Negative electrode active material composite particle, negative electrode mixture, lithium ion battery, and production method of negative electrode active material composite particle

Surface-modified silicon particles with an alkyl group and reduced binder resin in composite particles address the issue of aggregation, enhancing cycle characteristics and battery performance by maintaining contact and reducing resistance.

JP2024165002AActive Publication Date: 2024-11-28TOYOTA JIDOSHA KK
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023080801
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

Existing composite particles containing silicon particles and a binder resin exhibit poor cycle characteristics due to silicon particle aggregation, which reduces contact with the binder resin and leads to cracking and deterioration in performance.

Method used

Surface-modified negative electrode active material particles are produced by modifying silicon particles with an organic group, particularly an alkyl group, and using a reduced amount of binder resin, improving dispersibility and reducing resistance through appropriate void formation.

Benefits of technology

The modified particles enhance cycle characteristics by suppressing silicon particle aggregation and maintaining contact with the binder resin, resulting in improved battery performance even with a minimal amount of binder resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165002000001
    Figure 2024165002000001
  • Figure 2024165002000002
    Figure 2024165002000002
Patent Text Reader

Abstract

To provide: negative electrode active material composite particles including silicon particles and a binder resin and having high cycle properties; a negative electrode mixture including such negative electrode active material composite particles; a lithium ion battery including such negative electrode active material composite particles; a production method for such negative electrode active material composite particles; and a production method for such composite particles.SOLUTION: Negative electrode active material composite particles of the present disclosure include surface-modified negative electrode active material particles and a binder resin. In addition, the surface-modified negative electrode active material particles included in the negative electrode active material composite particles of the present disclosure have a silicon particle and an organic group that modifies the surface of the silicon particle. Furthermore, the ratio of the mass of the binder resin included in the negative electrode active material composite particles of the present disclosure to the total mass of the surface-modified negative electrode active material particles and the binder resin is 15 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a negative electrode active material composite particle, a negative electrode mixture, a lithium ion battery, and a method for producing a negative electrode active material composite particle. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as a negative electrode active material for batteries.

[0003] Patent Document 1 discloses an anode active material for an all-solid-state battery, which is composed of anode active material particles that are a composite of silicon and carbon and a binder, and is in the form of granulated particles having a median diameter (D50) of 25 μm or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-021571 A Summary of the Invention [Problem to be solved by the invention]

[0005] In composite particles containing silicon particles and a binder resin, it is desired to improve the cycle characteristics.

[0006] An object of the present disclosure is to provide a negative electrode active material composite particle that contains silicon particles and a binder resin and has high cycle characteristics, a negative electrode mixture that contains such a negative electrode active material composite particle, a lithium ion battery that contains such a negative electrode active material composite particle, and a method for producing such a negative electrode active material composite particle. [Means for solving the problem]

