Grease composition for heat fixing device and heat fixing device
A grease composition with perfluoropolyether oil and polytetrafluoroethylene addresses base oil leakage and sliding issues in heat fixing devices, enhancing durability by maintaining stable sliding properties and reducing frictional damage.
Patent Information
- Application Number
- JP2023080059
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Existing heat fixing devices face issues with base oil leakage and poor sliding properties between the fixing film and nip forming member, leading to potential damage due to high frictional forces, which are exacerbated by low kinematic viscosity at high temperatures.
A grease composition for heat fixing devices using perfluoropolyether oil with specific kinematic viscosity ranges and polytetrafluoroethylene as a thickener, ensuring stable sliding properties and preventing base oil leakage.
The grease composition maintains effective sliding properties and prevents base oil leakage, extending the lifespan of the heat fixing device by reducing frictional damage to components.
Smart Images

Figure 2024164520000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a grease composition for a heat fixing device and a heat fixing device. [Background technology]
[0002] 2. Description of the Related Art In recent years, heat fixing devices that are excellent in quick start characteristics and power saving properties have been proposed as fixing devices to be mounted on image forming apparatuses.
[0003] Patent Document 1 discloses a film heating type heat fixing device using a ceramic heater. The film heating type heat fixing device using a ceramic heater is composed of a fixing film as a flexible rotating body, a heater that contacts the inner surface of the fixing film and generates heat when electricity is applied, and a pressure roller that forms a fixing nip with the heater via the fixing film.
[0004] Moreover, Patent Document 2 discloses a heat fixing device of a radiation type film heating method using a halogen heater, and Patent Document 3 discloses a heat fixing device of an induction heating type film heating method. Although the heat sources of a radiative film heating type heat fixing device and a film heating type heat fixing device using induction heating are different, they consist of a fixing film to be heated and a nip forming member that comes into contact with the inner surface of the fixing film and forms a fixing nip with a pressure roller via the fixing film.
[0005] In either case of the heating and fixing device, the recording material on which an unfixed image has been formed is clamped and transported through the fixing nip, whereby the heat of the fixing film is imparted to the recording material, and the unfixed image on the recording material is fixed by the pressure applied at the fixing nip.
[0006] In these heating and fixing devices, a configuration is known in which a lubricant is interposed between the inner surface of the fixing film and the surface of the heater or nip forming member (hereinafter, the heater is also referred to as the nip forming member) in order to ensure sliding properties between the inner surface of the fixing film and the surface of the heater or nip forming member in the fixing nip. During operation of the heat fixing device, the inner surface of the fixing film and the surface of the nip forming member become hot, so a fluorine-based grease composition (hereinafter simply referred to as grease composition) that shows good stability even under high temperature conditions is used as the lubricant. The grease composition is basically composed of a base oil and a thickener, with the base oil being perfluoropolyether oil (PFPE) and the thickener being a homopolymer or copolymer of polytetrafluoroethylene (PTFE). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 5-27619 [Patent Document 2] JP 2012-237945 A [Patent Document 3] JP 2016-24348 A Summary of the Invention [Problem to be solved by the invention]
[0008] 2. Description of the Related Art In recent years, with the trend toward even longer life for electrophotographic image forming apparatuses (hereinafter also referred to as "image forming apparatuses") such as laser beam printers, even longer life is also being demanded for heat fixing devices. In order to extend the life of the heat fixing device, it is effective to ensure the slidability between the inner surface of the fixing film and the nip forming member in the fixing nip while the heat fixing device is in operation, in other words, to reduce the frictional force between the inner surface of the fixing film and the nip forming member. If the heat fixing device is continuously used in a state where the slidability is poor, i.e., in a state where the frictional force is large, it may lead to damage to the fixing film or the nip forming member (e.g., the heater).
[0009] In order to reduce the frictional force between the inner surface of the fixing film and the nip forming member, it is possible to reduce the kinetic viscosity of the base oil contained in the grease composition. In particular, in order to ensure the sliding property between the inner surface of the fixing film and the nip forming member when the heat fixing device is in a high temperature state during operation, it is considered to reduce the kinetic viscosity at high temperatures. However, if a base oil with a low kinetic viscosity is simply used, the viscosity of the base oil at room temperature will also be low, so the fluidity of the base oil will increase and the base oil will easily flow out from the end of the fixing film. Therefore, as time passes after the manufacture of the heat fixing device, the amount of base oil in the lubricant interposed between the inner surface of the fixing film and the nip forming member may decrease. If the base oil decreases or runs out, the sliding property between the inner surface of the fixing film and the nip forming member may deteriorate, leading to damage to the fixing film or the nip forming member.
