Negative photosensitive resin composition, and method for producing cured relief pattern, cured film and interlayer insulation film, utilizing the same
A negative photosensitive resin composition with polyimide and urethane (meth)acrylate addresses low-temperature curing challenges, enhancing elongation and copper adhesion, suitable for high-speed semiconductor devices.
Patent Information
- Application Number
- JP2024078888
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-27
AI Technical Summary
Conventional photosensitive resin compositions used in flip-chip mounting and fan-out wafer level packaging face challenges in achieving low-temperature curing without compromising mechanical strength, elongation, and copper adhesion, which are critical for preventing wafer warping and ensuring precise wiring in high-speed semiconductor devices.
A negative photosensitive resin composition combining polyimide precursors or polyimides with urethane (meth)acrylate, where the cured product has a glass transition temperature of 130°C or lower, enhancing elongation and copper adhesion, achieved by hydrogen bonding and flexible urethane (meth)acrylate interaction points.
The composition allows for excellent elongation and high adhesion to copper even at low curing temperatures, addressing the limitations of existing compositions and enabling precise wiring in high-speed semiconductor devices.
Smart Images

Figure 2024164833000001 
Figure 2024164833000002 
Figure 2024164833000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative photosensitive resin composition, a method for producing a cured relief pattern using the same, a cured film, and an interlayer insulating film. [Background technology]
[0002] Conventionally, polyimide resins, polybenzoxazole resins, phenolic resins, etc., which have excellent heat resistance, electrical properties, and mechanical properties, have been used as insulating materials for electronic components, and passivation films, surface protective films, interlayer insulating films, etc. for semiconductor devices. Among these resins, those provided in the form of a photosensitive resin composition can easily form a heat-resistant relief pattern film by coating, exposing, developing, and curing the composition to light, subjecting it to a ring-closing treatment (imidization, benzoxazole formation) or thermal crosslinking, and therefore have the characteristic of enabling a significant shortening of the process compared to conventional non-photosensitive materials, and are used in the manufacture of semiconductor devices.
[0003] Incidentally, semiconductor devices (hereinafter also referred to as "elements") are mounted on printed circuit boards by various methods according to the purpose. Conventional elements were generally fabricated by a wire bonding method in which thin wires connect the external terminals (pads) of the element to a lead frame. However, today, as elements have become faster and their operating frequencies have reached GHz, differences in the wiring length of each terminal during mounting have come to affect the operation of the element. As a result, when mounting elements for high-end applications, it has become necessary to precisely control the length of the mounting wiring, and it has become difficult to meet this requirement using wire bonding.
[0004] Therefore, flip-chip mounting has been proposed, in which a rewiring layer is formed on the surface of a semiconductor chip, bumps (electrodes) are formed thereon, and then the chip is flipped over and directly mounted on a printed circuit board. In this flip-chip mounting, since the wiring distance can be accurately controlled, it is adopted for elements for high-end applications that handle high-speed signals, and for mobile phones and the like because of the small mounting size, and the demand is rapidly expanding. More recently, a semiconductor chip mounting technology called fan-out wafer level package (FOWLP) has been proposed, in which individual chips are manufactured by dicing a wafer that has been subjected to a pre-processing process, the individual chips are reconstructed on a support, sealed with a molded resin, and a rewiring layer is formed after peeling off the support (for example, Patent Document 1). In FOWLP, the rewiring layer is formed with a thin film thickness, so that the height of the package can be thinned, and there are advantages in high-speed transmission and low cost. For example, Patent Documents 2 and 3 disclose photosensitive resin compositions used for such rewiring layers. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-167191 A [Patent Document 2] International Publication No. 2021 / 010028 [Patent Document 3] JP 2021-162834 A Summary of the Invention [Problem to be solved by the invention]
[0006] In FOWLP, it is desirable that the curing temperature (thermal imidization temperature) is lower than in the past, from the viewpoint of preventing warpage of the wafer during the process. However, in the photosensitive resin composition described in Patent Document 2, when the curing temperature is lowered, the mechanical strength such as elongation may deteriorate. In addition, since the rewiring layer is multi-layered in FOWLP, in the lithography process using a photoresist, if the flatness of the photosensitive resin composition is poor, the focus depth may shift and the resolution may be significantly deteriorated. In contrast, the photosensitive resin composition described in Patent Document 3 can suppress curing shrinkage and has good flatness, but there is a concern that the copper adhesion may deteriorate.
[0007] The present invention has been devised in view of the above circumstances, and has an object to provide a negative-type photosensitive resin composition which provides a cured film with excellent elongation and high adhesion to copper even when cured at a low temperature of 250° C. or less, and a method for producing a cured relief pattern using the same, a cured film, and an interlayer insulating film. [Means for solving the problem]
[0008] The present inventors have found that the above-mentioned problems can be solved by combining a polyimide precursor or a polyimide resin with a urethane (meth)acrylate having a glass transition temperature of a cured product equal to or lower than a specific temperature, and have thus completed the present invention. That is, the present invention is as follows. [1] The following components (A) to (D): (A) At least one selected from polyamic acid esters and polyimides (B) Photopolymerization initiator (C1) Urethane (meth)acrylate (D) Solvent Including, The negative photosensitive resin composition (C1) is characterized in that a cured product of the urethane (meth)acrylate has a glass transition temperature of 130° C. or lower. [2] The negative type photosensitive resin composition according to [1], wherein a cured product of the component (C1) has a glass transition temperature of 110° C. or lower. [3] The negative type photosensitive resin composition according to [1] or [2], wherein a cured product of the component (C1) has a glass transition temperature of 85° C. or lower. [4] The negative photosensitive resin composition according to any one of [1] to [3], wherein the component (C1) is an aliphatic urethane (meth)acrylate. [5] The negative photosensitive resin composition according to any one of [1] to [4], wherein the component (C1) has 1 to 3 (meth)acryloyl groups. [6] The negative photosensitive resin composition according to any one of [1] to [5], wherein the component (C1) has a weight average molecular weight of 7,000 or less. [7] The negative photosensitive resin composition according to any one of [1] to [6], wherein the component (C1) has a weight average molecular weight of 500 or more. [8] The negative photosensitive resin composition according to any one of [1] to [7], wherein the content of the component (C1) is 15 parts by mass or more per 100 parts by mass of the component (A). [9] The negative photosensitive resin composition according to any one of [1] to [8], wherein the content of the component (C1) is less than 30 parts by mass per 100 parts by mass of the component (A).
[10] The negative photosensitive resin composition according to any one of [1] to [9], wherein the component (A) is a polyamic acid ester represented by the following general formula (1): [ka] (In the formula, X 1 is a tetravalent organic group, Y 1 is a divalent organic group, R 1 and R 2 At least one of represents a monovalent organic group having a radically polymerizable group having 1 to 40 carbon atoms, and n is an integer of 2 to 100.
[11] The negative photosensitive resin composition according to any one of [1] to [9], wherein the component (A) is a polyimide represented by the following general formula (2): [ka] (In the formula, X 1 is a tetravalent organic group, Y 1 represents a divalent organic group, and n is an integer of 2 to 100.
[12] The negative photosensitive resin composition according to any one of [1] to [9], wherein the component (A) is a polyimide having no acidic group.
[13] The negative photosensitive resin composition according to any one of [1] to [9], wherein the component (A) is a polyimide having a (meth)acryloyl group at a main chain terminal.
[14] The negative photosensitive resin composition according to any one of [1] to
[13] , further comprising (C2) a radical polymerizable compound other than (C1) a urethane (meth)acrylate.
[15] The negative photosensitive resin composition according to any one of [1] to
[14] , further comprising (E) a rust inhibitor.
[16] The negative photosensitive resin composition according to any one of [1] to
[15] , which is used for forming a rewiring layer.
[17] The process is as follows: (1) A step of applying a negative type photosensitive resin composition according to any one of items [1] to
[16] onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising:
[18] A cured film comprising a cured product of the negative photosensitive resin composition according to any one of [1] to
[16] .
[19] An interlayer insulating film obtained by using the negative photosensitive resin composition according to any one of [1] to
[16] . Effect of the Invention
[0009] According to the present invention, it is possible to provide a negative type photosensitive resin composition which provides a cured film with excellent elongation even when cured at a low temperature of 250° C. or less and has high adhesion to copper, as well as a method for producing a cured relief pattern using the same, a cured film, and an interlayer insulating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail. The present invention is not limited to the following embodiments, and can be practiced with various modifications within the scope of the gist. Throughout this specification, structures represented by the same symbols in general formulas may be the same or different when multiple structures are present in a molecule. In addition, numerical ranges expressed using "to" in the specification are intended to include the upper and lower limit values.
[0011] <Negative-type photosensitive resin composition> The negative type photosensitive resin composition of the present invention comprises the following components (A) to (D): (A) At least one selected from polyimide precursors and polyimides (B) Photopolymerization initiator (C1) Urethane (meth)acrylate (D) Solvent and a cured product of the urethane (meth)acrylate (C1) has a glass transition temperature (hereinafter also referred to as Tg) of 130° C. or lower.
[0012] Without being limited to any theory, it is believed that the combined use of (A) polyimide precursor or polyimide and (C1) urethane (meth)acrylate improves elongation by constructing pseudo-crosslinks via hydrogen bonds with the polyimide precursor or polyimide. In addition, it is believed that the (C1) urethane (meth)acrylate used in the present invention has a flexible skeleton with a Tg of the cured product below a specific temperature, so that the distance between crosslinking points is appropriately maintained and high elongation is achieved.
[0013] Without being limited to theory, it is believed that urethane (meth)acrylate has an interaction site with copper, and therefore, when used as a polymerizable monomer, it exhibits high copper adhesion.
[0014] As a result, the negative photosensitive resin composition of the present invention provides a cured film with excellent elongation even when cured at a low temperature of 250° C. or less, and has high adhesion to copper.