[0007] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> The negative electrode active material includes surface-modified negative electrode active material particles and a binder resin, the surface-modified negative electrode active material particles have silicon particles and organic groups modifying the surfaces of the silicon particles; and a ratio of the mass of the binder resin to the total mass of the surface-modified negative electrode active material particles and the binder resin is 15 mass% or less; Negative electrode active material composite particles. <Aspect 2> The negative electrode active material composite particle according to aspect 1, wherein the organic group is an alkyl group. <Aspect 3> The negative electrode active material composite particle according to aspect 2, wherein the alkyl group has 5 or more and 20 or less carbon atoms. <Aspect 4> A negative electrode active material composite particle according to aspect 2, wherein the surface-modified negative electrode active material particle has a silicon-carbon bond, the silicon being the silicon of the silicon particle, and the carbon being the carbon of an alkyl group. <Aspect 5> A negative electrode mixture comprising the negative electrode active material composite particle according to any one of the first to fourth aspects. Aspect 6 A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to aspect 5. Lithium-ion battery. Aspect 7 (a) modifying the surfaces of silicon particles with organic groups to obtain surface-modified negative electrode active material particles; (b) forming droplets from a slurry containing the surface-modified negative electrode active material particles, a binder resin, and a solvent to obtain slurry droplets; and (c) flash drying the slurry droplets in a heated gas; The method for producing negative electrode active material composite particles comprising the steps of: <Aspect 8> 8. The method of claim 7, wherein in step (a), the surface of the silicon particles is modified with the organic groups by a hydrosilylation reaction in which the organic groups are added to hydrosilyl groups on the surface of the silicon particles. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a negative electrode active material composite particle that contains silicon particles and a binder resin and has high cycle characteristics, a negative electrode mixture that contains such a negative electrode active material composite particle, a lithium ion battery that contains such a negative electrode active material composite particle, and a method for producing such a negative electrode active material composite particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0010] 《Negative electrode active material composite particles》 The negative electrode active material composite particle of the present disclosure includes surface-modified negative electrode active material particles and a binder resin. The surface-modified negative electrode active material particles included in the negative electrode active material composite particle of the present disclosure have silicon particles and organic groups that modify the surfaces of the silicon particles. The ratio of the mass of the binder resin included in the negative electrode active material composite particle of the present disclosure to the total mass of the surface-modified negative electrode active material particles and the binder resin is 15 mass% or less.

[0011] The present inventors have considered that one of the causes of poor cycle characteristics in composite particles containing silicon particles and binder resin is that the silicon particles tend to aggregate within the composite particles. Specifically, without intending to be bound by any theory, it is believed that when the silicon particles aggregate within the composite particles, the silicon particles cannot make sufficient contact with the binder resin, causing cracks or the like in the composite particles, resulting in poor cycle characteristics.

[0012] In response to this, the present inventors have discovered that in composite particles containing silicon particles and a binder resin, the cycle characteristics of the composite particles can be improved by modifying the surfaces of the silicon particles with organic groups, particularly alkyl groups, and by reducing the amount of binder resin.

[0013] The reason for this is presumed to be as follows, without intending to be bound by any theory. That is, by modifying the surface of the silicon particles with an organic group, particularly an alkyl group, the dispersibility of the silicon particles in the composite particles is improved, and even if the amount of binder resin in the composite particles is reduced to a certain level or less, it is believed that the binder resin can be appropriately arranged even inside the composite particles. In this way, it is believed that by keeping the ratio of binder resin in the composite particles to a certain level or less, the resistance of the composite particles as a whole is reduced, thereby improving the cycle characteristics.

[0014] In addition, since the silicon particles and the binder resin are in sufficient contact with each other, aggregation of the silicon particles in the composite particles is suppressed, and appropriate gaps are formed between the silicon particles, the gaps can mitigate the volume change that occurs when the silicon particles expand during charging and discharging, thereby suppressing cracking of the composite particles and improving the cycle characteristics.

[0015] In the present disclosure, whether the negative electrode active material composite particles are properly prepared can be confirmed by the degree of particle size variation. That is, the value of (D90-D10) / D50 can be used as an index of particle size variation, and if this value is less than 4.0, 3.5 or less, 3.0 or less, 2.5 or less, or 2.0 or less, it can be determined that the negative electrode active material composite particles are properly prepared.

[0016] <Surface modified negative electrode active material particles> The negative electrode active material composite particles of the present disclosure contain surface-modified negative electrode active material particles and a binder resin.

[0017] (silicon particles) The surface-modified negative electrode active material particles include silicon particles.

[0018] The composition of the silicon particles is not particularly limited. The proportion of silicon element in all elements contained in the silicon particles may be, for example, 50 mol % or more, 70 mol % or more, or 90 mol % or more.

[0019] The silicon particles may contain other elements such as Li in addition to the Si element. Examples of the other elements include Sn, Fe, Co, Ni, Ti, Cr, B, and P in addition to the Li element.

[0020] The silicon particles may contain impurities such as oxides.

[0021] The silicon particles may be amorphous or crystalline, and the crystal phase contained in the silicon particles is not particularly limited.