[0010] At least one aspect of the present disclosure is directed to providing a grease composition for a heat fixing device that can prevent base oil from leaking out and ensure sliding properties between the inner surface of a fixing film and a nip forming member. Also, at least one aspect of the present disclosure is directed to providing a heat fixing device having a long service life. [Means for solving the problem]
[0011] According to at least one aspect of the present disclosure, Contains a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40°C is 800mm 2 / s~2500mm 2 / s, A grease composition for use in a heat fixing device is provided, which has a kinetic viscosity v200 at a temperature of 200° C. that is 1 / 50 or less of a kinetic viscosity v40.
[0012] [ka]
[0013] According to at least one aspect of the present disclosure, a heating rotor and a sliding portion on a heating side that slides due to rotation of the heating rotor; a pressure rotating body disposed opposite the heating rotating body, a grease composition is interposed between the sliding portion on the heating side and the heating rotor, The grease composition comprises a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by the above formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40°C is 800mm 2 / s~2500mm 2 / s, There is provided a heat fixing device in which the kinetic viscosity v200 at a temperature of 200° C. is 1 / 50 or less of the kinetic viscosity v40. Effect of the Invention
[0014] According to at least one aspect of the present disclosure, it is possible to obtain a grease composition for a heat fixing device that can prevent the outflow of the base oil and ensure the sliding property between the inner surface of the fixing film and the nip forming member. Also, according to at least one aspect of the present disclosure, it is possible to obtain a heat fixing device having a long durability. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic cross-sectional view of an image forming apparatus according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic configuration diagram of a heat fixing device according to an embodiment of the present disclosure. [Diagram 3] 1 is a schematic diagram of a heat fixing device according to an embodiment of the present disclosure in a longitudinal direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. However, the dimensions, materials, shapes, and relative positions of the components described in the embodiments should be appropriately changed depending on the configuration and various conditions of the device to which the present disclosure is applied. In other words, the scope of the present disclosure is not limited to the following embodiments. In addition, in the present disclosure, the description of "XX to YY" representing a numerical range means a numerical range including the lower limit and upper limit, which are the endpoints, unless otherwise specified.
[0017] (1) Grease composition The grease composition according to the present disclosure comprises the following components (A) and (B): (A) The kinetic viscosity ν40 at a temperature of 40°C is 800 mm 2 / s~2500mm 2 / s, and the kinetic viscosity ν200 at a temperature of 200°C is 1 / 50 or less of the kinetic viscosity ν40. (B) Polytetrafluoroethylene. In addition to the above components (A) and (B), additives that are usually blended, such as solid lubricants, thickeners, antioxidants, extreme pressure agents, oiliness agents, rust inhibitors, corrosion inhibitors, metal activators, dyes, color stabilizers, viscosity index improvers, and structure stabilizers, may be added depending on the application.
[0018] The component (A) contains a perfluoropolyether oil (PFPE) having at least one of the structures represented by the following formula (I) and formula (II) in the molecule.
[0019] [ka]
[0020] Since the PFPE is chemically inactive, it is not easily decomposed even at high temperatures, making it suitable as a base oil for grease compositions for use in heat fixing devices that are exposed to high temperatures.
