Solid-state battery

A two-layer negative electrode active material structure in solid state batteries, comprising a gallium-based layer on the solid electrolyte side and a magnesium-based layer on the current collector side, addresses the delamination issue, enhancing cycle characteristics and Li desorption, thereby improving battery performance.

JP2024164977AActive Publication Date: 2024-11-28TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023080746
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

Solid state batteries with metallic lithium as a negative electrode active material suffer from poor cycle characteristics due to delamination at the interface between the solid electrolyte and the negative electrode active material layer during discharge.

Method used

A solid battery design with a stacked structure of positive electrode current collector, positive electrode active material, solid electrolyte, negative electrode active material, and negative electrode current collector, where the negative electrode active material layer includes a gallium-based layer on the solid electrolyte side and a magnesium-based layer on the negative electrode current collector side, forming a two-layer structure.

Benefits of technology

The two-layer negative electrode active material layer enhances the cycle characteristics of the battery by preventing delamination and improving Li desorption, resulting in higher reversible capacity and improved cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164977000001_ABST
    Figure 2024164977000001_ABST
Patent Text Reader

Abstract

To provide a solid-state battery having high cycle characteristics.SOLUTION: In the solid-state battery of the present disclosure, a positive electrode current collector layer, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector layer are laminated in this order. The negative electrode active material layer of the solid-state battery of the present disclosure includes a gallium-based layer containing gallium or a lithium-gallium alloy, and a magnesium-based layer containing magnesium or a lithium-magnesium alloy. The gallium-based layer is arranged on the solid electrolyte layer side, and the magnesium-based layer is arranged on the negative electrode current collector layer side.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to solid-state batteries.

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. In the automobile industry, too, development of high-output, high-capacity batteries for electric vehicles or hybrid vehicles is underway.

[0003] Among batteries, lithium secondary batteries are attracting attention because they contain metallic lithium, which has the greatest ionization tendency of all metals, in the negative electrode active material layer, resulting in a large potential difference with the positive electrode active material layer and the ability to obtain a high output voltage.

[0004] In recent years, solid-state batteries using a solid electrolyte as an electrolyte have been attracting attention. Compared to batteries using an electrolyte, solid-state batteries are less susceptible to problems such as decomposition of the electrolyte caused by overcharging the battery, and have high cycle characteristics and energy density. [Background technology]

[0005] Patent Document 1 discloses a solid-state battery containing a β single-phase alloy of metallic lithium and metallic magnesium as a negative electrode active material.

[0006] Patent Document 2 discloses a secondary battery in which the negative electrode active material layer contains gallium and a resin.

[0007] Patent Document 3 discloses a lithium-aluminum alloy at the interface between a solid electrolyte and a lithium negative electrode. and an all-solid-state lithium battery comprising at least one lithium alloy layer selected from the group consisting of a lithium-gallium alloy, a lithium-indium alloy, a lithium-antimony alloy, and a lithium-bismuth alloy. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2020-184513 A [Patent Document 2] JP 2015-018799 A [Patent Document 3] Japanese Patent Application Publication No. 61-126770 Summary of the Invention [Problem to be solved by the invention]

[0009] There is still room for improvement in the cycle characteristics of solid-state batteries that contain, as a negative electrode active material, a material capable of forming an alloy with metallic lithium.

[0010] Therefore, an object of the present disclosure is to provide a solid-state battery with excellent cycle characteristics. [Means for solving the problem]

[0011] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A solid-state battery in which a positive electrode current collector layer, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector layer are laminated in this order, the negative electrode active material layer has a gallium-based layer containing gallium or a lithium gallium alloy, and a magnesium-based layer containing magnesium or a lithium magnesium alloy, The gallium-based layer is disposed on the solid electrolyte layer side, and The magnesium-based layer is disposed on the negative electrode current collector layer side. solid state battery. Effect of the Invention

