layer (anhydride equivalent) is preferably 0.03 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.5 parts by mass or more, and even more preferably 0.9 parts by mass or more, per 100 parts by mass of aggregate, from the viewpoint of improving storage stability and obtaining a high-strength casting mold. On the other hand, from the viewpoint of achieving both storage stability and strength, the content of metasilicate is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, even more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of aggregate.

[0061] (Inorganic fine particles) In this embodiment, the inorganic coated sand may further contain inorganic fine particles. When inorganic fine particles are included, it is preferable that the inorganic fine particles form a part of the second coating layer. Specifically, it is preferable that the second coating layer further includes inorganic fine particles at least on or in the layer, and it is more preferable that the second coating layer further includes inorganic fine particles on the layer. The inorganic fine particles may be included both on and in the second coating layer. In this way, the particles of the inorganic coated sand are more firmly bonded to each other via the inorganic fine particles, and as a result, the strength of the obtained mold can be further improved. The inorganic fine particles on the second coating layer may be partially embedded in the second coating layer.

[0062] The inorganic fine particles are not limited, and may be, for example, one or more fine particles selected from silica, silicon, zinc oxide, aluminum hydroxide, and tin oxide. Among them, silica particles are preferred from the viewpoint of improving the strength of the mold, and amorphous silica particles are more preferred from the viewpoint of large specific surface area and high reactivity with silicate. These inorganic fine particles may be used alone or in combination of two or more.

[0063] (Other additives) In addition to the above-mentioned components, the second coating layer may contain various additives as necessary, such as coupling agents, moisturizers, moisture resistance improvers, lubricants, surfactants, and mold release agents. The coupling agent is not limited, but examples thereof include silane coupling agents, zircon coupling agents, and titanium coupling agents. Examples of the moisturizing agent include polyhydric alcohols, water-soluble polymers, hydrocarbons, sugars, proteins, and inorganic compounds other than those mentioned above. Examples of the moisture resistance improver include metal oxides (other than those listed above), carbonates, borates, sulfates, phosphates, and the like. Examples of lubricants include waxes; fatty acid amides; alkylene fatty acid amides; stearic acid; stearyl alcohol; metal stearates such as lead stearate, zinc stearate, calcium stearate, and magnesium stearate; stearic acid monoglyceride; stearyl stearate; and hardened oils. Examples of the release agent include paraffin, wax, light oil, machine oil, spindle oil, insulating oil, waste oil, vegetable oil, fatty acid ester, organic acid, graphite particles, mica, vermiculite, fluorine-based release agents, and silicone-based release agents.

[0064] (moisture content) From the viewpoint of obtaining a high-strength mold, the content of water, including water of crystallization, in the second coating layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of silicate (anhydrous equivalent). In addition, from the viewpoint of filling into the molding die and obtaining a high-strength mold, the water content in the second coating layer is preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less, per 100 parts by mass of silicate.

[0065] The content of water, including water of crystallization, in the second coating layer contained in the inorganic coated sand can be adjusted depending on the type of silicate.

[0066] When the metasilicate is sodium metasilicate, from the viewpoint of obtaining a high-strength mold and from the viewpoint of easily manufacturing the mold, the content of water including water of crystallization in the second coating layer is preferably 60 parts by mass or more, more preferably 65 parts by mass or more, even more preferably 90 parts by mass or more, and even more preferably 110 parts by mass or more, relative to 100 parts by mass of sodium metasilicate (anhydrous equivalent); and from the viewpoint of improving fluidity and further improving the fillability into the molding die, it is preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less. For example, when the silicate constituting the second coating layer is only sodium metasilicate pentahydrate, the water content is 74 parts by mass per 100 parts by mass of sodium metasilicate, and when the silicate constituting the second coating layer is only sodium metasilicate nonahydrate, the water content is 133 parts by mass per 100 parts by mass of sodium metasilicate.

[0067] <Manufacturing method of reclaimed sand (A) / Method of reclaiming used casting sand> The method of regenerating the waste mold sand after casting can be based on known methods (for example, "Mold Making Method", 4th edition, Japan Foundry Technology Association, November 18, 1996, pp. 327-330). For example, methods such as dry grinding (mechanical abrasion), wet grinding, and roasting, as well as combinations of these processes, are known.