[0015] (A) Polyimide precursor, polyimide (A-1) Polyimide precursor The (A-1) polyimide precursor is a resin component contained in the negative photosensitive resin composition. There are no particular limitations on the type of resin that can form a polyimide upon thermal cyclization treatment. However, it is preferable that the (A) component has a polyamic acid ester structure represented by the following general formula (1): [ka] (In the formula, X 1 is a tetravalent organic group, Y 1 is a divalent organic group, R 1 and R 2 At least one of represents a monovalent organic group having a radically polymerizable group having 1 to 40 carbon atoms, and n is an integer of 2 to 100.
[0016] In general formula (1), X 1 The tetravalent organic group represented by the formula (I) is preferably an organic group having 6 to 40 carbon atoms, more preferably, -COOR 1 Group and -COOR 2 The X group and the -CONH- group are in the ortho position relative to each other, or the X group is an alicyclic aliphatic group. 1 Examples of the tetravalent organic group represented by the formula (X) include an organic group having 6 to 40 carbon atoms and containing an aromatic ring. 1 -1) and (X 1 -2) groups having the structures represented by the following formulae, but are not limited thereto. [ka] [ka]
[0017] Expression(X 1 -1) and (X 1 In -2), R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 10 carbon atoms, and a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, l is an integer selected from 0 to 2, m is an integer selected from 0 to 3, and n is an integer selected from 0 to 4. 1 The structure of the above formula (X) may be one type or a combination of two or more types. 1 -1) and (X 1 -2) 1 The group is particularly preferred in that it has both heat resistance and photosensitive properties, and more preferably has the above formula (X 1 -1).
[0018] In the above general formula (1), Y 1 The divalent organic group represented by the formula (Y 1 -1) and (Y 1 -2) structures, but are not limited thereto. [ka] [ka]
[0019] Formula (Y 1 -1) and (Y 1 In -2), R6 is a monovalent group selected from the group consisting of a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 10 carbon atoms, and a fluorine-containing hydrocarbon group having 1 to 10 carbon atoms, and n is an integer selected from 0 to 4. 1The structure of the formula (Y 1 -1) and (Y 1 -2) 1 The group is particularly preferred in that it has both heat resistance and photosensitive properties, and more preferably has the above formula (Y 1 -1).
[0020] R in the above general formula (1) 1 and R 2 At least one of the above is preferably a group containing a polymerizable group selected from the group consisting of an acid-polymerizable group, a base-polymerizable group, and a radical-polymerizable group, where the acid-polymerizable group, the base-polymerizable group, and the radical-polymerizable group respectively refer to a group that can be polymerized by the action of an acid, a base, or a radical.
[0021] From the perspective of resolution, R 1 and R 2 At least one of the groups is preferably a group containing a radically polymerizable group, more preferably a monovalent organic group having 1 to 40 carbon atoms, and further preferably a group represented by the following general formula (3). [ka]
[0022] In formula (3), R 3 , R 4 and R 5 are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms, and m 1 is an integer of 1 to 10, preferably an integer of 1 to 5, or an integer of 1 to 3. For example, the group represented by general formula (3) is preferably a group represented by the following formula (4). [ka] In formula (4), R 3 , R 4 and R 5are each independently a hydrogen atom or a monovalent organic group having 1 to 3 carbon atoms. More specific examples of the monovalent organic group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. R 3 is preferably a hydrogen atom or a methyl group, R 4 and R 5 is preferably a hydrogen atom.
[0023] (A-1) Method for preparing polyimide precursor The method for preparing the polyimide precursor (A-1) can be, for example, a method for preparing a polyimide precursor having the above-mentioned tetravalent organic group X 1 A partially esterified tetracarboxylic acid (hereinafter referred to as an acid / ester) is prepared by reacting a tetracarboxylic dianhydride containing the following with an alcohol having a polymerizable group selected from the group consisting of an acid-polymerizable group, a base-polymerizable group, and a radical-polymerizable group, and optionally with other alcohols. Next, the partially esterified tetracarboxylic acid (acid / ester) is reacted with the above-mentioned divalent organic group Y 1 and a diamine containing the same, to obtain a polyimide precursor (A-1).
[0024] (A-1) A tetravalent organic group X that is suitably used for preparing a polyimide precursor 1 As the tetracarboxylic dianhydride containing the above, a compound represented by the following general formula (5) is preferable. [ka] In formula (5), X 1 is defined in the above general formula (1). 1 is represented by the above general formula (X 1 -1) and (X 1 It is more preferable to select from the structures represented by the above general formula (X 1 It is more preferable that the structure is represented by the formula (1).
[0025] Particularly preferred examples of the tetracarboxylic dianhydride include pyromellitic anhydride, diphenylether-3,3',4,4'-tetracarboxylic dianhydride (also known as oxydiphthalic dianhydride, abbreviated as "ODPA"), benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride (abbreviated as "BPDA"), diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane. Particularly preferred are pyromellitic anhydride, diphenylether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, and biphenyl-3,3',4,4'-tetracarboxylic dianhydride, but are not limited thereto. These may be used alone or in combination of two or more.
[0026] Examples of alcohols having a polymerizable group selected from the group consisting of an acid-polymerizable group, a base-polymerizable group, and a radical-polymerizable group that are suitably used for preparing the (A-1) polyimide precursor include 2-hydroxyethyl methacrylate, 2-acryloyloxyethyl alcohol, 1-acryloyloxy-3-propyl alcohol, 2-acrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-t-butoxypropyl acrylate, 2-hydroxy-3-cyclohexyloxypropyl acrylate, 2-methacryloyloxypropyl acrylate, 1- ... Examples of the hydroxyethyl alcohol include 1-methacryloyloxy-3-propyl alcohol, 2-methacrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-t-butoxypropyl methacrylate, 2-hydroxy-3-cyclohexyloxypropyl methacrylate, glycerol diacrylate, 1-(acryloyloxy)-3-(methacryloyloxy)-2-propanol, glycerol dimethacrylate, pentaerythritol triacrylate, and pentaerythritol trimethacrylate.
[0027] The above-mentioned suitable tetracarboxylic dianhydride and the above-mentioned alcohol are dissolved and mixed in the presence of a suitable basic catalyst such as pyridine, preferably in a solvent as described below, preferably at a temperature of 20 to 50° C., preferably for 4 to 10 hours, with stirring, to cause an esterification reaction of the acid anhydride group of the tetracarboxylic dianhydride to proceed, thereby giving the desired acid / ester.
[0028] (Preparation of polyimide precursor) The acid / ester (typically in the form of a solution dissolved in a solvent described below) is mixed with an appropriate dehydration condensation agent, such as dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, or N,N'-disuccinimidyl carbonate, under ice cooling to convert the acid / ester into a polyacid anhydride, and then a diamine containing a divalent organic group Y1 preferably used in this embodiment, dissolved or dispersed in a separate solvent, is added dropwise to the acid / ester to carry out amide polycondensation to obtain the desired polyimide precursor. Depending on the reactivity of the substrate, 1-hydroxybenzotriazole or the like may also be used. Alternatively, the acid portion of the acid / ester is converted into an acid chloride using thionyl chloride or the like, and then the acid is reacted with a diamine in the presence of a base such as pyridine to obtain the desired polyimide precursor.
[0029] Divalent organic group Y preferably used in this embodiment 1 Diamines containing the formula: H 2 New York 1 -NH 2 {In the formula, Y 1 is defined in the above general formula (1). The compound represented by the formula Y is preferred. 1 is represented by the above general formula (Y 1 -1) and (Y 1 -2) is more preferable.
[0030] More preferred examples of the diamine include p-phenylenediamine, m-phenylenediamine, 4,4-diaminodiphenyl ether (also known as 4,4'-oxydianiline, abbreviated as "DADPE"), 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4' -Diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3 -aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[ 4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, ortho-tolidine sulfone, 9,9-bis(4-aminophenyl)fluorene, and those in which a part of the hydrogen atoms on the benzene ring is substituted with a methyl group, an ethyl group, a hydroxymethyl group, a hydroxyethyl group, a halogen, or the like, such as 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,Examples of the diaminodiphenylmethane include, but are not limited to, 3'-dimethyl-4,4'-diaminodiphenylmethane, 2,2'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethytoxy-4,4'-diaminobiphenyl, and 3,3'-dichloro-4,4'-diaminobiphenyl. These may be used alone or in combination of two or more.
[0031] In the above-mentioned (A-1) polyimide precursor production, a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can uniformly dissolve or suspend the tetracarboxylic dianhydride, the diamine, and the compound having a polymerizable group at the end, and examples of the reaction solvent include γ-butyrolactone, dimethylsulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0032] After the amide polycondensation reaction is completed, the water-absorbing by-product of the dehydration condensation agent coexisting in the reaction solution is filtered off as necessary, and then a poor solvent such as water, an aliphatic lower alcohol, or a mixture thereof is added to the resulting polymer component to precipitate the polymer component, and the polymer is purified by repeating redissolution and reprecipitation operations, and then vacuum drying is performed to isolate the desired polyimide precursor. In order to improve the degree of purification, the polymer solution may be passed through a column packed with an anion exchange resin, a cation exchange resin, or both of them swollen with an appropriate organic solvent to remove ionic impurities.
[0033] The molecular weight of the polyimide precursor (A-1) is preferably 8,000 to 150,000, more preferably 9,000 to 50,000, when measured by gel permeation chromatography in terms of polystyrene equivalent weight average molecular weight. When the weight average molecular weight is 8,000 or more, the mechanical properties are good, and when it is 150,000 or less, the dispersibility in the developer is good, and the resolution performance of the relief pattern is good. As the developing solvent for gel permeation chromatography, tetrahydrofuran and N-methyl-2-pyrrolidone are recommended. In addition, the weight average molecular weight is determined from a calibration curve prepared using standard monodisperse polystyrene. As the standard monodisperse polystyrene, it is recommended to select from the organic solvent-based standard sample "TSKstandard POLYSTYLENE" manufactured by TOSOH.
