Manufacturing method of electrode body for non-aqueous electrolyte secondary batteries, and manufacturing method of non-aqueous electrolyte secondary battery

By adjusting thickness and density parameters and using carbon nanotubes, the method addresses equipment costs and efficiency issues in electrode body manufacturing, ensuring separator integrity and reduced resistance without heating.

JP2024164710APending Publication Date: 2024-11-27TOYOTA BATTERY CO LTD +2

Patent Information

Application Number
JP2023080386
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Conventional methods for manufacturing non-aqueous electrolyte secondary battery electrode bodies require heating equipment, leading to high equipment costs and decreased production efficiency due to heating and cooling processes, and result in excessive plastic deformation of separators during pressing, increasing resistance.

Method used

A method for manufacturing the electrode body that involves adjusting thickness and density parameters to prevent separator deformation by pressing at room temperature, using a winding body shaping load of 11 MPa or less, without heating, and incorporating carbon nanotubes for improved conductivity.

Benefits of technology

The method effectively suppresses separator deformation, reduces internal resistance, and enhances production efficiency by eliminating the need for heating equipment and shortening production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164710000001_ABST
    Figure 2024164710000001_ABST
Patent Text Reader

Abstract

To suppress excessive plastic deformation of a separator in pressing an electrode body in a simple step.SOLUTION: In a wound body pressing step in which an electrode body 10 which is wound in manufacturing a lithium ion secondary battery is shaped flat, a thickness A [μm] after a cathode coating step, a cathode basis weight B [mg / cm2] and a thickness C [μm] after a cathode pressing step are adjusted in such a manner that a wound body shaping load PL [MPa] becomes equal to or less than 11 [MPa] regarding a load of the wound body pressing step with which a difference ΔT between thicknesses T1 and T2 [mm] of the electrode body 10 in a case where the electrode body is pressurized with 1.2 [MPa] and 0.03 [MPa] after the wound body pressing step and a thickness [mm] of the electrode body 10 is respectively measured becomes equal to or less than 0.4 [mm].SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an electrode assembly for a nonaqueous electrolyte secondary battery, and a method for manufacturing a nonaqueous electrolyte secondary battery, and more particularly, to a method for manufacturing an electrode assembly for a nonaqueous electrolyte secondary battery that suppresses excessive plastic deformation of a separator when the electrode assembly is pressed by a simple process, and a method for manufacturing a nonaqueous electrolyte secondary battery. [Background technology]

[0002] Non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries have high energy density, high voltage, and high output, and are therefore mounted on vehicles as power sources for driving electric vehicles and hybrid vehicles. A non-aqueous electrolyte secondary battery for vehicle use includes an electrode body, a non-aqueous electrolyte, and a rectangular battery case that houses them. In order to make the electrode body compact, a positive electrode plate and a negative electrode plate are stacked and wound with a separator interposed therebetween. The wound electrode body is then shaped into a flat shape in accordance with the inner dimensions of the battery case by a pressing process. The cell batteries thus manufactured are stacked and used as an assembled battery. At this time, the electrode body housed in the battery case is pressed at a certain pressure or higher in order to increase the stability and pressure resistance of the assembled battery.

[0003] In conventional methods, when pressing the wound electrode body flat, simply increasing the press load to compress the electrode body causes the pores in the separator to collapse, resulting in an increase in resistance. In response to this issue, the invention described in Patent Document 1 softens the electrodes by subjecting the positive and negative electrode plates to heat treatment in order to improve formability when pressing the electrode body. This process improves formability.

[0004] Moreover, in the invention described in Patent Document 2, the electrode body is heated in order to stabilize the shape of the electrode body, and the heated electrode body is then pressed. According to this invention, the positive electrode plate and the like are softened by heating, so that the electrode body can be pressed flat with a small load, and the pores of the separator are not crushed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-059491 A [Patent Document 2] JP 2013-206587 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, since heating equipment is required to heat the electrode body, there are problems in that equipment costs are incurred, and there are also problems in that the heating and cooling of the electrode body worsens the production tact time, thereby reducing production efficiency.

[0007] The problem to be solved by the method for manufacturing an electrode assembly for a nonaqueous electrolyte secondary battery and the method for manufacturing a nonaqueous electrolyte secondary battery of the present invention is to suppress excessive plastic deformation of the separator when the electrode assembly is pressed in a simple process. [Means for solving the problem]

[0008] In order to solve the above problems, the method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery of the present invention is a method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery comprising an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case that houses them, and the electrode body is manufactured through a positive electrode coating process of coating a positive electrode current collector foil with a positive electrode mixture layer, a positive electrode pressing process of pressing the positive electrode plate coated with the positive electrode mixture layer, a lamination process of laminating the pressed positive electrode plate, a negative electrode current collector foil, and a negative electrode plate including the negative electrode mixture layer with a separator made of a porous resin interposed therebetween, and a lamination process of winding the laminated electrode body. The method includes a winding step and a winding body pressing step in which the wound electrode body is shaped into a flat shape, and when the load in the winding body pressing step is defined as a winding body shaping load PL [MPa] such that a difference ΔT between the thicknesses T1 and T2 [mm] of the electrode body when the electrode body is pressurized at 1.2 [MPa] and 0.03 [MPa] after the winding body pressing step and the thicknesses [mm] of the electrode body are measured, respectively, the thickness A [μm] and the positive electrode basis weight B [mg / cm] after the positive electrode coating step are set so that the winding body shaping load PL [MPa] is 11 [MPa] or less. 2 ], and the thickness C [μm] after the positive electrode pressing process is adjusted.

