All-solid battery

By interposing a carbon sheet between metal leads and electrodes in all-solid-state batteries, the reliability issues caused by vibrations are mitigated, ensuring consistent battery performance.

JP2024165119APending Publication Date: 2024-11-28MAXELL LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023081000
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face reliability issues due to positional deviation and damage of metal leads during vibrations, leading to potential damage of electrodes and impaired battery characteristics.

Method used

Incorporating a carbon sheet between the metal leads and electrodes to prevent direct contact, allowing for flexible connection and reducing electrode damage during vibrations.

Benefits of technology

The carbon sheet interposition enhances the reliability of all-solid-state batteries by preventing electrode damage and maintaining consistent performance under vibrational stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165119000001_ABST
    Figure 2024165119000001_ABST
Patent Text Reader

Abstract

To provide an all-solid battery excellent in reliability.SOLUTION: An all-solid battery according to the present invention includes a plurality of unit cells that are constituted by stacking a positive electrode, a solid electrolyte layer and a negative electrode. Each of the unit cells is sequentially stacked in a thickness direction, and stored within the container. Either of the electrodes, possessed by the unit cell, has a metal lead which can derive electric power from the electrode and which is not fixed to the electrode, and a carbon sheet that is interposed between the electrode and the metal lead. The electrode and the metal lead are conductively connected together via the carbon sheet.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an all-solid-state battery with excellent reliability. [Background technology]

[0002] In recent years, with the development of portable electronic devices such as mobile phones and notebook personal computers, and the practical application of electric vehicles, there has been a demand for small, lightweight batteries with high capacity and high energy density.

[0003] Currently, lithium batteries that can meet this requirement, especially lithium-ion batteries, use lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 In these batteries, a lithium-containing composite oxide such as Graphite is used as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt is used as the non-aqueous electrolyte.

[0004] Furthermore, with the further development of devices in which lithium-ion batteries are used, there is a demand for lithium-ion batteries with longer life, higher capacity and higher energy density, as well as a high demand for the reliability of these longer life, higher capacity and higher energy density lithium-ion batteries.

[0005] However, the organic electrolyte used in lithium-ion batteries contains an organic solvent, which is a flammable substance, and therefore the organic electrolyte may generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium-ion batteries and an increasing amount of organic solvent in the organic electrolyte, there is a demand for even higher reliability in lithium-ion batteries.

[0006] In the above circumstances, all-solid-state lithium batteries that do not use organic solvents are also being considered. All-solid-state lithium batteries use a molded body of a solid electrolyte that does not use an organic solvent instead of the conventional organic solvent-based electrolyte, and are highly reliable without the risk of abnormal heat generation of the solid electrolyte. Therefore, there are high expectations for them, especially in the product field that requires a high-capacity secondary battery.

[0007] In addition, all-solid-state batteries are not only highly safe, but also highly reliable, highly environmentally resistant, and have a long lifespan, so they are expected to be maintenance-free batteries that can contribute to social development while also continuing to contribute to safety and security. By providing all-solid-state batteries to society, we can contribute to the achievement of Goal 3 (Ensure healthy lives and promote well-being for all at all ages), Goal 7 (Ensure access to affordable, reliable, sustainable and modern energy for all), Goal 11 (Make cities and human settlements inclusive, safe, resilient and sustainable), and Goal 12 (Ensure sustainable consumption and production patterns) out of the 17 Sustainable Development Goals (SDGs) established by the United Nations.

[0008] In an all-solid-state battery, for example, in order to increase capacity, a plurality of unit cells each composed of a positive electrode, a solid electrolyte layer, and a negative electrode may be used in one battery. In such an all-solid-state battery, it has been proposed to electrically connect the unit cells with each other by using a conductive internal current collecting layer or a carbon sheet (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2012 / 020699 [Patent Document 2] Patent Publication No. 2021-2457 Summary of the Invention [Problem to be solved by the invention]

[0010] Incidentally, when a battery is constructed by stacking a plurality of unit cells in the thickness direction and connecting the unit cells in series or parallel, a metal lead may be used to draw power from the electrode of the unit cell. In this case, if the lead is fixed to the surface of the electrode by welding or the like, the lead and the electrode will not be displaced due to vibrations received by the battery. However, if the lead is not fixed and is only in contact with the electrode and is electrically connected, the lead may be displaced when strong vibrations are applied, causing damage to the electrode. On the other hand, even if the lead is fixed to the surface of the electrode, if the battery is subjected to strong vibrations, the unit cell having the electrode to which the lead is fixed may rub against the unit cell adjacent to it, causing the lead to damage the electrode of the adjacent unit cell.

[0011] If the electrodes are damaged by the above-mentioned phenomena, there is a risk that the characteristics of the battery will be impaired. Therefore, in a battery having multiple unit cells, it is necessary to suppress the occurrence of such electrode damage and increase reliability.

[0012] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an all-solid-state battery with excellent reliability. [Means for solving the problem]

[0013] A first aspect of the all-solid-state battery of the present invention has a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, and each unit cell is stacked in order in the thickness direction and housed in a container, and at least one of the unit cells has at least one electrode which is electrically connected to the electrode and capable of drawing out electric power from the electrode and has a metal lead which is not fixed to the electrode, a carbon sheet is provided between the electrode and the metal lead, and the electrode and the metal lead are electrically connected via the carbon sheet.

[0014] A second aspect of the all-solid-state battery of the present invention is characterized in that it has a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, and each unit cell is stacked in order in the thickness direction and housed in a container, and at least one pair of electrodes of the same polarity is included among the two electrodes facing each other in adjacent unit cells, and at least one of the pair of electrodes is electrically connected to the two facing electrodes, is capable of drawing out electric power from the two electrodes, and has a metal lead fixed to one of the electrodes, and has a carbon sheet between the other of the two electrodes and the metal lead, and the other electrode and the metal lead are electrically connected via the carbon sheet. Effect of the Invention

[0015] According to the present invention, it is possible to provide an all-solid-state battery with excellent reliability. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a first embodiment of an all-solid-state battery of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of another example of the first embodiment of the all-solid-state battery of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view illustrating a schematic example of a second embodiment of the all-solid-state battery of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A first aspect of the all-solid-state battery of the present invention has a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, and each unit cell is stacked in order in the thickness direction and housed in a container, and in at least one unit cell, at least one electrode has a metal lead that is electrically connected to the electrode and capable of drawing out electric power from the electrode and is not fixed to the electrode, a carbon sheet is provided between the electrode and the metal lead, and the electrode and the metal lead are electrically connected via the carbon sheet.