[0068] In the dry grinding process, a part of the inorganic binder layer residue present on the surface of the refractory aggregate can be removed. For example, the removal can be performed using a sand reclaimer in which sand is raised in the device by a high-speed air current and collided with a collision plate to perform grinding by collision and friction between sand particles, a high-speed rotary reclaimer in which sand is charged onto a rotor rotating at high speed and grinded by collision and friction between the thrown sand generated by the centrifugal force and the falling charged sand, or an agitator mill in which grinding is performed by utilizing friction between sand particles. As an example of the wet grinding treatment, there is a method using a trough grinder in which grinding is performed by friction between sand grains in a trough with rotating blades.

[0069] The roasting treatment may be, for example, a method in which sand is continuously charged into a roasting furnace such as a fluidized roasting furnace or a rotary kiln and roasted at a temperature in the range of 200 to 1000° C. It is also known that roasting at a temperature of 600 to 800° C. is used to further improve accuracy.

[0070] Any method may be used for regeneration, but the wet treatment and roasting treatment are complicated steps and involve a large energy load, so among them, the dry grinding treatment is preferred.

[0071] <Manufacturing method of inorganic coated sand> Next, a method for producing the inorganic coated sand of this embodiment will be described. The method for producing inorganic coated sand of the present embodiment is a method for producing dry inorganic coated sand having foundry sand comprising one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), a first coating layer covering the aggregate and positioned on the surface thereof, and a second coating layer containing metasilicate on the first coating layer of the foundry sand, wherein the refractory aggregate (B) contains SiO2, and the cation exchange capacity (CEC) of the foundry sand satisfies the range of 3 mmol(+) / kg to 40 mmol(+) / kg.

[0072] According to the manufacturing method of this embodiment, by forming a first coating layer on the surface of the aggregate and controlling the cation exchange capacity (CEC) of the foundry sand, it is possible to improve storage stability while eliminating the need for a roasting process for the aggregate, thereby reducing thermal energy consumption and mitigating the environmental burden.

[0073] First, as an example of a method for producing the inorganic coated sand of this embodiment, the refractory aggregate (B) contains SiO2, and the method includes the following steps (1) to (3). Step (1): A step of mixing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, forming the first coating layer on the surface of the aggregate, and obtaining molding sand. Step (2): A step of mixing the obtained molding sand with a molten liquid of metasilicate hydrate to obtain a mixture. Step (3): cooling the mixture obtained to a temperature below the melting point of the metasilicate hydrate to form the second coating layer on the first coating layer.

[0074] In step (1), the aluminate or aluminum hydroxide is mixed with the aggregate to form a first coating layer so as to cover the surface of the aggregate. In particular, it is preferable to form the first coating layer by heating to 25°C or higher and lower than 400°C. Examples of the method for forming the first coating layer by heating to 25°C or more and less than 400°C in step (1) include a method in which an aluminate is added to aggregate heated to 25°C or more and less than 400°C, or a method in which an aluminate or aluminum hydroxide is added to the aggregate and then heated to 25°C or more and less than 400°C. Among these, the latter method is preferred from the viewpoint of forming a uniform coating layer. From the viewpoint of improving storage stability, the heating temperature is preferably 40° C. or higher and 300° C. or lower, and more preferably 70° C. or higher and 200° C. or lower.

[0075] Examples of the method for forming the first coating layer by heating to 25°C or more and less than 400°C in step (1) include a method in which an aluminate or aluminum hydroxide is added to aggregate heated to 25°C or more and less than 400°C, or a method in which an aluminate or aluminum hydroxide is added to the aggregate and then heated to 25°C or more and less than 400°C. Among these, the latter method is preferred from the viewpoint of forming a uniform coating layer. From the viewpoint of improving storage stability, the heating temperature is preferably 40° C. or higher and 300° C. or lower, and more preferably 70° C. or higher and 200° C. or lower. The mixing conditions such as the stirring speed and processing time when mixing the aggregate with the aluminate or aluminum hydroxide can be appropriately determined depending on the processing amount of the mixture. This results in molding sand with a cation exchange capacity (CEC) of 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.

[0076] In step (2), the foundry sand is mixed with a molten liquid of metasilicate hydrate to obtain a mixture. Examples of the method for mixing the molten metasilicate hydrate with the molding sand in step (2) include a method in which the metasilicate is poured into molding sand heated to the melting point of the metasilicate hydrate or higher, and a method in which the metasilicate heated to the melting point of the metasilicate hydrate or higher is poured into the molding sand. Among these, the latter method is preferred from the viewpoint of shortening the coating time. The mixing conditions, such as the stirring speed and processing time, when mixing the foundry sand and the metasilicate hydrate can be appropriately determined depending on the processing amount of the mixture.