[0009] In order to solve the above-mentioned problems, the present invention provides a method for producing an electrode body for a nonaqueous electrolyte secondary battery, the method comprising: an electrode body, a nonaqueous electrolyte, and a rectangular parallelepiped battery case that houses these; the electrode body includes a positive electrode coating step of coating a positive electrode current collector foil with a positive electrode mixture layer; a positive electrode pressing step of pressing the positive electrode plate coated with the positive electrode mixture layer; a lamination step of laminating the pressed positive electrode plate and a negative electrode plate including a negative electrode current collector foil and a negative electrode mixture layer with a separator made of a porous resin interposed therebetween; a winding step of winding the laminated electrode body; and a wound body pressing step of shaping the wound electrode body into a flat shape; and the thickness after the positive electrode coating step is set to A [μm] and the positive electrode basis weight is set to B [mg / cm]. 2 ], the thickness after the positive electrode pressing process is C [μm], and the thickness of the positive electrode current collector foil is D [μm]. 3 8 (Formula 1), the positive electrode density change amount ΔPD is 1.0 [g / cm3 In this case, the positive electrode density change amount ΔPD is adjusted to 0.63 [g / cm 3 It is desirable to adjust it so that it is equal to or greater than this.

[0010] In the wound body pressing step, the electrode body can be pressed at room temperature without heating. The positive electrode mixture layer contains a conductor, and it is preferable that the conductor is a carbon nanotube.

[0011] The present invention can include a method for producing an electrode assembly for a nonaqueous electrolyte secondary battery as part of a method for producing a nonaqueous electrolyte secondary battery. Effect of the Invention

[0012] According to the method for producing an electrode assembly for a nonaqueous electrolyte secondary battery and the method for producing a nonaqueous electrolyte secondary battery of the present invention, excessive plastic deformation of the separator during pressing of the electrode assembly can be suppressed by a simple process. [Brief description of the drawings]

[0013] [Figure 1] 1 is a perspective view of a lithium-ion secondary battery according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of a laminate of an electrode body of a lithium ion secondary battery. [Diagram 3] FIG. 2 is a schematic diagram showing the configuration of a laminate of an electrode body of a lithium ion secondary battery. [Figure 4] 4 is a schematic diagram showing the configuration of an end portion of an electrode body as viewed from the width direction W. FIG. [Diagram 5] 1 is a table showing test results of examples of the present embodiment and comparative examples. [Figure 6] 4 is a flowchart showing an example of a method for manufacturing the lithium-ion secondary battery 1 of the present embodiment. [Figure 7] 4 is a flowchart showing a charging process of the lithium ion secondary battery 1 of the present embodiment. [Figure 8] The amount of change in positive electrode density ΔPD [g / cm3] is derived as follows (Equation 1). [Figure 9] 1 is a table showing the relationship between the amount of change in positive electrode density ΔPD [g / cm3] and the winding body shaping load PL [MPa] in this embodiment. [Figure 10] 4 is a graph showing the relationship between the winding body shaping load PL [MPa] and the resistance increase rate [%] in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, a method for producing an electrode assembly for a nonaqueous electrolyte secondary battery and a method for producing a nonaqueous electrolyte secondary battery of the present invention will be described by way of an embodiment of a method for producing a lithium ion secondary battery 1 with reference to FIGS.

[0015] <Outline of this embodiment> Fig. 1 is a perspective view of a lithium ion secondary battery 1 of the present embodiment. Fig. 2 is a schematic diagram showing the configuration of a laminate of an electrode body 10 of the lithium ion secondary battery 1 of the present embodiment. Fig. 3 is a schematic diagram showing the configuration of a laminate of an electrode body 10 of the lithium ion secondary battery 1. Fig. 4 is a schematic diagram showing a wound body pressing process of the electrode body 10.

[0016] As described in the Background Art section, in the past, when pressing the wound electrode assembly 10 flat in the wound assembly pressing process, simply increasing the press load for compressing the electrode assembly could cause the pores in the separator 120 to collapse, resulting in an increase in resistance. To address this issue, the inventions described in Patent Documents 1 and 2, which are prior art, improve formability by softening the electrodes through heat treatment.

[0017] However, there is a problem in that equipment costs are incurred because heating equipment is required to heat the electrode body 10. In addition, there is also a problem in that the production tact time is worsened by heating and cooling the electrode body, thereby reducing production efficiency.

[0018] In this embodiment, the thickness A [μm] and the positive electrode coating weight B [mg / cm 2 ] after the positive electrode coating process are the same as those in the embodiment without such a heat treatment. 2], and the thickness C [μm] after the positive electrode pressing step is adjusted so that the wound body pressing step (FIG. 6: S4) is performed so as not to destroy the pores of the separator 120.

[0019] After the positive electrode coating process (S4), the thickness A [μm] and the positive electrode coating weight B [mg / cm 2 ], and in order to adjust the thickness C [μm] after the positive electrode press process, the "winding body shaping load PL [MPa]" is obtained. The "winding body shaping load PL [MPa]" is obtained by pressurizing the electrode body 10 with pressures of 1.2 [MPa] and 0.03 [MPa] after the winding body press process (S4). The load in the winding body press process (Fig. 6: S4) at which the difference ΔT between the thicknesses T1 and T2 [mm] of the electrode body 10 when the thicknesses [mm] of the electrode body 10 are measured respectively is 0.4 [mm] or less is defined as the winding body shaping load PL [MPa].

[0020] FIG. 5 is a graph showing the relationship between the wound body shaping load PL [MPa] and the resistance increase rate [%] in this embodiment. The horizontal axis of the graph is the wound body shaping load PL [MPa], and the vertical axis is the resistance increase rate [%]. Here, the "resistance increase rate [%]" is the internal resistance of the lithium ion secondary battery 1. When the pores of the separator 120 are crushed, lithium ions Li + Therefore, if the internal resistance increases, it can be assumed that the pores have been crushed during the roll pressing process (S4 in Fig. 6).

[0021] From this graph, it can be estimated that when the winding shaping load PL exceeds 11.0 [MPa], the pores are crushed in the winding press step (FIG. 6: S4). The inventors have found through experiments that, by setting the winding shaping load PL [MPa] to 11 [MPa] or less, the winding press step (S4) can be performed without destroying the pores of the separator 120 even at room temperature.