[0012] According to the present disclosure, a solid-state battery having excellent cycle characteristics can be provided. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a graph showing the cycle characteristics at 25° C. of the cells of Example 1 (Ga—Mg bilayer), Comparative Example 1 (Ga), and Comparative Example 2 (Mg). [Diagram 2] FIG. 2 is a cross-sectional SEM secondary electron image of the negative electrode active material layer of Example 1 after the initial charge / discharge at 60° C. [Diagram 3] FIG. 3 shows images showing the results of EDX mapping analysis by SEM-EDX for the negative electrode active material layer of Example 1 after the initial charge / discharge at 60° C., for each element (FIG. 3( a): Mg, FIG. 3( b): Ga, FIG. 3( c): O, FIG. 3( d): S). [Figure 4] FIG. 4 is a graph showing the cycle characteristics at 0.60 mA / cm2 at 25° C. after the initial charge and discharge of the cells of Example 1 (Ga-Mg bilayer), Comparative Example 1 (Ga), and Comparative Example 2 (Mg). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0015] 《Solid-state battery》 The solid-state battery of the present disclosure includes a positive electrode current collector layer, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector layer stacked in this order. The negative electrode active material layer of the solid-state battery of the present disclosure includes a gallium-based layer containing gallium or a lithium gallium alloy, and a magnesium-based layer containing magnesium or a lithium magnesium alloy, the gallium-based layer being disposed on the solid electrolyte layer side, and the magnesium-based layer being disposed on the negative electrode current collector layer side.

[0016] As a method for improving the energy density of a solid-state battery, there is a method of using metallic lithium (Li) as the negative electrode active material to make the battery anode-free. However, the present inventors have found that the cycle characteristics of an anode-free solid-state battery may deteriorate. Although it is not intended to be bound by any theory, it is presumed that the cause of this is that the loss of Li in the negative electrode active material layer during discharge causes peeling at the interface between the solid electrolyte layer and the negative electrode active material layer.

[0017] As shown in Patent Document 1, anode-free solid-state batteries containing a β single-phase alloy of metallic Li and metallic magnesium (Mg) as the negative electrode active material are known. The present inventors have found that by disposing a Ga-based layer containing metallic gallium (Ga) or a lithium gallium (Li-Ga) alloy between a solid electrolyte layer and an Mg-based layer in addition to the Mg-based layer containing metallic Mg or a lithium magnesium (Li-Mg) alloy, and forming a two-layer negative electrode active material layer, the cycle characteristics of a battery containing such a negative electrode active material layer are improved. Although not intending to be bound by any theory, the reason for this is presumed to be that even at the end of the discharge of the battery, the Ga-based layer is held between the solid electrolyte layer and the Mg-based layer, thereby suppressing peeling at the interface between the negative electrode active material layer and the solid electrolyte layer.

[0018] The solid-state battery of the present disclosure has a positive electrode current collector layer, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector layer laminated in this order.

[0019] <Positive electrode current collector layer> The positive electrode current collector may be a known metal that can be used as a current collector for solid-state batteries, such as a metal material containing one or more elements selected from the group consisting of Cu, Ni, Al, V, Au, Pt, Mg, Fe, Ti, Co, Cr, Zn, Ge, and In.

[0020] The shape of the positive electrode current collector is not particularly limited, and it may be in various shapes such as a foil shape, a mesh shape, or the like.

[0021] <Cathode active material layer> The positive electrode active material layer contains a positive electrode active material, and may optionally contain a solid electrolyte, a conductive material, a binder, and the like.

[0022] (Cathode active material) There is no particular limitation on the type of the positive electrode active material, and any material that can be used as an active material for a solid-state battery can be used. The positive electrode active material may contain lithium element or may not contain lithium element.

[0023] Examples of the positive electrode active material containing lithium include metallic lithium (Li), lithium alloys, and LiCoO 2 , LiNi x Co 1-x O 2 (0 <x<1)、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , LiMnO 2 , hetero-element substituted Li-Mn spinels (e.g. LiMn 1.5 Ni 0.5 O 4 , LiMn 1.5 Al 0.5 O 4 , LiMn 1.5 Mg 0.5 O 4 , LiMn 1.5 Co 0.5 O 4 , LiMn 1.5 Fe 0.5 O 4 , and LiMn 1.5 Zinc 0.5 O 4 etc.), lithium titanate (e.g. Li 4 Ti 5 O 12 ), lithium metal phosphate (e.g. LiFePO 4 , LiMnPO 4 , LiCoPO 4 , and LiNiPO 4 etc.), LiCoN, Li 2 SiO 3 , and Li 4SiO 4 etc. can be mentioned.