[0034] As the polyimide precursor (A), a non-photosensitive polyimide precursor prepared using only the alcohol having no polymerizable group may be used by mixing with the photosensitive polyimide precursor of the present invention. In this case, from the viewpoint of resolution, the amount of the non-photosensitive polyimide precursor is preferably 200 parts by mass or less based on 100 parts by mass of the photosensitive polyimide precursor.
[0035] (A-2) Polyimide The (A-2) polyimide is a resin component contained in the negative photosensitive resin composition, and preferably has a structure represented by the above general formula (2). By including the polyimide represented by the general formula (2) as the (A) component in the negative photosensitive resin composition of the present embodiment, cure shrinkage can be more effectively reduced. [ka] (In the formula, X 1 is a tetravalent organic group, Y 1 represents a divalent organic group, and n is an integer of 2 to 100.
[0036] Since the negative photosensitive resin composition of the present invention can be developed with an organic solvent, it is preferable that the component (A) does not have an acidic group, and in the general formula (2), X1 , and Y 1 It is more preferable that the compound does not have an acidic group. Examples of the acidic group include a carboxyl group, a phenolic hydroxyl group, a mercapto group, and a sulfo group.
[0037] In general formula (2), X 1 Examples of the tetravalent organic group represented by the formula (X) include an organic group having 6 to 40 carbon atoms and containing an aromatic ring. 2 Examples of the alkyl group include, but are not limited to, groups having a structure represented by the following formula: [ka]
[0038] In the above general formula (2), Y 1 The divalent organic group represented by the formula (Y 2 -1), but is not limited thereto. [ka] From the viewpoint of mechanical strength (elongation), it is preferable that the (A-2) polyimide has a (meth)acryloyl group at the end of the main chain. Although the theory is not limited to this, it is considered that by having a (meth)acryloyl group at the end of the main chain of the polyimide, a crosslinked structure can be formed with the urethane (meth)acrylate, thereby improving the mechanical strength.
[0039] The structure of the (meth)acryloyl group that may be present at the main chain terminal of the polyimide (A-2) is not particularly limited, but examples thereof include the structure represented by the following general formula (M-1). [ka]
[0040] The method for preparing the polyimide (A-2) is, for example, 1and a tetracarboxylic dianhydride containing the divalent organic group Y 1 The polyamic acid is obtained by reacting the polyimide with a diamine containing the compound, and then dehydrating and ring-closing the polyamic acid by heat treatment. In the case of obtaining a polyimide having a (meth)acryloyl group at the main chain end, the process includes a step of reacting a compound having a (meth)acryloyl group capable of reacting with the functional group at the main chain end (amino group or carboxyl group) of the polyimide obtained in the above step.
[0041] The temperature at which the polyamic acid is dehydrated and cyclized by heat treatment is not particularly limited, but since the cyclization reaction is not completed at a low temperature, the lower limit is preferably 150° C. or more, and more preferably 160° C. or more. On the other hand, since side reactions proceed at a high temperature, the upper limit is preferably 200° C. or less, and more preferably 180° C. or less.
[0042] (A-2) A tetravalent organic group X that is suitably used for preparing a polyimide 1 As the tetracarboxylic dianhydride containing the above, a compound represented by the following general formula (5) is preferable. [ka] In formula (5), X 1 is defined in the above general formula (1). 1 is represented by the above general formula (X 2 It is preferable that the structure is selected from the structures represented by the formula (1).
[0043] The tetracarboxylic dianhydride is not particularly limited, but specific examples include oxydiphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, etc. These can be used alone, or two or more of them can be mixed and used.
[0044] The diamine containing a divalent organic group Y1 preferably used in this embodiment is a diamine represented by the formula: H 2 New York 1 -NH 2 {In the formula, Y 1 is defined in the above general formula (1). The compound represented by the formula Y is preferred. 1 is represented by the above general formula (Y 2 It is more preferable that the structure is represented by the formula (1).
[0045] The diamine is not particularly limited, but specific examples include 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene, 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]sulfone, 9,9-bis(4-aminophenyl)fluorene, 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)benzidine, and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
[0046] Specific examples of the compound having a (meth)acryloyl group capable of reacting with the functional group at the main chain end of the polyimide include isocyanate-based compounds such as 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate; chloride-based compounds such as acryloyl chloride and methacryloyl chloride; and alcohol-based compounds such as 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 4-hydroxyethyl methacrylate, and 4-hydroxyethyl acrylate.
[0047] The isocyanate-based compound reacts with the amino group of the dehydrated, ring-closed polyimide to form a urea bond, the chloride-based compound reacts with the amino group of the dehydrated, ring-closed polyimide to form an amide bond, and the alcohol-based compound reacts with the carboxyl group of the dehydrated, ring-closed polyimide to form an ester bond.
[0048] The method for reacting the isocyanate compound is not particularly limited, but the compound can be reacted with the amino groups of the dehydrated ring-closed polyimide by stirring at room temperature.
[0049] The method for reacting the chloride compound is not particularly limited, but the reaction can be carried out by ice-cooling the dehydrated ring-closed polyimide solution and adding the chloride compound dropwise thereto.
[0050] The method for reacting the alcohol compound is not particularly limited, but it can be reacted with the carboxyl group of the dehydration-ring-closed polyimide using a condensing agent such as N,N'-dicyclohexylcarbodiimide or an esterification catalyst such as p-toluenesulfonic acid.
[0051] In the production of the polyimide (A-2), a reaction solvent may be used to efficiently carry out the reaction in a homogeneous system. The reaction solvent is not particularly limited as long as it can dissolve or suspend the tetracarboxylic dianhydride and the diamine homogeneously, and examples of the reaction solvent include γ-butyrolactone, dimethylsulfoxide, N,N-dimethylacetoacetamide, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide.
[0052] The polyimide (A-2) may be purified by a known method such as that described in JP 2012-194520 A. For example, a method of dropping the polyimide (A-2) solution into water to reprecipitate and remove unreacted materials, a method of removing condensing agents insoluble in the reaction solvent by filtration, a method of removing the catalyst using an ion exchange resin, etc. After purification, the polyimide (A-2) may be dried by a known method and isolated in a powder state.
[0053] The molecular weight of the polyimide (A-2) is preferably 4,000 to 200,000, more preferably 4,100 to 15,000, when measured by gel permeation chromatography in terms of polystyrene equivalent weight average molecular weight. When the weight average molecular weight is 4,000 or more, the mechanical properties are good, and when it is 20,000 or less, the dispersibility in the developer is good, and the resolution performance of the relief pattern is good. As the developing solvent for gel permeation chromatography, tetrahydrofuran and N-methyl-2-pyrrolidone are recommended. In addition, the weight average molecular weight is determined from a calibration curve prepared using standard monodisperse polystyrene. As the standard monodisperse polystyrene, it is recommended to select from the organic solvent-based standard sample "TSKstandard POLYSTYRENE" manufactured by TOSOH.
[0054] (B) Photopolymerization initiator The photopolymerization initiator (B) used in this embodiment will be described below. The photopolymerization initiator is preferably a photoradical polymerization initiator.
[0055] Examples of the photoradical polymerization initiator include benzophenone compounds such as benzophenone, o-benzoyl methyl benzoate, 4-benzoyl-4'-methyldiphenyl ketone, dibenzyl ketone, and fluorenone; acetophenone compounds such as 2,2'-diethoxyacetophenone, 2-hydroxy-2-methylpropiophenone, and 1-hydroxycyclohexyl phenyl ketone; thioxanthone compounds such as thioxanthone, 2-methylthioxanthone, 2-isopropylthioxanthone, and diethylthioxanthone; benzyl compounds such as benzil, benzil dimethyl ketal, and benzyl-β-methoxyethyl acetal; benzoin compounds such as benzoin and benzoin methyl ether; 1-phenyl Examples of the compounds include oxime compounds such as 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl)oxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, and 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime; N-arylglycine compounds such as N-phenylglycine; peroxides such as benzoyl perchloride, aromatic biimidazole compounds, and titanocene compounds.
[0056] The photopolymerization initiator (B) used in the present embodiment is not limited to the above examples, but is more preferably an oxime compound, particularly in terms of photosensitivity.
[0057] The content of the (B) photopolymerization initiator is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the (A) polyimide precursor and / or polyimide. When the (A) component is a mixture of a polyimide precursor and a polyimide, the above content is based on 100 parts by mass of the mixture. The blend amount is preferably 0.1 parts by mass or more from the viewpoint of photosensitivity or patterning ability, and 30 parts by mass or less from the viewpoint of the physical properties of the photosensitive resin layer after curing of the negative photosensitive resin composition.
[0058] (C1) Urethane (meth)acrylate The urethane (meth)acrylate (C1) used in this embodiment will be described. In this embodiment, it is considered that the use of (C1) urethane (meth)acrylate improves elongation by constructing pseudo-crosslinks via hydrogen bonds with (A) polyimide precursor or polyimide. In addition, since urethane (meth)acrylate has an interaction site with copper, it is considered that the use of it as a polymerizable monomer will result in high copper adhesion.
[0059] In particular, the urethane (meth)acrylate (C1) used in this embodiment is characterized in that the cured product has a glass transition temperature (Tg) of 130° C. or lower. This allows the distance between crosslinking points to be appropriately maintained, resulting in high elongation. As a result, the negative type photosensitive resin composition of the present embodiment provides a cured film with excellent elongation even when cured at a low temperature of 250° C. or less.
[0060] The glass transition temperature (Tg) of the cured product of the (C1) urethane (meth)acrylate is preferably not higher than 110° C., more preferably not higher than 85° C., and even more preferably not higher than 70° C. This results in a cured film with superior elongation.
[0061] The cured product of the urethane (meth)acrylate can be obtained by a photopolymerization reaction or a thermal polymerization reaction. The method is not particularly limited, but can be, for example, the method described in JP-A-9-40741.
[0062] The glass transition temperature can be measured by a known method, and the measurement method is not particularly limited. For example, the glass transition temperature can be measured by the method described in JP-A-2015-520122.