[0022] Specifically, the thickness after the positive electrode coating process is A [μm], and the positive electrode weight is B [mg / cm 2], the thickness after the positive electrode pressing process is C [μm], and the thickness of the positive electrode current collector foil is D [μm]. The change in positive electrode density ΔPD [g / cm 3 ] is calculated using the formula (1) shown in FIG. 8. At this time, the positive electrode density change amount ΔPD is 1.0 [g / cm 3 In addition, the positive electrode density change amount ΔPD is adjusted to 0.6 [g / cm 3 By making such an adjustment, the winding body shaping load PL [MPa] can be easily adjusted to 11 [MPa] or less.

[0023] <Lithium-ion secondary battery 1 of this embodiment> First, the configuration of a lithium ion secondary battery 1 that is the premise of this embodiment will be briefly described. FIG. 1 is a perspective view of a lithium ion secondary battery 1. As shown in FIG. 1, the lithium ion secondary battery 1 is configured as a cell battery. It includes a rectangular parallelepiped battery case 11 having an opening on the upper side. The battery case 11 includes a lid 12 that seals the opening of the battery case 11. An electrode body 10 is housed inside the battery case 11. The battery case 11 is filled with a nonaqueous electrolyte 17. The battery case 11 and the lid 12 are made of a metal such as an aluminum alloy. The lithium ion secondary battery 1 is configured as a sealed battery case by attaching the lid 12 to the battery case 11. The lithium ion secondary battery 1 also includes a negative electrode external terminal 14 and a positive electrode external terminal 16 on the lid 12, which are used for charging and discharging power. The negative electrode external terminal 14 and the negative electrode connection part 103 (see FIG. 2) of the electrode body 10 are connected by a negative electrode current collector 13 via the lid 12. The positive electrode external terminal 16 and the positive electrode connection part 113 (see FIG. 2) of the electrode body 10 are connected by the positive electrode current collector 15 via the lid body 12 .

[0024] <Electrode body 10> Fig. 2 is a schematic diagram showing the configuration of a laminate of an electrode body 10 of a lithium ion secondary battery 1. As shown in Fig. 2, the electrode body 10 of the lithium ion secondary battery 1 includes a negative electrode plate 100, a positive electrode plate 110, and a separator 120. The negative electrode plate 100 includes a negative electrode composite layer 102 on both sides of a negative electrode current collector foil 101. The positive electrode plate 110 includes a positive electrode composite layer 112 on both sides of a positive electrode current collector foil 111. The negative electrode plate 100 and the positive electrode plate 110 are stacked with the separator 120 interposed therebetween to form a laminated electrode body 10. This laminate is wound in the length direction Z around a winding axis and shaped into a flat electrode body 10.

[0025] Negative electrode connection portion 103 functions as a current collector that extracts electricity from negative electrode mixture layer 102 of negative electrode plate 100. Positive electrode connection portion 113 functions as a current collector that extracts electricity from positive electrode mixture layer 112 of positive electrode plate 110.

[0026] <End Configuration of Electrode Body 10> FIG. 3 is a perspective view showing the end of the wound electrode body 10 on the negative electrode side in the width direction. The electrode body 10 laminated in the lamination process (FIG. 6: S2) is wound in the winding process (FIG. 6: S3) with the center Ct supported around the winding axis. Next, in the wound body pressing process (FIG. 6: S4), the end as viewed from the width direction W is shaped into a flat shape like a racing track by a pair of opposing press machines 2 (see FIG. 4) from the thickness direction T perpendicular to the width direction W. Then, the flat electrode body 10 is housed in a battery case 11 as shown in FIG. 1, and the negative electrode current collector 13 is welded to the negative electrode connection part 103. The positive electrode current collector 15 is welded to the positive electrode connection part 113. Examples of the welding method between the connection part and the current collector include ultrasonic welding, resistance welding, and electric welding. A negative electrode external terminal 14 is connected to the negative electrode current collector 13 through the lid 12 , and a positive electrode external terminal 16 is connected to the positive electrode current collector 15 .

[0027] Here, the direction parallel to the winding axis of the electrode body 10 is referred to as the "width direction W." Moreover, the direction perpendicular to the winding axis of the electrode body 10 and perpendicular to the surface of the flat portion F is referred to as the "thickness direction T." Moreover, the direction perpendicular to the width direction W and the thickness direction T is referred to as the "length direction Z."

[0028] <Flat section F and curved section R> 4 is a schematic diagram showing the configuration of the end portion of the electrode body 10 as viewed from the width direction W. The wound body of the electrode body 10 is formed by repeatedly stacking negative electrode plates 100 and positive electrode plates 110 with separators 120 interposed therebetween. The center portion of the electrode body 10, which has been pressed flat, is linear, and a planar "flat portion F" (see FIG. 3) is formed by the negative electrode plates 100, the positive electrode plates 110, and the separators 120.

[0029] In addition, the upper and lower ends of the flat portion F are curved into a semi-cylindrical shape by bending the electrode body 10, which is made up of the stacked negative electrode plate 100, positive electrode plate 110, and separator 120, into a curved portion R (see FIG. 3). When viewed from the width direction W, the curved portion R is in the shape of a nearly concentric semicircle, and the position at the center of these semicircles is defined as the "center Ct." This center Ct can be thought of as a straight line continuing in the width direction W.

[0030] <Negative electrode plate 100> In the negative electrode plate 100, a negative electrode mixture layer 102 is formed on both sides of a negative electrode current collector foil 101. In this embodiment, the negative electrode current collector foil 101 is made of Cu foil. The negative electrode current collector foil 101 serves as a base as an aggregate for the negative electrode mixture layer 102, and also functions as a current collecting member that collects electricity from the negative electrode mixture layer 102. In the negative electrode plate 100, the negative electrode mixture layer 102 is formed on the metallic negative electrode current collector foil 101. In the first embodiment, the negative electrode active material is a material capable of absorbing and releasing lithium ions, and a powdered carbon material made of graphite or the like is used.