[0018] Fig. 1 shows a cross-sectional view that shows a schematic example of a first embodiment of an all-solid-state battery. The all-solid-state battery 10 shown in Fig. 1 has four unit cells 20 stacked in the thickness direction (vertical direction in the figure) and connected in parallel, which are housed in a container (exterior body) having a cylindrical bottomed metal exterior can 80 and a metal lid 90. The exterior can and the lid can be made of aluminum, stainless steel, or the like.

[0019] A metal terminal 100 is attached to the lid body 90 via an insulating packing 110 made of resin (such as polypropylene), and a metal (such as stainless steel) lead plate 130 is attached to the terminal 100. A resin (such as polypropylene) insulator 120 is attached to the terminal 100 to prevent the lead plate 130 from contacting the inner surface of the lid plate 90 when the lid body 90 is combined with the outer can 80. The lid body 90 is inserted into the opening of the outer can 80, and the opening of the outer can 80 is sealed by welding the joint between the two, etc., to hermetically seal the inside of the battery. A resin (such as polypropylene or polytetrafluoroethylene) insulator 140 is disposed at the bottom of the outer can 80.

[0020] Each unit cell 20 of the all-solid-state battery 1 is configured by sequentially stacking a positive electrode 30, a solid electrolyte layer 50, and a negative electrode 40.

[0021] In addition, each unit cell 20 is stacked so that electrodes of the same polarity of adjacent unit cells 20 face each other (for example, the unit cell 20 located at the top and the unit cell 20 adjacent thereto below are stacked so that the positive electrodes 30, 30 face each other).

[0022] Furthermore, a metal lead 31 that is not fixed to any of the positive electrodes 30, 30 is disposed between the positive electrode 30 of the unit cell 20 located at the top and the positive electrode 30 of the unit cell 20 adjacent thereto below, for conducting with these positive electrodes 30, 30 to extract power. Carbon sheets 60, 60 are disposed between the positive electrodes 30, 30 and the metal lead 31, and the positive electrodes 30, 30 and the metal lead 31 are electrically connected by these carbon sheets 60, 60.

[0023] Furthermore, a metal lead 32 that is not fixed to any of the positive electrodes 30, 30 is disposed between the positive electrode 30 of the unit cell 20 located at the bottom and the positive electrode 30 of the unit cell 20 adjacent thereto above, for conducting with these positive electrodes 30, 30 to extract power. Carbon sheets 60, 60 are disposed between the positive electrodes 30, 30 and the metal lead 32, and the positive electrodes 30, 30 and the metal lead 32 are electrically connected by these carbon sheets 60, 60.

[0024] Furthermore, metal lead 31 and metal lead 32 are conductively connected to a metallic connection lead 33 by welding or the like, and this connection lead 33 is conductively connected to the inner surface of an outer casing 80 which also serves as a positive electrode terminal by welding or the like.

[0025] Moreover, a metal lead 41 that is not fixed to the negative electrode 40 is disposed above the negative electrode 40 of the unit cell 20 located at the top, in order to conduct electricity with the negative electrode 40 and output power. A carbon sheet 60 is disposed between the negative electrode 40 and the metal lead 41, and the negative electrode 40 and the metal lead 41 are electrically connected by this carbon sheet 60.

[0026] Furthermore, a metal lead 42 that is not fixed to any of the negative electrodes 40, 40 is disposed between the negative electrode 40 of the unit cell 20 positioned second from the top and the negative electrode 40 of the unit cell 20 adjacent thereto below, for conducting electricity with these negative electrodes 40, 40 to draw out electric power. Carbon sheets 60, 60 are disposed between the negative electrodes 40, 40 and the metal lead 42, and the negative electrodes 40, 40 and the metal lead 42 are conductively connected by these carbon sheets 60, 60.

[0027] Further, a metal lead 43 that is not fixed to the negative electrode 40 is disposed below the negative electrode 40 of the unit cell 20 located at the bottom, in order to conduct electricity with the negative electrode 40 and output power. A carbon sheet 60 is disposed between the negative electrode 40 and the metal lead 43, and the negative electrode 40 and the metal lead 43 are electrically connected by this carbon sheet 60.

[0028] Furthermore, metal lead 41, metal lead 42 and metal lead 43 are conductively connected to a metallic connection lead 44 by welding or the like, and this connection lead 44 is conductively connected to a lead plate 130 connected to a terminal 100 that functions as a negative terminal by welding or the like.

[0029] Moreover, a cross-sectional view showing a schematic diagram of another example of the first embodiment of the all-solid-state battery is shown in Fig. 2. The all-solid-state battery 11 shown in Fig. 2 is an example in which four unit cells 20 are stacked in the thickness direction (vertical direction in the figure) and connected in series, and are housed in a container.

[0030] The unit cells 20 are stacked such that the electrodes of opposite polarity of adjacent unit cells 20 face each other. That is, adjacent unit cells 20, 20 are stacked such that the positive electrode 30 of the upper unit cell 20 faces the negative electrode 40 of the lower unit cell 20. A current collector 150 is disposed between adjacent unit cells 20, 20, and the positive electrode 30 of the upper unit cell 20 and the negative electrode 40 of the lower unit cell 20 are conductively connected by this current collector 150.

[0031] A metal lead 41 is disposed above the negative electrode 40 of the unit cell 20 located at the top via a carbon sheet 60 (i.e., the metal lead 41 is not fixed to the negative electrode 40), and the negative electrode 40 and the metal lead 41 are conductively connected via the carbon sheet 60. The metal lead 41 is also conductively connected via a connection lead 44 to a lead plate 130 that is connected to a terminal 100 that functions as a negative electrode terminal.

[0032] Moreover, a metal lead 31 is disposed below the positive electrode 30 of the unit cell 20 located at the bottom via a carbon sheet 60 (i.e., the metal lead 31 is not fixed to the positive electrode 30), and the positive electrode 30 and the metal lead 31 are conductively connected via the carbon sheet 60. Moreover, the metal lead 31 is conductively connected via a connection lead 33 to the inner surface of an exterior can 80 that also serves as a positive electrode terminal.

