Non-aqueous secondary battery and method of manufacturing non-aqueous secondary battery
The non-aqueous secondary battery design addresses cell expansion and electrolyte impregnation issues by setting the cell compression parameter to 0.000 to 0.007, enhancing stability and performance through controlled cell expansion and electrolyte distribution.
Patent Information
- Application Number
- JP2023080737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing non-aqueous secondary batteries face issues with cell thickness expansion and electrolyte impregnation due to the mismatch in hardness between the negative electrode and the spacer, leading to potential swelling and reduced electrolyte distribution.
A non-aqueous secondary battery design that sets the cell compression parameter to a range of 0.000 to 0.007, balancing the cell compression force with the spring constant of the case to control cell expansion and maintain electrolyte impregnation, using a specific configuration of electrode sheets, separators, and electrolyte composition.
The solution effectively suppresses cell thickness expansion and maintains electrolyte impregnation, ensuring stable battery performance by controlling cell compression forces and internal pressure.
Smart Images

Figure 2024164974000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonaqueous secondary battery and a method for manufacturing a nonaqueous secondary battery. [Background technology]
[0002] The battery pack described in Patent Document 1 includes a plurality of arranged single cells and a spacer interposed between the single cells. The single cells include an electrode group in which a positive electrode and a negative electrode are stacked facing each other with a separator interposed therebetween, and a rectangular case that houses the electrode group. The electrode group expands in the stacking direction as the electrodes are charged and discharged. The negative electrode plate described in Patent Document 1 is harder than the spacer. Therefore, when the electrode group expands, the spacer, which is softer than the negative electrode plate, deforms and absorbs the strain. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-84550 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, in the battery pack (cell) described in the above Patent Document 1, the hardness of the negative electrode plate needs to be set in accordance with the spacer, and therefore there is a need to suppress the expansion of the cell thickness when it is not constrained. [Means for solving the problem]
[0005] The nonaqueous secondary battery that solves the above problem is a nonaqueous secondary battery that includes an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator between them, a nonaqueous electrolyte, and a case that contains the electrode assembly and the nonaqueous electrolyte, and has a cell compression parameter that is equal to or greater than 0.000 and equal to or less than 0.007, the cell compression parameter being calculated by multiplying the area of a flat portion of the electrode assembly by the differential pressure between the internal pressure of the case and the atmospheric pressure and the area of the flat portion of the electrode assembly.
[0006] According to the above configuration, by setting the cell compression parameter to 0.000 or more, the cell can be compressed by atmospheric pressure to suppress the expansion of the cell thickness when unconstrained. Also, by setting the cell compression parameter to 0.007 or less, it is possible to suppress the deterioration of the impregnation of the electrolyte into the electrode body due to the reduced pressure inside the cell.
[0007] A method for manufacturing a nonaqueous secondary battery that solves the above-mentioned problems includes an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator between them, a nonaqueous electrolyte, and a case that contains the electrode assembly and the nonaqueous electrolyte, and adjusts a cell compression parameter obtained by dividing a cell compression force, which is calculated by the product of a pressure difference between an internal pressure of the case and the atmospheric pressure and an area of a flat portion of the electrode assembly, by a spring constant of the case, to be greater than or equal to 0.000 and less than or equal to 0.007.
[0008] According to the above method, by setting the cell compression parameter to 0.000 or more, the cell can be compressed by atmospheric pressure to suppress the expansion of the cell thickness when unconstrained. Also, by setting the cell compression parameter to 0.007 or less, it is possible to suppress the deterioration of the impregnation of the electrolyte into the electrode body due to the reduced pressure inside the cell. Effect of the Invention
[0009] According to the present invention, it is possible to suppress the expansion of the cell thickness when unconstrained. [Brief description of the drawings]
[0010] [Figure 1] 1 is a perspective view showing a schematic configuration of a cell battery of an embodiment of a nonaqueous secondary battery. [Diagram 2] FIG. 4 is a view showing a part of the electrode body of the embodiment in an expanded form. [Diagram 3] FIG. 2 is a cross-sectional view of the cell battery of the same embodiment. [Figure 4] 4 is a graph showing unconstrained cell thickness and Li precipitation resistance versus cell compression parameter of the nonaqueous secondary battery of the embodiment. [Diagram 5] 1 is a table showing examples and comparative examples of nonaqueous secondary batteries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Present embodiment] An embodiment of a nonaqueous secondary battery and a method for manufacturing a nonaqueous secondary battery will be described below with reference to Figures 1 to 4. As an example of the nonaqueous secondary battery, a lithium ion secondary battery will be described.