[0077] In step (3), the mixture obtained in step (2) is cooled to a temperature below the melting point of the metasilicate hydrate to reduce the fluidity of the metasilicate hydrate and fix the metasilicate hydrate to the surface of the foundry sand, thereby forming a metasilicate hydrate layer, i.e., a second coating layer. In this way, the inorganic coated sand according to this embodiment can be obtained.

[0078] Next, as another example of the method for producing the inorganic coated sand of this embodiment, the refractory aggregate (B) contains SiO2, and the method includes the following steps (4) to (5). Step (4): A step of mixing one or two types of aggregate selected from the recycled sand (A) and the refractory aggregate (B) with an aluminate or aluminum hydroxide, forming the first coating layer on the surface of the aggregate, and obtaining molding sand. Step (5): mixing the foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing sodium metasilicate hydrate.

[0079] Step (4) can be carried out in the same manner as step (1) above.

[0080] In step (5), a metasilicate hydrate having a desired amount of water of hydration can be formed by adjusting the molar ratio of SiO2 / M2O (M represents an alkali metal) / H2O in a solution containing water glass, caustic alkali, and water to 1:1:n (5≦n≦9). Furthermore, by mixing the above-mentioned solution containing water glass, caustic alkali, and water with the above-mentioned molding sand, the surface of the molding sand can be coated with metasilicate hydrate to form a second coating layer. The conditions for mixing the water glass, the caustic alkali, and the water are not particularly limited, and a known method can be used. For example, the mixing may be performed at ambient temperature, and if the molten liquid generates heat, the mixing may be continued and then allowed to stand until the temperature reaches the ambient temperature.

[0081] In this way, the inorganic coated sand according to this embodiment can be obtained.

[0082] <Mold> The casting mold of this embodiment includes the inorganic coated sand of this embodiment and is formed using the inorganic coated sand. Examples of a molding method for the casting mold include a molding method using a heated molding die, and a molding method in which water vapor is passed through the heated molding die and then hot air is passed through the heated molding die.

[0083] <Method for improving storage stability> The method for improving the storage stability of the inorganic coated sand of the present embodiment includes: A foundry sand containing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate coating the foundry sand, comprising: The refractory aggregate (B) contains SiO2, The method includes a step of preparing dry inorganic coated sand so that the cation exchange capacity (CEC) of the foundry sand satisfies the range of 3 mmol(+) / kg to 40 mmol(+) / kg. This improves the storage stability of the inorganic coated sand. The step of adjusting the cation exchange capacity (CEC) of the foundry sand to 3 mmol(+) / kg or more and 40 mmol(+) / kg or less is carried out by adjusting the manufacturing method of the inorganic coated sand and the foundry sand. The details are the same as those explained in the above-mentioned manufacturing method of the inorganic coated sand. The details of the composition of the inorganic coated sand and the foundry sand are also the same as those explained above.

[0084] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted.

[0085] In relation to the above-mentioned embodiments, the present invention further discloses the following inorganic coated sand, a method for manufacturing the inorganic coated sand, and a method for manufacturing a casting mold.