[0024] Lithium alloys include Li-Au, Li-Mg, Li-Sn, Li-Si, Li-Al, Li-Ge, Li-Sb, Li-B, Li-C, Li-Ca, Li-Ga, Li-As, Li-Se, Li-Ru, Examples include Li-Rh, Li-Pd, Li-Ag, Li-Cd, Li-Ir, Li-Pt, Li-Hg, Li-Pb, Li-Bi, Li-Zn, Li-Tl, Li-Te, Li-At, and Li-In.

[0025] Examples of the positive electrode active material that does not contain lithium include transition metal oxides (e.g., V 2 O 5 , and MoO 3 etc.), sulfur, TiS 2 , Si, SiO 2 , and lithium storage intermetallic compounds (e.g. Mg 2 Sn, Mg 2 Ge, Mg 2 Sb and Cu 3 Sb, etc.

[0026] The shape of the positive electrode active material is not particularly limited, but may be in the form of particles.

[0027] A coating layer containing a Li-ion conductive oxide may be formed on the surface of the positive electrode active material, because this can suppress the reaction between the positive electrode active material and the solid electrolyte.

[0028] Examples of Li-ion conductive oxides include LiNbO 3 , Li 4 Ti 5 O 12 , and Li 3 PO 4 The thickness of the coating layer is, for example, 0.1 nm or more, and may be 1 nm or more. Meanwhile, the thickness of the coating layer is, for example, 100 nm or less, and may be 20 nm or less. The coverage of the coating layer on the surface of the positive electrode active material is, for example, 70% or more, and may be 90% or more.

[0029] (Solid electrolyte) Examples of the solid electrolyte include sulfide solid electrolytes and oxide-based solid electrolytes.

[0030] Examples of the sulfide solid electrolyte include, for example, Li 2 S-P 2 S 5 , Li 2 S-SiS 2 , LiX-Li 2 S-SiS 2 , LiX-Li 2 S-P 2 S 5 , LiX-Li 2 O-Li 2 S-P 2 S 5 , LiX-Li 2 S-P 2 O 5 , LiX-Li 3 PO 4 -P 2 S 5 , and Li 3 PS 4 and the like. The description of "Li 2 S-P 2 S 5 " means a material formed using a raw material composition containing Li 2 S and P 2 S 5 , and the same applies to other descriptions. In addition, "X" in the above LiX represents a halogen element. The raw material composition containing the above LiX may contain one or more kinds of LiX. When two or more kinds of LiX are contained, the mixing ratio of the two or more kinds is not particularly limited.

[0031] Examples of the oxide-based solid electrolyte include, for example, Li 6.25 La 3 Zr 2 A l0.25 O 12 , Li 3 PO 4 , and Li 3+x PO 4-x N x (0 < x ≤ 3) and the like.

[0032] The proportion of the solid electrolyte in the positive electrode active material layer is not particularly limited, but may be, for example, 1% by mass to 80% by mass when the total mass of the positive electrode active material layer is taken as 100% by mass.

[0033] (Conductive material) The conductive material may be a known one, for example, a carbon material, metal particles, etc. The carbon material may be at least one selected from the group consisting of carbon black such as acetylene black and furnace black, carbon nanotubes, and carbon nanofibers, and among them, from the viewpoint of electronic conductivity, at least one selected from the group consisting of carbon nanotubes and carbon nanofibers is preferable. The carbon nanotubes and carbon nanofibers may be VGCF (vapor grown carbon fiber). The metal particles may be particles of Ni, Cu, Fe, SUS, etc.

[0034] The content of the conductive material in the positive electrode active material layer is not particularly limited.

[0035] (binder) Examples of the binder include acrylonitrile butadiene rubber (ABR), butadiene rubber (BR), polyvinylidene fluoride (PVdF), and styrene butadiene rubber (SBR).

[0036] The content of the binder in the positive electrode active material layer is not particularly limited.

[0037] The thickness of the positive electrode active material layer is not particularly limited.

[0038] <Solid electrolyte layer> The solid electrolyte layer includes a solid electrolyte and, optionally, a binder.

[0039] (solid electrolyte) For the solid electrolyte, reference can be made to the above description regarding the positive electrode active material layer of the present disclosure.

[0040] The solid electrolyte may be used alone or in combination of two or more kinds. When two or more kinds of solid electrolytes are used, the two or more kinds of solid electrolytes may be mixed, or two or more layers of the solid electrolyte may be formed to form a multilayer structure.