[0021] (A) The kinetic viscosity ν40 of PFPE at 40 ° C. is 800 mm 2If the kinematic viscosity ν40 is less than 2500 mm / s, the base oil flows out from the end of the fixing film even when the heat fixing device is not in operation, and the amount of base oil in the grease composition is significantly reduced. If the amount of base oil is reduced, the sliding property between the inner surface of the fixing film and the surface of the nip forming member is deteriorated, which may lead to damage to the fixing film or the heater as the nip forming member. 2 If the viscosity exceeds 900 mm / s, the driving torque required to drive the heat fixing device from a cold state in a low-temperature environment becomes excessively large. 2 / s~2000mm 2 / s, and preferably in the range of 1000 mm 2 / s~1500mm 2 It is more preferable that the range is / s. In addition, if the kinetic viscosity v200 of the PFPE at 200°C is greater than 1 / 50 of the kinetic viscosity v40, the frictional force between the fixing film and the nip forming member during the operation of the heat fixing device increases, and the sliding property deteriorates. Therefore, the fixing film and the nip forming member are loaded, and may be damaged by continued use. This is because, during the operation of the heat fixing device, the temperature of the fixing film and the heater as the nip forming member becomes high, so in order to ensure the sliding property between the fixing film and the nip forming member during the operation of the heat fixing device, it is better to have a small kinetic viscosity at high temperatures. Furthermore, it is preferable that the kinetic viscosity v200 of the PFPE is 1 / 75 or less of the kinetic viscosity v40. The kinetic viscosity of the PFPE is a value measured by a method in accordance with JIS K2283. Such PFPEs can be obtained as commercial products. For example, PFPEs having a structure represented by formula (I) include "FOMBLIN Y" (trade name, manufactured by Solvay). PFPEs having a structure represented by formula (II) include "FOMBLIN Y" (trade name, manufactured by Solvay) and "Krytox" (trade name, manufactured by Chemours). Furthermore, PFPEs having both a structure represented by formula (I) and a structure represented by formula (II) include "FOMBLIN Y" (trade name, manufactured by Solvay). Among these, those that satisfy the above-mentioned kinetic viscosity conditions may be appropriately selected and used.
[0022] Polytetrafluoroethylene as component (B) is chemically inactive like PEPF, and therefore does not decompose easily even at high temperatures, making it suitable as a thickener for grease compositions for heat fixing devices that are exposed to high temperatures. The polytetrafluoroethylene can be appropriately selected from those used as thickeners for lubricants and the like. Usable commercial polytetrafluoroethylene products include the following: "Lubron L-5F" manufactured by Daikin Industries, Ltd., and "L173JE" manufactured by AGC, Ltd.
[0023] The blending ratio of component (B) to component (A) is preferably within the range of 10 to 100 parts by mass, and more preferably within the range of 20 to 80 parts by mass, of component (B) per 100 parts by mass of component (A). By setting the blending ratio of component (B) to component (A) within the above range, it becomes easier to maintain the grease composition in a semi-solid state, and the outflow, falling off, and drying up of the grease composition can be more effectively prevented.
[0024] The grease composition of the present embodiment can be produced by various methods known in the art. Specifically, for example, it can be produced by distilling perfluoropolyether oil under reduced pressure and then mixing it with polytetrafluoroethylene. At this time, various additives can be added and mixed as necessary. In addition, additives such as stabilizers contained in each product may also be contained within a range that does not impair the effects of the present disclosure.
[0025] (2) Image forming device The configuration of an image forming apparatus according to an embodiment of the present disclosure will be described with reference to the schematic cross-sectional view of Fig. 1. The image forming apparatus 1 is a laser printer that forms an image on a recording material P by utilizing an electrophotographic system. The image forming apparatus 1 includes a process cartridge 10 that is detachably attached to the main body of the apparatus. The process cartridge 10 includes a photosensitive drum 19 as an image carrier, a charging roller 16 as a charging means, a developing roller 17 as a developing means, and a cleaning unit including a cleaning blade 18 as a cleaning means. The image forming apparatus 1 also includes a paper feed cassette 21, a pickup roller 22, a paper feed roller 23, a pair of registration rollers 24, a transfer roller 12 as a transfer member, and a heat fixing device 13. The image forming apparatus 1 also includes a pair of fixing paper discharge rollers 25, a pair of main body paper discharge rollers 26, an operation control unit 40, a motor 20 as a driving means for the heat fixing device, and a motor 100 as a driving means for the other members.
[0026] The photosensitive drum 19 is rotated clockwise at a predetermined peripheral speed (process speed). The charging roller 16 uniformly charges the peripheral surface of the photosensitive drum 19 to a predetermined polarity and potential. The charged surface of the charged photosensitive drum 19 is scanned and exposed to a laser beam emitted from the laser scanner 11. The laser scanner 11, which serves as an image exposure means, outputs a laser beam that is on / off modulated in response to a time-series electric digital pixel signal of the image information to be formed from an external device (not shown) such as an image scanner or computer. This scanning exposure removes the charge from the exposed light portion of the peripheral surface of the photosensitive drum 19, and an electrostatic latent image corresponding to the image information to be formed on the peripheral surface of the photosensitive drum 19.