[0031] The negative electrode plate 100 is made, for example, by kneading a negative electrode active material, a solvent, and a binder to prepare a negative electrode composite paste (FIG. 7: S21). The prepared negative electrode composite paste is applied to the negative electrode current collector foil 101 (FIG. 7: S22), and is dried in a drying process (FIG. 7: S23). Then, a predetermined thickness and density are achieved in a negative electrode pressing process (FIG. 7: S24).

[0032] <Positive electrode plate 110> Positive electrode mixture layers 112 are formed on both sides of positive electrode current collector foil 111 to form positive electrode plate 110. In this embodiment, positive electrode current collector foil 111 is made of Al foil or Al alloy foil. Positive electrode current collector foil 111 serves as a base for the aggregate of positive electrode mixture layer 112, and also functions as a current collector that collects electricity from positive electrode mixture layer 112.

[0033] In the positive electrode plate 110, a positive electrode composite layer 112 is formed on the surface of a positive electrode current collector foil 111. The positive electrode composite layer 112 has a positive electrode active material. The positive electrode active material is a material capable of absorbing and releasing lithium, and for example, lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), etc. may be used. Alternatively, a material in which LiCoO2, LiMn2O4, and LiNiO2 are mixed in any ratio may be used.

[0034] The positive electrode mixture layer 112 also contains a conductive material. As the conductive material, for example, carbon black such as acetylene black (AB) or ketjen black, or graphite can be used. In this embodiment, the positive electrode area weight B [mg / cm 2 To reduce the amount of carbon nanotubes and carbon nanofibers that have high electrical conductivity, the amount of additive required to achieve the same level of electrical conductivity is small, allowing the solid content of the positive electrode mixture paste to be reduced.

[0035] The positive electrode plate 110 is made, for example, by kneading a positive electrode active material, a conductive material, a solvent, and a binder to create a positive electrode composite paste (FIG. 7: S11). The kneaded positive electrode composite paste is applied to the positive electrode current collector foil 111 (FIG. 7: S12). It is then dried (FIG. 7: S13). Finally, a positive electrode pressing process (FIG. 7: S14) is carried out to obtain a predetermined thickness and density.

[0036] <Separator 120> The separator 120 is a highly insulating nonwoven fabric made of polypropylene or the like, which is a porous resin for holding the nonaqueous electrolyte 17 between the negative electrode plate 100 and the positive electrode plate 110. As the separator 120, a porous polymer membrane such as a porous polyethylene membrane, a porous polyolefin membrane, and a porous polyvinyl chloride membrane, or a lithium ion or ion conductive polymer electrolyte membrane can be used alone or in combination. When the electrode body 10 is immersed in the nonaqueous electrolyte 17, the nonaqueous electrolyte 17 permeates the separator 120 from the end toward the center.

[0037] The resin separator 120 has a certain elasticity, and even if it is subjected to a temporary pressing force such as in the wound body pressing process (S4 in FIG. 6), it will return to its original thickness when the pressing force is removed. However, if the pressing force exceeds a certain value (11 [MPa] in this embodiment), the material will plastically deform and the crushed pores will not return to their original size, the porosity [%] will decrease, and the lithium ion Li + This causes the internal resistance to increase irreversibly.

[0038] In the method of manufacturing the separator 120, a porous sheet is stretched in the length direction and width direction to adjust the size of the pores, thereby achieving a desired porosity. The separator 120 may be a single layer or may be composed of multiple layers. In this embodiment, the core sheet is made of a porous polyethylene sheet, and when it becomes hot, it melts and closes the pores to release the lithium ion Li + This prevents the movement of the core, shutting down the circuit. In addition, both sides of the core sheet are made of porous polypropylene sheets, which have high mechanical strength and are highly resistant to heat and corrosion, thereby suppressing micro-short circuits.

[0039] <Method of Manufacturing Lithium-Ion Secondary Battery 1> FIG. 6 is a flow chart showing an example of a method for manufacturing the lithium ion secondary battery 1 of this embodiment. In the lithium ion secondary battery 1, which is a cell battery, first, in a source step (S1), the negative electrode plate 100, the positive electrode plate 110, and the separator 120, which are power generating elements, are produced. The source step (S1) will be described in detail later with reference to FIG. 7. After the negative electrode plate 100, the positive electrode plate 110, and the separator 120 are produced in the source step (S1), the negative electrode plate 100 and the positive electrode plate 110 are stacked and integrated with the separator 120 in the stacking step (S2). The stack produced in this way is wound in the length direction Z as shown in FIG. 2 in the winding step (S3). When wound, the stack has a shape roughly like a track for athletics when viewed from the width direction W as shown in FIG. 3. In the winding step (S3), the wound stack is roughly plate-shaped. In a winding pressing step (S4), such a wound body is pressed in the thickness direction T indicated by the arrow by the pressing surfaces 2a of a pair of opposing presses 2 as shown in FIG. 4. In the winding pressing step (S4), the wound body is pressed until it has a specified thickness [mm] in order to fit the electrode body 10 into the battery case 11 shown in FIG. 1 without any gaps. At this time, the composition in the positive electrode composite paste preparation step (S11 in FIG. 7) and the positive electrode coating weight B [mg / cm2] in the positive electrode coating step (S12) are determined based on the following factors: 2 The wound body shaping load PL [kN] varies depending on the thickness A [μm] after the positive electrode coating process (S12), the thickness C [μm] after the positive electrode pressing process (S14), and the like.

[0040] After the thickness of the electrode body 10 is adjusted in the winding pressing step (S4), an assembly step (S5) is performed. In the assembly step (S5), as shown in FIG. 1, a negative electrode current collector 13 and a positive electrode current collector 15 are attached to the electrode body 10, and a negative electrode external terminal 14 and a positive electrode external terminal 16 are further attached via a lid body 12. The electrode body 10 is then housed in a battery case 11. The lid body 12 is then welded to the battery case 11 to seal the opening. At this stage, the liquid injection port 18 of the lid body 12 is open, so the cell is heated in a cell drying step (S6) to dry the inside of the cell. After the inside of the cell is dried in the cell drying step (S6), a nonaqueous electrolyte 17 is injected in a liquid injection / sealing step (S7), and the liquid injection port 18 is sealed and hermetically sealed. This completes the assembly of the lithium ion secondary battery 1.