[0012] [Lithium-ion secondary battery 10] 1, a lithium-ion secondary battery 10 is a cell battery that is combined with a plurality of lithium-ion secondary batteries 10 and sealed in a resin or metal case to form a battery pack. The battery pack is used in hybrid vehicles and electric vehicles.
[0013] The lithium ion secondary battery 10 includes a battery case 11 and a lid 12. The battery case 11 has a rectangular parallelepiped shape with an opening on the upper side. The lid 12 seals the opening of the battery case 11. The battery case 11 and the lid 12 are made of a metal such as aluminum or an aluminum alloy. The lithium ion secondary battery 10 is configured as a sealed battery container by attaching the lid 12 to the battery case 11.
[0014] The lid 12 is provided with two positive external terminals 13A and a negative external terminal 13B. The positive external terminal 13A and the negative external terminal 13B are used for charging and discharging power. The electrode body 20 is accommodated inside the battery case 11. An external film (not shown) is inserted between the battery case 11 and the electrode body 20. The positive electrode side current collector 20A, which is the end of the electrode body 20 on the positive electrode side, is electrically connected to the positive electrode external terminal 13A via the positive electrode side current collector 14A. The negative electrode side current collector 20B, which is the end of the electrode body 20 on the negative electrode side, is electrically connected to the negative electrode external terminal 13B via the negative electrode side current collector 14B. In addition, a nonaqueous electrolyte is injected into the battery case 11 through a liquid injection hole (not shown). The shapes of the positive electrode external terminal 13A and the negative electrode external terminal 13B are not limited to those shown in FIG. 1 and may be any shape.
[0015] [Electrode body 20] 2, the electrode body 20 is a flat wound body obtained by winding a laminate in which a long positive electrode sheet 21 and a negative electrode sheet 24 are stacked with a separator 27 interposed therebetween. The positive electrode sheet 21, the negative electrode sheet 24, and the separator 27 are stacked such that their respective longitudinal directions coincide with the longitudinal direction D1. In the laminate before winding, the positive electrode sheet 21, the separator 27, the negative electrode sheet 24, and the separator 27 are stacked in this order.
[0016] [Positive electrode sheet 21] The positive electrode sheet 21 includes a positive electrode current collector 22 and a positive electrode composite layer 23. The positive electrode current collector 22 is a foil-like positive electrode base material formed in an elongated shape. The positive electrode composite layer 23 is provided on each of two opposing surfaces of the positive electrode current collector 22. The positive electrode current collector 22 includes a positive electrode-side uncoated portion 22A at one end in the width direction D2 where the positive electrode composite layer 23 is not formed and the positive electrode current collector 22 is exposed.
[0017] A metal foil made of aluminum or an alloy mainly composed of aluminum is used for the positive electrode current collector 22. The positive electrode current collector 22 functions as a current collector for the positive electrode. In the wound state, the positive electrode side uncoated portion 22A of the positive electrode current collector 22 is pressed against each other at opposing surfaces to form the positive electrode side current collector 20A.
[0018] The positive electrode mixture layer 23 is a hardened body of a liquid positive electrode mixture paste. The positive electrode mixture paste includes a positive electrode active material, a positive electrode solvent, a positive electrode conductive material, and a positive electrode binder. The positive electrode mixture layer 23 is formed by drying the positive electrode mixture paste and evaporating the positive electrode solvent. Therefore, the positive electrode mixture layer 23 includes a positive electrode active material, a positive electrode conductive material, and a positive electrode binder.