[0086] <1> A foundry sand comprising one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B), and a first coating layer covering the aggregate and positioned on the surface; A dry inorganic coated sand having a second coating layer containing a metasilicate on the first coating layer of the foundry sand, The refractory aggregate (B) contains SiO2, The cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more, preferably 6 mmol(+) / kg or more, and 40 mmol(+) / kg or less, preferably 20 mmol(+) / kg or less, more preferably 10 mmol(+) / kg or less. <2> <1> The inorganic coated sand according to claim 1, The content of the first coating layer is 0.02 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, and is 10 parts by mass or less, preferably 9.5 parts by mass or less, per 100 parts by mass of the aggregate, of the inorganic coated sand. <3> <1> or <2> The inorganic coated sand according to claim 1, The content of the second coating layer is 0.05 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, per 100 parts by mass of the aggregate, and is 10 parts by mass or less, preferably 8 parts by mass or less, and more preferably 6 parts by mass or less. <4> <1> ~ <3> The inorganic coated sand according to any one of the preceding claims, The first coating layer of the foundry sand contains an aluminosilicate, the aluminosilicate containing a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, with an aluminate or aluminum hydroxide. <5> <1> ~ <4> The inorganic coated sand according to any one of the preceding claims, The aluminosilicate comprises at least one of a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, and sodium aluminate or aluminum hydroxide. <6> <1> ~ <5> The inorganic coated sand according to any one of the above, The inorganic coated sand has a dynamic angle of repose of preferably 80° or less, more preferably 45° or less, and further preferably 30° or less. <7> <1> ~ <6> The inorganic coated sand according to any one of the above, The degree of amorphization of the refractory aggregate (B) is preferably 30% or more, more preferably 50% or more, even more preferably 65% ​​or more, and even more preferably 80% or more, while it is preferably 100% or less, and more preferably 99% or less. <8> <1> ~ <7> The inorganic coated sand according to any one of the above, The SiO2 content of the refractory aggregate (B) is preferably 10% or more, preferably 20% or more, more preferably 30% or more, while it is preferably 99% or less, more preferably 80% or less, even more preferably 70% or less, particularly preferably 50% or less, and even more particularly preferably 40% or less. <9> <1> ~ <8> The inorganic coated sand according to any one of the above, The aluminum content in the first coating layer, calculated as Al2O3, is preferably 0.1 parts by mass or more, and more preferably 0.4 parts by mass or more, per 100 parts by mass of the aggregate, and is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less. <10> <1> ~ <9> The inorganic coated sand according to any one of the above, The content of metasilicate in the second coating layer is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, still more preferably 98% by mass or more, and even more preferably substantially 100% by mass of the inorganic coated sand. <11> <1> ~ <10> The inorganic coated sand according to any one of the above, The content of water, including water of crystallization, in the second coating layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, relative to 100 parts by mass of silicate (anhydrous equivalent), while being preferably 180 parts by mass or less, more preferably 160 parts by mass or less, even more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less. <12> <1> ~ <11> A casting mold comprising the inorganic coated sand according to any one of the preceding claims. <13> A method for producing inorganic coated sand, comprising the steps of: A step (1) of mixing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming the first coating layer on the surface of the aggregate to obtain the foundry sand; (2) mixing the obtained foundry sand with a molten liquid of metasilicate hydrate to obtain a mixture; (3) cooling the mixture to a temperature below the melting point of the metasilicate hydrate; Including, The method for producing inorganic coated sand, wherein the refractory aggregate (B) contains SiO2. <14> A method for producing inorganic coated sand, comprising the steps of: (4) mixing one or two aggregates selected from the group consisting of recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming the first coating layer on the surface of the aggregate to obtain the foundry sand; and (5) mixing the obtained foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate, The method for producing inorganic coated sand, wherein the refractory aggregate (B) contains SiO2. <15> <13> or <14> A method for producing the inorganic coated sand according to claim 1, A method for producing inorganic coated sand, in which in step (1) or (4), the first coating layer is formed by heating to a temperature of 25°C or higher but lower than 400°C, preferably 40°C or higher but lower than 300°C, and more preferably 70°C or higher but lower than 200°C. <16> <14> A method for producing the inorganic coated sand according to claim 1, A method for producing inorganic coated sand, wherein in step (5), the molar ratio of SiO2 / M2O (M represents an alkali metal) / H2O in a solution containing water glass, caustic alkali, and water is 1:1:n (5≦n≦9). <17> A foundry sand containing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate coating the foundry sand, comprising: The refractory aggregate (B) contains SiO2, A method for improving the storage stability of inorganic coated sand, comprising preparing the dry inorganic coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less. EXAMPLES

[0087] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.

[0088] (1) Material The materials used in the following examples and comparative examples will be described. [Fire-resistant aggregate] Fireproof aggregate 1: Espearl #60L (manufactured by Yamakawa Sangyo Co., Ltd., average particle size: 241 μm, degree of amorphization: 45%) Refractory aggregate (B1): Spherical fused silica (natural silica sand spheroidized by the flame fusion method, average particle size: 200 μm, degree of amorphization: 95% or more) Fireproof aggregate (B2): Naigai Cera Beads 60 #650 (manufactured by Itochu Ceratec Co., Ltd., average particle size: 200 μm, degree of amorphization: 30%)

