Manufacturing method of press die, and press die

The press mold manufacturing method addresses warpage and waviness issues by incorporating a rough surface with specific depth and height ratios, enhancing the quality and appearance of press-formed products.

JP2024164461APending Publication Date: 2024-11-27TOCALO CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023079947
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Existing press forming methods result in molded products with warpage, deformation, and surface waviness due to springback, particularly in automobile steel sheets, which affect the appearance and quality.

Method used

A press mold manufacturing method that includes forming a rough surface region with convex and concave portions on the molding surface, where the average depth of the concave portions exceeds the average height of the convex portions, to mitigate springback and waviness during press molding.

Benefits of technology

The method effectively suppresses warpage and deformation caused by springback, while reducing surface waviness, resulting in improved product quality and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164461000001_ABST
    Figure 2024164461000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a press die, in which generation of springback in molded articles can be suppressed, and undulation does not occur.SOLUTION: A manufacturing method of a press die includes a roughening process for forming a rough surface region at a part of a molding surface of a press die used for molding a steel plate. In the roughening process, a rough surface region including protrusions protruding from a molding surface before roughening, and recesses depressed from the molding surface before roughening is formed. In the rough surface region formed, an average depth of the recesses is larger than an average height of the protrusions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a press die, and a press die. [Background technology]

[0002] Press forming is a commonly known method for forming steel sheets for automobiles. When steel sheets for automobiles are press-molded using a press die, unexpected warping or deformation can occur in the molded product after the press-molded part is released from the press die due to springback (also known as elastic recovery) that occurs in the molded product, which is considered problematic.

[0003] Therefore, as a method for reducing elastic recovery, for example, Patent Document 1 proposes a press-molding method in which a second mold having a second mold surface is moved relative to a first mold having a first molding surface, and a raw metal plate is shaped by cooperation between the first molding surface and the second molding surface, in which linear protrusions are provided on the first molding surface and / or the second molding surface, and the linear protrusions are caused to bite into areas that have been subjected to bending deformation or bending back deformation during press molding, thereby forming linear recesses of a predetermined shape corresponding to the plate thickness of the press-molded part. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-087816 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that when a molded product (press-molded part) is produced using the method described in Patent Document 1, waviness may occur on the surface of the obtained molded product opposite to the surface on which the linear recesses are formed. If waviness occurs on the outer surface of an automotive steel sheet, the molded product will have a poor appearance.

[0006] FIG. 5 is a diagram for explaining the principle of waviness generation. As shown in Fig. 5, when a steel plate 53 is press-molded using a first molding die (lower die) 51 having protrusions on the molding surface and a second molding die (upper die) 52 having a flat molding surface, the obtained molded product 55 may have undulations 56 on a surface 55a (the upper surface in the figure) opposite to a surface 55b facing the first molding die 51. This is thought to be because the linear protrusions 64 of the first molding die 51 pierce the steel plate 53 during pressing, causing internal stress to accumulate in the steel plate 53, and the internal stress is released when the steel plate is released, causing the undulations 56 on the surface of the steel plate 53 facing the second molding die 52.

[0007] The present invention has been made in consideration of the above-described circumstances, and has an object to provide a method for manufacturing a press die, and a press die, which can suppress the occurrence of warping and deformation due to springback while avoiding the occurrence of the above-mentioned swell. [Means for solving the problem]

[0008] (1) The method for manufacturing a press die of the present invention comprises the steps of: A roughening process is provided for forming a roughened surface area on a part of a molding surface of a press die used for molding a steel sheet, The surface roughening step includes: This is a process for forming a roughened surface region having convex portions protruding from the molded surface before roughening and concave portions recessed from the molded surface before roughening, and the roughened surface region is formed in which the average depth of the concave portions is greater than the average height of the convex portions.

[0009] The above-mentioned method for manufacturing a press die forms a rough surface region having a predetermined uneven shape on a part of the molding surface. By performing press molding using the press die manufactured in this way, it is possible to suppress the occurrence of warping or deformation due to springback in the molded product. The method for manufacturing the press die forms a rough surface region in which the average depth of the recesses is greater than the average height of the protrusions. By performing press molding using the press die manufactured in this manner, it is possible to suppress the occurrence of waviness in the molded product.

[0010] (2) In the method for producing a press die according to (1) above, it is preferable that the roughened surface region has a surface roughness Rz of 500 μm or less and an average height of protrusions of 12 μm or more. (3) In the method for producing a press die according to (1) or (2) above, it is preferable that the roughened surface region has a surface roughness Rsm of 150 μm or more. (4) In any one of the above methods for manufacturing a press die (1) to (3), the surface roughening step is suitably performed using a laser. (5) Any of the above methods for manufacturing a press die (1) to (4) is suitable for a steel plate having a thickness of 1.5 mm or less. (6) Any of the above methods for manufacturing a press die (1) to (5) is suitable for use in a case where the steel sheet is an automotive steel sheet.