[0019] The positive electrode active material is a lithium-containing composite oxide capable of absorbing and releasing lithium ions, which are charge carriers in the lithium-ion secondary battery 10. The lithium-containing composite oxide is an oxide containing lithium and a metal element other than lithium. The metal element other than lithium is at least one selected from the group consisting of nickel, cobalt, manganese, vanadium, magnesium, molybdenum, niobium, titanium, tungsten, aluminum, and iron contained in the lithium-containing composite oxide as iron phosphate.
[0020] For example, the lithium-containing composite oxide is lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or lithium manganese oxide (LiMn2O4). For example, the lithium-containing composite oxide is a ternary lithium-containing composite oxide containing nickel, cobalt, and manganese, and is lithium nickel cobalt manganese oxide (LiNiCoMnO2). For example, the lithium-containing composite oxide is lithium iron phosphate (LiFePO4).
[0021] The positive electrode solvent is an NMP (N-methyl-2-pyrrolidone) solution, which is an example of an organic solvent. The positive electrode conductive material is, for example, carbon black such as acetylene black or ketjen black, carbon fiber such as carbon nanotube or carbon nanofiber, or graphite. The positive electrode binder is an example of a resin component contained in the positive electrode mixture paste. The positive electrode binder is, for example, polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), or the like.
[0022] The positive electrode sheet 21 may have an insulating layer at the boundary between the positive electrode uncoated portion 22A and the positive electrode mixture layer 23. The insulating layer contains an inorganic component having insulating properties and a resin component that functions as a binder. The inorganic component is at least one selected from the group consisting of powdered boehmite, titania, and alumina. The resin component is at least one selected from the group consisting of PVDF, PVA, and acrylic.
[0023] [Negative electrode sheet 24] The negative electrode sheet 24 includes a negative electrode current collector 25 and a negative electrode composite layer 26. The negative electrode current collector 25 is a foil-like negative electrode base material formed in an elongated shape. The negative electrode composite layer 26 is provided on each of two opposing surfaces of the negative electrode current collector 25. The negative electrode current collector 25 includes a negative electrode-side uncoated portion 25A at one end in the width direction D2, which is located opposite the positive electrode-side uncoated portion 22A, where the negative electrode composite layer 26 is not formed and the negative electrode current collector 25 is exposed.
[0024] A metal foil made of copper or an alloy mainly composed of copper is used for the negative electrode current collector 25. The negative electrode current collector 25 functions as a current collector for the negative electrode. In the wound body state, the negative electrode uncoated portion 25A has opposing surfaces pressed against each other to form the negative electrode current collector 20B.
[0025] The negative electrode mixture layer 26 is a hardened body of the liquid negative electrode mixture paste. The negative electrode mixture paste includes a negative electrode active material, a negative electrode solvent, a negative electrode thickener, and a negative electrode binder. The negative electrode mixture layer 26 is formed by drying the negative electrode mixture paste and evaporating the negative electrode solvent. Therefore, the negative electrode mixture layer 26 includes the negative electrode active material, and further includes a negative electrode thickener and a negative electrode binder as additives. The negative electrode mixture layer 26 may further include an additive such as a conductive material.
[0026] The negative electrode active material is a material capable of absorbing and releasing lithium ions. For example, carbon materials such as graphite, non-graphitizable carbon, graphitizable carbon, and carbon nanotubes are used as the negative electrode active material. An example of the negative electrode solvent is water. For example, CMC (carboxymethyl cellulose) can be used as the negative electrode thickener, which is a thickener containing a sodium salt. For example, the negative electrode binder can be the same as the positive electrode binder. For example, SAR (styrene acrylic acid copolymer) can be used as the negative electrode binder, which is a binder containing a sodium salt.