[0089] [Inorganic fine particles] Amorphous silica particles: Denka fused silica SFP-20M (manufactured by Denka, average particle size: 0.4 μm, degree of amorphization: 99.5% or more) Calcined kaolin: Satinton W (BASF, average particle size: 0.4 μm)

[0090] [Recycled sand (A)] Reclaimed sand (A1) was prepared according to the following procedure. (i) Preparation of inorganic coated sand 100 parts by mass of refractory aggregate 1 (Espearl #60L) was put into the mixer as the refractory aggregate. Next, sodium metasilicate nonahydrate (2.00 parts by mass) that had been heated to 80°C and melted was put into the mixer and kneaded for 4 minutes to obtain dry sand with room temperature fluidity. Then, amorphous silica fine particles (0.6 parts by mass) were added and kneaded for 2 minutes to obtain dry inorganic coated sand to be used for producing reclaimed sand (A1). (ii) Preparation of the template A portion of the obtained 10 kg of inorganic coated sand was poured into the center of a truncated cone mold for producing a test mold, with an upper diameter of 298 mm, a lower diameter of 205 mm, and a height of 265 mm, to a height of 50 mm. Next, a truncated cone metal core with an upper diameter of 280 mm, a lower diameter of 200 mm, and a height of 220 mm, which had been heated to 180°C, was placed in the mold. The remaining inorganic coated sand was poured into the space between the mold and the metal core, and the mold was heated in a heating furnace at 180°C for 20 minutes to obtain a test mold. (iii) Casting 10 kg of aluminum alloy AC4C material (720℃) was poured into the obtained test mold. After pouring, it was left to stand at room temperature and cooled. (iv) Preparation of recycled sand After casting, the casting was removed from the test mold, and the test mold was crushed with a hammer or the like, and further crushed in a mini crusher (manufactured by Taiyo Machinery Co., Ltd.) until the mold became single particles, and recovered sand was obtained. (v) Preparation of recycled sand 100 kg of the recycled sand was put into a dry-type foundry sand reclamation device equipped with a fluidized bed (Hybrid Sand Master manufactured by Nippon Foundry Co., Ltd.) and batch-processed for 60 minutes at a rotor speed of 2400 rpm to obtain recycled sand (A1). Fine powder derived from the binder generated during the process was removed by a dust collector.

[0091] [Material for first coating layer] 50% sodium aluminate: Sodium aluminate #2019 (50% sodium aluminate aqueous solution manufactured by Asada Chemical Industry Co., Ltd.) Aluminum hydroxide (Al(OH)3): Aluminum hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, powder form, average particle size: 2.01 μm) No. 2 water glass: No. 2 sodium silicate (manufactured by Fuji Chemical Co., Ltd., Si / Na molar ratio 2.4)

[0092] [Material for second coating layer] Sodium metasilicate nonahydrate: Sodium metasilicate nonahydrate (manufactured by Nippon Chemical Industry Co., Ltd.)

[0093] (2) Preparation of inorganic coated sand Each inorganic coated sand having the composition shown in Table 1 was prepared by the following procedure.

[0094] <Example 1> 100 parts by mass of reclaimed sand (A1) was put into a mixer as a refractory aggregate. Next, 2.3 parts by mass of 50% sodium aluminate aqueous solution was put in and stirred for 2 minutes to obtain a mixture. The mixture was then heat-treated in a calciner at a roasting temperature of 80°C for 12 hours, cooled to room temperature, and then sieved through a sieve (20 mesh) to remove aggregates in the mixture, thereby obtaining a foundry sand having a first coating layer made of aluminosilicate formed on the surface of the reclaimed sand (A1). Next, the foundry sand and sodium metasilicate nonahydrate (3.50 parts by mass) that had been heated to 80°C and melted were charged into a mixer and kneaded for 4 minutes to form a second coating layer on the first coating layer, thereby obtaining the inorganic coated sand of Example 1. Table 1 shows the blending composition of the inorganic coated sand.

[0095] <Examples 2 to 3> The inorganic coated sands of Examples 2 and 3 listed in Table 1 were obtained in the same manner as Example 1, except that the amount of 50% sodium aluminate aqueous solution added when forming the first coating layer made of aluminosilicate on the surface of the reclaimed sand (A1) was changed to the mass parts shown in Table 1.

[0096] <Example 4> The inorganic coated sand of Example 4 shown in Table 1 was obtained in the same manner as in Example 1, except that 0.1 parts by mass of No. 2 water glass was added when the 50% sodium aluminate aqueous solution was added to form the first coating layer made of aluminosilicate on the surface of the reclaimed sand (A1).