[0022] The shape and size of the silicon particles are not particularly limited. The average particle size of the silicon particles may be, for example, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average particle size can be determined by observation with an electron microscope such as an SEM, and is determined, for example, as the average value of the maximum Feret diameters of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. The average particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the silicon particles described later or by performing a classification process.

[0023] The silicon particles contained in the surface-modified negative electrode active material particles may be porous silicon particles. The porous silicon particles contain silicon having a plurality of voids. There is no particular limitation on the shape of the voids in the porous silicon particles.

[0024] The porous silicon particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with pore diameters on the nanometer order (less than 1000 nm, preferably 100 nm or less).

[0025] (organic group) The surface-modified negative electrode active material particles of the present disclosure have organic groups that modify the surfaces of the silicon particles.

[0026] The organic group may be a group consisting of one or more carbon atoms and one or more atoms selected from the group consisting of H, O, S, N, B, P, Si, and halogen atoms, and is preferably an alkyl group.

[0027] The number of carbon atoms of the alkyl group may be 5 or more and 20 or less. The number of carbon atoms may be 6 or more, 19 or less, or 18 or less. The alkyl group may have a linear, branched, or cyclic structure, but is preferably a linear alkyl group. Specific examples of such alkyl groups include pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, and eicosyl groups.

[0028] The modification of the surface of silicon particles with alkyl groups can be confirmed by measuring the amount of carbon and hydrogen on the surface of the silicon particles after the treatment of modifying the surface with alkyl groups, and by analyzing the surface functional group state of the particles, etc. An example of a method for measuring the amount of carbon on the surface is high-frequency combustion infrared absorption method, an example of a method for measuring the amount of hydrogen on the surface is inert gas induction infrared absorption method, and an example of a method for analyzing the surface functional group state is time-of-flight secondary ion mass spectrometry (TOF-SIMS), but these are not limited thereto.

[0029] The surface-modified negative electrode active material particles may have a silicon-carbon bond, in which the silicon is that of a silicon particle and the carbon is that of an alkyl group, i.e., the carbon of the alkyl group may be directly bonded to the silicon on the surface of the silicon particle.

[0030] <Binder resin> The negative electrode active material composite particle of the present disclosure includes a binder resin. The binder binds a plurality of silicon particles together. The type of binder is not particularly limited. For example, the binder may be selected from butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, carboxymethyl cellulose (CMC)-based binders, polyacrylate-based binders, polyacrylic acid ester-based binders, and the like. Only one type of binder may be used alone, or two or more types may be used in combination.

[0031] The ratio of the mass of the binder resin contained in the negative electrode active material composite particle of the present disclosure to the total mass of the surface-modified negative electrode active material particle and the binder resin is 15% by mass or less. This ratio may be 14% by mass or less, 13% by mass or less, 12% by mass or less, 11% by mass or less, or 10% by mass or less. Even if the amount of the binder resin in the negative electrode active material composite particle of the present disclosure is small, the cycle characteristics of the obtained battery are high.

[0032] <<Method for producing negative electrode active material composite particles>> The method of the present disclosure for producing negative electrode active material composite particles includes: (a) modifying the surfaces of silicon particles with organic groups to obtain surface-modified negative electrode active material particles; (b) forming droplets from a slurry containing the surface-modified negative electrode active material particles, a binder resin, and a solvent to obtain slurry droplets; and (c) flash-drying the slurry droplets in a heated gas.

[0033] According to this method, even when drying is performed by spray drying in step (c), for example, the dispersibility of the silicon particles in the composite particles is improved, and the binder resin is present in the center of the composite particles, allowing the silicon particles to be appropriately bonded together, thereby producing the composite particles of the present disclosure.

[0034] In step (a), the surface of the silicon particles may be modified with an organic group by a hydrosilylation reaction in which an organic group is added to the hydrosilyl group on the surface of the silicon particles. For example, when the organic group is an alkyl group, the method of carrying out this hydrosilylation reaction includes a method of mixing and reacting hydrogen fluoride-treated silicon particles, an alkene, and optionally a catalyst in a solvent.