[0041] The proportion of the solid electrolyte in the solid electrolyte layer is not particularly limited, but may be, for example, 50% by mass or more, 60% by mass or more and 100% by mass or less, or 70% by mass or more and 100% by mass or less, or may be 100% by mass.

[0042] (binder) The solid electrolyte layer may contain a binder from the viewpoint of expressing plasticity, etc. For the binder, the above description regarding the positive electrode active material layer of the present disclosure may be referred to. However, in order to facilitate high output, the binder may be contained in the solid electrolyte layer in an amount of 5 mass% or less from the viewpoint of preventing excessive aggregation of the solid electrolyte and enabling the formation of a solid electrolyte layer having a uniformly dispersed solid electrolyte.

[0043] The thickness of the solid electrolyte layer is not particularly limited, and is usually 0.1 μm or more and 1 mm or less.

[0044] <Negative electrode active material layer> The negative electrode active material layer includes a Ga-based layer and an Mg-based layer.

[0045] (Gallium-based layer) The Ga-based layer contains metallic Ga or a Li—Ga alloy as a negative electrode active material.

[0046] The Ga metal may be Ga metal itself or a material obtained by vapor deposition of Ga metal.

[0047] The Li-Ga alloy may be an alloy produced by charging a solid-state battery including the negative electrode active material layer of the present disclosure, or may be an alloy prepared separately.

[0048] The method of producing a Li-Ga alloy by charging a solid-state battery includes the following methods. First, a battery precursor having a positive electrode active material layer containing at least one positive electrode active material selected from the group consisting of metal Li, Li alloys, and Li compounds, a solid electrolyte layer, a metal Ga layer, and a negative electrode current collector layer in this order is prepared. By charging this battery precursor, Li ions transferred from the positive electrode active material layer to the metal Ga layer react with metal Ga of the metal Ga layer to obtain a Li-Ga alloy. In addition, from the viewpoint of alloying all of the metal Ga of the metal Ga layer with metal Li, the precursor battery may be charged and discharged multiple times. The number of times of charging and discharging is not particularly limited and can be appropriately set according to the thickness of the metal Ga layer.

[0049] The Ga-based layer is disposed on the solid electrolyte layer side. By disposing the Ga-based layer between the solid electrolyte layer and the Mg-based layer described later to form a two-layer negative electrode active material layer, the cycle characteristics of a battery including such a negative electrode active material layer are improved.

[0050] The Ga-based layer may contain other conventionally known negative electrode active materials as long as it contains metallic Ga or a Li-Ga alloy as the main component of the negative electrode active material. In the present disclosure, the main component means a component contained in an amount of 50% by mass or more when the total mass of the Ga-based layer is taken as 100% by mass.

[0051] (Magnesium-based layer) The Mg-based layer includes metallic Mg or a Li-Mg alloy.

[0052] The Mg metal may be the Mg metal itself or a material obtained by vapor deposition of the Mg metal.

[0053] The Li-Mg alloy may be an alloy produced by charging a solid-state battery including the negative electrode active material layer of the present disclosure, or may be an alloy prepared separately.

[0054] For the method of producing a Li-Mg alloy by charging a solid-state battery, reference may be made to the above description of the method of producing a Li-Ga alloy in the present disclosure.

[0055] The Mg-based layer is disposed on the negative electrode current collector layer side.

[0056] The Mg-based layer may contain other conventionally known negative electrode active materials as long as it contains metallic Mg or a Li-Mg alloy as the main negative electrode active material. In the present disclosure, the main component means a component contained in an amount of 50% by mass or more when the total mass of the Mg-based layer is taken as 100% by mass.

[0057] (Solid electrolyte, conductive material, and binder) The negative electrode active material layer may contain a solid electrolyte, a conductive material, a binder, etc. For the solid electrolyte, the conductive material, and the binder, the above description regarding the positive electrode active material layer of the present disclosure can be referred to.

[0058] The thickness of the negative electrode active material layer is not particularly limited, but may be 30 nm or more and 50 μm or less.

[0059] <Negative electrode current collector layer> The negative electrode current collector may be made of a material that does not alloy with Li, such as SUS, copper, and nickel.

[0060] The negative electrode current collector may be in the form of, for example, a foil or a plate.