[0033] In an all-solid-state battery, when a metal lead for deriving power from an electrode of each unit cell is not fixed to any electrode, a carbon sheet is interposed between the metal lead and the electrode adjacent to the metal lead, and the metal lead and the electrode are conductively connected by this carbon sheet, as shown in Figures 1 and 2. By adopting such a configuration, even if the metal lead that is not fixed to the electrode moves due to vibration, etc., the action of the carbon sheet can prevent the electrode from being damaged, resulting in a highly reliable all-solid-state battery.

[0034] A spacer 70 is disposed between the uppermost unit cell 20 and the terminal 100, and each stacked unit cell 20 is pressed toward the bottom of the exterior can 80 by this spacer 70. This allows the metal leads and the electrodes to be well connected via the carbon sheet even when the metal leads are not fixed to the electrodes, resulting in an all-solid-state battery with superior characteristics. The spacer 70 can be a rubber plate or a metal spring (such as a leaf spring).

[0035] A second aspect of the all-solid-state battery of the present invention includes a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, the unit cells being stacked in order in the thickness direction and housed in a container, and adjacent unit cells have at least one pair of electrodes of the same polarity among the two electrodes facing each other, and at least one of the pair of electrodes is electrically connected to the two opposing electrodes, is capable of drawing out electric power from the two electrodes, and has a metal lead fixed to one of the electrodes, and has a carbon sheet between the other of the two electrodes and the metal lead, and the other electrode and the metal lead are electrically connected via the carbon sheet.

[0036] A cross-sectional view showing a schematic example of the second embodiment of the all-solid-state battery is shown in Fig. 3. The all-solid-state battery 12 shown in Fig. 3 is configured such that, like the all-solid-state battery 10 shown in Fig. 1, four unit cells 20 are stacked in the thickness direction (vertical direction in the figure) and connected in parallel, and these are housed in a container (exterior body) having a cylindrical bottomed metal exterior can 80 and a metal lid 90.

[0037] The four unit cells 20 of the all-solid-state battery 12 are stacked such that electrodes of the same polarity of adjacent unit cells 20 face each other, similar to the all-solid-state battery 10 shown in FIG.

[0038] The second unit cell 20 from the top and the bottom unit cell 20 have metal leads 31, 32 fixed to the surfaces of the respective positive electrodes 30, 30, and these metal leads 31, 32 are conductively connected to a metal connection lead 33 by welding or the like. This connection lead 33 is conductively connected to the inner surface of an exterior can 80 that also serves as a positive electrode terminal by welding or the like.

[0039] A carbon sheet 60 is disposed between the positive electrode 30 of the uppermost unit cell 20 and the metal lead 31, and the positive electrode 30 and the metal lead 31 are conductively connected by this carbon sheet 60. Furthermore, a carbon sheet 60 is also disposed between the positive electrode 30 of the third unit cell 20 from the top and the metal lead 32, and the positive electrode 30 and the metal lead 32 are conductively connected by this carbon sheet 60.

[0040] On the other hand, the uppermost unit cell 20 and the third unit cell 20 from the top have metal leads 41, 42 fixed to the surfaces of the respective negative electrodes 40, 40. A carbon sheet 60 is disposed between the negative electrode 40 and the metal lead 42 of the second unit cell 20 from the top, and the negative electrode 40 and the metal lead 42 are conductively connected by this carbon sheet 60. Furthermore, a metal lead 43 is disposed on the underside of the negative electrode 40 of the bottommost unit cell 20 via the carbon sheet 60, and the negative electrode 40 and the metal lead 43 are conductively connected by this carbon sheet 60.

[0041] Metal lead 41, metal lead 42 and metal lead 43 are conductively connected to a metallic connection lead 44 by welding or the like, and this connection lead 44 is conductively connected to a lead plate 130 connected to a terminal 100 that functions as a negative terminal by welding or the like.

[0042] In an all-solid-state battery, when a metal lead for deriving power from an electrode of each unit cell is fixed to one of two opposing electrodes as shown in Fig. 3, the metal lead may rub against the electrode to which the metal lead is not fixed due to the movement of the metal lead caused by vibration of the battery, etc., and the electrode may be damaged. However, by interposing a carbon sheet between the metal lead and the electrode to which the metal lead is not fixed, the electrode can be prevented from being damaged, resulting in a highly reliable all-solid-state battery.

[0043] Next, the configuration and structure common to the first and second aspects of the all-solid-state battery will be described.

[0044] The all-solid-state battery of the present invention includes a primary battery and a secondary battery.

[0045] <Positive electrode> Examples of the positive electrode of the all-solid-state battery include a structure in which a layer (positive electrode mixture layer) made of a molded body of a positive electrode mixture containing a positive electrode active material and a solid electrolyte is formed on a current collector, a structure made of only a molded body of a positive electrode mixture (pellets, etc.), and a structure in which a positive electrode mixture containing a positive electrode active material and a solid electrolyte is filled into the pores of a conductive porous substrate.

[0046] When the all-solid-state battery is a primary battery, the positive electrode active material can be the same as the positive electrode active material used in conventionally known non-aqueous electrolyte primary batteries. Specifically, for example, manganese dioxide, lithium-containing manganese oxide (e.g., LiMn 3 O 6 or a composite oxide having the same crystal structure as manganese dioxide (e.g., β-type, γ-type, or a mixed structure of β-type and γ-type) and a Li content of 3.5 mass% or less, preferably 2 mass% or less, more preferably 1.5 mass% or less, and particularly preferably 1 mass% or less); a Ti 5 / 3 O 4 (4 / 3≦a<7 / 3) and other lithium-containing composite oxides; vanadium oxides; niobium oxides; titanium oxides; sulfides such as iron disulfide; graphite fluoride; Ag 2 Silver sulfides such as S;NiO 2 Such as nickel oxide:

[0047] In addition, when the all-solid-state battery is used as the positive electrode of the secondary battery, the positive electrode active material can be the same as the positive electrode active material used in conventionally known non-aqueous electrolyte secondary batteries. r Mn 2-r O 4(However, M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, and 0 ≦ r ≦ 1) Spinel-type lithium manganese composite oxide, Li r Mn (1-s-r) Ni s M t O (2-u) F v (However, M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, and 0.8 ≦ r ≦ 1.2, 0 < s < 0.5, 0 ≦ t ≦ 0.5, u + v < 1, -0.1 ≦ u ≦ 0.2, 0 ≦ v ≦ 0.1) Layered compound, LiCo 1-r M r O 2 (However, M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5) Lithium cobalt composite oxide, LiNi 1-r M r O 2 (However, M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5) Lithium nickel composite oxide, Li 1+s M 1-r N r PO 4 F s (However, M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0 ≦ r ≦ 0.5, 0 ≦ s ≦ 1) Olivine-type composite oxide, Li 2 M 1-r N r P 2 O 7(wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5), and one or more types of particles of various positive electrode active materials used in conventionally known nonaqueous electrolyte secondary batteries can be mentioned.