[0063] Examples of the urethane (meth)acrylate (C1) used in this embodiment include EBECRYL230, EBECRYL270, EBECRYL284, EBECRYL4491, EBECRYL4683, EBECRYL4858, EBECRYL8402, EBECRYL8411, EBECRYL8413, EBECRYL8804, EBECRYL8807, EBECRYL9270, EBECRYL8800, KRM2000, KRM7735, and KRM896 manufactured by Daicel-Allnex Corporation. 1, KRM8191, EBECRYL4220, EBECRYL4513, EBECRYL4740, EBECRYL8465, EBECRYL9260, EBECRYL8701, KRM8667, KRM8296, EBECRYL4265, EBECRYL4587, EBECRYL4666, EBECRYL8210, EBECRYL8405, EBECRYL8606, EBECRYL8254, EBECRYL8301R, EBECRYL210, EBECRYL220, and the like.
[0064] The (C1) urethane (meth)acrylate used in this embodiment is not limited to the above examples. Among the above urethane (meth)acrylates, aliphatic urethane (meth)acrylates are preferred from the viewpoint of elongation. Since aliphatic urethane (meth)acrylates have a flexible skeleton, they can further improve elongation.
[0065] Furthermore, from the viewpoint of elongation, it is more preferable to use a urethane (meth)acrylate having 1 to 3 (meth)acryloyl groups. By having 1 to 3 (meth)acryloyl groups, the crosslinking density can be kept below a certain level, and as a result, the elongation can be further improved.
[0066] Furthermore, from the viewpoint of cure shrinkage, it is more preferable to use a urethane (meth)acrylate having a molecular weight of 7000 or less. By having a molecular weight of the above or less, the concentration of (meth)acryloyl groups in the resin composition is increased, and a decrease in the residual film rate after curing due to subsequent polymerization (curing) can be further suppressed. Further, from the viewpoint of storage stability, urethane (meth)acrylates having a molecular weight of at least 500 are more preferable. When the molecular weight is at least as high as the above, the concentration of urethane bonds in the composition does not become too high, and aggregation between the urethane bonds is suppressed, thereby making it possible to suppress an increase in the viscosity of the composition over time.
[0067] From the standpoint of elongation, the content of the (C1) component is preferably 10 parts by mass, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the (A) component. Furthermore, from the viewpoint of storage stability, the amount of the urethane (meth)acrylate added is preferably less than 30 parts by mass per 100 parts by mass of component (A). When the amount of the urethane (meth)acrylate added is less than 30 parts by mass, the concentration of the urethane bonds in the composition does not become too high, and aggregation between the urethane bonds is suppressed, thereby suppressing an increase in the viscosity of the composition over time.
[0068] The negative photosensitive resin composition of the present invention may contain a urethane (meth)acrylate having a Tg of more than 130° C. in a cured product, as long as the effects of the present invention are not impaired.
[0069] (C2) Radical polymerizable compound In order to improve the resolution of the relief pattern and suppress the cure shrinkage during thermal curing, the photosensitive resin composition may optionally contain (C2) a radical polymerizable compound other than the (C1) urethane (meth)acrylate. The (C2) radical polymerizable compound does not contain the above-mentioned (C1) urethane (meth)acrylate. As such a compound, a (meth)acrylate compound that undergoes a radical polymerization reaction by a photopolymerization initiator is preferable. The (C2) radical polymerizable compound may be a monofunctional monomer or a polyfunctional monomer.
[0070] Examples of monofunctional monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexyl (meth)acrylate, butoxydiethylene glycol methacrylate, isobornyl (meth)acrylate, m-phenoxybenzyl acrylate, o-phenylphenoxyethyl acrylate, 4-methacryloyloxybenzophenone, EO-modified paracumylphenol acrylate, nonylphenoxyethyl acrylate, and 6-acrylamidohexanoic acid. Examples of polyfunctional monomers include di(meth)acrylates of ethylene glycol or polyethylene glycol, such as diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate, di(meth)acrylates of propylene glycol or polypropylene glycol, di(meth)acrylates or tri(meth)acrylates of glycerol, cyclohexane di(meth)acrylate, di(meth)acrylates of 1,4-butanediol, di(meth)acrylates of 1,6-hexanediol, di(meth)acrylates of neopentyl glycol, di(meth)acrylates of bisphenol A, (meth)acrylamide, derivatives thereof, trimethylolpropane tri(meth)acrylate, di(meth)acrylates or tri(meth)acrylates of glycerol, di(meth)acrylates, tri(meth)acrylates or tetra(meth)acrylates of pentaerythritol, and ethylene oxide or propylene oxide adducts of these compounds.
[0071] The amount of the radical polymerizable compound (C2) is preferably 4 parts by mass or more to 100 parts by mass, more preferably 5 parts by mass or more to 60 parts by mass or less, based on 100 parts by mass of the polyimide precursor (A) and / or polyimide. The amount is preferably 4 parts by mass or more from the viewpoint of the residual film rate after curing, and 100 parts by mass or less from the viewpoint of photosensitivity or patterning property.
[0072] (D) Solvent The (D) solvent is not limited as long as it can uniformly dissolve or suspend (A) polyimide precursor or polyimide, (B) photopolymerization initiator, and (C1) urethane (meth)acrylate. Examples of such solvents include γ-butyrolactone, dimethyl sulfoxide, tetrahydrofurfuryl alcohol, ethyl acetoacetate, N,N-dimethylacetoacetamide, ε-caprolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and N,N-dimethylacetamide. These solvents may be used alone or in combination of two or more.
[0073] The above (D) solvent can be used in an amount of, for example, 30 to 1,000 parts by mass, preferably 100 to 1,000 parts by mass, per 100 parts by mass of the (A) polyimide precursor and / or polyimide, depending on the desired coating film thickness and viscosity of the negative photosensitive resin composition.
[0074] When the (D) solvent contains an alcohol having no olefinic double bond, the content of the alcohol having no olefinic double bond in the total solvent is preferably 5 to 50 mass %. The lower limit is more preferably 10 mass % or more from the viewpoint of storage stability of the negative photosensitive resin composition. The upper limit is more preferably 30 mass % or less from the viewpoint of solubility of the (D) polyimide precursor and polyimide.
[0075] (E) Rust inhibitor The (E) rust inhibitor used in this embodiment will be described. When a cured film is formed on a substrate made of copper or a copper alloy using a negative photosensitive resin composition, the negative photosensitive resin composition may optionally contain (E) a rust inhibitor in order to increase the adhesion between copper and the polyimide film. Examples of (E) rust inhibitors include azole compounds and purine compounds.
[0076] Examples of the azole compound include 1H-triazole, 5-methyl-1H-triazole, 5-ethyl-1H-triazole, 4,5-dimethyl-1H-triazole, 5-phenyl-1H-triazole, 4-t-butyl-5-phenyl-1H-triazole, 5-hydroxyphenyl-1H-triazole, phenyltriazole, p-ethoxyphenyltriazole, 5-phenyl-1-(2-dimethylaminoethyl)triazole, 5-benzyl-1H-triazole, hydroxyphenyltriazole, 1,5-dimethyltriazole, 4,5-diethyl-1H-triazole, 1H-benzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, and the like. benzotriazole, 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole, 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-benzotriazole, 2-(3,5-di-t-amyl-2-hydroxyphenyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, hydroxyphenylbenzotriazole, tolyltriazole, 5-methyl-1H-benzotriazole, 4-methyl-1H-benzotriazole, 4-carboxy-1H-benzotriazole, 5-carboxy-1H-benzotriazole, 1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 5-amino-1H-tetrazole, 1-methyl-1H-tetrazole, and the like.
[0077] Particularly preferred are 5-amino-1H-tetrazole, tolyltriazole, 5-methyl-1H-benzotriazole, and 4-methyl-1H-benzotriazole. These azole compounds may be used alone or in combination of two or more.
[0078] Specific examples of purine compounds include purine, adenine, guanine, hypoxanthine, xanthine, theobromine, caffeine, uric acid, isoguanine, 2,6-diaminopurine, 9-methyladenine, 2-hydroxyadenine, 2-methyladenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminopurine, 9-methyladenine, 2-hydroxyadenine, 1-methyladenine, N-methyladenine, N,N-dimethyladenine, 2-fluoroadenine, 9-(2-hydroxyethyl)adenine, guanine oxime, N-(2-hydroxyethyl)adenine, 8-aminopurine, 9 ... Aminoadenine, 6-amino-8-phenyl-9H-purine, 1-ethyladenine, 6-ethylaminopurine, 1-benzyladenine, N-methylguanine, 7-(2-hydroxyethyl)guanine, N-(3-chlorophenyl)guanine, N-(3-ethylphenyl)guanine, 2-azaadenine, 5-azaadenine, 8-azaadenine, 8-azaguanine, 8-azapurine, 8-azaxanthine, 8-azahypoxanthine, and the like, and derivatives thereof.
[0079] When the negative photosensitive resin composition contains (E) a rust inhibitor, the amount of the rust inhibitor is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of (A) polyimide precursor and / or polyimide. The lower limit is more preferably 0.03 parts by mass or more, and even more preferably 0.05 parts by mass or more, because adhesion to copper is improved when the negative photosensitive resin composition is formed on copper or a copper alloy. The upper limit is more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, from the viewpoint of photosensitivity.
[0080] The negative photosensitive resin composition may further contain components other than the above components (A) to (E). The components other than the components (A) to (E) are not limited, but examples thereof include an adhesion promoter, a hindered phenol compound, an organic titanium compound, a thermal crosslinking agent, a sensitizer, and a thermal polymerization inhibitor.
[0081] Adhesive Aid In order to improve the adhesion between the film formed using the negative photosensitive resin composition and the substrate, the negative photosensitive resin composition may optionally contain an adhesive aid. As the adhesive aid, an aluminum-based adhesive aid, a silane coupling agent, etc. can be used.