[0011] (7) The press die of the present invention is A press die used for forming a steel plate, The molding surface of the mold has a roughened area; The rough surface region has convex portions protruding from a reference surface corresponding to the molded surface before roughening, and concave portions recessed from the reference surface, and the average depth of the concave portions is greater than the average height of the convex portions.

[0012] The press die has a rough surface region with a predetermined uneven shape on a part of the molding surface. By performing press molding using this press die, it is possible to suppress the occurrence of warping or deformation due to springback in the molded product. The press die has a rough surface region in which the average depth of the recesses is greater than the average height of the protrusions, and therefore, by using this press die for press molding, it is possible to suppress the occurrence of waviness in the molded product.

[0013] (8) The press die of (7) above preferably has, as the roughened surface region, a surface roughness Rz of 500 μm or less and an average height of protrusions of 12 μm or more. (9) The press die of (7) or (8) above preferably has, as the roughened surface region, a roughened surface region having a surface roughness Rsm of 150 μm or more. (10) In any of the press dies described above in (7) to (9), the thickness of the steel plate is preferably 1.5 mm or less. (11) In any one of the press dies described above in (7) to (10), the steel sheet is preferably an automotive steel sheet. Effect of the Invention

[0014] According to the present invention, it is possible to provide a press die capable of manufacturing a molded product in which warping and deformation due to springback are unlikely to occur and in which the occurrence of waviness is also suppressed. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a diagram illustrating an example of a press die according to an embodiment of the present invention. [Diagram 2] 2 is a diagram showing a schematic view of a part of a molding surface of the press die of FIG. 1. [Diagram 3] 4A to 4C are diagrams illustrating the surface state of a molded product obtained using a press die according to an embodiment of the present invention. [Figure 4] FIG. 1 is a diagram showing a method for evaluating the springback suppression effect. [Diagram 5] 1A to 1C are diagrams for explaining the principle of waviness that occurs in conventional press molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described, but the embodiment of the present invention is not limited to the following embodiment.

[0017] (Press mold) Fig. 1 is a diagram showing an example of a press die according to an embodiment of the present invention, Fig. 2 is a diagram showing a part of a molding surface of the press die of Fig. 1. The press die 10 has a lower die 11 having an upper surface 11a as a molding surface, and an upper die 12 having a lower surface 12a as a molding surface. The press die 10 can press-mold the steel plate 13 by placing the steel plate 13 between the lower die 11 and the upper die 12 and moving the upper die 12 or the lower die 11 toward the opposite die.

[0018] The upper surface (molding surface) 11a of the lower mold 11 has a roughened area 22 and a non-roughened area . The rough surface area 22 has projections and recesses formed thereon by, for example, laser processing. The rough area 22 and the non-rough area 21 can be distinguished from each other by, for example, visual observation, observation with a magnifying glass, observation with a microscope, or the like. As shown in Figure 2, the roughened surface region 22 has a convex portion 24 protruding from a reference surface 25 (i.e., a surface obtained by extending the non-roughened surface region 21 in parallel toward the roughened surface region 22) corresponding to the molded surface before roughening, and a concave portion 23 recessed from the reference surface 25.

[0019] In the rough surface region 22, the average depth of the recesses 23 is greater than the average height of the protrusions 24. The reason why the occurrence of waviness can be suppressed when the rough surface region 22 has such an uneven shape is as follows.

[0020] FIG. 3 is a diagram illustrating the surface state of a molded product obtained using the press die according to the embodiment of the present invention. When press molding is performed using the press die according to this embodiment, when the convex portion 24 of the lower die 11 pierces the steel sheet 13, a gap S exists between the lower die 11 and the steel sheet 13. Therefore, when the convex portion 24 of the lower die 11 pierces the steel sheet 13, a force acts on the steel sheet around the portion where the convex portion 24 pierces so as to move into the gap S (see the arrows in FIG. 3). Therefore, when the press die according to this embodiment is used, it is possible to suppress the generation of undulations on the surface on the upper die side, and by using the surface on the upper die side as the outer plate surface of the automotive steel sheet, an automotive steel sheet with excellent design can be obtained.