[0048] In the case where the all-solid-state battery is a secondary battery, the average particle size of the positive electrode active material is preferably 1 μm or more, more preferably 2 μm or more, and preferably 10 μm or less, more preferably 8 μm or less. The positive electrode active material may be either primary particles or secondary particles formed by agglomeration of primary particles. When a positive electrode active material having an average particle size in the above range is used, a large interface with the solid electrolyte contained in the positive electrode can be obtained, and therefore the output characteristics of the battery are further improved.

[0049] The average particle diameter of various particles (positive electrode active material, solid electrolyte, etc.) in this specification is the 50% diameter value (D) in the volume-based integrated fraction when calculating the integral volume from small particles using a particle size distribution measurement device (such as the Microtrac particle size distribution measurement device "HRA9320" manufactured by Nikkiso Co., Ltd.). 50 )

[0050] When the all-solid-state battery is a secondary battery, the positive electrode active material preferably has a reaction suppression layer on its surface for suppressing reaction with the solid electrolyte contained in the positive electrode.

[0051] In the positive electrode, if the positive electrode active material and the solid electrolyte come into direct contact with each other, the solid electrolyte may oxidize to form a resistance layer, which may reduce the ionic conductivity in the positive electrode. By providing a reaction suppression layer that suppresses the reaction with the solid electrolyte on the surface of the positive electrode active material and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in the ionic conductivity in the positive electrode due to the oxidation of the solid electrolyte.

[0052] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the particles of the electrode active material (positive electrode active material) and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, Zr, Ta, and W, more specifically, LiNbO 3 Nb-containing oxides such as Li 3 PO 4 , Li 3 BO 3 , Li 2 SO 4 , Li 4 SiO 4 , Li 4 GeO 4 , LiTiO 3 , LiZrO 3 , Li 2 WO 4 The reaction suppression layer may contain only one of these oxides, or may contain two or more of these oxides, or may contain a composite compound of two or more of these oxides. Among these oxides, it is preferable to use an Nb-containing oxide, and LiNbO 3 It is more preferable to use

[0053] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 1.0 part by mass per 100 parts by mass of the positive electrode active material, in order to effectively suppress the reaction between the positive electrode active material and the solid electrolyte.

[0054] Methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, the mechanofusion method, the CVD method, the PVD method, and the ALD method.

[0055] The content of the positive electrode active material in the positive electrode mixture is preferably 60 to 85 mass % from the viewpoint of increasing the energy density of the all-solid-state battery.

[0056] The positive electrode mixture may contain a conductive assistant. Specific examples of the conductive assistant include carbon materials such as graphite (natural graphite, artificial graphite), graphene, carbon black, carbon nanofiber, and carbon nanotubes. For example, Ag 2 When S is used, conductive Ag is generated during the discharge reaction, so the conductive additive does not need to be included. When the conductive additive is included in the positive electrode mixture, the content thereof is preferably 1.0 part by mass or more, preferably 7.0 parts by mass or less, and more preferably 6.5 parts by mass or less, when the content of the positive electrode active material is 100 parts by mass.

[0057] The positive electrode mixture may contain a binder. Specific examples of such binders include fluororesins such as polyvinylidene fluoride (PVDF). In addition, the positive electrode mixture may not contain a binder if good moldability can be ensured in forming the positive electrode without using a binder, such as when a sulfide-based solid electrolyte is contained in the positive electrode mixture (described later).

[0058] When the positive electrode mixture requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, when the positive electrode mixture requires no binder and can obtain moldability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0059] The positive electrode mixture may contain a solid electrolyte.

[0060] The solid electrolyte contained in the positive electrode mixture is not particularly limited as long as it has lithium ion conductivity. For example, a sulfide-based solid electrolyte, a hydride-based solid electrolyte, a halide-based solid electrolyte, an oxide-based solid electrolyte, etc. can be used.

[0061] As a sulfide-based solid electrolyte, Li 2 SP2 S 5 , Li 2 S-SiS 2 , Li 2 SP 2 S 5 -GeS 2 , Li 2 S.B. 2 S 3 In addition to particles such as thio-LISICON type particles, which have been attracting attention in recent years for their high Li-ion conductivity, 10 GeP 2 S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 Li 12-12a-b+c+6d-e M 1 3+a-b-c-d M 2 b M 3 c M 4 d M 5 12-e X e (However, M 1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca, Ba, M 5 is either S or S and O, and X is F, Cl, Br or I, 0≦a<3, 0≦b+c+d≦3, 0≦e≦3], or those having an argyrodite type crystal structure can also be used.

[0062] Examples of hydride-based solid electrolytes include LiBH 4 , LiBH 4 and the following alkali metal compounds (e.g., LiBH 4Those having a molar ratio of 1:1 to 20:1 with an alkali metal compound) and the like can be mentioned. Examples of the alkali metal compound in the solid solution include at least one selected from the group consisting of lithium halides (such as LiI, LiBr, LiF, LiCl), rubidium halides (such as RbI, RbBr, RbF, RbCl), cesium halides (such as CsI, CsBr, CsF, CsCl), lithium amide, rubidium amide, and cesium amide.

[0063] Examples of the halide-based solid electrolyte include, for example, monoclinic LiAlCl 4 , defective spinel-type or layered LiInBr 4 , monoclinic Li 6-3m Y m X 6 (where 0 < m < 2 and X = Cl or Br) and the like can be mentioned. In addition, for example, known ones described in International Publication No. 2020 / 070958 and International Publication No. 2020 / 070955 can also be used.

[0064] Examples of the oxide-based solid electrolyte include, for example, Li 2 O - Al 2 O 3 -SiO 2 -P 2 O 5 -TiO 2 -based glass ceramics, Li 2 O - Al 2 O 3 -SiO 2 -P 2 O 5 -GeO 2 -based glass ceramics,, Li 3 PO 4 -Li 3 BO 3 -Li 2 SO 4 -based glass, garnet-type Li 7 La 3 Zr 2 O 12 , NASICON-type Li 1+O Al 1+O Ti 2-O (PO 4 )3 , Li 1+p Al 1+p Ge 2-p (PO 4 ) 3 , perovskite-type Li 3q La 2 / 3-q TiO 3 , the reverse perovskite Li 3 Examples include HX (X=O, S, Se, Te).