[0082] Examples of aluminum-based adhesion promoters include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0083] Examples of the silane coupling agent include γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3- (triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamido)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, N-phenylaminopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-(trialkoxysilyl)propyl succinic anhydride, 3-mercaptopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name) KBM803, manufactured by Chisso Corporation: trade name SilaAce S810), 3-mercaptopropyltriethoxysilane (manufactured by Azmax Corporation: trade name SIM6475.0), 3-mercaptopropylmethyldimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS1375, manufactured by Azmax Corporation: trade name SIM6474.0), mercaptomethyltrimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.5C), mercaptomethylmethyldimethoxysilane (manufactured by Azmax Corporation: trade name SIM6473.0), 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptoethyltrimethoxysilane,2-mercaptoethyldiethoxymethoxysilane, 2-mercaptoethylethoxydimethoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltripropoxysilane, N-(3-triethoxysilylpropyl)urea (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS3610, manufactured by Azmax Corporation: trade name SIU9055.0), N-(3-trimethoxysilylpropyl)urea (manufactured by Azmax Corporation: trade name SIU9058.0), N-(3-diethoxymethoxysilylpropyl)urea, N-(3-ethoxydimethoxysilylpropyl)urea, N-(3-tripropoxysilylpropyl)urea, N-(3-diethoxypropoxysilylpropyl)urea, N-(3-ethoxydipropoxysilylpropyl)urea, N-(3-dimethoxypropoxysilylpropyl)urea, N-(3-methoxydipropoxysilylpropyl)urea, N-(3-trimethoxysilylethyl)urea, N-(3-ethoxydimethoxysilylethyl) Urea, N-(3-trippropoxysilylethyl)urea, N-(3-trippropoxysilylethyl)urea, N-(3-ethoxydipropoxysilylethyl)urea, N-(3-dimethoxypropoxysilylethyl)urea, N-(3-methoxydipropoxysilylethyl)urea, N-(3-trimethoxysilylbutyl)urea, N-(3-triethoxysilylbutyl)urea, N-(3-trippropoxysilylbutyl)urea, 3-(m-aminophenoxy)propyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0598.0), m-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.0), p-aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.1) aminophenyltrimethoxysilane (manufactured by Azmax Corporation: trade name SLA0599.2),2-(Trimethoxysilylethyl)pyridine (manufactured by Azmax Corporation: trade name SIT8396.0), 2-(triethoxysilylethyl)pyridine, 2-(dimethoxysilylmethylethyl)pyridine, 2-(diethoxysilylmethylethyl)pyridine, (3-triethoxysilylpropyl)-t-butylcarbamate, (3-glycidoxypropyl)triethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, tetrakis(methoxyethoxy) Silane), tetrakis(methoxy-n-propoxysilane), tetrakis(ethoxyethoxysilane), tetrakis(methoxyethoxyethoxysilane), bis(trimethoxysilyl)ethane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)methane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)ethylene, bis(triethoxysilyl)octane, bis(triethoxysilyl)octadiene, bis[3-(triethoxysilyl)propyl]disulfide, bis[3-(triethoxysilyl)propyl] propyl]tetrasulfide, di-t-butoxydiacetoxysilane, di-i-butoxyaluminoxytriethoxysilane, phenylsilanetriol, methylphenylsilanediol, ethylphenylsilanediol, n-propylphenylsilanediol, isopropylphenylsilanediol, n-butyldiphenylsilanediol, isobutylphenylsilanediol, tert-butylphenylsilanediol, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolyl Rylsilane, ethyl methylphenylsilanol, n-propyl methylphenylsilanol, isopropyl methylphenylsilanol, n-butyl methylphenylsilanol, isobutyl methylphenylsilanol, tert-butyl methylphenylsilanol, ethyl n-propyl phenylsilanol, ethyl isopropyl phenylsilanol, n-butyl ethyl phenylsilanol, isobutyl ethyl phenylsilanol, tert-butyl ethyl phenylsilanol, methyl diphenylsilanol, ethyl diphenylsilanol,Examples of the silane coupling agent include, but are not limited to, silane coupling agents having structures represented by the following formula (S-1): [ka]
[0084] Among these adhesion aids, it is more preferable to use a silane coupling agent from the viewpoint of adhesive strength.As the silane coupling agent, among the above-mentioned silane coupling agents, it is preferable to use one or more selected from the group consisting of phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, and the silane coupling agents having the structure represented by each of the above formula (S-1), from the viewpoint of storage stability.
[0085] When the negative photosensitive resin composition contains an adhesive aid, the amount of the adhesive aid is preferably 0.01 to 25 parts by mass, or more preferably 0.5 to 20 parts by mass, based on 100 parts by mass of the (A) polyimide precursor and / or polyimide. When a silane coupling agent is used, the amount is 0.2 to 10% by mass based on 100 parts by mass of the (A) polyimide precursor and / or polyimide, and the lower limit is more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, based on copper adhesion. From the viewpoint of suppressing the generation of foreign matter due to precipitation, the upper limit is more preferably 8% by mass or less, and even more preferably 6% by mass or less.
[0086] Hindered phenol compounds In order to suppress discoloration on the copper surface, the negative photosensitive resin composition may optionally contain a hindered phenol compound. Examples of the hindered phenol compound include 2,6-di-t-butyl-4-methylphenol, 2,5-di-t-butyl-hydroquinone, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-thio-bis(3-methyl-6-t-butylphenol), 4,4'-butylidene-bis(3-methyl-6-t-butyl Phenol), triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 2,2'-methylene-bis(4-methyl-6-t-butylphenyl)propionate 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-isopropylbenzyl)-1,3,5-triazine-2,4, 6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-s-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-(1-ethylpropyl)-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris[4-triethylmethyl-3-hydroxy-2,6-dimethylbenzyl]-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3-hydroxy-2,6-dimethyl-4-phenylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2,5,6-trimethylbenzyl)-1,3, 5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-6-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris( 4-t-butyl-6-ethyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5,6-diethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine Examples of the hydroxyl group include 1,3,5-tris(4-t-butyl-3-hydroxy-2,5-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(4-t-butyl-5-ethyl-3-hydroxy-2-methylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, but are not limited thereto. Among these, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione is particularly preferred.
[0087] When the negative photosensitive resin composition contains a hindered phenol compound, the amount of the compound is preferably 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the (A) polyimide precursor and / or polyimide. The lower limit is more preferably 0.5 parts by mass or more because discoloration and corrosion of copper or copper alloys are prevented when the negative photosensitive resin composition is formed on copper or copper alloys. The upper limit is more preferably 10 parts by mass or less from the viewpoint of photosensitivity.
[0088] Organotitanium Compounds The negative photosensitive resin composition may contain an organotitanium compound. By containing an organotitanium compound in the negative photosensitive resin composition, a photosensitive resin layer having excellent chemical resistance can be formed even when cured at a low temperature.
[0089] Usable organotitanium compounds include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organotitanium compounds are shown in I) to VII) below: I) Titanium chelate compounds: Specific examples include titanium(IV) oxide acetylacetonate, titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), titanium diisopropoxide bis(ethylacetoacetate), and the like. II) Tetraalkoxytitanium compounds: For example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], and the like. III) Titanocene compounds: For example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and the like. IV) Monoalkoxytitanium compounds: For example, titanium tris(dioctylphosphate) isopropoxide, titanium tris(dodecylbenzenesulfonate) isopropoxide, etc. V) Titanium oxide compounds: For example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, and the like. VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate. VII) Titanate coupling agents: For example, isopropyl tridodecylbenzenesulfonyl titanate.
[0090] Among them, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds, from the viewpoint of exhibiting better chemical resistance. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, and titanium(IV) oxide acetylacetonate are preferred.
[0091] When the negative photosensitive resin composition contains an organic titanium compound, the amount of the organic titanium compound is preferably 0.05 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the (A) polyimide precursor. The lower limit is more preferably 0.2 parts by mass or more from the viewpoint of the heat resistance and chemical resistance of the resulting cured film. The upper limit is more preferably 2 parts by mass or less from the viewpoint of the storage stability of the negative photosensitive resin composition.
[0092] Thermal Crosslinking Agent In order to suppress the cure shrinkage of the cured film, the negative photosensitive resin composition may optionally contain a thermal crosslinking agent.
[0093] The thermal crosslinking agent means a compound that undergoes an addition reaction or a condensation polymerization reaction by heat. These reactions occur in combination with (A) the polyimide precursor or polyimide and a thermal crosslinking agent, between thermal crosslinking agents, or between a thermal crosslinking agent and other components, and the reaction temperature is preferably 150°C or higher.
[0094] Examples of the thermal crosslinking agent include an alkoxymethyl compound, an epoxy compound, an oxetane compound, a bismaleimide compound, an allyl compound, and a blocked isocyanate compound. From the viewpoint of suppressing cure shrinkage, the thermal crosslinking agent preferably contains a nitrogen atom.