[0097] <Examples 5 to 8> Inorganic coated sand was obtained in the same manner as in Example 1, except that the roasting temperature for forming a first coating layer made of an aluminosilicate on the surface of the reclaimed sand (A1) was changed to the temperatures shown in Table 1. Table 1 shows the blending compositions of the inorganic coated sands of Examples 5 to 8.

[0098] <Example 9> Inorganic coated sand was obtained in the same manner as in Example 1, except that a suspension of aluminum hydroxide previously suspended in water (aluminum hydroxide:water=1:1 mass ratio) was used instead of the 50% aqueous sodium aluminate solution. Table 1 shows the blending composition of the inorganic coated sand of Example 9.

[0099] <Examples 10 and 12> Inorganic coated sand was obtained in the same manner as in Example 2, except that the reclaimed sand (A1) used as the refractory aggregate was changed to the refractory aggregate shown in Table 2. Table 2 shows the mix compositions of the inorganic coated sands of Examples 10 and 12.

[0100] <Example 11> Inorganic coated sand was obtained in the same manner as in Example 3, except that the reclaimed sand (A1) as the refractory aggregate was changed to the refractory aggregate shown in Table 2. Table 2 shows the mix composition of the inorganic coated sand of Example 11.

[0101] <Example 13> Using the inorganic coated sand obtained in Example 2, regenerated sand (A2) was obtained in the same manner as in Example 2, following the steps (ii) to (v) of the regenerated sand (A1). Using this regenerated sand (A2), inorganic coated sand was produced in the same manner as in Example 2, and the steps (ii) to (v) of the regenerated sand (A1) were repeated again to obtain regenerated sand (A3). Furthermore, using the regenerated sand (A3), the process of obtaining regenerated sand (A3) from the regenerated sand (A2) was repeated twice to obtain regenerated sand (A5). Reclaimed sand (A5) was used to obtain inorganic coated sand in the same manner as in Example 2. The results of storage stability are shown in Table 3.

[0102] <Comparative Example 1> Except for not adding 50% sodium aluminate or carrying out heat treatment, the inorganic coated sand of Comparative Example 1 containing the inorganic binder and not containing the first coating layer made of aluminosilicate was obtained in the same manner as in Example 1. Table 1 shows the composition of the inorganic coated sand of Comparative Example 1.

[0103] <Comparative Examples 2 to 3> Inorganic coated sands of Comparative Examples 2 and 3 were obtained in the same manner as in Example 1, except that 50% sodium aluminate was not added and heat treatment was carried out at the temperatures shown in Table 1. Table 1 shows the blending compositions of the inorganic coated sands of Comparative Examples 2 and 3.

[0104] <Comparative Example 4> 100 parts by mass of reclaimed sand (A1) was prepared as a refractory aggregate and put into a mixer. Then, 0.25 parts by mass of calcined kaolin, 0.25 parts by mass of amorphous silica fine particles, and 0.50 parts by mass of water were put in and mixed for 2 minutes. After that, the obtained mixture was heat-treated in an electric furnace at 730°C for 1 hour, then the heating of the electric furnace was stopped and the mixture was left in the electric furnace for 4 hours, and then the mixture was taken out of the electric furnace and cooled to room temperature at room temperature, and then the aggregates were removed from the mixture through a sieve (20 mesh). The obtained mixture and sodium metasilicate nonahydrate (3.50 parts by mass) heated to 80°C and melted were put into a mixer and kneaded for 4 minutes to obtain the inorganic coated sand of Comparative Example 4. Table 1 shows the composition of the inorganic coated sand.

[0105] <Comparative Examples 5 to 6> The inorganic coated sands of Comparative Examples 5 and 6 were obtained in the same manner as in Comparative Example 1, except that the reclaimed sand (A1) used as the refractory aggregate was changed to the type of refractory aggregate shown in Table 2. Table 2 shows the mix compositions of the inorganic coated sands of Comparative Examples 5 and 6.

[0106] (3) Evaluation and measurement The following evaluations and measurements were carried out using the obtained inorganic coated sand. The results are shown in Tables 1 and 2.