[0065] Among these solid electrolytes, sulfide-based solid electrolytes are preferred due to their high lithium ion conductivity, sulfide-based solid electrolytes containing Li and P are more preferred, and sulfide-based solid electrolytes having an argyrodite-type crystal structure are even more preferred due to their higher lithium ion conductivity and high chemical stability.

[0066] As an example of a sulfide-based solid electrolyte having an argyrodite-type crystal structure, Li 6 P.S. 5 Particularly preferred are those represented by the following general composition formula (1) or the following general composition formula (2), such as Cl.

[0067] Li 7-x+y P.S. 6-x Cl x+y (1)

[0068] In the general composition formula (1), 0.05≦y≦0.9 and −3.0x+1.8≦y≦−3.0x+5.7.

[0069] Li 7-a P.S. 6-a Cl b Br c (2)

[0070] In the general composition formula (2), a=b+c, ​​0 <a≦1.8、0.1≦b / c≦10.0である。

[0071] The average particle size of the solid electrolyte is preferably 0.1 μm or more, and more preferably 0.2 μm or more, from the viewpoint of reducing grain boundary resistance, while it is preferably 10 μm or less, and more preferably 5 μm or less, from the viewpoint of forming a sufficient contact interface between the active material and the solid electrolyte.

[0072] The content of the solid electrolyte in the positive electrode mixture is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, when the content of the positive electrode active material is 100 parts by mass, from the viewpoint of further increasing the ion conductivity in the positive electrode and further improving the output characteristics of the all-solid-state battery. However, if the amount of the solid electrolyte in the positive electrode mixture is too large, the amount of other components may be reduced, and the effects of these components may be reduced. Therefore, the content of the solid electrolyte in the positive electrode mixture is preferably 65 parts by mass or less, more preferably 60 parts by mass or less, when the content of the positive electrode active material is 100 parts by mass.

[0073] When a current collector is used for the positive electrode, the current collector can be a metal foil such as aluminum or stainless steel; a sheet-like conductive porous substrate such as punched metal, net, expanded metal, or foamed metal; or a carbon sheet. As the sheet-like conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of the foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd.

[0074] The positive electrode can be produced by a method in which a positive electrode mixture-containing composition (paste, slurry, etc.) obtained by dispersing a positive electrode active material and a solid electrolyte, and optionally added conductive additives, a binder, and the like, in a solvent is applied to a current collector, dried, and then pressure-molded, as required, by calendaring or the like, to form a positive electrode mixture compact (positive electrode mixture layer) on the surface of the current collector.

[0075] As the solvent for the positive electrode mixture-containing composition, organic solvents such as water and N-methyl-2-pyrrolidone (NMP) can be used, but when using a solid electrolyte that is highly reactive to water, it is desirable to select a solvent that does not easily deteriorate the solid electrolyte. In particular, since sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions with a small amount of water, it is preferable to use non-polar aprotic solvents such as hydrocarbon solvents such as hexane, heptane, octane, nonane, decane, decalin, toluene, and xylene. In particular, it is more preferable to use an ultra-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less. In addition, fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by Mitsui DuPont Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Nippon Zeon Co., Ltd., and "Novec (registered trademark)" manufactured by Sumitomo 3M Co., Ltd., as well as non-aqueous organic solvents such as dichloromethane and diethyl ether can also be used.

[0076] In addition to the above-mentioned method, the molded body of the positive electrode mixture may be formed by compressing a positive electrode mixture prepared by mixing a conductive assistant, a binder, etc., which are added as necessary, with a positive electrode active material and a solid electrolyte, by pressure molding, etc. As described above, the molded body of the positive electrode mixture obtained by such a method can be used as a positive electrode as it is, or it can be used as a positive electrode by bonding it to a current collector by pressing it, etc.

[0077] The thickness of the positive electrode mixture compact (positive electrode mixture layer) formed using the solvent-containing positive electrode mixture-containing composition (thickness per one side of the current collector when a current collector is included) is preferably 10 to 1000 μm. Also, the thickness of the positive electrode mixture compact obtained by pressure molding is preferably 0.15 to 4 mm.

[0078] The thickness of the positive electrode current collector is preferably 0.01 to 0.1 mm.

[0079] In addition, when a conductive porous substrate is used for the positive electrode current collector, the positive electrode can be produced, for example, by filling the pores of the conductive porous substrate with the positive electrode mixture-containing composition, drying the composition, and then subjecting the resulting mixture to pressure molding, such as calendaring, as necessary.

[0080] Furthermore, instead of the above-mentioned positive electrode mixture-containing composition, a positive electrode mixture that contains a positive electrode active material, a solid electrolyte, and further a conductive assistant and a binder, and does not contain a solvent, may be dry-filled into the pores of a conductive porous substrate, and the positive electrode may be produced by a method in which pressure molding, such as calendaring, is performed as necessary.

[0081] In the case of a positive electrode obtained by filling the pores of a conductive porous substrate with a positive electrode mixture-containing composition or a positive electrode mixture, the thickness is preferably 30 to 4000 μm.

[0082] <Negative electrode> The negative electrode of the all-solid-state battery has, for example, a molded body of a negative electrode mixture containing a negative electrode active material, a lithium sheet, or a lithium alloy sheet. Also, a conductive porous substrate having a negative electrode mixture containing a negative electrode active material filled in its pores can be used as the negative electrode.

[0083] When the negative electrode is a molded body of a negative electrode mixture containing a negative electrode active material, examples of the negative electrode include a structure in which a layer (negative electrode mixture layer) made of a molded body of the negative electrode mixture is formed on a current collector, and a structure consisting only of a molded body (pellet, etc.) made by molding the negative electrode mixture.

[0084] Examples of the negative electrode active material include carbon materials such as graphite, lithium titanium oxides (lithium titanate, etc.), simple substances containing elements such as Si and Sn, compounds (oxides, etc.), and alloys thereof, etc. In addition, lithium metal and lithium alloys (lithium-aluminum alloys, lithium-indium alloys, etc.) can also be used as the negative electrode active material.

[0085] The content of the negative electrode active material in the negative electrode mixture is preferably 40 to 80 mass % from the viewpoint of increasing the energy density of the battery.