[0095] Examples of the alkoxymethyl compound include, but are not limited to, the following compounds: [ka] [ka]
[0096] Examples of epoxy compounds include 4-hydroxybutyl acrylate glycidyl ether, epoxy compounds containing bisphenol A type groups, and hydrogenated bisphenol A diglycidyl ether (e.g., Epolite 4000 manufactured by Kyoeisha Chemical Co., Ltd.). Examples of oxetane compounds include 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, bis[1-ethyl(3-oxetanyl)]methyl ether, 4,4'-bis[(3-ethyl-3-oxetanyl)methyl]biphenyl, 4,4'-bis(3-ethyl-3-oxetanylmethoxy)biphenyl, ethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, diethylene glycol bis(3-ethyl-3-oxetanylmethyl)ether, and bis(3-ethyl-3-oxetanylmethyl). Examples of such oxetanes include diphenoate, trimethylolpropane tris(3-ethyl-3-oxetanylmethyl)ether, pentaerythritol tetrakis(3-ethyl-3-oxetanylmethyl)ether, poly[[3-[(3-ethyl-3-oxetanyl)methoxy]propyl]silasesquioxane] derivatives, oxetanyl silicate, phenol novolac-type oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, OXT121 (manufactured by Toagosei, trade name), and OXT221 (manufactured by Toagosei, trade name). Examples of bismaleimide compounds include 1,2-bis(maleimide)ethane, 1,3-bis(maleimide)propane, 1,4-bis(maleimide)butane, 1,5-bis(maleimide)pentane, 1,6-bis(maleimide)hexane, 2,2,4-trimethyl-1,6-bis(maleimide)hexane, N,N'-1,3-phenylenebis(maleimide), 4-methyl-N,N'-1,3-phenylenebis(maleimide), and 5-methyl-N,N'-1,3-phenylenebis(maleimide). Examples of the 4-maleimide-1,4-phenylene bis(maleimide) include N,N'-1,4-phenylene bis(maleimide), 3-methyl-N,N'-1,4-phenylene bis(maleimide), 4,4'-bis(maleimide)diphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-bis(maleimide)diphenylmethane, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane.Examples of the allyl compound include allyl alcohol, allyl anisole, allyl benzoate ester, allyl cinnamate ester, N-allyloxyphthalimide, allylphenol, allyl phenyl sulfone, allyl urea, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl maleate, diallyl isocyanurate, triallyl amine, triallyl isocyanurate, triallyl cyanurate, triallyl amine, triallyl 1,3,5-benzenetricarboxylate, triallyl trimellitate, triallyl phosphate, triallyl phosphite, and triallyl citrate. Examples of the blocked isocyanate compound include hexamethylene diisocyanate-based blocked isocyanates (e.g., Duranate SBN-70D, SBB-70P, SBF-70E, TPA-B80E, 17B-60P, MF-B60B, E402-B80B, MF-K60B, and WM44-L70G manufactured by Asahi Kasei Corporation, Takenate B-882N manufactured by Mitsui Chemicals, Inc., and 7960, 7961, 7982, 7991, and 7992 manufactured by Baxenden), tolylene diisocyanate-based blocked isocyanates (e.g., Takenate B-830 manufactured by Mitsui Chemicals, Inc.), 4 ,4'-diphenylmethane diisocyanate-based blocked isocyanates (e.g., Takenate B-815N manufactured by Mitsui Chemicals, Inc., Bronate PMD-OA01 and PMD-MA01 manufactured by Daiei Sangyo Co., Ltd., etc.), 1,3-bis(isocyanatemethyl)cyclohexane-based blocked isocyanates (e.g., Takenate B-846N manufactured by Mitsui Chemicals, Inc., Coronate BI-301, 2507, and 2554 manufactured by Tosoh Corporation, etc.), and isophorone diisocyanate-based blocked isocyanates (e.g., 7950, 7951, and 7990 manufactured by Baxenden, etc.). Among these, blocked isocyanates and bismaleimide compounds are preferred from the viewpoint of storage stability. (F) Thermal crosslinking agents may be used alone or in combination of two or more kinds.
[0097] The content of the thermal crosslinking agent in the negative photosensitive resin composition is preferably 0.2% by mass to 40% by mass based on 100 parts by mass of the (A) polyimide precursor and / or polyimide. From the viewpoint of chemical resistance, the lower limit is more preferably 1% by mass or more, and even more preferably 5% by mass or more. From the viewpoint of storage stability of the negative photosensitive resin composition, the upper limit is more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0098] Sensitizer The negative photosensitive resin composition may optionally contain a sensitizer to improve photosensitivity. Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylidene indane, and the like. Non, p-dimethylaminobenzylidene indanone, 2-(p-dimethylaminophenylbiphenylene)-benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetone ethyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin, N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, Np-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, and the like. These may be used alone or in combination of, for example, 2 to 5 types.
[0099] When the negative type photosensitive resin composition contains a sensitizer for improving photosensitivity, the amount of the sensitizer is preferably 0.1 parts by mass or more and 25 parts by mass or less per 100 parts by mass of the (A) polyimide precursor and / or polyimide.
[0100] The negative photosensitive resin composition may optionally contain a thermal polymerization inhibitor in order to improve the stability of viscosity and photosensitivity, particularly when stored in the form of a solution containing a solvent. Examples of the thermal polymerization inhibitor that can be used include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt.
[0101] <Method for Producing Cured Relief Pattern> The method for producing a cured relief pattern of the present invention comprises the steps of: (1) a step of applying the above-mentioned negative type photosensitive resin composition of the present invention onto a substrate to form a photosensitive resin layer on the substrate (a resin layer forming step); (2) a step of exposing the photosensitive resin layer to light (exposure step); (3) developing the exposed photosensitive resin layer to form a relief pattern (relief pattern formation step); (4) a step of heat-treating the relief pattern to form a cured relief pattern (cured relief pattern forming step); Includes.
[0102] (1) Resin layer formation process In this step, the negative photosensitive resin composition is applied onto a substrate, and then dried as necessary to form a photosensitive resin layer. As the application method, a method that has been conventionally used for applying negative photosensitive resin compositions, such as a method of applying with a spin coater, a bar coater, a blade coater, a curtain coater, a screen printer, etc., or a method of spray application with a spray coater, etc., can be used.
[0103] If necessary, the coating film containing the negative photosensitive resin composition can be dried. Examples of the drying method include air drying, heat drying using an oven or a hot plate, and vacuum drying. Specifically, in the case of air drying or heat drying, drying can be performed under conditions of 20°C to 150°C for 1 minute to 1 hour. In this manner, a photosensitive resin layer can be formed on a substrate.
[0104] (2) Exposure process In this step, the photosensitive resin layer formed above is exposed to an ultraviolet light source or the like through a photomask or reticle having a pattern, or directly, using an exposure device such as a contact aligner, mirror projection, or stepper. This exposure causes the polymerizable groups of the (A) polyimide precursor and polyimide contained in the negative photosensitive resin composition to crosslink due to the action of the (C) photopolymerization initiator. This crosslinking makes the exposed portion insoluble in the developer described below, making it possible to form a relief pattern.
[0105] Thereafter, for the purpose of improving the photosensitivity, etc., a post-exposure bake (PEB) or a pre-development bake, or both, may be performed at any combination of temperature and time, as necessary. The baking conditions are preferably a temperature of 40° C. to 120° C. and a time of 10 seconds to 240 seconds, but are not limited to these ranges as long as they do not impair the various properties of the negative-type photosensitive resin composition of the present invention.
[0106] (3) Relief pattern formation process In this process, the unexposed portion of the exposed photosensitive resin layer is developed and removed. As a development method for developing the exposed (irradiated) photosensitive resin layer, any method can be selected from conventionally known photoresist development methods, such as a rotary spray method, a paddle method, and a dipping method accompanied by ultrasonic treatment. After development, post-development baking may be performed at any combination of temperature and time, as necessary, for the purpose of adjusting the shape of the relief pattern, etc.
[0107] The developer used for development is preferably, for example, a good solvent for the negative photosensitive resin composition, or a combination of the good solvent and a poor solvent. As the good solvent, for example, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, etc. are preferable. As the poor solvent, for example, toluene, xylene, methanol, ethanol, isopropyl alcohol, ethyl lactate, propylene glycol methyl ether acetate, water, etc. are preferable. When a good solvent and a poor solvent are used in combination, it is preferable to adjust the ratio of the poor solvent to the good solvent according to the solubility of the polymer in the negative photosensitive resin composition. Two or more types of solvents, for example, several types, can also be used in combination.
[0108] (4) Hardened relief pattern formation process In this step, the relief pattern obtained by the above development is heat-treated to dissolve the photosensitive component, and when a polyimide precursor (A) is used, it is imidized to convert it into a cured relief pattern made of polyimide. As the method of heat treatment, various methods can be selected, such as a method using a hot plate, a method using an oven, or a method using a temperature-programmable heating oven. The heat treatment can be performed, for example, under conditions of 160°C to 350°C for 30 minutes to 5 hours. The temperature of the heat treatment is preferably 300°C or less, more preferably 250°C or less. The atmospheric gas during heat curing may be air, or an inert gas such as nitrogen or argon.
[0109] <Polyimide cured film> The present invention also provides a cured film formed from the negative photosensitive resin composition of the present invention. The cured film formed from the negative photosensitive resin composition is considered to contain a polyimide having a structure represented by general formula (2). Such a cured film has excellent elongation and high adhesion to copper.
[0110] <Semiconductor device> The present invention also provides a semiconductor device having a cured relief pattern obtained from the above-mentioned negative photosensitive resin composition. More specifically, a semiconductor device having a substrate that is a semiconductor element and a cured relief pattern is provided. The cured relief pattern may be produced by the above-mentioned method for producing a cured relief pattern using the above-mentioned negative photosensitive resin composition. Such a semiconductor device has excellent reliability because it has a cured relief pattern with excellent elongation of the cured film and high adhesion to copper. The present invention also provides a method for manufacturing a semiconductor device, which uses a semiconductor element as a substrate and includes the method for manufacturing a cured relief pattern of the present embodiment as part of the steps. In this case, the cured relief pattern formed by the method for manufacturing a cured relief pattern of the present disclosure can be formed as a surface protective film, an interlayer insulating film, an insulating film for a redistribution layer, a protective film for a flip chip device, or a protective film for a semiconductor device having a bump structure, or the like, of a semiconductor device, and can be manufactured by combining the method with a known method for manufacturing a semiconductor device.
[0111] <Display device> The present disclosure also provides a display device comprising a display element and a cured film provided on the upper portion of the display element, the cured film being the above-mentioned cured relief pattern. Here, the cured relief pattern may be laminated in direct contact with the display element, or may be laminated with another layer sandwiched therebetween. The cured film can be applied to, for example, surface protection films, insulating films, planarizing films, etc. of TFT liquid crystal display elements and color filter elements; protrusions for MVA type liquid crystal display devices; partition walls for cathodes of organic EL elements; and the like. EXAMPLES
[0112] The present embodiment will be described in detail below with reference to examples, but the present embodiment is not limited thereto. In the examples, comparative examples, and synthesis examples, the physical properties of the polyamic acid ester, polyimide, or negative photosensitive resin composition were measured and evaluated according to the following methods.