[0021] The reference surface 25 corresponds to the molded surface before roughening, and after roughening, it can be derived from the waviness curve when the roughened region 22 is viewed in cross section. The waviness curve is obtained, for example, based on JIS B 0601 (2013) by the following method. First, a measured profile curve including a boundary point between a non-rough region and a rough region is obtained using a surface roughness measuring device, with at least one end of the measured profile curve being located on the non-rough region. Next, a profile curve is obtained by applying a profile curve filter with a cutoff value λs=8 μm to the measured profile curve. Then, a profile curve filter with a cutoff value λc of 2.5 mm and λf of no upper limit is applied to the measured profile curve to obtain a waviness curve. Then, by overlapping the acquired cross-sectional curve and undulation curve so that their ends located on the non-rough surface area coincide with each other, the undulation curve can be regarded as the position of the reference surface. In addition, a roughness curve can also be obtained from the measured profile curve by applying appropriate cutoff values ​​λs and λc. The numerical values ​​of the cutoff value λs, the cutoff value λc, and the cutoff value λf may be appropriately set based on JIS B 0633 (2013) and JIS B 0651 (2013).

[0022] In the rough surface region 22, the average height of the projections 24 is preferably 12 μm or more. In this case, it is more suitable for suppressing the occurrence of springback. More preferably, the average height of the projections is 26 μm or more. A preferred upper limit of the average height of the protrusions 24 is 60 μm.

[0023] In the rough surface region 22, the average depth of the recesses 23 and the average height of the protrusions 24 can be obtained by superimposing the cross-sectional curve and the waviness curve using the method described above. The average depth of the recesses 23 is the average value of the depths of the portions recessed below the waviness curve. The average height of the protrusions 24 is the average value of the heights of the portions protruding above the waviness curve.

[0024] The surface roughness Rz of the rough surface region 22 is preferably 500 μm or less. The surface roughness Rz is one of the roughness parameters defined in JIS B 0601 (2013), and is a parameter in the height direction called the maximum height. If the surface roughness Rz is 500 μm or less, deformation of the protrusions of the press die can be suppressed. A preferred lower limit of the surface roughness Rz is 25 μm.

[0025] The surface roughness Rsm of the roughened region 22 is preferably 150 μm or more. The surface roughness Rsm is one of the roughness parameters defined in JIS B 0601 (2013). When the surface roughness Rsm is 150 μm or more, the protrusions 24 of the rough surface region 22 are formed thick, so that deformation of the protrusions 24 during press molding can be suppressed. A preferred upper limit of the surface roughness Rsm is 500 μm.

[0026] The surface roughness Rz and the surface roughness Rsm in the rough surface region 22 are calculated based on the roughness curve obtained by the above-mentioned method.

[0027] The non-rough region 21 typically has a surface roughness Ra of 1 μm or less. The surface roughness Ra is one of the roughness parameters defined in JIS B 0601 (2013), and is a parameter in the height direction called the arithmetic mean roughness. The surface roughness Rz (JIS B 0601 (2013)) of the non-rough region 21 is typically 10 μm or less. The non-rough surface region 21 is provided in a region where springback is unlikely to occur or where the occurrence of springback will not cause any problems. The surface roughness Ra and surface roughness Rz of the non-roughened region 21 are not particularly limited as long as they are within the above-mentioned normal ranges.

[0028] In the press die 10, the protrusions 24 of the rough surface region 22 preferably have an HRC (Rockwell hardness) of 52 or more. In this case, since the hardness of the protrusions 24 is high, deformation of the shape of the protrusions 24 can be suppressed even if press molding is performed repeatedly.

[0029] The HRC of the protrusions 24 is preferably 60 or more when the tensile strength of the steel plate to be press-formed exceeds 440 MPa. When a steel plate with high tensile strength is press-molded, deformation of the shape of the protrusions 24 is likely to occur during press molding. In response to this, by setting the HRC to 60 or more, deformation of the shape of the protrusions 24 can be easily suppressed.

[0030] The press die 10 is made of a steel material such as spheroidal graphite cast iron or flame hardened steel. Therefore, in order to achieve the above HRC, for example, quenching or the like may be carried out.

[0031] In the press die 10, the rough surface region 22 may be provided at a position where springback is likely to occur during press molding and where the occurrence of springback would be problematic. Locations where springback becomes a problem include, for example, the outer plate surface and the joining surface with the mating member in the case of steel sheets for automobiles.

[0032] Although there is no particular limitation on the thickness of the steel sheet to be molded by the press die 10, springback is particularly likely to occur when the thickness of the steel sheet is 1.5 mm or less, so it is effective to apply the press die 10 to steel sheets of such a thickness. More preferably, the thickness is 0.7 mm or less. The lower limit of the thickness of the steel sheet is, for example, 0.3 mm. An example of a steel sheet having a thickness in this range is a steel sheet for automobiles.