[0086] The negative electrode mixture may contain a conductive assistant. Specific examples thereof include the same conductive assistants as those exemplified above as those that may be contained in the positive electrode mixture. The content of the conductive assistant in the negative electrode mixture is preferably 10 to 30 parts by mass when the content of the negative electrode active material is 100 parts by mass.

[0087] The negative electrode mixture may contain a binder. Specific examples thereof include the same binders as those exemplified above as those that may be contained in the positive electrode mixture. For example, when a sulfide-based solid electrolyte is contained in the negative electrode mixture (described later), in cases where good moldability can be ensured in forming the negative electrode mixture layer without using a binder, the negative electrode may be used. The mixture may not contain a binder.

[0088] In the case where the negative electrode mixture requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, in the case where the negative electrode mixture requires no binder and can obtain moldability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0089] The negative electrode mixture can contain a solid electrolyte. Specific examples thereof include the same solid electrolytes as those exemplified above as those that can be contained in the positive electrode mixture. Among the above-mentioned solid electrolytes, it is preferable to use a sulfide-based solid electrolyte because it has high lithium ion conductivity and also has a function of increasing the moldability of the negative electrode mixture, and it is more preferable to use a sulfide-based solid electrolyte having an argyrodite-type crystal structure, and it is even more preferable to use one represented by the general composition formula (1) or the general composition formula (2).

[0090] For the same reasons as in the case of the positive electrode mixture, the average particle size of the solid electrolyte in the negative electrode mixture is preferably 0.1 μm or more, and more preferably 0.2 μm or more, and is preferably 10 μm or less, and more preferably 5 μm or less.

[0091] The content of the solid electrolyte in the negative electrode mixture is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, when the content of the negative electrode active material is 100 parts by mass, from the viewpoint of further increasing the ion conductivity in the negative electrode and further improving the output characteristics of the all-solid-state battery. However, if the amount of the solid electrolyte in the negative electrode mixture is too large, the amount of other components may be reduced, and the effects of these components may be reduced. Therefore, the content of the solid electrolyte in the negative electrode mixture is preferably 130 parts by mass or less, more preferably 110 parts by mass or less, when the content of the negative electrode active material is 100 parts by mass.

[0092] When a current collector is used for the negative electrode having a molded body of the negative electrode mixture, the current collector can be a sheet-like conductive porous substrate such as copper or nickel foil, punched metal, net, expanded metal, or foamed metal; a carbon sheet; or the like. As the sheet-like conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of the foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd.

[0093] The negative electrode can be produced by a method in which a negative electrode mixture-containing composition (paste, slurry, etc.) in which a negative electrode active material, and further, if necessary, a conductive assistant, a solid electrolyte, a binder, etc. are dispersed in a solvent is applied to a current collector, dried, and then, if necessary, pressure-molded by calendaring or the like to form a molded body of the negative electrode mixture (negative electrode mixture layer) on the surface of the current collector.

[0094] As the solvent for the negative electrode mixture-containing composition, an organic solvent such as water or NMP can be used. However, when the negative electrode mixture-containing composition also contains a solid electrolyte, it is preferable to select a solvent that does not deteriorate the solid electrolyte, and it is preferable to use the same solvent as the various solvents exemplified above for the positive electrode mixture-containing composition.

[0095] In addition to the above-mentioned method, the negative electrode mixture compact may be formed by compressing a negative electrode mixture prepared by mixing the negative electrode active material, and further the conductive assistant, solid electrolyte, and binder, which are added as necessary, by pressure molding, etc. As described above, the negative electrode mixture compact obtained by such a method can be used as a negative electrode as it is, or it can be used as a negative electrode by bonding a current collector by pressing it.

[0096] The thickness of the negative electrode mixture compact (negative electrode mixture layer) formed using the solvent-containing negative electrode mixture-containing composition (thickness per one side of the current collector when a current collector is included) is preferably 10 to 1000 μm. Also, the thickness of the negative electrode mixture compact obtained by pressure molding is preferably 0.15 to 4 mm.

[0097] The thickness of the negative electrode current collector is preferably 0.01 to 0.1 mm.

[0098] In addition, when a conductive porous substrate such as a punched metal is used as the negative electrode current collector, the negative electrode can be manufactured, for example, by filling the pores of the conductive porous substrate with the negative electrode mixture-containing composition, drying the composition, and then, if necessary, performing pressure molding such as calendaring. A negative electrode manufactured by such a method can ensure high strength, and therefore can hold a solid electrolyte sheet having a larger area.

[0099] Furthermore, instead of the above-mentioned negative electrode mixture-containing composition, a negative electrode mixture that contains a negative electrode active material, a solid electrolyte, a binder, a conductive assistant, and the like, but does not contain a solvent, may be dry-filled into the pores of a conductive porous substrate, and the negative electrode may be produced by a method in which pressure molding, such as calendaring, is performed as necessary.

[0100] In the case of a negative electrode obtained by filling the pores of a conductive porous substrate with a negative electrode mixture-containing composition or a negative electrode mixture, the thickness is preferably 30 to 4000 μm.

[0101] In the case of a negative electrode having a lithium sheet or a lithium alloy sheet, one consisting of only this sheet or one consisting of this sheet laminated with a current collector is used.

[0102] Examples of alloying elements for the lithium alloy include aluminum, lead, bismuth, indium, and gallium, with aluminum and indium being preferred. The ratio of the alloying elements in the lithium alloy (when multiple alloying elements are included, the total ratio of the alloying elements) is preferably 50 atomic % or less (in this case, the balance is lithium and inevitable impurities).

[0103] In the case of a negative electrode having a lithium alloy sheet, a laminate is used in which a layer containing an alloying element for forming a lithium alloy is laminated on the surface of a lithium layer (a layer containing lithium) composed of a metallic lithium foil or the like by pressure bonding, and the laminate is brought into contact with a solid electrolyte in a battery to form a lithium alloy on the surface of the lithium layer to form a negative electrode. In the case of such a negative electrode, a laminate having a layer containing an alloying element on only one side of the lithium layer may be used, or a laminate having layers containing an alloying element on both sides of the lithium layer may be used. The laminate can be formed, for example, by pressure bonding a metallic lithium foil and a foil composed of an alloying element.