[0035] One method for obtaining hydrogen fluoride-treated silicon particles is to add a hydrogen fluoride solution to silicon particles dispersed in a dispersion medium, stir the mixture, separate the resulting suspension into solid and liquid, and then dry it. This removes silicon oxide from the surfaces of the silicon particles, and simultaneously generates hydrosilyl groups (-SiH) on the surfaces of the silicon particles.

[0036] This hydrosilyl group can undergo a hydrosilylation reaction with the double bond of the alkene.

[0037] For alkenes, see the above description of the alkyl groups of the present disclosure and alkenes of the corresponding carbon numbers can be used.

[0038] 《Negative electrode mixture》 The negative electrode mixture of the present disclosure includes the negative electrode active material composite particles of the present disclosure. The negative electrode mixture of the present disclosure also optionally includes an electrolyte, a conductive additive, and a binder.

[0039] In the present disclosure, the term "negative electrode mixture" refers to a composition that can constitute a negative electrode active material layer as it is or by further containing other components. In the present disclosure, the term "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can be applied and dried to form a negative electrode active material layer.

[0040] <Negative electrode active material> The negative electrode active material includes the negative electrode active material composite particles of the present disclosure.

[0041] <Electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0042] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0043] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0044] In addition, when the negative electrode mixture contains a solid electrolyte, the mass ratio of the negative electrode active material composite particles to the solid electrolyte in the negative electrode mixture (mass of the negative electrode active material composite particles:mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0045] The electrolyte preferably contains a supporting salt and a solvent.

[0046] Examples of supporting salts (lithium salts) for electrolytes having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3.

[0047] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0048] <Conductive assistant> The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0049] <binder> The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0050] Lithium-ion battery The lithium ion battery of the present disclosure has a negative electrode active material layer. The negative electrode active material layer contains the negative electrode mixture of the present disclosure. The lithium ion battery of the present disclosure may have, in this order, a negative electrode current collector layer, a negative electrode active material layer containing the negative electrode mixture of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

[0051] The lithium ion battery of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0052] The lithium ion battery may be a primary battery or a secondary battery.

[0053] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type.

[0054] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0055] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0056] <Negative electrode active material layer> The negative electrode active material layer contains the negative electrode mixture of the present disclosure. For the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referenced.

[0057] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0058] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode mixture of the present disclosure can be referred to.

[0059] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0060] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.

[0061] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y Li-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.

[0062] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O12 , Li3PO4, etc., but are not limited to these.

[0063] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0064] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode mixture of the present disclosure.

[0065] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0066] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0067] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0068] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred. EXAMPLES

[0069] <<Preparation of surface-modified negative electrode active material particles>> <Adjustment of silicon particles> (Comparative Synthesis Example 1) Silicon particles were prepared as a silicon (Si) source. The silicon particles and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed silicon particles and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere to obtain porous silicon particles.

[0070] 10 g of porous silicon particles were dispersed in 100 mL of ethanol. Then, 3.7 mL of 46 wt% aqueous hydrogen fluoride (HF) solution was added dropwise and stirred at room temperature for 3 hours. After stirring, the solution was suction filtered, washed with 50 mL of ethanol, and filtered, and this operation was repeated 8 times. The obtained solid was vacuum dried at 100°C for 12 hours to obtain HF-treated porous silicon particles.

[0071] Modification with alkyl groups (Synthesis Example 1) In an argon (Ar)-substituted glove box, 2 g of the HF-treated porous silicon particles, 30 g of mesitylene (Nacalai Tesque), 0.18 g of 1-hexene (Fujifilm Wako Pure Chemical Industries, Ltd.), and 10 μL of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex xylene solution (Sigma-Aldrich Co., Ltd.) were weighed and placed in a sealed reaction vessel, and the mixture was stirred at 50° C. for 24 hours to react (hydrosilylation reaction). The solution after stirring was suction filtered, washed with 30 mL of mesitylene, and filtered three times, and then washed once with 30 mL of ethanol and filtered. The solid obtained was vacuum-dried at 100° C. for 12 hours to convert some of the Si-H bonds on the silicon particle surface to Si-CH 13 That is, the surface of the silicon particles was covered with hexyl groups (-CH 13 ) to prepare surface-modified negative electrode active material particles.