[0027] The developing roller 17 carries a developer (toner) on its surface and supplies the toner to the peripheral surface of the photoconductor drum 19, thereby sequentially developing the electrostatic latent image formed on the peripheral surface of the photoconductor drum 19 into a toner image. Laser printers generally use a reversal development method in which toner is deposited on exposed light portions of the electrostatic latent image for development.
[0028] The paper feed cassette 21 is detachably attached to the image forming apparatus 1, and stacks and stores recording materials P. The recording materials P in the paper feed cassette 21 are transported to the paper feed roller 23 by the pickup roller 22 based on a paper feed start signal, and are separated and fed one by one into the main body of the image forming apparatus 1 by the paper feed roller 23. The recording materials P fed into the image forming apparatus by the paper feed roller 23 pass through a transport path 30 and are transported to the pair of registration rollers 24. The recording materials P transported to the pair of registration rollers 24 are transported to the transport path 31 by the pair of registration rollers 24 and introduced into the transfer nip T formed by the photosensitive drum 19 and the transfer roller 12.
[0029] The recording material P introduced into the transfer nip T is nipped and transported through the transfer nip T, during which a transfer voltage controlled to a predetermined value is applied to the transfer roller 12 from a transfer voltage application power source (not shown). By applying a transfer voltage of the opposite polarity to that of the toner to the transfer roller 12, the toner image formed on the circumferential surface of the photosensitive drum 19 is electrostatically transferred to the surface of the recording material P. The recording material P with the toner image transferred thereto is transported from the transfer nip T through a transport path 32 and introduced into the heat fixing device 13.
[0030] The heat fixing device 13 includes a fixing film 14 and a pressure roller 15. The recording material P introduced into the heat fixing device 13 is nipped and conveyed through a fixing nip F formed by the fixing film 14 and the pressure roller 15. During this time, the recording material P is heated by the fixing film 14, which is controlled to a predetermined temperature (fixing temperature), and the toner image on the recording material P is fixed to the recording material P. The recording material P, on which the toner image has been fixed by the heat fixing device 13, is discharged from the heat fixing device 13 by a fixing discharge roller pair 25 that discharges the recording material P, and is conveyed along a conveying path 33. Thereafter, the recording material P is discharged from the image forming apparatus to a paper discharge tray 27 by a main body paper discharge roller pair 26, and image formation is completed. On the other hand, after the toner image is transferred to the recording material P, the peripheral surface of the photosensitive drum 19 is cleaned of untransferred toner and paper dust by a cleaning blade 18 and is charged again for use in the next image formation.
[0031] By repeating the above operations, continuous image formation can be performed. Note that the image forming apparatus 1 of this embodiment can print 60 black and white images per minute on A4 size [210 mm x 297 mm] paper at a process speed of 340 mm / sec.
[0032] (3) Heat fixing device 2 and 3 are schematic diagrams showing a heat fixing device 13 according to an embodiment of the present disclosure. The heat fixing device 13 has a fixing film 14 as a heating rotator, a pressure roller 15 as a pressure rotator disposed opposite the fixing film 14, and a ceramic heater 60 as a heating body. The fixing film 14 is a highly heat-resistant member having a multi-layer structure formed in a cylindrical shape, and has a base layer of a heat-resistant resin such as polyimide having a thickness of 100 μm or less. The surface layer of the fixing film 14 is a release layer coated with a fluororesin having excellent release properties such as perfluoroalkoxyalkane (PFA). The pressure roller 15 has a core metal made of iron, aluminum or the like, and an elastic layer made of a highly heat-resistant rubber material such as silicone rubber. The ceramic heater 60 is a heating element disposed inside the fixing film 14, and heats the fixing nip F where the toner on the recording material P is melted and fixed. The ceramic heater 60 is formed by applying a heating element made of silver paste or the like to a ceramic substrate such as alumina as a base material by screen printing or the like, and then applying a glass coating as an insulating protective layer thereon. The fixing film 14 rotates while the inner circumferential surface of the fixing film 14 rubs against the ceramic heater 60 disposed inside the fixing film 14. The sliding contact portion of the ceramic heater 60 constitutes the sliding portion on the heating side. In this sliding portion, it is necessary to suppress the frictional resistance between the ceramic heater 60 and the fixing film 14 to a small value. Therefore, a lubricant is applied in advance to the glass coating of the ceramic heater 60, and the lubricant is interposed between the inner surface of the fixing film 14 and the glass coating of the ceramic heater 60, thereby reducing the frictional resistance and ensuring the sliding property. The grease composition described in detail above is used as the lubricant.