[0104] The current collector can also be used when a lithium alloy is formed in a battery to form a negative electrode, and for example, a laminate having a lithium layer on one side of the negative electrode current collector and a layer containing an alloying element on the side of the lithium layer opposite the negative electrode current collector may be used, or a laminate having lithium layers on both sides of the negative electrode current collector and each lithium layer having a layer containing an alloying element on the side opposite the negative electrode current collector may be used. The negative electrode current collector and the lithium layer (metallic lithium foil) may be laminated by compression bonding or the like.

[0105] The layer containing the alloying elements in the laminate to be used as the negative electrode may be, for example, a foil composed of these alloying elements. The thickness of the layer containing the alloying elements is preferably 1 μm or more, more preferably 3 μm or more, and is preferably 20 μm or less, more preferably 12 μm or less.

[0106] The lithium layer of the laminate for use as the negative electrode may be, for example, a metallic lithium foil. The thickness of the lithium layer is preferably 0.1 to 1.5 mm. The thickness of the sheet of lithium or lithium alloy for the negative electrode is also preferably 0.1 to 1.5 mm.

[0107] When a negative electrode having a lithium sheet or a lithium alloy sheet has a current collector, the current collector can be the same as the current collector exemplified above as one that can be used for a negative electrode having a molded body of a negative electrode mixture.

[0108] <Solid electrolyte layer> The solid electrolyte layer may be one or more of the sulfide-based solid electrolyte, hydride-based solid electrolyte, and oxide-based solid electrolyte exemplified above as the solid electrolyte that may be contained in the positive electrode mixture. Among the above-exemplified solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte, and it is even more preferable to use an argyrodite-type sulfide-based solid electrolyte, in order to improve the battery characteristics.

[0109] The solid electrolyte layer can be formed by a method of compressing a solid electrolyte by pressure molding or the like; a method of applying a composition for forming a solid electrolyte layer, which is prepared by dispersing a solid electrolyte in a solvent, onto a substrate, a positive electrode, or a negative electrode, drying the composition, and, if necessary, performing pressure molding such as pressing.

[0110] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.

[0111] It is desirable to select a solvent for use in the composition for forming a solid electrolyte layer that is unlikely to deteriorate the solid electrolyte, similar to the solvent for use in the positive electrode mixture-containing composition. It is preferable to use the various solvents exemplified above as the solvent for the positive electrode mixture-containing composition, and it is particularly preferable to use an ultra-dehydrated solvent with a water content of 0.001 mass % (10 ppm) or less.

[0112] The thickness of the solid electrolyte layer is preferably 10 to 500 μm.

[0113] <Carbon sheet> As the carbon sheet, for example, a porous carbon sheet made of fibrous carbon such as carbon paper, carbon cloth, or carbon felt can be preferably used. These sheets may have a single layer structure, a multilayer structure in which carbon papers, carbon cloths, or carbon felts are laminated, or a multilayer structure in which two or more of carbon paper, carbon cloth, and carbon felt are laminated. Also, a porous sheet made of expanded graphite can be used as the carbon sheet.

[0114] Taking into consideration electrical conductivity and the like, the fiber diameter of the fibrous carbon constituting the sheet is preferably 2 to 30 μm.

[0115] The thickness of the carbon sheet is preferably 0.5 mm or less from the viewpoint of increasing the energy density of the battery, and the lower limit of the thickness of the porous carbon sheet is usually 0.05 mm, taking into consideration the ease of handling, availability, and ensuring the current collecting function.

[0116] When the carbon sheet is porous, the porosity is preferably 50% or more and 95% or less.

[0117] The carbon sheet to be used may be selected from commercially available products that satisfy the above physical property values.

[0118] <Unit cell> The unit cell can be constructed by stacking a positive electrode and a negative electrode with a solid electrolyte layer interposed therebetween. When forming a unit cell including a positive electrode having a compact of a positive electrode mixture and a negative electrode having a compact of a negative electrode mixture, it is preferable to pressure-mold the positive electrode, the negative electrode, and the solid electrolyte layer in a stacked state from the viewpoint of increasing the mechanical strength of the unit cell.

[0119] The shape of the unit cell in a plan view is not particularly limited, and examples of the shape include a circle and a polygon such as a square.

[0120] The number of unit cells to be stacked in an all-solid-state battery is not particularly limited as long as it is a plurality (two or more), and can be appropriately set according to the characteristics and productivity required of the battery.

[0121] <Metal leads, connecting leads and current collectors> Metal leads for extracting power from the electrodes of the unit cells, connection leads for connecting the metal leads together, and current collectors placed between the unit cells to electrically connect them can be made of metal foils (plates) such as stainless steel, nickel, aluminum, iron, copper, clad materials combining these, or materials plated with nickel, chromium, nickel chromium, etc.

[0122] The thickness of the metal lead or connection lead made of a metal foil (plate) and the current collector is preferably 10 to 100 μm.

[0123] When a metal lead is fixed to an electrode of a unit cell, an electrode having a metal current collector is used, and the current collector and the metal lead may be joined by welding or the like.

[0124] In addition, for the current collector interposed between the unit cells for conductive connection between them, the same carbon sheet as exemplified above can be used as the current collector interposed between the metal lead and the electrode of the unit cell.

[0125] <Container> There is also no particular limitation on the container (exterior body) of the all-solid-state battery, and various containers that have been conventionally used in various batteries can be used, such as cylindrical or rectangular metal containers, flat containers having an exterior can and a sealed can that are used in batteries called coin batteries or button batteries, sheet-like containers made of a resin film such as a metal laminate film, and box-shaped ceramic containers.

[0126] The all-solid-state battery of the present invention can be used for applications similar to those of conventionally known primary batteries and secondary batteries. However, since the all-solid-state battery of the present invention has a solid electrolyte instead of an organic electrolyte solution, it has excellent heat resistance and can be preferably used for applications in which the battery is exposed to high temperatures. EXAMPLES

[0127] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.

[0128] Example 1 Lithium titanate (Li 4 Ti 5 O 12 , negative electrode active material) and a sulfide-based solid electrolyte with an average particle size of 0.7 μm (Li 6 P.S. 5 Cl) and graphene (conductive assistant) were mixed in a mass ratio of 50:41:9 to prepare a negative electrode mixture.

[0129] In addition, LiNbO 3 The LiCoO with an average particle size of 5 μm is coated with the 2 (positive electrode active material) and a sulfide-based solid electrolyte (Li 6 P.S. 5 Cl) and graphene in a mass ratio of 65:30.7:4.3 to prepare a positive electrode mixture.