[0072] (Synthesis Example 2) The same procedure as in Synthesis Example 1 was repeated except that the alkene was changed to 0.30 g of 1-decene (Fujifilm Wako Pure Chemical Industries, Ltd.), and some of the Si-H bonds on the silicon particle surface were converted to Si-C 10 H 21 In other words, the surface of the silicon particles was treated with decyl groups (-C 10 H 21 ) to prepare surface-modified negative electrode active material particles.

[0073] (Synthesis Example 3) Surface-modified negative electrode active material particles. The procedure was the same as in Synthesis Example 1, except that the alkene was changed to 0.55 g of 1-octadecene (Fujifilm Wako Pure Chemical Industries, Ltd.). Some of the Si-H bonds on the silicon particle surface were converted to Si-C. 18 H 37 In other words, the surface of the silicon particles was treated with octadecyl groups (-C 18 H 37 ) to prepare surface-modified negative electrode active material particles.

[0074] <<Preparation of negative electrode active material composite particles>> (PVdF-HFP is used as the binder resin) (Comparative Examples 1 to 3 and Examples 1 to 9) Polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) (KF8300 manufactured by Kureha Corporation) was dissolved in dimethyl carbonate to a concentration of 1 wt%. Either the silicon particles of Comparative Synthesis Example 1 or the surface-modified negative electrode active material particles of Synthesis Examples 1 to 3 were stirred in this solution so that the weight ratio of silicon particles:PVdF-HFP was 94:6, 92:8, or 90:10, respectively, and the mixture was dispersed using a homogenizer. The solution was then spray-dried using a spray dryer (ADL311S-A manufactured by Yamato Scientific Co., Ltd.) to obtain the negative electrode active material composite particles of Comparative Examples 1 to 3 and Examples 1 to 9.

[0075] (SBR is used as the binder resin) (Comparative Example 4 and Example 10) Styrene butadiene (SBR) was dissolved in butyl butyrate to a concentration of 1 wt %. Either the silicon particles of Comparative Synthesis Example 1 or the surface-modified negative electrode active material particles of Synthesis Example 3 was stirred into this solution to a weight ratio of silicon particles:SBR=92:8, and then dispersed with a homogenizer. The solution was then spray-dried using a spray dryer (Yamato Scientific, ADL311S-A) to obtain negative electrode active material composite particles of Comparative Example 4 and Example 10.

[0076] The relationship between the alkyl groups modifying the surfaces of the obtained negative electrode active material composite particles, the type of binder resin, and the amount of binder resin is as shown in Table 2.

[0077] Making a Battery Preparation of Positive Electrode Mixture A polypropylene (PP) container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi as a positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (average particle size: 6 μm), Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and vapor-grown carbon fiber (VGCF) as a conductive additive were added to the container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) and stirred for 30 seconds with an ultrasonic disperser. It was further shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).

[0078] <Formation of Positive Electrode Active Material Layer> The obtained slurry was applied to an aluminum (Al) foil (manufactured by Showa Denko) as a positive electrode current collector layer by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. As a result, a positive electrode active material layer was formed on the positive electrode current collector layer.

[0079] <Preparation of negative electrode mixture> Dibutyl ether, mesitylene, 5wt% mesitylene solution of SBR binder, VGCF as conductive assistant, Li2S-P2S5 glass ceramic as solid electrolyte, and each example of negative electrode active material composite particles were added to a polypropylene (PP) container, and stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Furthermore, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry).

[0080] <Formation of negative electrode active material layer> The obtained slurry was applied onto a nickel (Ni) foil as a negative electrode current collector by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. This formed a negative electrode active material layer on the negative electrode current collector layer.