[0061] The shape of the negative electrode current collector in a plan view is not particularly limited, but examples thereof include a circle, an ellipse, a rectangle, and any polygonal shape.

[0062] The thickness of the negative electrode current collector varies depending on the shape, but may be, for example, 1 μm to 50 μm, or 5 μm to 20 μm. EXAMPLES

[0063] Creating a cell <Preparation of Positive Electrode Active Material Layer> A positive electrode composite slurry was prepared using butyl butyrate as a solvent with a weight composition ratio of lithium nickel oxide (NCA): solid electrolyte: binder: conductive additive = 84.7: 13.4: 0.6: 1.27, and coated on an aluminum (Al) foil with a coating gap of 225 μm, then pre-dried at 60 ° C and finally dried at 165 ° C for 1 hour. Thus, the basis weight was 18.7 mg / cm 2 , design capacity 3.0mAh / cm 2 Thus, a positive electrode active material layer of the above structure was obtained.

[0064] (Preparation of solid electrolyte layer) A solid electrolyte slurry was prepared using butyl butyrate as a solvent with a weight composition ratio of solid electrolyte:binder = 92.6:7.4, and coated onto a release film with a coating gap of 325 μm. It was then pre-dried at room temperature for about 3 hours and then fully dried at 165°C for 1 hour. Two pieces with a diameter of φ14.5 mm were punched out from the dried coated foil, and the coated surfaces were overlapped and pressed at 7 tons. After pressing, the release film was peeled off to obtain a free-standing sulfide solid electrolyte layer.

[0065] <Preparation of negative electrode active material layer> As negative electrode active material layers, gallium (Ga) evaporated foil (thickness: 0.84 μm), magnesium (Mg) evaporated foil (thickness: 1.0 μm), and Ga-Mg double-layer evaporated foil (Ga evaporated foil thickness: 1.0 μm, Mg evaporated foil thickness: 1.0 μm) were prepared.

[0066] Cell assembly Comparative Example 1 The prepared positive electrode active material layer was punched out to φ11.28 mm. Also, Ga vapor deposition foil as the negative electrode active material layer was punched out to φ14.5 mm. The prepared self-supporting solid electrolyte layer of φ14.5 mm was placed between the positive electrode active material layer and the negative electrode active material layer, and was vacuum sealed in a laminate film using Al foil as the positive electrode current collector and Ni as the negative electrode current collector. The sealed cell was isostatically pressed at 392 MPa using cold isostatic pressing (CIP) to prepare a laminate cell. The prepared cell was restrained at 1 MPa using a constant pressure jig with a spring inserted so that the restraining pressure was constant regardless of the volume change of the cell. This resulted in the cell of Comparative Example 1 being obtained.

[0067] Comparative Example 2 A cell of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the negative electrode active material layer was a Mg evaporated foil.

[0068] Example 1 A cell of Example 1 was obtained in the same manner as in Comparative Example 1, except that the negative electrode active material layer was a Ga-Mg bilayer evaporated foil. The Ga evaporated foil was placed on the solid electrolyte layer side, and the Mg evaporated foil was placed on the negative electrode current collector layer side.

[0069] "evaluation" <Measurement of charge / discharge curve> The cutoff voltage is in the range of 4.2V-3.0V, and the constant current (current density: 0.15mA / cm 2 , equivalent to 0.05C) - constant voltage (cutoff current density: 0.03mA / cm 2 In the test, the initial charge and discharge of the restrained cell was performed at 60°C, and the charge and discharge curve was obtained.

[0070] <SEM-EDX measurement> The cross section of the Ga-Mg bilayer evaporated foil after the initial charging at 60°C was subjected to SEM observation and EDX mapping using secondary electron images at an applied voltage of 5 kV.

[0071] Measurement of cycle characteristics After the initial charge and discharge at 60°C, the battery was charged at a constant current (current density: 0.60mA / cm2) at 25°C with the cutoff voltage in the range of 4.2V-3.0V. 2 , equivalent to 0.05C) - constant voltage (only when charging, cut-off current density: 0.03mA / cm 2 The cycle characteristics were measured in a test at 25° C. (equivalent to 0.01 C). However, since Ga has a low melting point (melting point: 29.7° C.), the initial charge / discharge was also performed at 25° C. for the cycle characteristic test of the cell of Comparative Example 1 in which the negative electrode active material layer was a Ga evaporated foil.