[0033] <Another embodiment of the press die> In the press dies described so far, the lower die has a rough surface area. On the other hand, in the press die according to the embodiment of the present invention, the upper die may have a rough surface region. Moreover, the press die according to the embodiment of the present invention may be a press die having a cam mechanism.

[0034] (Method of manufacturing press dies) A method for manufacturing a press die according to an embodiment of the present invention includes a roughening step of forming a roughened region on a part of the molding surface of the press die. In this roughening step, a roughened surface region is formed having protruding portions protruding from the molded surface before roughening and recessed portions recessed from the molded surface before roughening.

[0035] In the formed rough surface region, the average depth of the recesses is greater than the average height of the projections. Therefore, in press molding using a press die manufactured according to an embodiment of the present invention, it is possible to prevent the occurrence of waviness while suppressing the occurrence of springback.

[0036] In the roughening step, for example, the roughened surface region is formed by laser processing in which the molding surface of the press die is irradiated with laser light. Laser processing is suitable for forming an uneven shape in which the average depth of the recesses is greater than the average height of the projections.

[0037] There are no particular limitations on the laser used in the above laser processing, and any laser that can roughen the surface of the steel material can be used. Specific examples of the laser include semiconductor lasers, solid-state lasers such as YAG lasers, and fiber lasers. In addition, the conditions for irradiating the laser light are not particularly limited. However, unlike normal groove cutting, it is necessary to form a convex portion that protrudes above the reference surface, and therefore it is necessary to devise a method for forming the convex portion by appropriately adjusting the timing of the laser light oscillation and the scanning speed, etc. The convex portion can be formed, for example, by utilizing the flow of molten metal in a molten pool.

[0038] The average height of the projections formed in the surface roughening step is preferably 12 μm or more. In this case, the resulting mold is suitable for suppressing springback. More preferably, the average height of the projections is 26 μm or more. A preferred upper limit of the average height of the protrusions 24 is 60 μm.

[0039] The surface roughness Rz of the roughened area formed in the roughening step is preferably 500 μm or less, which can suppress deformation of the protrusions of the press die. A preferred lower limit of the surface roughness Rz is 25 μm.

[0040] The surface roughness Rsm of the roughened surface region formed in the roughening step is preferably 150 μm or more. In this case, the protrusions are formed thick, so that the protrusions 24 are less likely to deform during press molding. A preferred upper limit of the surface roughness Rsm is 500 μm.

[0041] The surface roughness Rz and the surface roughness Rsm can be obtained by the method already explained.

[0042] In the manufacturing method of this embodiment, the molded surface before the roughening step usually has a surface roughness Ra (JIS B 0601 (2013)) of 1 μm or less, and a surface roughness Rz (JIS B 0601 (2013)) of 10 μm or less. In the press die manufactured by the manufacturing method of this embodiment, the area that has not been subjected to the surface roughening treatment becomes a non-roughened area.

[0043] The method for producing the press die may be the same as the conventional method, except that it includes a surface roughening step for forming a roughened region on a part of the molding surface of the press die.

[0044] (Evaluation test) The springback suppression effect according to the embodiment of the present invention was evaluated below. This evaluation was performed by simulation using simulation software (product name: JSTAMP) manufactured by JSOL Corporation. FIG. 4 is a diagram illustrating the evaluation method.

[0045] (Test Examples 1 to 5) An evaluation (simulation) was performed under the following conditions, and the amount of springback after forming (simply referred to as the amount of springback in Table 1) was calculated. (1) Evaluation sample A strip-shaped steel sheet having a thickness of 0.3 mm, 0.5 mm, 0.7 mm, 1.0 mm, or 1.5 mm and bent into a dogleg was used as an evaluation sample 33. Here, the bending angle θ (see FIG. 4(a)) was 20°.

[0046] (2) Evaluation mold The evaluation mold was a press mold for molding the bent evaluation sample 33 into a flat plate shape. This evaluation mold was a press mold consisting of a lower mold 31 and an upper mold 32, with the molding surface 31a of the lower mold 31 and the molding surface 32a of the upper mold 32 serving as molding surfaces. The evaluation molds in Test Examples 1 to 5 were set so that no irregularities were formed on either the molding surfaces 31a, 32a of the lower mold 31 or the upper mold 32.

[0047] (3) Evaluation of springback amount The evaluation sample 33 in (1) above was molded into a flat plate shape using the evaluation mold in (2) above (see FIG. 4(b)). After that, it was released from the evaluation mold, and the amount of springback after release was calculated. The above-mentioned springback amount was measured by placing the molded evaluation sample (molded product) 35 on a flat surface so that the inner surface of the evaluation sample 33 was facing down when it was bent, as shown in Figure 4(c), and measuring the distance from the flat surface to the bending position of the evaluation sample as distance B. The results are shown in Table 1.