[0033] The ceramic heater 60 is held by a heater holding member 61 , and the heater holding member 61 holding the ceramic heater 60 is held by a metal stay member 63 . As shown in FIG. 3, a fixing flange 70 is provided at the longitudinal end of the heater holding member 61 and the metal stay member 63. The fixing flange 70 is attached to both longitudinal ends of the fixing film 14 and regulates both longitudinal ends of the fixing film 14. A pressure spring 71 is arranged to apply pressure to the fixing flange 70, and the fixing nip F is formed by pressing the ceramic heater 60 toward the pressure roller 15 through the fixing film 14. The core metal of the pressure roller 15 is connected to the motor 20 shown in FIG. 1 by a coupling gear or the like, and the fixing film 14 is rotated by the motor 20 as the pressure roller 15 is rotated. The recording material P is nipped and conveyed through the fixing nip F, so that the unfixed toner image on the recording material P is fixed.
[0034] A thermistor 62 serving as a temperature detection element is in contact with the ceramic heater 60, and the control unit 40 controls the power supply to the ceramic heater 60 based on the detection result of the temperature detection element so that the temperature detected by the thermistor 62 becomes a desired target temperature. The control unit 40 performs image formation and fixing operations under image formation conditions and at a fixing temperature according to the print mode set by the user. EXAMPLES
[0035] The grease composition according to the present disclosure will be explained in more detail below using examples and comparative examples, but the present disclosure is not limited to these examples. <Example 1> Preparation of the Grease Composition of Example 1 A perfluoropolyether oil having at least one of the structures represented by formula (I) and formula (II) in the molecule was subjected to reduced pressure distillation for 30 hours under the conditions of temperature: 230°C to 240°C and pressure: 60 kPa. In addition, a PFPE (trade name: Krytox GPL107, manufactured by Chemours) having a constitutional unit represented by the following formula (III) was used. Then, low molecular weight components were removed, and the viscosity was adjusted to obtain a base oil, which was mixed with polytetrafluoroethylene (trade name: Lubron L-5F, manufactured by Daikin Industries, Ltd.) to prepare a grease composition. The mixing ratio of the base oil and polytetrafluoroethylene was 75:25 (mass ratio). This is a ratio of 18.8 parts by mass of polytetrafluoroethylene to 100 parts by mass of the base oil.
[0036] [ka]
[0037] <Comparative Example 1> A grease composition was prepared in the same manner as in Example 1, except that the perfluoropolyether oil used in Example 1 was used as the base oil without being distilled under reduced pressure.
[0038] <Comparative Example 2> A grease composition was prepared in the same manner as in Example 1, except that a perfluoropolyether oil (product name: b1800, manufactured by Valbis) having a structural unit represented by formula (IV) in its molecule was used as the base oil without being distilled under reduced pressure.
[0039] [ka] In formula (IV), n and m are each a positive number.
[0040] Table 1 shows the kinematic viscosity v40 at 40°C and the kinematic viscosity v200 at 200°C of the base oil (perfluoropolyether oil) used in Example 1, Comparative Example 1, and Comparative Example 2, as well as the ratio v200 / v40. v200 / v40 is 0.02 or less, and 1 / 50 or less. The kinetic viscosity was measured at each temperature according to a method in accordance with JIS K2283.
[0041] [Table 1]
[0042] The heat fixing device was a laser beam printer having the configuration shown in FIGS. 1 and 2, and was prepared as follows. In the heat fixing device, a pressure roller 15 having an outer diameter of 25 mm and including a core metal made of iron, an elastic layer made of silicone rubber, and a surface layer made of PFA was used. The fixing film 14 used was a base layer of 70 μm thick polyimide resin coated with a release layer of 12 μm thick fluorine resin. Between the glass coat of the ceramic heater 60 and the inner surface of the fixing film 14, 250 mg of each of the grease compositions of Example 1, Comparative Example 1, and Comparative Example 2 shown in Table 1 was interposed.