[0113] <Measurement and evaluation methods> (1) Weight average molecular weight The weight average molecular weight (Mw) of each resin was measured by gel permeation chromatography (converted into standard polystyrene) under the following conditions. Equipment: HLC-8320GPC (Tosoh Corporation) Eluent: N-methyl-2-pyrrolidone Lithium bromide monohydrate 30mmol / L Phosphate 50mmol / L Flow rate: 0.5mL / min Column: 2 TSK-GEL SUPER HM-H / 1 TSK-GEL SUPER H-RC Column temperature: 40℃ Detector: UV-8320
[0114] (2) Preparation of cured film for elongation measurement A negative photosensitive resin composition prepared by the method described below was spin-coated on a 6-inch silicon wafer that had been previously sputtered with Al using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.) so that the film thickness after drying would be 10 μm. The wafer was then pre-baked on a hot plate at 110°C for 180 seconds to form a coating film with a thickness of 10 μm. The resulting photosensitive resin film was then irradiated with 800 mJ / cm2 of a high-pressure mercury lamp. 2 Then, the film was heated in a temperature programmable curing oven (VF-2000 type, manufactured by Koyo Lindberg) at 230° C. for 2 hours in a nitrogen atmosphere to obtain a cured film for elongation measurement.
[0115] (3) Measurement of elongation The cured film on the Al wafer obtained in (2) above was cut into strips with a width of 3 mm using a dicing machine (DISCO, DAD3350) and treated with 10% hydrochloric acid to obtain a polyimide tape with a width of 3 mm. The obtained polyimide tape was left to stand for 24 hours or more in an atmosphere with a temperature of 23°C and a humidity of 50%. The elongation of the polyimide tape that had been left to stand was measured using a tensile tester (UTM-II-20 type, manufactured by Orientec Co., Ltd.) under conditions of a test speed of 40 mm / min and an initial load of 0.5 fs, and the elongation and average elongation were obtained according to the following definitions. In this application, the test was performed 10 times. Elongation (%) = 100 x {(specimen length at break - specimen length before test) / specimen length before test} Average elongation (%) = elongation / number of tests
[0116] The average elongation determined above was evaluated based on the following criteria. Excellent: Average elongation of 35% or more Good: Average elongation is 20% or more and less than 35% Acceptable: Average elongation is 10% or more but less than 20% Unacceptable: Average elongation is less than 10%
[0117] (4) Measurement of cure shrinkage rate A negative photosensitive resin composition prepared by the method described below was spin-coated on a 6-inch silicon wafer (manufactured by Fujimi Electronics Co., Ltd., thickness 625±25 μm) using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.) so that the film thickness after drying would be 10 μm. The wafer was then pre-baked on a hot plate at 110° C. for 180 seconds to form a coating film with a thickness of 10 μm. The resulting photosensitive resin film was then irradiated with 400 mJ / cm 2 from a high-pressure mercury lamp. 2 Then, the film was heated in a temperature programmable curing oven (VF-2000 type, manufactured by Koyo Lindberg) at 230° C. for 2 hours in a nitrogen atmosphere to obtain a cured film.
[0118] The cure shrinkage of the resulting cured film was calculated according to the following definition. Curing shrinkage rate [%] = {(film thickness after curing [μm]) ÷ (film thickness before curing [μm])} × 100 The remaining film rate obtained by the above formula was evaluated according to the following criteria. Excellent: Curing shrinkage rate is 85% or more Good: Curing shrinkage rate is 75% or more and less than 85% Acceptable: Curing shrinkage rate is 65% or more and less than 75% Not acceptable: Curing shrinkage rate is less than 65%
[0119] (5) Copper adhesion evaluation A negative photosensitive resin composition prepared by the method described below was spin-coated onto a 6-inch silicon wafer that had been previously sputtered with Ti and Cu using a coater developer (D-Spin60A model, manufactured by SOKUDO Co., Ltd.) so that the film thickness after drying would be 10 μm, and then the wafer was pre-baked on a hot plate at 110°C for 180 seconds to form a coating film with a thickness of 10 μm. The resulting photosensitive resin film was then irradiated with 400 mJ / cm2 of a high-pressure mercury lamp. 2 The exposed film was then heated at 230° C. for 2 hours in a nitrogen atmosphere using a temperature-programmed curing furnace (VF-2000, manufactured by Koyo Lindberg Co., Ltd.) to obtain a cured film of resin having a thickness of approximately 6 μm on the Cu.
[0120] The heat-treated film was evaluated for adhesion properties between the copper substrate and the cured resin coating film according to the cross-cut method of JIS K 5600-5-6 standard, based on the following criteria. "Excellent": The lattice number of the cured resin coating adhered to the substrate is 100 "Good": The lattice number of the cured resin coating adhered to the substrate is 80 or more and less than 100. "Acceptable": The lattice number of the cured resin coating adhered to the substrate is 60 or more and less than 80. "Not acceptable": The number of lattices in the cured resin coating adhered to the substrate is less than 60.
[0121] (6) Storage stability evaluation After preparing the photosensitive resin composition, the composition was stirred at room temperature (23.0°C ± 0.5°C, relative humidity 50% ± 10%) for 3 days to be the initial state, and then left to stand at room temperature for 4 weeks. The viscosity of the initial PI precursor resin composition was measured using a viscometer (VISCOMETER RE-85, manufactured by TOKI SANGYO), and the viscosity of the PI precursor resin composition left to stand at room temperature for 4 weeks was measured in the same manner. The viscosity change rate was calculated according to the following formula. Viscosity change rate = (viscosity of PI precursor resin composition left standing for 4 weeks / initial PI precursor resin composition) x 100 The viscosity change rate obtained by the above formula was evaluated according to the following criteria. Excellent: Viscosity change rate is less than 1% Good: Viscosity change rate is 1% or more but less than 5% Acceptable: Viscosity change rate is 5% or more but less than 10% Unacceptable: Viscosity change rate is 10% or more
[0122] <Synthesis Example 1> ((A-1) Synthesis of Polyimide Amic Acid Ester A-1-1) 24.8g (0.08mol) of 4,4'-oxydiphthalic dianhydride (ODPA) and 26.2g (0.12mol) of pyromellitic dianhydride (PMDA) were placed in a 1L separable flask and 74.9g of γ-butyrolactone was added. Next, 52.1g (0.40mol) of 2-hydroxyethyl methacrylate (HEMA) was added, and 31.6g (0.40mol) of pyridine was added while stirring. The mixture was stirred at 40°C for 5 hours using an oil bath to obtain a reaction mixture. After the reaction was completed, the mixture was allowed to cool to room temperature and left for 16 hours.
[0123] Next, while stirring the resulting reaction mixture, a solution of 81.3 g of dicyclohexylcarbodiimide (DCC) dissolved in 100 g of γ-butyrolactone was added over 40 minutes under ice cooling, followed by the addition of a suspension of 38.2 g (0.18 mol) of m-tolidine (m-TB) suspended in 300 g of γ-butyrolactone over 60 minutes. After stirring at room temperature for 2 hours, 18 g of ethyl alcohol was added and stirred for another hour, and then 140 g of γ-butyrolactone was added. The reaction mixture was filtered to remove the precipitate formed in the reaction system, and a reaction liquid was obtained.
[0124] The obtained reaction solution was added to 1.2 kg of ethyl alcohol to precipitate a crude polymer. The precipitated crude polymer was collected by filtration and dissolved in 600 g of γ-butyrolactone to obtain a crude polymer solution. The obtained crude polymer solution was dropped into 7 kg of water to reprecipitate the polymer. The obtained reprecipitate was collected by filtration and then vacuum dried to obtain a powdered polymer (polymer A-1-1). The molecular weight of polymer A-1-1 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 23,000.
[0125] <Synthesis Example 2> (A-1) Synthesis of Polyimide Amic Acid Ester A-1-2 Except for changing 24.8g (0.08mol) of ODPA and 26.2g (0.12mol) of PMDA in Synthesis Example 1 to 62.0g (0.2mol) of ODPA, and changing 38.2g of m-TB to 37.2g (0.19mol) of 4,4'-diaminodiphenyl ether (DADPE), the reaction was carried out in the same manner as in Synthesis Example 1 to obtain polymer A-1-2. The molecular weight of polymer A-1-2 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 19,000.
[0126] <Synthesis Example 3> ((A-1) Synthesis of Polyimide Amic Acid Ester A-1-3) The reaction was carried out in the same manner as described in Synthesis Example 1, except that 24.8 g (0.08 mol) of ODPA and 26.2 g (0.12 mol) of PMDA in Synthesis Example 1 were replaced with 49.6 g (0.16 mol) of ODPA and 11.8 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) (0.04 mol), and 38.2 g of m-TB was replaced with 34.3 g (0.17 mol) of 4,4'-diaminodiphenyl ether (DADPE), to obtain polymer A-1-3. The molecular weight of polymer A-1-3 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that the weight average molecular weight (Mw) was 19,000.
[0127] <Synthesis Example 4> ((A-1) Synthesis of Polyimide Amic Acid Ester A-1-4) Polymer A-1-4 was obtained by carrying out the reaction in the same manner as in Synthesis Example 2, except that 37.2 g of DADPE in Synthesis Example 2 was replaced with 19.7 g of p-phenylenediamine (p-PD). The molecular weight of Polymer A-1-4 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 25,000.
[0128] <Synthesis Example 5> ((A-2) Synthesis of Polyimide A-2-1) A Dean-Stark extraction apparatus was attached to a three-neck flask purged with nitrogen, and 100.0 g of N-methylpyrrolidone (hereinafter NMP) and 34.9 g (0.1 mol) of 9,9'-bis(4-aminophenyl)fluorene (hereinafter BAFL) were added and dissolved, to which 15.6 g (0.05 mol) of 4,4'-oxydiphthalic dianhydride (ODPA) and 25.0 g of toluene were added and heated to 180°C. After confirming that the theoretical amount of water (1.80 g) and the added toluene (25.0 g) had been extracted in the Dean-Stark extraction apparatus, heating was stopped and the mixture was cooled to room temperature.