[0027] [Separator 27] The separator 27 prevents contact between the positive electrode sheet 21 and the negative electrode sheet 24, and retains a nonaqueous electrolyte between the positive electrode sheet 21 and the negative electrode sheet 24. When the electrode body 20 is immersed in the nonaqueous electrolyte, the nonaqueous electrolyte permeates from the ends of the separator 27 in the width direction D2 toward the center.
[0028] The separator 27 is a nonwoven fabric made of polypropylene, etc. As the separator 27, for example, a porous polymer membrane such as a porous polyethylene membrane, a porous polyolefin membrane, a porous polyvinyl chloride membrane, an ion-conductive polymer electrolyte membrane, etc. can be used.
[0029] [Nonaqueous electrolyte] The non-aqueous electrolyte is a composition in which a supporting salt is contained in a non-aqueous solvent. As the non-aqueous solvent, one or more materials selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. can be used. In addition, as the supporting salt, one or more lithium compounds (lithium salts) selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, LiBOB (lithium bis(oxalate)borate), etc. can be used.
[0030] In this embodiment, ethylene carbonate is used as the non-aqueous solvent. LiBOB is added to the non-aqueous electrolyte as a lithium salt of the film forming agent. For example, LiBOB is added to the non-aqueous electrolyte so that the concentration of LiBOB in the non-aqueous electrolyte is 0.001 to 0.1 [mol / L].
[0031] [Manufacturing method] Next, a method for manufacturing the lithium ion secondary battery 10 will be described with reference to FIGS.
[0032] As shown in FIG. 3, if the thickness T of the electrode body 20 exceeds the inner dimension W of the battery case 11, the thickness of the cell battery will expand. Therefore, in order to prevent the thickness of the cell battery from expanding, the cell compression parameter is set to 0.000 or more and 0.007 or less. The cell compression parameter is obtained by dividing the cell compression force by the cell spring constant. The cell spring constant is calculated from the thickness displacement amount at 2 kN to 5 kN when the battery cell is compressed by an autograph (precision universal testing machine). The cell compression parameter is shown in formula (1). The cell compression force is obtained by the product of the difference in internal pressure with respect to the atmospheric pressure of the battery case 11 and the flat area of the electrode body 20. The cell compression force is shown in formula (2). The flat area of the electrode body 20 is obtained by the product of the positive electrode coating width and the electrode body flat area height. The flat area of the electrode body 20 is shown in formula (3). For example, the innermost positive electrode length is used as the electrode body flat area height.
[0033] Cell compression parameter = cell compression force ÷ cell spring constant [kN / mm] (1) Cell compression force = -cell internal pressure [MPa] × electrode body flat area [mm 2 ]···(2) Electrode body flat area = positive electrode coating width [mm] × electrode body flat part height [mm] (3)
[0034] As shown in Fig. 4, by setting the cell compression parameter to a range exceeding 0.000, it is possible to apply a cell compression force due to atmospheric pressure and suppress the expansion of the cell thickness when unconstrained. The cell thickness when unconstrained is the thickness measured when the probe of a digimatic indicator (e.g., pressed with 1.5 N) comes into contact with the maximum value of the convex part on the side of the battery cell. The cell thickness when there is no swelling is the sum of the plate thickness (both sides) of the battery case 11, the thickness (both sides) of the extrapolation film 15, and the thickness of the electrode body 20 (see Fig. 3).
[0035] Furthermore, when the cell internal pressure decreases and the cell compression parameter becomes 0.007 or more, the inside of the cell is in a reduced pressure state, which deteriorates the impregnation of the electrolyte into the electrode body 20. When the impregnation of the electrolyte deteriorates, unevenness occurs in the formation of the coating on the negative electrode, and the Li deposition resistance decreases. The Li deposition resistance is an index of the Li deposition resistance of each battery cell, with the Li deposition limit current value when the cell compression parameter is 0.000 being set to 100.
[0036] Therefore, by setting the cell compression parameter to be 0.000 or more and 0.007 or less, it is possible to suppress the fluctuation in the cell thickness when unconstrained, and to suppress the decrease in Li precipitation resistance caused by the reduced pressure state inside the cell.