[0081] <Formation of solid electrolyte layer> Heptane, a 5 wt% heptane solution of an SBR binder, and Li2S-P2S5 glass ceramic as a solid electrolyte were added to a polypropylene (PP) container and stirred for 30 seconds with an ultrasonic dispersing device (UH-50, manufactured by SMT). The container was then shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry. The obtained slurry was applied to an Al foil by a blade method using an applicator. The applied slurry was dried on a hot plate at 100°C for 30 minutes. This formed a solid electrolyte layer. Three solid electrolyte layers were produced.

[0082] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. in the first pressing step to obtain a positive electrode laminate.

[0083] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. in the second pressing step to obtain a negative electrode laminate.

[0084] The negative electrode laminate and the positive electrode laminate were fabricated so that the area of ​​the negative electrode laminate was larger than the area of ​​the positive electrode laminate.

[0085] Further, an Al foil as a release sheet, an intermediate solid electrolyte layer formed on the Al foil, and the negative electrode laminate were laminated so that the solid electrolyte layers were in contact with each other. The laminate was set in a flat uniaxial press and temporarily pressed for 10 seconds at a pressure of 100 MPa and a temperature of 25° C. The Al foil was peeled off from the intermediate solid electrolyte layer of the laminate to obtain a negative electrode laminate further laminated with an intermediate solid electrolyte layer.

[0086] The positive electrode laminate and the negative electrode laminate further having an intermediate solid electrolyte layer laminated thereon were laminated so that the solid electrolyte layers were in contact with each other. This laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a temperature of 120°C in the third pressing step. This produced an all-solid-state battery.

[0087] "evaluation" Analysis of the surface properties of silicon particles The amount of carbon on the surface of silicon particles in the synthesis example and the comparative synthesis example was measured by high-frequency combustion infrared absorption method (apparatus used: LECO, CSLS600). Also, the amount of hydrogen in silicon particles in each example was measured by inert gas fusion infrared absorption method (apparatus used: LECO, TCH600).

[0088] Furthermore, the silicon particles of each example were subjected to surface analysis by time-of-flight secondary ion mass spectrometry (TOF-SIMS) (apparatus used: ION-TOF, TOF.SIMS5, primary ion source: bismuth (Bi)).

[0089] <Measurement of particle size distribution of negative electrode active material composite particles> The negative electrode active material composite particles of each example were dispersed in water and measured with a particle size distribution meter.

[0090] <Battery capacity retention rate> The fabricated battery was restrained at a predetermined restraining pressure using a restraining jig, charged at a constant current and constant voltage at 1 / 10C to 4.55V, and then discharged at 1C to 3.0V. The battery was then charged at a constant current and constant voltage at 1 / 3C to 4.35V, and discharged at a constant current and constant voltage at 1 / 3C to 3.00V to determine the initial capacity, and then the charge and discharge test was repeated 100 times at 1C. The capacity retention rate was calculated by subtracting the initial capacity from the capacity after the charge and discharge test was repeated 100 times.

[0091] "result" Analysis of the surface properties of silicon particles Table 1 shows the results of the quantitative analysis of the carbon and hydrogen amounts on the surfaces of the silicon particles of the Comparative Synthesis Example and the Synthesis Example, as well as the results of the TOF-SIMS analysis.

[0092] [Table 1]

[0093] As shown in Table 1, the silicon particles of the synthesis example, whose surfaces were modified with alkyl groups, had a higher carbon content on the particle surface compared to the silicon particles of the comparative synthesis example. Also, the m / z value was larger as the alkyl group had more carbon atoms. From these findings, it is believed that the surfaces of the silicon particles were successfully modified with alkyl groups.

[0094] <Measurement of particle size distribution of negative electrode active material composite particles> Table 2 shows the results of particle size distribution measurement of the negative electrode active material composite particles.

[0095] <Battery capacity retention rate> Table 2 shows the calculation results of the battery capacity retention rate.