[0041] Then, in the activation step (S8), an SEI film is formed by initial charging, and in the aging step, the battery is stored at high temperature for a long period of time to eliminate micro-short circuits. Once this activation process (S8) is complete, an inspection process (S9) is carried out to check the battery capacity, internal resistance, self-discharge, OCV, etc., and those that pass are shipped as products.

[0042] <Source process (S1)> FIG. 7 is a flowchart showing the source step (S1) of the lithium ion secondary battery 1 of this embodiment.

[0043] The source step (S1) is a step of producing the negative electrode plate 100, the positive electrode plate 110, and the separator 120, which are power generating elements. In the positive electrode mixture paste preparation step (S11), a positive electrode active material, a conductive material, a solvent, and a binding agent (binder) are mixed together to prepare a positive electrode mixture paste.

[0044] In this embodiment, the thickness A [μm] and the positive electrode coating weight B [mg / cm 2 ] after the positive electrode coating step (S12) are determined by the blending in the positive electrode composite paste preparation step (S11). 2 The winding shaping load PL [kN] can be changed by adjusting the thickness C [μm] after pressing the positive electrode, etc.

[0045] The thickness A [μm] after the positive electrode coating step (S12) can be adjusted by, for example, increasing the amount of the solvent. 2 ] is required in a certain amount for the positive electrode active material in relation to the battery capacity of the positive electrode. Therefore, if the conductive material is, for example, carbon nanotubes, their mass can be smaller than that of particulate carbon due to their shape and conductivity. Therefore, the solid content rate of the positive electrode mixture paste can be reduced, and the positive electrode basis weight B [mg / cm] of the positive electrode mixture paste can be reduced. 2 ] can be made smaller.

[0046] In the positive electrode coating step (S12), the composition of the positive electrode composite paste is adjusted in this manner, thereby adjusting the thickness A [μm] after the positive electrode coating step (S12). After the positive electrode coating step (S12), the positive electrode mixture layer 112 is dried in a drying step (S13) to volatilize volatile components such as the solvent of the positive electrode mixture layer 112 and solidify the positive electrode mixture layer 112. The positive electrode plate 110 dried in the drying step (S13) is pressed to have a predetermined thickness in a positive electrode pressing step (S14).

[0047] In the source step (S1), the negative electrode plate 100 is manufactured in parallel with the manufacture of the positive electrode plate 110. Although not described in detail here, the negative electrode plate 100 is manufactured by a negative electrode composite paste preparation step (S21), a negative electrode coating step (S22), a drying step (S23), and a negative electrode pressing step (S24).

[0048] Although a detailed description is omitted, in parallel with the manufacture of the positive electrode plate 110, the separator 120 is also manufactured in a separator manufacturing step (S31). In the above source process (FIG. 6: S1), the negative electrode plate 100, the positive electrode plate 110, and the separator 120 which are power generating elements of the lithium ion secondary battery 1 are manufactured.

[0049] <Lamination process (S2)> The negative electrode plate 100, the positive electrode plate 110, and the separator 120 manufactured in the source process (S1) as described above are laminated in the order of the negative electrode plate 100-separator 120-positive electrode plate 110-separator 120, as shown in FIGS.

[0050] <Winding process (S3)> The negative electrode plate 100, the positive electrode plate 110, and the separator 120 stacked in the stacking step (S2) are wound as shown in FIGS.

[0051] <Winding body pressing process (S4)> In the wound body pressing step (S4), the wound body of the electrode body 10 is pressed in the thickness direction T by a press surface 2a of a press machine 2 as shown in FIG.

[0052] Here, after the wound body pressing step (S4), the electrode body 10 is pressurized at 1.2 [MPa] and 0.03 [MPa], and the thickness [mm] of the electrode body 10 is measured. The load in the wound body pressing step (S4) at which the difference ΔT between the measured thicknesses T1 and T2 [mm] of the electrode body 10 is 0.4 [mm] or less is defined as the wound body shaping load PL [MPa].

[0053] The thickness A [μm] after the positive electrode coating process and the positive electrode basis weight B [mg / cm2] are set so that the roll forming load PL [MPa] is 11 [MPa] or less. 2 ] and adjust the thickness C [μm] after the positive electrode pressing process.

[0054] In this embodiment, the thickness after the positive electrode coating step (S12) is A [μm], and the positive electrode basis weight is B [mg / cm 2 ], the thickness after the positive electrode pressing process is C [μm], and the thickness of the positive electrode current collector foil is D [μm]. The amount of change in the positive electrode density at this time, ΔPD [g / cm 3 ] is calculated using the formula (1) shown in FIG. 8, the positive electrode density change ΔPD is 1.0 [g / cm 3 By adjusting in this manner, the wound body shaping load PL [MPa] can be set to 11 [MPa] or less in the wound body pressing step (S4).

[0055] The change in the positive electrode density, ΔPD, is 0.63 [g / cm 3 By adjusting in this manner, the particles of the positive electrode active material and the conductive material are brought into close contact with each other, and the contact resistance therebetween can be reduced.

[0056] (Action of this embodiment) As shown in FIG. 4, when the wound body of the electrode body 10 is pressed by a pair of press surfaces 2a, 2a of a press machine 2 in the wound body pressing step (FIG. 6: S4), the reaction force characteristics of the positive electrode plate 110 have a dominant effect on formability. The separator 120 is made of a porous polyolefin such as polyethylene (PE) or polypropylene (PP) and has a certain degree of elasticity. However, if it is subjected to a large pressure exceeding a certain pressure, it will be irreversibly plastically deformed. Once plastically deformed, the pores will be crushed, and the permeability will be deteriorated, resulting in the incorporation of lithium ions Li + This will have a negative impact on battery performance.