[0037] Next, the effects of this embodiment will be described. (1) By setting the cell compression parameter to 0.000 or more, the cell can be compressed by atmospheric pressure to suppress the expansion of the cell thickness when unconstrained. Also, by setting the cell compression parameter to 0.007 or less, it is possible to suppress the deterioration of the impregnation of the electrolyte into the electrode body 20 due to the reduced pressure inside the cell.
[0038] (Other embodiments) The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.
[0039] In the above embodiment, the cell spring constant may be adjusted to be softer by increasing the number of separators. In the above embodiment, the battery cell may be made negative pressure by sealing the lid 12 immediately after the electrolyte is placed in the battery case 11. Alternatively, the negative pressure may be created by increasing the space between the electrode body 20 of the battery case 11 and the lid 12 and allowing the electrolyte to impregnate the electrode body 20.
[0040] In the above embodiment, the electrode body 20 is a wound body obtained by winding a laminate in which the positive electrode sheet 21 and the negative electrode sheet 24 are laminated with the separator 27 interposed therebetween. However, the electrode body may be a laminate in which a plurality of positive electrode sheets 21 and a plurality of negative electrode sheets 24 are alternately stacked with the separator 27 interposed therebetween.
[0041] The lithium ion secondary battery 10 may be mounted on an automatic transport vehicle, a special vehicle for loading and unloading, an electric vehicle, a hybrid vehicle, a computer, or other electronic device, or may be part of other systems. For example, it may be mounted on a moving object such as a ship or an aircraft, or may be a power supply system that supplies power from a power plant via a substation to a building or home in which a secondary battery is installed.
[0042] [Example] Next, examples and comparative examples of the lithium ion secondary battery 10 will be described with reference to Fig. 5. Note that these examples and comparative examples do not limit the manufacturing method of the nonaqueous secondary battery.
[0043] In the following, lithium ion secondary batteries 10 of examples and comparative examples were prepared in which the combinations of the cell internal pressure, the positive electrode coating width, the innermost circumferential positive electrode length, and the cell spring constant were changed as shown in Fig. 5. Then, for each example and each comparative example, the cell compression parameter was calculated, and the cell thickness [mm] and the precipitation limit current [%] when not constrained were evaluated.
[0044] [Comparative Example 1] The cell internal pressure is set to 0.030 MPa, which is higher than atmospheric pressure, and the flat area of the electrode body is set to 3632 mm 2 ], the cell spring constant was 37.0 [kN / mm], and the cell compression parameter was -0.003.
[0045] [Comparative Example 2] The cell internal pressure was set to 0.028 MPa, which is higher than atmospheric pressure, and the flat area of the electrode body was set to 3636 mm 2 ], the cell spring constant was set to 40.6 [kN / mm], and the cell compression parameter was set to -0.002.
[0046] [Comparative Example 3] The cell internal pressure is set to 0.023 MPa, which is higher than atmospheric pressure, and the flat area of the electrode body is set to 3612 mm 2 ], the cell spring constant was 28.5 [kN / mm], and the cell compression parameter was -0.003.
[0047] [Comparative Example 4] The cell internal pressure was set to 0.019 MPa, which is higher than atmospheric pressure, and the flat area of the electrode body was set to 3620 mm 2 ], the cell spring constant was set to 40.6 [kN / mm], and the cell compression parameter was set to -0.002.
[0048] [Comparative Example 5] The cell internal pressure is set to 0.013 MPa, which is higher than atmospheric pressure, and the flat area of the electrode body is set to 3608 mm 2 ], the cell spring constant was 23.6 [kN / mm], and the cell compression parameter was -0.002.
[0049] [Comparative Example 6] The cell internal pressure is set to -0.050 [MPa], which is less than atmospheric pressure, and the flat area of the electrode body is set to 4450 [mm 2 ], the cell spring constant was 25.2 [kN / mm], and the cell compression parameter was 0.009.