[0043] [Evaluation of spillability of grease composition] A heat fixing device having the same configuration except for using the grease compositions of Example 1, Comparative Example 1, and Comparative Example 2 was prepared, and left without operation for 10 days (240 hours) in an environment of 23°C / 50% while attached to an image forming apparatus. After that, the heat fixing device was removed from the image forming apparatus, and it was observed whether the grease composition had flowed out.
[0044] [Durability test of heat fixing device] Heat fixing devices of the same configuration were prepared except that the grease compositions of Example 1, Comparative Example 1, and Comparative Example 2 were used, and were attached to an image forming apparatus to perform printing operations, which were continued until a malfunction occurred in the fixing film or heater. The printing operation conditions were such that 5,000 sheets were continuously fed in one day, and after printing of 5,000 sheets was completed, printing was stopped until the next day (the heat fixing device was also stopped), and another 5,000 sheets were fed the next day, and this operation was repeated. The paper used was A4 size paper "Red Label Presentation 80g / mm2 " (Canon Inc.) was used. In all of the heat fixing devices, the first defect observed was that the surface layer of the fixing film was worn away, exposing the base layer, and the durability of the heat fixing device was evaluated based on the number of sheets of paper that had been passed before the surface layer of the fixing film was no longer worn away.
[0045] [Table 2]
[0046] When the grease compositions of Comparative Example 1 and Comparative Example 2 were used in the outflow of the grease composition, outflow of the base oil of the grease composition from the end of the fixing film was observed. Specifically, it was confirmed that the base oil leaked out from the end of the fixing film and adhered to the surface of the fixing flange 70 and the longitudinal end region of the fixing film 14 shown in FIG. 3. On the other hand, when the lubricant of Example 1 was used, only a small amount of base oil adhered to the fixing flange, and the outflow level of the base oil was minor. This is because the base oils of the grease compositions of Comparative Example 1 and Comparative Example 2 have a smaller kinetic viscosity at 40°C than the base oil of the grease composition of Example 1, and therefore are likely to have flowed out from the end of the fixing film while the heat fixing device is stopped. On the other hand, the base oil of the lubricant of Example 1 has a larger kinetic viscosity at 40°C, and therefore is likely to have flowed out less easily.
[0047] Regarding the durability of the heat fixing device, when the grease composition of Example 1 was used, the surface layer of the fixing film was worn away and the base layer was exposed after 382,000 sheets had been passed through. On the other hand, when the grease composition of Comparative Example 1 was used, the base layer was exposed after 333,000 sheets had been passed through, and when the grease composition of Comparative Example 2 was used, the base layer was exposed after 311,000 sheets had been passed through. The wear of the surface layer of the fixing film is more likely to progress as the sliding property between the inner surface of the fixing film and the heater glass coating surface becomes poor. This is because, when the sliding property between the inner surface of the fixing film and the heater glass coating surface is poor and the frictional force is large, the frictional force between the pressure roller and the paper and the surface of the fixing film also becomes large during the rotation of the fixing film. Therefore, there is a correlation between the wear of the surface layer of the fixing film and the sliding property between the inner surface of the fixing film and the heater glass coating layer. The sliding property between the inner surface of the fixing film and the heater glass coating layer can be ensured by appropriately maintaining the amount and kinetic viscosity of the base oil of the intervening grease composition.
[0048] Compared with Example 1, Comparative Examples 1 and 2 showed that wear of the surface layer of the fixing film progressed more rapidly. As shown in Table 1, the kinetic viscosity at 40°C of the base oils of the grease compositions of Comparative Examples 1 and 2 is smaller than that of the base oil of the grease composition of Example 1. Therefore, it can be assumed that the base oil has higher fluidity than the base oil used in Example 1 and is more likely to flow out from the end of the fixing film during the operation stop time of the heat fixing device. This is consistent with the results of the comparison of the outflow of the lubricant shown in Table 2, as described above. When the base oil leaks out, the amount of base oil between the inner surface of the fixing film and the heater glass coat decreases, and the sliding property between the inner surface of the fixing film and the heater glass coat deteriorates. As a result, the wear of the surface layer of the fixing film progresses faster in Comparative Examples 1 and 2 than in Example 1.