[0057] Therefore, the inventors discovered through experiments that by setting the winding shaping load PL [MPa] to 11 [MPa] or less, the winding press process can be performed without destroying the pores of the separator 120 even at room temperature.

[0058] In addition, the inventors have determined that in order to set the winding body forming load PL [MPa] to 11 [MPa] or less, the positive electrode density change amount ΔPD [g / cm 3 ] to 1.0 [g / cm 3 It has been found that this can be achieved by:

[0059] Therefore, the change in the positive electrode density ΔPD [g / cm 3 ] to 1.0 [g / cm 3 For this reason, it is necessary to prove the condition that the thickness after coating of the positive electrode is A [μm], the weight of the positive electrode per unit area is B [mg / cm 2 ], thickness after positive electrode pressing process C [μm], thickness of positive electrode current collector foil D [μm], and change in positive electrode density ΔPD [g / cm 3 ] The following experiment was conducted to examine the relationship between

[0060] <Experimental Example> Here, an experimental example of this embodiment will be shown. Fig. 9 is a table showing the test results of the example and comparative examples of this embodiment. In the experiment, the following items were measured for the "comparative example" and "Examples 1 to 4".

[0061] First, a thickness D [μm] is measured in advance of the positive electrode current collector foil 111. The positive electrode current collector foil 111 used was a common one, and its thickness D was 12.00 [μm]. Next, in a positive electrode composite paste preparation step (S11), a positive electrode composite paste of a predetermined composition is prepared. Next, in a positive electrode coating step (S12), the positive electrode composite paste is applied to the positive electrode current collector foil 111 at a predetermined positive electrode basis weight B [mg / cm 2 ]. Here, the thickness A [μm] of the positive electrode after coating is measured. Thereafter, the positive electrode mixture layer 112 is dried, and the positive electrode pressing step (S14) is performed. Then, the thickness C [μm] of the positive electrode after pressing is measured.

[0062] Here, the thickness after the positive electrode coating step (S12) is A [μm]. The weight of the positive electrode is B [mg / cm 2 The thickness after the positive electrode pressing step (S14) is C [μm]. The thickness of the positive electrode current collector foil 111 is D [μm]. The amount of change in the positive electrode density at this time, ΔPD [g / cm 3 ] is calculated using Equation 1 shown in Figure 8. Here, the numerator on the right side is multiplied by 10 to make the units uniform.

[0063] Then, the "Comparative Example" and "Examples 1 to 5" were compared. <Experimental conditions> Comparison example: The thickness A of the positive electrode after coating is 86.1 [μm], and the weight B of the positive electrode is 11.33 [mg / cm 2 The thickness C of the positive electrode after the pressing process is 53.5 [μm], and the thickness D of the positive electrode current collector foil is 12.00 [μm]. The amount of change in the positive electrode density ΔPD calculated from the above (Equation 1) is 1.20 [g / cm 3 In addition, the winding body shaping load PL at this time was 13.0 [MPa].

[0064] Example 1: The thickness A of the positive electrode after coating is 79.1 [μm], and the weight B of the positive electrode is 11.15 [mg / cm 2 The thickness C of the positive electrode after the pressing process is 55.5 [μm], and the thickness D of the positive electrode current collector foil is 12.00 [μm]. The amount of change in the positive electrode density ΔPD calculated from the above (Equation 1) is 0.90 [g / cm 3 In addition, the winding body shaping load PL at this time was 9.7 [MPa].

[0065] Example 2: The thickness A of the positive electrode after coating is 75.5 [μm], and the weight B of the positive electrode is 11.11 [mg / cm 2 The thickness C of the positive electrode after the pressing process is 58.0 [μm], and the thickness D of the positive electrode current collector foil is 12.00 [μm]. The amount of change in the positive electrode density ΔPD calculated from the above (Equation 1) is 0.67 [g / cm 3 In addition, the winding body shaping load PL at this time was 7.7 [MPa].

[0066] Example 3: The thickness A of the positive electrode after coating is 82.6 [μm], and the weight B of the positive electrode is 11.10 [mg / cm 2 The thickness C of the positive electrode after the pressing process is 55.4 [μm], and the thickness D of the positive electrode current collector foil is 12.00 [μm]. The amount of change in the positive electrode density ΔPD calculated from the above (Equation 1) is 1.00 [g / cm 3 In addition, the winding body shaping load PL at this time was 11.0 [MPa].

[0067] Example 4: The thickness A after coating on the positive electrode is 74.4 [μm], and the weight B of the positive electrode is 11.03 [mg / cm 2 The thickness C of the positive electrode after the pressing process is 58.0 [μm], and the thickness D of the positive electrode current collector foil is 12.00 [μm]. The amount of change in the positive electrode density ΔPD calculated from the above (Equation 1) is 0.63 [g / cm 3 In addition, the winding body shaping load PL at this time was 6.9 [MPa].

[0068] <Summary of the experiment> As shown in FIG. 4, when the wound body of the electrode body 10 is pressed by a pair of press surfaces 2a, 2a of a press machine 2 in the wound body pressing step (FIG. 6: S4), the reaction force characteristics of the positive electrode plate 110 have a dominant effect on formability. The separator 120 is made of a porous polyolefin such as polyethylene (PE) or polypropylene (PP) and has a certain degree of elasticity. However, it undergoes plastic deformation when subjected to a certain amount of pressure. Once plastic deformation occurs, the pores are crushed, and the permeability and other properties deteriorate, resulting in the incorporation of lithium ions Li + The present inventors have found that if the wound body shaping load PL [MPa] is 11 [MPa] or less, the plastic deformation of the separator 120 can be avoided and the pores can be prevented from collapsing, allowing the lithium ions Li to flow smoothly. + Through experiments, we confirmed that the exchange of data was carried out smoothly.