[0048] (4) Presence or absence of swell The occurrence of waviness was judged by visually observing the top surface of the evaluation sample 35 visualized based on the simulation results.

[0049] (Test Examples 6 to 15) Except for changing the evaluation mold, the amount of springback after molding was calculated in the same manner as in Test Examples 1 to 5. In addition, the presence or absence of waviness was also determined in the same manner as in Test Examples 1 to 5. The evaluation mold employed was one in which a rough surface region was formed over the entire molding surface 31a of the lower mold 31. In the simulation, the rough surface region was represented by a plurality of protrusions formed thereon, and the protrusions were adjusted so that the steel plate would pierce only a portion of the height direction of the protrusions, thereby reproducing the protrusions and recesses of the present invention. In other words, the parts of the protrusions of the rough surface region that pierce the steel plate were regarded as the protrusions of the present invention, and the parts of the protrusions of the rough surface region that do not pierce the steel plate were regarded as the recesses of the present invention, and the experiment was performed. At this time, the uneven shape (height of the projections, Rsm, and Rz) in the rough surface region had the dimensions shown in Table 1.

[0050] The effect of providing the rough surface region was evaluated with "◎", "◯" or "△". Here, test examples 6 to 15 with a rough surface region and test examples 1 to 5 without a rough surface region were compared for test examples with the same plate thickness, and the percentage of the reduced springback amount was calculated as the reduction rate (%). A reduction rate of 70% or more was evaluated as "◎", a reduction rate of 50% or more but less than 70% was evaluated as "◯", and a reduction rate other than the above was evaluated as "△". The results are shown in Table 1.

[0051] [Table 1]

[0052] As shown in Table 1, it has become clear that the occurrence of springback can be suppressed by performing press molding using the press die according to the embodiment of the present invention. It was also revealed that the occurrence of swells could be avoided. In addition, when a press die with the same specifications as in Test Example 10 was manufactured as an actual machine, the results showed that the occurrence of springback could be similarly suppressed and the occurrence of waviness could be avoided. [Industrial Applicability]

[0053] The present invention can be suitably used in the field of automobile manufacturing and the like. [Explanation of symbols]

[0054] 10 Press mold 11, 31, 51 Lower mold 11a Molding surface (upper surface of lower mold) 12, 32, 52 Upper mold 12a Molding surface (lower surface of upper mold) 13, 53 steel plate 15 Molded products 21 Non-rough area 22 Rough surface area 23 Recess 24, 64 convex part 25 Reference plane 33, 35 Evaluation sample

Claims

1. A roughening process is provided for forming a roughened surface area on a part of a molding surface of a press die used for molding a steel sheet, The surface roughening step includes: A method for manufacturing a press die, comprising a step of forming a roughened surface region having convex portions protruding from a molding surface before roughening and concave portions recessed from a molding surface before roughening, the roughened surface region being formed such that the average depth of the concave portions is greater than the average height of the convex portions.

2. The method for manufacturing a press die according to claim 1 , wherein the rough surface region has a surface roughness Rz of 500 μm or less and an average height of protrusions of 12 μm or more.

3. The method for manufacturing a press die according to claim 1 or 2, wherein the rough surface region has a surface roughness Rsm of 150 μm or more.

4. The method for manufacturing a press die according to claim 1 or 2, wherein the surface roughening step is performed by using a laser.

5. The method for manufacturing a press die according to claim 1 or 2, wherein the steel plate has a thickness of 1.5 mm or less.

6. The method for manufacturing a press die according to claim 1 or 2, wherein the steel plate is a steel plate for an automobile.

7. A press die used for forming a steel plate, The molding surface of the mold has a roughened area; A press mold, wherein the rough surface region has a convex portion protruding from a reference surface corresponding to the molding surface before roughening, and a concave portion recessed from the reference surface, and the average depth of the concave portion is greater than the average height of the convex portion.

8. The press die according to claim 7 , wherein the rough surface region has a surface roughness Rz of 500 μm or less and an average height of protrusions of 12 μm or more.

9. The press die according to claim 7 or 8, wherein the rough surface region has a surface roughness Rsm of 150 μm or more.

10. 9. The press die according to claim 7 or 8, wherein the steel plate has a thickness of 1.5 mm or less.

11. The press die according to claim 7 or 8, wherein the steel plate is a steel plate for automobiles.

Citation Information

Patent Citations

  • Press formed member and press forming method

    JP2001087816A