[0107] <Storage stability; Measurement of time until moisture buildup> Immediately after preparing the inorganic coated sand, the dynamic angle of repose of the inorganic coated sand was measured by the following procedure. Separately, immediately after preparing the inorganic coated sand, 2 kg of the inorganic coated sand was placed in a plastic bag, sealed, and left in a constant temperature room at 25°C / 55%RH, and the dynamic angle of repose of the inorganic coated sand was measured every 24 hours using the following procedure, and the condition of the inorganic coated sand (dry or wet) was confirmed as follows: If the inorganic coated sand had become wet, the time from placing it in the plastic bag until it became wet was recorded as the "time until wet" (days).

[0108] (i) Procedure (Measurement of dynamic angle of repose) Half the volume of inorganic coated sand was placed in a cylindrical transparent plastic bottle with a diameter of 76 mm and a height of 125 mm, and the bottle was rotated around the horizontal axis at room temperature (25°C) and a speed of 60 rpm. The inclined surface of the inorganic coated sand layer flowing inside the cylinder became flat, and the angle formed between the inclined surface and the horizontal plane (dynamic angle of repose) was measured. (ii) Verification (determination of dry or wet state) In the above procedure, the case where the angle could be measured was deemed to be "dry state", and the case where the inorganic coated sand did not flow inside the cylinder, or even if it did flow, the slope of the inorganic coated sand layer did not form a flat surface, and as a result, the dynamic angle of repose could not be measured was deemed to be "wet state".

[0109] [Table 1]

[0110] [Table 2]

[0111] [Table 3]

Claims

1. A dry inorganic coated sand comprising: foundry sand in which a first coating layer is disposed on a surface of one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate on the first coating layer of the foundry sand, The refractory aggregate (B) is SiO 2 and The cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less, and the dry inorganic coated sand is thus obtained.

2. The inorganic coated sand according to claim 1, The content of the first coating layer is 0.02 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the aggregate.

3. The inorganic coated sand according to claim 1 or 2, The content of the second coating layer is 0.05 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the aggregate.

4. The inorganic coated sand according to claim 1 or 2, The inorganic coated sand, wherein the first coating layer contains an aluminosilicate, the aluminosilicate containing a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, and an aluminate or aluminum hydroxide.

5. The inorganic coated sand according to claim 4, The aluminosilicate comprises at least one of a reaction product of one or more selected from the group consisting of silicates and reaction products of silicates, and sodium aluminate or aluminum hydroxide.

6. A casting mold made of the inorganic coated sand according to claim 1 or 2.

7. A step (1) of mixing one or two aggregates selected from recycled sand (A) and refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming a first coating layer on the surface of the aggregate to obtain molding sand; (2) mixing the obtained foundry sand with a molten liquid of metasilicate hydrate to obtain a mixture; (3) cooling the mixture to a temperature below the melting point of the metasilicate hydrate; Including, The refractory aggregate (B) is SiO 2 The method for producing inorganic coated sand comprises:

8. (4) mixing one or two aggregates selected from the recycled sand (A) and the refractory aggregate (B) with an aluminate or aluminum hydroxide, and forming a first coating layer on the surface of the aggregate to obtain molding sand; (5) mixing the obtained foundry sand with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate; Including, The refractory aggregate (B) is SiO 2 The method for producing inorganic coated sand comprises the steps of:

9. A method for producing the inorganic coated sand according to claim 7 or 8, The method for producing inorganic coated sand, wherein in the step (1) or (4), the first coating layer is formed by heating to a temperature of 25° C. or higher and lower than 400° C.

10. A foundry sand containing one or two types of aggregate selected from recycled sand (A) and refractory aggregate (B); and a second coating layer containing a metasilicate coating the foundry sand, comprising: The refractory aggregate (B) is SiO 2 and The method for improving the storage stability of inorganic coated sand comprises preparing the dry inorganic coated sand so that the cation exchange capacity (CEC) of the foundry sand is 3 mmol(+) / kg or more and 40 mmol(+) / kg or less.

Citation Information

Patent Citations

  • Porous masses or moulded bodies consisting of inorganic polymers and production thereof

    US20160068440A1

  • Particulate refractory compositions for use in the manufacture of foundry moulds and cores, methods of preparing same and corresponding uses

    WO2014019726A1

  • Coated sand, method for producing same, and method for producing casting mold using same

    WO2018097180A1

  • Inorganic coated sand

    WO2020012934A1

  • Thermal regeneration of foundry sand

    JP2010519042A