[0069] Therefore, the inventors set the wound body shaping load PL [MPa] to be equal to or less than the threshold PLth [MPa] of 11 [MPa], and analyzed the conditions under which the wound body pressing step (FIG. 6: S4) can be performed without destroying the pores of the separator 120 even at room temperature.

[0070] <Experimental Results> As a result of the experiment, it was found that in the "Comparative Example", the winding shaping load PL was 13.0 [MPa], which exceeded the threshold value PLth [MPa], and therefore plastic deformation of the separator 120 could not be avoided. On the other hand, in "Example 1" to "Example 4", the winding shaping load PL was 6.9 to 11.0 [MPa], which did not exceed the threshold value PLth [MPa], and therefore plastic deformation of the separator 120 could be avoided.

[0071] As the conditions, the positive electrode density change amount ΔPD of the "Comparative Example" is 1.20, and that of "Example 1" to "Example 4" is 0.63 to 1.00 [g / cm 3 ] was the case. From this result, the positive electrode density change amount ΔPD was set to 1.00 [g / cm 3It was found that by setting the load PL [MPa] to be equal to or less than the reference threshold value PLth of 11 [MPa], the winding shaping load PL [MPa] can be set to be equal to or less than the reference threshold value PLth of 11 [MPa].

[0072] That is, the positive electrode density change amount ΔPD is 1.00 [g / cm 3 In (Equation 1), the thickness A [μm] of the positive electrode after coating, the positive electrode coating weight B [mg / cm 2 ] and the value of the thickness C [μm] after the positive electrode pressing process are determined. This makes it easy to set the winding body shaping load PL [MPa] to 11 [MPa] or less, which is the threshold value PLth [MPa].

[0073] In addition, the specific thickness A [μm] of the positive electrode after coating, the positive electrode coating weight B [mg / cm 2 ] and the value of the thickness C [μm] after the positive electrode pressing process are as follows. It was found that by setting the thickness A after coating of the positive electrode to 74.4 to 82.6 [μm], the winding body shaping load PL [MPa] becomes equal to or less than 11 [MPa], which is the reference threshold value PLth.

[0074] The positive electrode weight B is 11.03 to 11.05 [mg / cm 2 It was found that by setting the value of [MPa], the winding shaping load PL [MPa] can be made equal to or less than the reference threshold value PLth of 11 [MPa].

[0075] It was also found that by setting the post-press step thickness C of the positive electrode to 55.4 to 58.0 [μm], the winding body shaping load PL [MPa] became equal to or less than 11 [MPa], which is the reference threshold value PLth.

[0076] <Action of this embodiment> FIG. 10 shows the amount of change in the positive electrode density ΔPD [g / cm 3 ] and the winding forming load PL [MPa]. The horizontal axis shows the amount of change in positive electrode density ΔPD [g / cm 3 The experimental results were plotted on a graph with the vertical axis representing the load at which the winding was formed, PL [MPa], and the relationship between the load and the load was shown. 3It can be seen that there is a strong positive correlation between the winding shaping load PL [MPa] and the plastic deformation load of the separator 120, which is 11 [MPa] or less. Therefore, in order to make the winding shaping load PL [MPa] of the separator 120 11 [MPa] or less, the positive electrode density change amount ΔPD needs to be 1.0 [g / cm 3 ]You can see that what you need to do is the following.

[0077] (Effects of this embodiment) (1) The method for manufacturing the lithium-ion secondary battery 1 of this embodiment has the advantage that excessive plastic deformation of the separator 120 can be suppressed when the electrode body 10 is pressed using a simple process.

[0078] (2) After the winding press process (S4), the thickness A [μm] after the positive electrode coating process and the positive electrode basis weight B [mg / cm] are adjusted so that the winding shaping load PL [MPa] is 11 [MPa] or less. 2 ] and the thickness C [μm] after the positive electrode pressing process were adjusted. Therefore, in the winding body pressing process, the lithium ion Li + This has the effect of effectively suppressing the movement resistance.

[0079] (3) After the positive electrode coating process (S12), the thickness is A [μm], and the positive electrode weight is B [mg / cm 2 ], the thickness after the positive electrode pressing step (S14) is C [μm], and the thickness of the positive electrode current collector foil 111 is D [μm]. The amount of change in the positive electrode density at this time ΔPD [g / cm 3 8. In this case, the positive electrode density change amount ΔPD was calculated using the formula 1 shown in FIG. 3 This has the effect of easily adjusting the wound body shaping load PL [MPa] to 11 [MPa] or less.

[0080] (4) The change in positive electrode density ΔPD is 0.63 [g / cm 3 By adjusting in this manner, the particles of the positive electrode active material and the conductive material are brought into close contact with each other, and the contact resistance between them can be reduced.

[0081] (5) In this embodiment, the winding shaping load PL [MPa] can be set to 11 [MPa] or less at room temperature without heating, which has the advantage that the process can be carried out using simple equipment.

[0082] (6) Furthermore, since no time is required for heating, there is an effect that the production takt time can be shortened and production efficiency can be improved. (7) The positive electrode mixture layer 112 of this embodiment contains a conductor, and the conductor is a carbon nanotube. Carbon nanotubes have high conductivity and are fibrous in shape, so that the amount of carbon nanotubes added as a conductive material for forming a conductive network can be small, and the density of the positive electrode mixture layer 112 can be reduced. This has the effect of facilitating the blending of the positive electrode mixture paste.

[0083] (8) The production method of the present embodiment has the advantage that it can be suitably applied to the lithium ion secondary battery 1. (Modification) The above embodiment is an example of the present invention, and the present invention can be modified as follows.

[0084] In the present embodiment, the lithium ion secondary battery 1, which is a plate-shaped cell battery for vehicle use, has been illustrated as an example of a nonaqueous electrolyte secondary battery. However, the present invention is not limited to this and can be used for other purposes such as stationary use.