[0072] "result" <Charge / discharge curve measurement results> The current density in each example cell was 0.15 mA / cm 2The initial charge / discharge curve at 60°C (~C / 20) is shown in Figure 1.

[0073] As shown in FIG. 1, the charge capacity and discharge capacity were 213-215mAh / g and 179-189mAh / g, respectively, based on the positive electrode active material. The cell of Comparative Example 1, which used Ga vapor-deposited foil as the negative electrode active material layer, had a lower cell voltage than Mg vapor-deposited foil in the region of 3.2V-3.5V in the early stage of charging and in the region of 3.6V-3.0V in the late stage of discharging. This suggests that in the cell of Comparative Example 1, Li insertion and alloying into Ga occurs in the early stage of charging, and Li desorption from Ga occurs in the late stage of charging, before the deposition of metallic lithium (Li) occurs at the negative electrode potential of 0V vs. Li.

[0074] In contrast, the cell of Example 1 using Ga-Mg bilayer evaporated foil as the negative electrode active material layer showed additional reversible capacity in the discharge curve at 3.5 V or less compared to the cell of Comparative Example 2 using Mg evaporated foil as the negative electrode active material layer, and the reversible capacity derived from the constant voltage step at the lower cutoff voltage of 3.0 V was reduced. This suggests that the presence of the Ga layer in the Ga-Mg bilayer evaporated foil does not cause a drop in cell voltage in the early stage of charging, and enables more Li desorption in the constant current step in the final stage of discharge.

[0075] <SEM-EDX measurement results> 2 and 3 show a cross-sectional SEM secondary electron image and the results of EDX mapping analysis of the cell of Example 1 using a Ga-Mg double-layer evaporated foil as the negative electrode active material layer after the initial charge / discharge at 60° C.

[0076] As shown in Figures 2 and 3, a distribution rich in Mg, Ga, and S was confirmed from the bottom negative electrode current collector layer. This indicates that a Ga-based layer exists between the Mg-based layer and the solid electrolyte layer even after Li insertion and desorption during the initial charge and discharge. It is believed that this Ga-based layer serves as a Li desorption reaction site at the end of discharge, contributing to the maintenance of the negative electrode active material layer-solid electrolyte interface and the increase in reversible capacity during the constant current step.

[0077] <Measurement results of cycle characteristics> 0.60mA / cm after the first charge / discharge for each example cell 2 The results of the 25°C cycle characteristics at (~C / 5) are shown in Figure 4. The reversible capacity after 50 cycles is shown in Table 1.

[0078] [Table 1]

[0079] As shown in FIG. 4 and Table 1, the cell of Example 1, which used a Ga-Mg bilayer evaporated foil as the negative electrode active material layer, had a larger reversible capacity than the cells of the comparative examples. Even compared to Comparative Example 2, which had the largest reversible capacity among the comparative examples, the reversible capacity after both the first cycle and the 50th cycle was about twice that of Comparative Example 2.

[0080] 4 and Table 1, the cell of Comparative Example 2 using Mg-deposited foil had a larger reversible capacity than the cell of Comparative Example 1 using Ga-deposited foil as the negative electrode active material layer. From this, it is considered that the reversible capacity was improved in the cell including the negative electrode active material layer of the present disclosure because the Mg-deposited foil was provided on the negative electrode current collector layer side and the Ga-deposited foil, which is the second negative electrode active material layer, was provided between the Mg-deposited foil and the solid electrolyte layer.

Claims

[Claim 1] A solid-state battery in which a positive electrode current collector layer, a positive electrode active material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector layer are laminated in this order, the negative electrode active material layer has a gallium-based layer containing gallium or a lithium gallium alloy, and a magnesium-based layer containing magnesium or a lithium magnesium alloy, The gallium-based layer is disposed on the solid electrolyte layer side, and The magnesium-based layer is disposed on the negative electrode current collector layer side. solid state battery.

Citation Information

Patent Citations

  • All-solid battery

    JP2021051866A

  • All-solid type secondary battery, and manufacturing method thereof

    JP2021068706A

  • All-solid-state secondary battery and method for producing same

    JP2023517913A

  • All solid type lithium cell

    JP1986126770A

  • Secondary battery, and method for manufacturing the same

    JP2015018799A