[0049] Furthermore, the reason why the wear of the surface layer of the fixing film in Comparative Example 2 progressed more quickly than in Comparative Example 1 will be described in detail below. The kinetic viscosity at 200°C of the base oil of the grease composition of Comparative Example 2 is higher than that of the base oil of the grease composition of Example 1 and Comparative Example 1. Therefore, in the case of Comparative Example 2, the frictional force between the fixing film and the glass surface of the heater during the operation of the heat fixing device is higher than that in the cases of Example 1 and Comparative Example 1, and the frictional force between the pressure roller surface and the paper surface increases when the fixing film is rotating. Therefore, the wear of the surface layer of the fixing film in Comparative Example 2 progresses quickly.
[0050] By interposing the grease composition having the composition shown in Example 1 as a lubricant between the inner surface of the fixing film and the heater glass coated surface, it is possible to ensure the sliding properties and the durability of the heat fixing device. [Industrial Applicability]
[0051] In the present embodiment, the heat fixing device has been described as a film heating type heat fixing device using a ceramic heater, but the heat fixing device is not limited to this. In addition, the base layer of the fixing film as the heating rotator is not limited to resin and may be made of metal. As a modified example of the heat fixing device of the film heating type using a ceramic heater, a metal plate may be placed on the metal heater, and the metal plate and the fixing film may slide against each other. The present invention can also be applied to a heat fixing device of a radiation type film heating method using a conventional halogen heater, and a heat fixing device of an induction heating method. In either case of the heat fixing device, as long as the nip forming member and the inner surface of the fixing film slide against each other, the configuration of the present disclosure can be applied as the grease composition to be interposed in the sliding portion.
[0052] Furthermore, in the present embodiment, a configuration in which a lubricant is applied in advance to the glass coat of the ceramic heater has been described, but the present invention is not limited to this. As long as a lubricant is present in the sliding portion between the fixing film and the nip forming member, for example, a configuration in which a lubricant is applied in advance to the inner surface of the fixing film may be used.
[0053] The present disclosure includes the following configurations. [Configuration 1] Contains a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40°C is 800mm 2 / s~2500mm 2 / s, A grease composition for use in a heat fixing device, characterized in that the kinetic viscosity v200 at a temperature of 200°C is 1 / 50 or less of the kinetic viscosity v40.
[0054] [ka]
[0055] [Configuration 2] a heating rotor and a sliding portion on a heating side that slides due to rotation of the heating rotor; a pressure rotating body disposed opposite the heating rotating body, a grease composition is interposed between the sliding portion on the heating side and the heating rotor, The grease composition comprises a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40°C is 800mm 2 / s~2500mm 2 / s, A heat fixing device, characterized in that a kinetic viscosity v200 at a temperature of 200° C. is 1 / 50 or less of a kinetic viscosity v40.
[0056] [ka] [Explanation of symbols]
[0057] 1. Image forming device 13 Heat fixing device 14 Fixing film 15 Pressure roller P Recording material F Fixing nip 60 Ceramic heater 61 Heater holding member 62 Thermistor 63 Metal stay member 40 Control section
Claims
1. Contains a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40° C. is 800 mm 2 / s~2500mm 2 / s, A grease composition for use in a heat fixing device, characterized in that a kinetic viscosity v200 at a temperature of 200° C. is 1 / 50 or less of a kinetic viscosity v40. 【Chemistry 1】
2. a heating rotor and a sliding portion on a heating side that slides due to rotation of the heating rotor; a pressure rotating body disposed opposite the heating rotating body, a grease composition is interposed between the sliding portion on the heating side and the heating rotor, The grease composition comprises a base oil and polytetrafluoroethylene, The base oil contains a perfluoropolyether having at least one of the structures represented by formula (I) and formula (II) in the molecule, The kinetic viscosity ν40 at a temperature of 40° C. is 800 mm 2 / s~2500mm 2 / s, A heat fixing device, characterized in that a kinetic viscosity v200 at a temperature of 200° C. is 1 / 50 or less of a kinetic viscosity v40. 【Chemistry 2】
Citation Information
Patent Citations
Heater device
JP1993027619A
Fixing apparatus
JP2012237945A
Heat-fixing device
JP2016024348A