[0096] In Table 2, "resin" means binder resin, and "Si" means surface-modified silicon particles in the examples and non-surface-modified silicon particles in the comparative examples.

[0097] [Table 2]

[0098] As shown in Table 2, the particles of the examples, including silicon particles whose surfaces are modified with alkyl groups, had a (D90-D10) / D50 value of 2.0 or less. From this, it is considered that the particles of the examples were prepared as composite particles. In contrast, the particles of Comparative Examples 1 and 2 had a large (D90-D10) / D50, and therefore were not appropriately prepared as composite particles.

[0099] The batteries containing the particles of Examples 1 to 3 and 4 to 6 had a higher capacity retention rate, i.e., better cycle characteristics, than the corresponding batteries of Comparative Examples 1 and 2. As described above, this is believed to be because in these Examples, the composite particles were appropriately prepared even though the amount of binder resin was small. In particular, the high capacity retention rate of the batteries of Examples 1 to 3 is believed to be due to the fact that the resistance of the battery was suppressed due to the small amount of binder resin.

[0100] In addition, the batteries containing the particles of Examples 7 to 9 also had a higher capacity retention rate than the corresponding battery of Comparative Example 3. Thus, even when the amount of binder resin was relatively large and it was estimated that the particles of the Examples and Comparative Examples were both prepared as composite particles, a difference occurred in the capacity retention rate. This is thought to be because, in the composite particles of the Examples, the surface modification of the alkyl groups suppresses the aggregation of the silicon particles in the composite particles, and appropriate voids are formed between the silicon particles, so that the volume change when the silicon particles expand during charging and discharging can be alleviated by these voids, and cracking of the composite particles is suppressed.

[0101] Furthermore, the battery of Example 10, in which the type of binder resin was changed, also had a larger capacity retention rate than the corresponding battery of Comparative Example 4.

Claims

1. The negative electrode active material includes surface-modified negative electrode active material particles and a binder resin, the surface-modified negative electrode active material particles have silicon particles and organic groups modifying the surfaces of the silicon particles; and a ratio of the mass of the binder resin to the total mass of the surface-modified negative electrode active material particles and the binder resin is 15 mass% or less; Negative active material composite particles.

2. The negative electrode active material composite particle according to claim 1 , wherein the organic group is an alkyl group.

3. The negative electrode active material composite particle according to claim 2 , wherein the alkyl group has 5 or more and 20 or less carbon atoms.

4. 3. The negative electrode active material composite particle according to claim 2, wherein the surface-modified negative electrode active material particle has a silicon-carbon bond, the silicon being the silicon of the silicon particle, and the carbon being the carbon of an alkyl group.

5. A negative electrode mixture comprising the negative electrode active material composite particles according to any one of claims 1 to 4.

6. A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to claim 5. Lithium-ion battery.

7. (a) modifying the surfaces of silicon particles with organic groups to obtain surface-modified negative electrode active material particles; (b) forming droplets from a slurry containing the surface-modified negative electrode active material particles, a binder resin, and a solvent to obtain slurry droplets; and (c) flash drying the slurry droplets in a heated gas; The method for producing negative electrode active material composite particles comprising the steps of:

8. The method according to claim 7, wherein in step (a), the surface of the silicon particle is modified with the organic group by a hydrosilylation reaction in which the organic group is added to a hydrosilyl group on the surface of the silicon particle.

Citation Information

Patent Citations

  • Organic matter / silicon composite material, battery negative electrode prepared from organic matter / silicon composite material and preparation method

    CN112382763A

  • Negativee active material for lithium secondary battery, manufacturing method therefor, and lithium secondary battery containing the material

    JP2008130570A

  • Negative electrode material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2013069531A

  • Negative electrode active material for lithium ion secondary batteries, negative electrode for lithium ion secondary batteries, and lithium ion secondary battery

    JP2015111514A

  • Stabilized electrodes for ion batteries and methods of making the same

    US20200223704A1