[0129] To the resulting reaction solution, 15.5 g (0.1 mol) of 2-methacryloyloxyethyl isocyanate (Karenz MOI, product name; Resonac Corporation) was added and stirred to obtain a polymer solution. The resulting polymer solution was dropped into 3 kg of water to precipitate the polymer, which was then filtered and vacuum dried to obtain terminally modified polyimide A-2-1 in powder form. The molecular weight of polyimide A-2-1 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 4,400. The terminal modification rate was confirmed to be 95% from the integral ratio of proton NMR.
[0130] <Synthesis Example 6> (A-2) Synthesis of Polyimide A-2-2 Polymer A-2-2 was obtained by carrying out the reaction in the same manner as in Synthesis Example 5, except that Karenz MOI in Synthesis Example 5 was not added. The molecular weight of Polymer A-2-2 was measured by gel permeation chromatography (standard polystyrene equivalent) and found to have a weight average molecular weight (Mw) of 4,200.
[0131] <Synthesis Example 7> ((A-2) Synthesis of Polyimide A-2-3) The reaction was carried out in the same manner as in Synthesis Example 5, except that BAFL in Synthesis Example 5 was replaced with 27.7 g of 6-(4-aminophenoxy)[1,1'-biphenyl]-3-amine (hereinafter referred to as PDPE), to obtain polyimide A-2-3. The molecular weight of polyimide A-2-3 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 5,500. The modification rate of the terminals was confirmed to be 100% based on the integral ratio of proton NMR.
[0132] <Synthesis Example 8> ((A-2) Synthesis of Polyimide A-2-4) The reaction was carried out in the same manner as described in Synthesis Example 5, except that ODPA was replaced with 14.89 g (0.06 mol) of bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (hereinafter: BCD), BAFL was replaced with 22.11 g (0.08 mol) of PDPE, and the amount of Karenz MOI was replaced with 18.6 g, to obtain polyimide A-2-4. The molecular weight of polyimide A-2-4 was measured by gel permeation chromatography (standard polystyrene equivalent) to find that Mw was 8,700. In addition, it was confirmed that the modification rate of the terminals was 100% based on the integral ratio of proton NMR.
[0133] <Example 1> A negative photosensitive resin composition was prepared by the following method, and the prepared composition was evaluated. (A) 100 g of A-1-1 as a polymer, (B) 5 g of KZ-941 (trade name, B-1) as a photopolymerization initiator, (C-1) 20 g of KRM7735 (trade name, Daicel Allnex Corporation, C-1-1, Tg of cured product: 22°C) as a urethane (meth)acrylate were dissolved in 160 g of γ-butyrolactone (hereinafter referred to as GBL, D-1) and 40 g of dimethyl sulfoxide (hereinafter referred to as DMSO, D-2) to prepare a negative photosensitive resin composition. The composition was evaluated according to the above-mentioned method. The results are shown in Table 1.
[0134] <Examples 2 to 22 and Comparative Examples 1 to 4> Negative photosensitive resin compositions were prepared similarly to Example 1, except that polymers and other additives were used as shown in Tables 1 to 3, and evaluations were carried out similarly to Example 1. The results are shown in Tables 1 to 3.
[0135] The (A-1) polyimide precursor, (A-2) polyimide, (B) photopolymerization initiator, (C-1) urethane (meth)acrylate, (C-2) polymerizable monomer, (D) solvent, and (E) rust inhibitor listed in Tables 1 to 3 are as follows. B-2: PBG3057 (product name, manufactured by Changzhou Strong Electronics New Materials Co., Ltd.) C-1-2: EBECRYL4740 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 35°C, molecular weight: 1250, number of (meth)acryloyl groups: 2 C-1-3: KRM8667 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 85°C, molecular weight: 2000, number of (meth)acryloyl groups: 3 C-1-4: EBECRYL230 (trade name, manufactured by Daicel-Allnex), Tg of cured product: -55°C, molecular weight: 5000, number of (meth)acryloyl groups: 2 C-1-5: EBECRYL4491 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: -45°C, molecular weight: 7000, number of (meth)acryloyl groups: 2 C-1-6: KRM9276 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 5°C, molecular weight: 215, number of (meth)acryloyl groups: 1 C-1-7: EBECRYL4858 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 54°C, molecular weight: 450, number of (meth)acryloyl groups: 2 C-1-8: EBECRYL4738 (trade name, manufactured by Daicel-Allnex Corporation), Tg of cured product: 105°C, molecular weight: 800, number of (meth)acryloyl groups: 3 C-1-9: EBECRYL4859 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 136°C, molecular weight: 500, number of (meth)acryloyl groups: 2 C-1-10: KRM8528 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: 150°C, molecular weight: 1600, number of (meth)acryloyl groups: 4 C-1-11: EBECRYL210 (trade name, manufactured by Daicel Allnex Corporation), Tg of cured product: -19°C, molecular weight: 1500, number of (meth)acryloyl groups: 2 C-1-12: EBECRYL8301R (trade name, manufactured by Daicel Allnex), Tg of cured product: 63°C, number of meth)acryloyl groups: 6 C-1-13: EBECRYL8413 (trade name, manufactured by Daicel Allnex), Tg of cured product: -35°C, molecular weight: 36000, number of (meth)acryloyl groups: 2 C-2-1: Tetraethylene glycol dimethacrylate C-2-2: Tris-(2-acryloxyethyl) isocyanurate E-1: 8-azaadenine
[0136] [Table 1]
[0137] [Table 2]
[0138] [Table 3]
[0139] As shown in Tables 1 and 2, the negative photosensitive resin composition of Example 1 had excellent elongation, a pass rating in the cure residual film evaluation, and good adhesion. The photosensitive resin compositions of Examples 2 to 25 all had pass or better ratings in elongation, cure residual film evaluation (curing shrinkage rate), and adhesion.
[0140] On the other hand, as shown in Table 3, the adhesion was unsatisfactory in Comparative Example 1, the cure residual film evaluation and adhesion were unsatisfactory in Comparative Example 2, the elongation and adhesion were unsatisfactory in Comparative Example 3, the elongation was unsatisfactory in Comparative Example 4, and the elongation and adhesion were unsatisfactory in Comparative Example 5. [Industrial Applicability]
[0141] The negative photosensitive resin composition of the present disclosure is useful not only for application to the semiconductor device described above, but also for applications such as an interlayer insulating film in a multilayer circuit, a cover coat for a flexible copper-clad board, a solder resist film, and a liquid crystal alignment film.
Claims
1. The following components (A) to (D): (A) At least one selected from polyamic acid esters and polyimides (B) Photopolymerization initiator (C1) Urethane (meth)acrylate (D) Solvent Including, The negative photosensitive resin composition (C1), wherein a cured product of the urethane (meth)acrylate has a glass transition temperature of 130° C. or lower.
2. 2. The negative photosensitive resin composition according to claim 1, wherein a cured product of the component (C1) has a glass transition temperature of 110° C. or lower.
3. 2. The negative type photosensitive resin composition according to claim 1, wherein a cured product of the component (C1) has a glass transition temperature of 85° C. or lower.
4. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (C1) is an aliphatic urethane (meth)acrylate.
5. 3. The negative type photosensitive resin composition according to claim 1, wherein the number of (meth)acryloyl groups in the component (C1) is 1 to 3.
6. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (C1) has a weight average molecular weight of 7,000 or less.
7. 7. The negative type photosensitive resin composition according to claim 6, wherein the weight average molecular weight of the component (C1) is 500 or more.
8. 3. The negative type photosensitive resin composition according to claim 1, wherein the content of the component (C1) is 15 parts by mass or more per 100 parts by mass of the component (A).
9. 9. The negative type photosensitive resin composition according to claim 8, wherein the content of the component (C1) is less than 30 parts by mass per 100 parts by mass of the component (A).
10. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (A) is a polyamic acid ester represented by the following general formula (1): 【Chemistry 1】 (In the formula, X 1 is a tetravalent organic group, Y 1 is a divalent organic group, R 1 and R 2 At least one of represents a monovalent organic group having a radical polymerizable group having 1 to 40 carbon atoms, and n is an integer of 2 to 100.
11. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (A) is a polyimide represented by the following general formula (2): 【Chemistry 2】 (In the formula, X 1 is a tetravalent organic group, Y 1 represents a divalent organic group, and n is an integer from 2 to 100.
12. The negative type photosensitive resin composition according to claim 11, wherein the component (A) is a polyimide having no acidic group.
13. 3. The negative type photosensitive resin composition according to claim 1, wherein the component (A) is a polyimide having a (meth)acryloyl group at a main chain terminal.
14. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (C2) a radical polymerizable compound other than (C1) a urethane (meth)acrylate.
15. The negative type photosensitive resin composition according to claim 1 or 2, further comprising (E) a rust inhibitor.
16. The negative type photosensitive resin composition according to claim 1 or 2, which is used for forming a rewiring layer.
17. The following steps: (1) applying the negative type photosensitive resin composition according to claim 1 or 2 onto a substrate to form a photosensitive resin layer on the substrate; (2) exposing the photosensitive resin layer to light; (3) developing the exposed photosensitive resin layer to form a relief pattern; (4) heat treating the relief pattern to form a hardened relief pattern; 2. A method for producing a cured relief pattern comprising:
18. A cured film comprising a cured product of the negative photosensitive resin composition according to claim 1 or 2.
19. An interlayer insulating film formed by using the negative photosensitive resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Fanout wafer-level-package structure and method of manufacturing same
JP2005167191A
Photosensitive resin composition, method for producing electronic device, and electronic device
JP2021162834A
Method for producing composite material conjugate
WO2021010028A1
Cited By
Semiconductor integrated circuit
CN121725848A