[0130] Next, we used a sulfide-based solid electrolyte (Li 6 P.S. 5A powder of 1,2-dichlorophenyl chloride (Cl) was placed in a powder molding die and pressure-molded at a surface pressure of 70 MPa using a press to form a provisionally molded layer of a solid electrolyte layer. Furthermore, the negative electrode mixture was placed on the upper surface of the provisionally molded layer of the solid electrolyte layer and pressure-molded at a surface pressure of 50 MPa to form a provisionally molded layer of the negative electrode mixture on the provisionally molded layer of the solid electrolyte layer.

[0131] Next, a nickel-made porous metal foam (nickel "Celmet" (registered trademark)) made by Sumitomo Electrochemical Industries, Ltd., cut to a diameter of 7.25 mm (thickness: 1.2 mm, porosity: 98%) was placed on the provisionally molded layer of the negative electrode mixture formed on the provisionally molded layer of the solid electrolyte layer, and pressure molding was performed at a surface pressure of 300 MPa to form an integrated body of the solid electrolyte layer and the negative electrode. The negative electrode is constituted by integrating the negative electrode mixture layer and the porous metal body.

[0132] Furthermore, after the mold was turned upside down, the positive electrode mixture was placed on the upper surface of the solid electrolyte layer in the mold (the surface opposite to the surface having the negative electrode), and pressure molding was performed with a surface pressure of 50 MPa, thereby forming a provisionally molded layer of the positive electrode mixture on the solid electrolyte layer.

[0133] Next, a cut piece of the same nickel foamed metal porous body used for the negative electrode was placed on the provisionally molded layer of the positive electrode mixture formed on the solid electrolyte layer, and pressure molding was performed at a surface pressure of 1400 MPa to obtain a unit cell consisting of a molded body in which the negative electrode, the solid electrolyte layer, and the positive electrode were laminated. The positive electrode is configured by integrating the positive electrode mixture layer and the metal porous body.

[0134] Four of the unit cells were stacked together and used as a carbon sheet, a flexible graphite sheet called "PERMA-FOIL (product name)" (thickness: 0.1 mm, apparent density: 1.1 g / cm) manufactured by Toyo Tanso Co., Ltd. 3 ) was punched out to the same size as the molded body, and nickel metal pieces were used as the metal leads and connecting leads for the positive and negative electrodes to assemble the all-solid-state battery shown in Fig. 1. Although not shown, a resin film was interposed between the metal leads and connecting leads and the unit cell for insulation.

[0135] Example 2 The all-solid-state battery shown in Fig. 3 was assembled in the same manner as in Example 1, except that each metal lead was welded to the metal porous body of the electrode, and the same flexible graphite sheet as used in Example 1 was placed between the metal leads, except for the metal leads at both the top and bottom ends, and the opposing electrodes. Although not shown, a resin film was interposed between the metal leads and the connection leads and the unit cell for insulation.

[0136] Comparative Example 1 An all-solid-state battery was assembled in the same manner as in Example 1, except that no flexible graphite sheet was placed between each metal lead and electrode, and the metal leads were in direct contact with the electrodes.

[0137] Comparative Example 2 An all-solid-state battery was assembled in the same manner as in Example 2, except that no flexible graphite sheet was placed between each metal lead and the electrode, and the welded metal lead was in direct contact with the opposing electrode.

[0138] A vibration test was carried out under the following conditions for the all-solid-state batteries of the Examples and Comparative Examples to examine whether or not there was any deterioration in characteristics due to damage to the electrodes.

[0139] [Vibration test] A test was conducted on each of the all-solid-state batteries of the examples and comparative examples by applying a sine wave vibration in three directions, length, width, and height, in order. The sine wave was swept in a logarithmic manner, with the frequency varying between 7 Hz and 200 Hz, and reciprocating in 15 minutes, and the sweep was repeated 12 times in each of the three directions.

[0140] Between 7 Hz and 18 Hz, the frequency was swept so that the peak acceleration was maintained at 1 G. From 18 Hz, the frequency was swept up to the frequency (approximately 50 Hz) where the peak acceleration reached 8 G while maintaining the total amplitude at 0.8 mm. Furthermore, the frequency was swept up to 200 Hz so that the peak acceleration was maintained at 1 G.

[0141] The open circuit voltage (OCV) of the battery subjected to the vibration test was measured, and the results are shown in Table 1.

[0142] [Table 1]

[0143] In the all-solid-state batteries of Examples 1 and 2, the OCV showed normal values ​​because damage to the electrodes could be prevented by interposing a carbon sheet between the metal lead and the electrode. However, in Comparative Examples 1 and 2, the metal lead rubbed against the surface of the electrode, causing some of the electrode components to detach, which is believed to have caused a slight short circuit or poor conductivity, and a decrease in the OCV of the batteries was observed. [Explanation of symbols]

[0144] 10, 11, 12 All-solid-state battery 20 unit cells 30 positive electrode 31, 32 Metal lead 33 Connection Lead 40 negative electrode 41, 42, 43 Metal lead 44 Connection Lead 50 Solid electrolyte layer 60 Carbon Sheet 70 Spacer 80 Outer can 90 Lid 100 Terminals 110 Insulating packing 120, 140 Insulator 130 Lead plate 150 Current collector

Claims

1. An all-solid-state battery comprising a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, the unit cells being stacked in order in a thickness direction and housed in a container, In at least one of the unit cells, at least one of the electrodes is provided with a metal lead that is electrically connected to the electrode to allow electrical power to be derived from the electrode and is not fixed to the electrode; 1. An all-solid-state battery comprising: a carbon sheet between the electrode and the metal lead; and the electrode and the metal lead are conductively connected via the carbon sheet.

2. An all-solid-state battery comprising a plurality of unit cells each formed by stacking a positive electrode, a solid electrolyte layer, and a negative electrode, the unit cells being stacked in order in a thickness direction and housed in a container, Among the two electrodes facing each other in adjacent unit cells, at least one pair of electrodes having the same polarity is provided; At least one of the pair of electrodes is electrically connected to the two opposing electrodes, is capable of drawing out electric power from the two electrodes, and includes a metal lead fixed to one of the electrodes; An all-solid-state battery comprising: a carbon sheet between the other of the two electrodes and the metal lead; and the other electrode and the metal lead are conductively connected via the carbon sheet.

Citation Information

Patent Citations

  • Solid electrolyte battery

    JP2021002457A

  • Layered solid-state battery

    WO2012020699A1