[0085] The drawings are for explaining the present embodiment, and numbers may be omitted or dimensional balance may be exaggerated for ease of understanding, so the drawings are not intended to be limiting.

[0086] The flowcharts shown in FIGS. 6 and 7 are merely examples of the present invention, and steps may be added, deleted, or changed in order or interchanged. Various numerical values ​​and ranges are merely examples and can be optimized and implemented by those skilled in the art.

[0087] The composition of the positive electrode mixture paste and the characteristics of the materials are merely examples of the present invention and may be optimized by those skilled in the art. The present embodiment is one embodiment of the present invention, and it goes without saying that those skilled in the art can add, delete, or modify the configuration without being limited to the embodiment, as long as it does not deviate from the scope of the claims. [Explanation of symbols]

[0088] A [μm]…Thickness after positive electrode coating process B [mg / cm 2 ]…Positive electrode weight C [μm]…Thickness after positive electrode pressing process D [μm]…Thickness of positive electrode current collector foil ΔPD[g / cm 3 ]…Positive electrode density change PL [MPa]…Winding body forming load PLth: Winding body shaping load standard threshold F...Flat area R: (a pair of semi-cylindrical curved sections formed on both ends of the flat section) Ct: Center of curved portion R (point located on the central axis of curved portion R formed in a semi-cylindrical shape) W: (The direction parallel to the axis around which the electrode body is wound) Width direction D: (direction perpendicular to the axis around which the electrode body is wound and perpendicular to the surface of the flat part) thickness direction Z... (the direction perpendicular to the width and thickness directions) length direction 1...Lithium-ion secondary battery 2. Press machine 2a…Press surface 10...Electrode body 11…Battery case 12…Lid body 13...Negative electrode current collector 14...Negative external terminal 15...Positive electrode current collector 16…Positive external terminal 17...Nonaqueous electrolyte 18…Filling port 100: Negative plate 101...Negative electrode current collector foil 102...Negative electrode composite material layer 103...Negative electrode connection part 110…Positive electrode plate 111...Positive current collector foil 112: Positive electrode mixture layer 113…Positive electrode connection part 120…Separator

Claims

1. A method for manufacturing an electrode assembly for a non-aqueous electrolyte secondary battery, comprising: an electrode assembly, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating these, the method comprising the steps of: a positive electrode coating step of coating a positive electrode mixture layer on the positive electrode current collector foil of the electrode body; a positive electrode pressing step of pressing the positive electrode plate coated with the positive electrode mixture layer; a lamination step in which the pressed positive electrode plate and a negative electrode plate including a negative electrode current collector foil and a negative electrode mixture layer are laminated with a separator made of a porous resin interposed therebetween; and a winding step in which the laminated electrode body is wound; a wound body pressing process in which the wound electrode body is shaped into a flat shape, After the wound body pressing step, the electrode body was pressed at 1.2 [MPa] and 0.03 [MPa], and the thickness [mm] of the electrode body was measured. 1 , T 2 When the load in the winding press process at which the difference ΔT in [mm] is 0.4 [mm] or less is defined as a winding shaping load PL [MPa], The thickness A [μm] and the positive electrode basis weight B [mg / cm] after the positive electrode coating step are adjusted so that the wound body shaping load PL [MPa] is 11 [MPa] or less. 2 and a thickness C [μm] of the positive electrode after the pressing step.

2. A method for manufacturing an electrode assembly for a non-aqueous electrolyte secondary battery, comprising: an electrode assembly, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating these, the method comprising the steps of: a positive electrode coating step of coating a positive electrode mixture layer on the positive electrode current collector foil of the electrode body; a positive electrode pressing step of pressing the positive electrode plate coated with the positive electrode mixture layer; a lamination step in which the pressed positive electrode plate and a negative electrode plate including a negative electrode current collector foil and a negative electrode mixture layer are laminated with a separator made of a porous resin interposed therebetween; and a winding step in which the laminated electrode body is wound; a wound body pressing process in which the wound electrode body is shaped into a flat shape, The thickness after the positive electrode coating process is A [μm], and the positive electrode basis weight is B [mg / cm 2 ], the thickness after the positive electrode pressing process is C [μm], and the thickness of the positive electrode current collector foil is D [μm]. 3 ]of [0010] When you search for it with The positive electrode density change amount ΔPD is 1.0 [g / cm 3 4. A method for producing an electrode assembly for a non-aqueous electrolyte secondary battery, comprising adjusting the content of each component so that the content of each component satisfies the following:

3. The positive electrode density change amount ΔPD is 0.63 [g / cm 3 3. The method for producing an electrode assembly for a non-aqueous electrolyte secondary battery according to claim 2, wherein the content of the non-aqueous electrolyte in the electrode assembly is adjusted so that the content of the non-aqueous electrolyte in the electrode assembly is equal to or greater than 1.

4. 4. The method for producing an electrode assembly for a non-aqueous electrolyte secondary battery according to claim 1, wherein the wound body pressing step presses the electrode assembly at room temperature without heating the electrode assembly.

5. 4. The method for producing an electrode assembly for a non-aqueous electrolyte secondary battery according to claim 1, wherein the positive electrode mixture layer contains a conductor, and the conductor is a carbon nanotube.

6. 4. The method for producing an electrode assembly for a non-aqueous electrolyte secondary battery according to claim 1, wherein the non-aqueous electrolyte secondary battery is a lithium ion secondary battery.

7. A method for producing a non-aqueous electrolyte secondary battery, comprising the method for producing an electrode assembly for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Electrode group for flat-type secondary battery and flat-type secondary battery using the same

    JP2012059491A

  • Method for manufacturing battery with flat electrode body

    JP2013206587A

  • Method for manufacturing nonaqueous electrolyte secondary battery

    JP2015204282A

  • Secondary cell and battery assembly

    WO2012111077A1

  • Positive electrode for secondary batteries, and secondary battery using same

    WO2013094100A1

Cited By

  • Trimming device

    US12343779B2