[0050] [Example 1] The cell internal pressure is set to -0.004 [MPa], which is less than atmospheric pressure, and the flat area of the electrode body is set to 3620 [mm 2 ], the cell spring constant was set to 24.5 [kN / mm], and the cell compression parameter was set to 0.001.
[0051] [Example 2] The cell internal pressure is set to -0.002 [MPa], which is less than atmospheric pressure, and the flat area of the electrode body is set to 3620 [mm 2 ], the cell spring constant was set to 39.3 [kN / mm], and the cell compression parameter was set to 0.000.
[0052] [Example 3] The cell internal pressure is set to -0.010 [MPa], which is less than atmospheric pressure, and the flat area of the electrode body is set to 3636 [mm 2 ], the cell spring constant was set to 40.6 [kN / mm], and the cell compression parameter was set to 0.001.
[0053] [Example 4] The cell internal pressure is set to -0.040 [MPa], which is less than atmospheric pressure, and the flat area of the electrode body is set to 4463 [mm 2 ], the cell spring constant was 25.3 [kN / mm], and the cell compression parameter was 0.007.
[0054] [evaluation] The cell thickness [mm] and deposition limiting current [%] when unconstrained were evaluated for each of the above examples and comparative examples. The cell thickness [mm] and deposition limiting current [%] when unconstrained with no bulging were 12.50 [mm].
[0055] In Comparative Examples 1 to 5, in which the internal cell pressure is higher than atmospheric pressure, the unconstrained cell thickness is greater than 12.50 [mm]. On the other hand, in Comparative Example 6 and Examples 1 to 4, in which the internal cell pressure is lower than atmospheric pressure, the unconstrained cell thickness is approximately 12.50 [mm] or less. Therefore, it is desirable that the internal cell pressure is lower than atmospheric pressure, and thus the cell compression parameter is 0.000 or more.
[0056] In Comparative Examples 1 to 5 and Examples 1 to 4, in which the cell compression parameter is 0.007 or less, the deposition limit current is 100.0[%]. In Comparative Example 6, in which the cell compression parameter is 0.009, which is greater than 0.007, the deposition limit current is 85.6[%]. Therefore, it is desirable that the cell compression parameter is 0.007 or less. In Examples 1 to 4, excellent results were obtained. [Explanation of symbols]
[0057] 10...Lithium-ion secondary battery 11…Battery case 12…Lid body 13A…Positive external terminal 13B…Negative external terminal 14A…Positive electrode side current collecting member 14B: Negative electrode side current collecting member 15…Extrapolation film 20...Electrode body 20A…Positive electrode current collector 20B: Negative electrode current collector 21...Positive electrode sheet 22...Positive electrode current collector 22A: Positive electrode uncoated area 23...Positive electrode mixture layer 24...Negative electrode sheet 25...Negative electrode current collector 25A…Negative electrode uncoated area 26…Negative electrode composite material layer 27…Separator
Claims
1. A non-aqueous secondary battery comprising: an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator interposed therebetween; a non-aqueous electrolyte; and a case that accommodates the electrode assembly and the non-aqueous electrolyte, A cell compression parameter obtained by dividing a cell compression force obtained by the product of the internal pressure difference with respect to the atmospheric pressure of the case and the area of the flat portion of the electrode body by a spring constant of the case is set to 0.000 or more and 0.007 or less. Non-aqueous secondary battery.
2. A method for producing a non-aqueous secondary battery comprising: an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator interposed therebetween; a non-aqueous electrolyte; and a case that contains the electrode assembly and the non-aqueous electrolyte, A cell compression parameter obtained by dividing a cell compression force obtained by the product of the internal pressure difference with respect to the atmospheric pressure of the case and the area of the flat portion of the electrode body by a spring constant of the case is adjusted to be 0.000 or more and 0.007 or less. A method for manufacturing a non-aqueous secondary battery.
Citation Information
Patent Citations
Manufacturing method of secondary battery
JP2021182508A
Battery pack
JP2017084550A